Hot rolling facility and hot rolling method
The hot rolling equipment and method address red heat embrittlement cracking by removing Cu-enriched layers during the rolling process, enhancing surface quality and reducing costs, thus enabling more efficient and environmentally friendly steel production with copper-containing iron scrap.
Patent Information
- Application Number
- PCT/JP2024/012448
- Authority / Receiving Office
- WO · WO
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2023-03-29
- Filing Date
- 2024-03-27
- Publication Date
- 2024-10-03
AI Technical Summary
The use of iron scrap as an iron source in steel manufacturing can lead to surface defects due to copper (Cu) enrichment, causing red heat embrittlement cracking, which hinders the adoption of environmentally friendly steel production methods and increases costs with the addition of expensive alloying elements like Ni and REM.
A hot rolling equipment and method that includes a heating furnace, rough rolling, and finish rolling, with a removing device to address Cu-enriched layers by removing the affected surface area during or after rough rolling, using techniques such as melt cutting or mechanical removal, to prevent red embrittlement cracking.
This approach effectively suppresses red embrittlement cracking, improves surface quality, and reduces production costs by eliminating the need for expensive alloy additions, while maintaining productivity and allowing for increased use of copper-containing iron scrap.
Smart Images

Figure JP2024012448_03102024_PF_FP_ABST
Abstract
Description
Hot rolling equipment and hot rolling method
[0001] The present disclosure relates to hot rolling equipment and hot rolling methods.
[0002] Japanese Patent Laid-Open Publication No. 7-242938 describes a method for producing a hot-rolled steel sheet having excellent workability, which comprises, by weight %, C: 0.01 to 0.20%, Si: 2.0% or less, Mn: 0.05 to 2.0%, and Ni: 0 to 0.50%, and further contains, as tramp elements, Cu: 0.01 to 0.50%, Sn: 0.001 to 0.050%, Pb: 0.001 to 0.010%, and As: 0.001 to 0.050%, and the steel is hot-rolled and then coiled at 500°C or less.
[0003] Furthermore, Japanese Patent Laid-Open Publication No. 6-297026 describes a method for preventing hot cracking of steel containing Cu and Sn, which is characterized by adding Si as an alloying component to steel containing Cu and Sn, then heating the steel to form scale, and then rolling the steel.
[0004] Furthermore, Japanese Patent Application Laid-Open No. 2005-29886 describes a Cu-containing steel material characterized in that, in a steel material containing 0.06 mass% or more of Cu, the solute concentration of one or more of Ti, Nb, and V is 0.01 mass% or more and 0.15 mass% or less, and further contains one or more of a P concentration of 0.01 mass% or more and 0.1 mass% or less, a REM concentration of 0.002 mass% or more and 0.15 mass% or less, and a S concentration of 0.01 mass% or more and 0.05 mass% or less.
[0005] In recent years, in order to reduce carbon dioxide emissions in the steel manufacturing process, iron sources other than iron ore have been used. For example, increasing the proportion of scrap iron used as the iron source has been considered.
[0006] However, when scrap iron is used as an iron source, surface defects due to copper (Cu) contained in the scrap iron may occur during the steel production stage. For example, during the hot rolling process, red embrittlement cracking may occur due to the concentration of Cu on the surface of the steel, resulting in a deterioration in the surface quality of the steel. For this reason, it is difficult to increase the proportion of scrap iron containing Cu used as an iron source, making it difficult to realize an environmentally friendly steel production process.
[0007] The techniques described in JP-A-7-242938, JP-A-6-297026, and JP-A-2005-29886 suppress red embrittlement cracking by adding an alloy to the steel material. In JP-A-7-242938, expensive Ni is added to the steel material, which increases costs.
[0008] In addition, in the technology described in JP-A-6-297026, Si is added to the steel material, which leads to a decrease in the workability of the steel material. Therefore, the technology described in JP-A-6-297026 limits the range of use of the steel material, making it difficult to use the steel material as outer plates, in particular. Furthermore, in the technology described in JP-A-6-297026, the steel material is processed at a temperature range higher than the temperature of normal hot rolling, which reduces the productivity of the steel material.
[0009] Furthermore, in the technology disclosed in JP 2005-29886 A, elements that affect the material properties, such as Ti, V, and Nb, are added to the steel material. Furthermore, in the technology disclosed in JP 2005-29886 A, expensive REM is added to the steel material, which increases costs. As such, there is room for improvement in the technologies disclosed in JP 7-242938 A, JP 6-297026 A, and JP 2005-29886 A.
[0010] Therefore, an object of the present disclosure is to provide hot rolling equipment and a hot rolling method that can suppress red embrittlement cracking.
[0011] The hot rolling equipment according to the first aspect is a hot rolling equipment for hot rolling a steel material containing Cu, and includes a heating furnace for heating the steel material after casting to a predetermined temperature, a rough rolling device including a plurality of rolling mills for rough rolling the steel material heated in the heating furnace, and a finish rolling device for performing finish rolling on the steel material rough rolled by the rough rolling device. The equipment includes: a removal device for removing a target area including cracks caused by a Cu-enriched layer that is present on the surface side of the steel material during or after the rough rolling and has a higher concentration of Cu component than in the base material of the steel material; and the removal device is provided downstream of the rolling mill located most upstream of the plurality of rolling mills in the rough rolling device in the conveying direction of the steel material, and upstream of the finish rolling device.
[0012] The hot rolling equipment of the second aspect is the hot rolling equipment of the first aspect, but is provided with a post-removal descaling device that is located downstream of the removal device and upstream of the finishing rolling device in the conveying direction of the steel material and that removes scale from the steel material using cooling water.
[0013] The hot rolling equipment of the third aspect is the hot rolling equipment of the first or second aspect, and is provided with a rolling mill among the plurality of rolling mills in the rough rolling device that is located upstream of the removal device in the conveying direction of the steel material and adjacent to the removal device, and a pre-removal descaling device that is provided between the removal device and removes scale from the steel material using cooling water.
[0014] The hot rolling equipment according to the fourth aspect is the hot rolling equipment according to any one of the first to third aspects, wherein the removal device is provided between one of the plurality of rolling mills in the roughing rolling device and another rolling mill adjacent to the one rolling mill.
[0015] The hot rolling equipment according to the fifth aspect is the hot rolling equipment according to the fourth aspect, wherein the removal device is provided after the rolling mill located most upstream of the plurality of rolling mills in the roughing rolling device in the conveying direction of the steel material.
[0016] The hot rolling equipment of the sixth aspect is the hot rolling equipment of any one of the first to third aspects, wherein the removal device is provided downstream of the roughing rolling device and upstream of the finishing rolling device in the conveying direction of the steel material.
[0017] A hot rolling facility according to a seventh aspect is the hot rolling facility according to any one of the first to sixth aspects, wherein the removal device removes the target area from the steel material by laser cutting, or removes the target area from the steel material by mechanical removal.
[0018] A hot rolling facility according to an eighth aspect is the hot rolling facility according to any one of the first to seventh aspects, wherein the heating furnace is provided separately from a production line of a casting machine that casts the steel material.
[0019] A hot rolling facility according to a ninth aspect is the hot rolling facility according to any one of the first to seventh aspects, wherein the heating furnace is provided on a production line of a casting machine that casts the steel material.
[0020] A hot rolling method according to a tenth aspect is a hot rolling method for hot rolling a steel material containing Cu, and includes a heating step in which the steel material after casting is heated to a predetermined temperature, a rough rolling step in which rough rolling is performed multiple times on the steel material heated in the heating step, and a finish rolling step in which finish rolling is performed on the steel material rough rolled in the rough rolling step. A removal step is provided in which a target region including cracks caused by a Cu-enriched layer that is present on the surface side of the steel material during the rough rolling or that has been rough rolled and has a higher concentration of Cu component than in the base material of the steel material is removed, and the removal step is performed after the first rough rolling of the multiple rough rollings and before the finish rolling step.
[0021] A hot rolling method according to an eleventh aspect is the hot rolling method according to the tenth aspect, further comprising a post-removal descaling step of removing scales from the steel material using cooling water after the removing step and before the finish rolling step.
[0022] The hot rolling method according to a twelfth aspect is the hot rolling method according to the tenth or eleventh aspect, further including a pre-removal descaling step of removing scales from the steel material using cooling water after a rolling step immediately preceding the removing step among the plurality of rough rolling steps and before the removing step.
[0023] A hot rolling method according to a thirteenth aspect is the hot rolling method according to any one of the tenth to twelfth aspects, wherein the removing step is performed when the surface temperature of the steel material during or after the rough rolling is 1000°C or less.
[0024] A hot rolling method according to a fourteenth aspect is the hot rolling method according to any one of the tenth to thirteenth aspects, wherein, in the removing step, when the target area is removed by surface cutting, the conveying speed of the steel material during or after the rough rolling is 20 m / min or more.
[0025] A hot rolling method according to a fifteenth aspect is the hot rolling method according to any one of the tenth to fourteenth aspects, wherein the target region is a region of 1 mm or less in the thickness direction from the surface of the steel material during or after the rough rolling.
[0026] As described above, according to the present disclosure, there are provided hot rolling equipment and a hot rolling method that are capable of suppressing red embrittlement cracking.
[0027] FIG. 1 is a schematic diagram showing an example of a schematic configuration of a hot rolling facility according to a first embodiment of the present disclosure. FIG. 2 is a schematic diagram showing an example of a thermal history of the hot rolling facility according to the first embodiment of the present disclosure. FIG. 3 is a cross-sectional view showing a steel material to be laser-cut by the laser-cutting device according to the first embodiment of the present disclosure. FIG. 4 is a schematic diagram showing an example of a schematic configuration of a laser-cutting device according to the first embodiment of the present disclosure. FIG. 5 is a schematic diagram showing an example of a schematic configuration of a target region according to the first embodiment of the present disclosure. FIG. 6 is a flowchart showing an example of a hot rolling process according to the first embodiment of the present disclosure. FIG. 7 is a schematic diagram showing an example of a schematic configuration of a hot rolling facility and a laser-cutting device according to a first modified example. FIG. 8 is a schematic diagram showing an example of a schematic configuration of a hot rolling facility and a laser-cutting device according to a second modified example. FIG. 9 is a schematic diagram showing an example of a schematic configuration of a hot rolling facility and a laser-cutting device according to a fourth modified example. FIG. 10 is a schematic diagram showing an example of a schematic configuration of a cutting device according to the second embodiment of the present disclosure. 1 is a schematic diagram showing an example of a schematic configuration of a hot rolling facility according to a third embodiment of the present disclosure. 2 is a schematic diagram showing an example of a thermal history of the hot rolling facility according to the third embodiment of the present disclosure. 3 is a graph showing the relationship between the Cu concentration in the steel plate and the depth of surface cracks in the steel plate for each steel plate according to the examples and comparative examples.
[0028] Preferred embodiments of the present disclosure will be described in detail below with reference to the accompanying drawings. In this specification and the drawings, components having substantially the same functional configurations are designated by the same reference numerals, and redundant description will be omitted. Furthermore, unless otherwise specified, each component is not limited to one, and may be present in multiple numbers.
[0029] First Embodiment First, a schematic configuration of a hot rolling facility 10 according to a first embodiment of the present disclosure will be described with reference to Fig. 1. Fig. 1 is a diagram showing a schematic configuration of the hot rolling facility 10.
[0030] As an example, as shown in Figure 1, hot rolling equipment 10 is equipment for hot rolling steel material 1. As an example, this hot rolling equipment 10 is provided separately from a production line of a continuous casting machine 11 that continuously casts the steel material 1. The hot rolling equipment 10 includes a heating furnace 20, a laser cutting device 30, a descaling device 40, a roughing rolling device 50, and a finishing rolling device 60. Note that the steel material 1 is not limited to being continuously cast, and may also be cast individually.
[0031] The heating furnace 20 heats the steel material 1 (for example, a slab 1A) obtained by cutting the steel material 1 discharged from the continuous casting machine 11 to a predetermined length, to a predetermined temperature. The "predetermined temperature" here is, for example, 1100°C or higher. The slab 1A is heated by the heating furnace 20 while being transported by the transport rolls 22. Note that, although the slab 1A is used as an example of the steel material 1 here, this is merely an example, and the steel material 1 may also be a billet.
[0032] The steel material 1 is a steel material containing Cu, for example, a steel material containing 0.15 wt% (mass%) or more of Cu, particularly a steel material containing 0.25 wt% or more of Cu. Note that the Cu content here refers to the average Cu content in the base material of the steel material 1, which will be described later, or the average Cu content in the molten steel that becomes the steel material 1. The Cu content of the steel material 1 is, for example, 5.6 wt% or less.
[0033] The descaling device 40 removes scale (i.e., oxide film) formed on both surfaces of the slab 1A in the thickness direction and on both surfaces (side end faces) of the slab 1A in the width direction before rough rolling by the roughing rolling device 50. The descaling device 40 removes scale by spraying a fluid (e.g., cooling water) onto the slab 1A from a nozzle 42. That is, the descaling device 40 sprays cooling water W, which is supplied, for example, from a cooling water tank (not shown) and adjusted to a predetermined water pressure using a pump (not shown), onto the surface of the slab 1A from the nozzle 42. The descaling device 40 removes scale from the surface of the slab 1A, and the surface temperature of the slab 1A is reduced to less than 1100°C due to heat removal by the cooling water. Here, the surface temperature of the slab 1A (e.g., the surface in the width direction of the slab 1A) after scale removal by the descaling device 40 is measured using a radiation thermometer.
[0034] The roughing rolling device 50 performs rough rolling (hot rough rolling) on the slab 1A to thin the slab 1A to a predetermined thickness. Specifically, the roughing rolling device 50 rolls the slab 1A, which has been rolled down in the width direction by the vertical rolls 24, from above and below to form a rough bar 1B. In the example shown in FIG. 1, the roughing rolling device 50 includes four rolling mills 51, 52, 53, and 54. Each of the rolling mills 51 to 54 has multiple rolls that sandwich the slab 1A from both sides in the thickness direction. The roughing rolling device 50 continuously rolls the slab 1A using the rolling mills 51 to 54. In the roughing rolling device 50, the slab 1A is thinned to a plate thickness of, for example, about 25 to 50 mm and formed into a rough bar 1B.
[0035] The rake-cutting device 30 removes a surface portion (surface layer) of the steel material 1 by rake-cutting the steel material 1 after the rough rolling process (i.e., during or after rough rolling). The configuration of the rake-cutting device 30 will be described in detail later. In the example shown in FIG. 1 , the rake-cutting device 30 is provided downstream of the rolling mill 51, which is located most upstream in the conveying direction of the steel material 1, among the multiple rolling mills 51 to 54 included in the rough rolling device 50. Furthermore, the rake-cutting device 30 is provided upstream of the finish rolling device 60 in the conveying direction of the steel material 1. When the steel material 1 is rake-cut by the rake-cutting device 30, the surface temperature of the steel material 1 is set to 1000°C or less. Note that, in this specification, "removal" does not necessarily mean complete removal, but also includes insufficient removal within a range generally acceptable in the technical field to which the present disclosure pertains, and does not contradict the spirit of the present disclosure. Note that the rake-cutting device 30 is an example of a removal device.
[0036] The scalding device 30 is provided between the rolling mill 51 provided on the most upstream side of the roughing rolling device 50 and the rolling mill 52 provided on the second stage (i.e., after the rolling mill 51 provided on the most upstream side) in the conveying direction of the steel material 1. In other words, the scalding device 30 is provided between the rolling mill 51 and the rolling mill 52 adjacent to the rolling mill 51.
[0037] The finish rolling device 60 further hot finish rolls the rough bar 1B to a predetermined thickness. Specifically, the finish rolling device 60 finish rolls the rough bar 1B, which has been reheated by the rough bar heating device 62, to a thickness of about several mm (e.g., 1 to 2 mm). The finish rolling device 60 has multiple groups of finish rolling rolls 64 across 6 to 7 stands. Each group of finish rolling rolls 64 has multiple rolls aligned vertically. The finish rolling device 60 gradually reduces the rough bar 1B by passing it through the gaps between the multiple groups of finish rolling rolls 64. The steel strip 1C obtained by finish rolling the rough bar 1B to a predetermined thickness by the finish rolling device 60 is sent to a cooling device 70. Here, an example is shown in which the finishing rolling device 60 has 6 to 7 stands, but this example is merely one example, and the finishing rolling device 60 may have, for example, a group of finishing rolling rolls 64 with 5 stands.
[0038] The cooling device 70 cools the steel strip 1C after finish rolling with cooling water W. The cooling device 70 is, for example, a pipe laminar nozzle type cooling device. The steel strip 1C cooled by the cooling device 70 is wound into a coil by a winding device 80 and transported as a hot-rolled coil 1D from the hot rolling facility 10 to the next process.
[0039] Figure 2 shows an example of the thermal history of the steel material 1 in a series of processes including continuous casting, hot rolling, and cold rolling. As shown in Figure 2, at the start of continuous casting, the temperature of the steel material 1 is about 1500°C, and scale is generated on the surface of the steel material 1. This is because, when the temperature of the steel material 1 reaches 1100°C or higher, the surface of the steel material 1 is heated to 2Fe+O 2 This is because the reaction of Cu = 2FeO mainly proceeds, forming iron oxide (i.e., FeO) on the surface of the steel material 1 and turning it into scale. At this time, Cu remains in the steel material 1 without oxidizing. However, if the base material of the steel material 1 contains a relatively large amount of Cu in this temperature range (for example, if the average concentration of the Cu component in the base material is 0.15 wt % (mass %) or more), Cu is locally swept out of the iron oxide and infiltrates into the interface between the iron oxide and the bare metal portion of the steel material 1. The Cu swept out from the iron oxide mainly infiltrates and concentrates in the grain boundaries in the surface layer of the bare metal portion of the steel material 1. In this way, a region (hereinafter referred to as a "Cu-enriched layer") where the concentration of the Cu component is higher than the average concentration of the Cu component in the base material of the steel material 1 is formed in the surface layer (surface side) of the bare metal portion of the steel material 1 (i.e., a Cu concentration phenomenon occurs).
[0040] The Cu-enriched layer refers to a region in the unoxidized base metal of a steel material where, when a scale formed on the surface of the steel material due to oxidation, the concentration of Cu is higher than the average concentration of Cu in the base material of the steel material. In other words, the Cu-enriched layer refers to the region extending from the interface between the scale formed on the surface of the steel material and the base metal of the steel material, i.e., the surface of the unoxidized base metal of the steel material, toward the center of the thickness direction of the steel material, until the Cu component enriched at the grain boundaries is no longer observed. Here, the "region where the Cu component enriched at the grain boundaries is not observed" refers to a region where the concentration of Cu component present at the grain boundaries is equal to or less than the average concentration in the steel material + 1%. The base material of the steel material refers to the portion of the steel material excluding the Cu-enriched layer.
[0041] When Cu is present at the grain boundaries in a liquid phase (for example, at 1100°C or higher), the ductility of the grain boundaries decreases. Therefore, when a Cu-enriched layer is formed in the steel material 1, the steel material 1 exhibits red embrittlement, and red embrittlement cracking due to the Cu-enriched layer occurs on the surface of the steel material 1. The red embrittlement cracking that occurs on the surface of the steel material 1 becomes a quality defect and needs to be removed. In particular, in high-quality steel materials, automotive steel sheets, and the like, where surface quality is important, it is necessary to remove the surface cracks of the steel material 1.
[0042] In conventional surface treatment methods, surface defects such as iron oxide formed on the surface of the slab 1A, inclusions and casting powder embedded in the surface layer of the slab 1A during casting, or air bubble marks on the surface layer of the slab 1A are removed using a machine scarifier or the like. The removal of these surface defects is performed before the heating step (i.e., heating in the heating furnace 20) in the hot rolling process. That is, the surface defects are removed from the slab 1A before the hot rolling process. However, in the heating step in the hot rolling process, the slab 1A is heated again to 1100°C or higher (e.g., approximately 1300°C), and scale is re-formed on the surface of the slab 1A. As a result, the Cu concentration phenomenon recurs in the slab 1A, and red embrittlement cracking also recurs.
[0043] Therefore, after extensive research, the inventors came up with the idea of removing red embrittlement cracking caused by the Cu-enriched layer on the surface of the slab 1A during the rough rolling process in the hot rolling process. That is, in the thermal history of the steel material 1 shown in FIG. 2, after leaving the heating furnace 20, the steel material 1 is heated to 1000 ° C or less during the rough rolling process, and is not heated to 1100 ° C or more thereafter. Therefore, in the processes after the rough rolling process, the Cu enrichment phenomenon is suppressed, and red embrittlement cracking is also suppressed. Therefore, if red embrittlement cracking is removed from the steel material 1 during or after the rough rolling process, it is not necessary to remove red embrittlement cracking from the steel material 1 again in subsequent processes.
[0044] In addition, even if the steel material 1 is heated to 1100°C or higher in the rough rolling process or the finish rolling process, the heating of the steel material 1 during rolling is short, so scale that causes a Cu-enriched layer is not formed on the surface of the steel material 1.
[0045] Furthermore, red embrittlement due to the Cu concentration phenomenon mainly occurs at 1100°C to 1250°C. The upper limit of the temperature at which red embrittlement occurs increases as the Cu concentration in the steel material 1 increases. In addition, in the relationship between the heating temperature of the steel material 1 and the depth of red embrittlement cracking in the steel material 1, the higher the heating temperature of the steel material 1, the more the γ (austenite) grain boundaries coarsen, and therefore the depth of red embrittlement cracking caused by Cu concentrated at the grain boundaries also increases. On the other hand, in the relationship between the heating temperature of the steel material 1 and the number of red embrittlement cracking in the steel material 1, the higher the heating temperature of the steel material 1, the fewer the number of grain boundaries, and therefore the fewer the number of red embrittlement cracking in the steel material 1.
[0046] Here, the depth of penetration of Cu from the iron oxide into the base metal portion of the steel material 1 is relatively shallow, at most about 50 μm. The reason for this is thought to be as follows: When a crack that has occurred on the surface of the steel material 1 propagates, liquid-phase Cu infiltrates the tip of the crack in the early stage of crack propagation. This reduces the ductility of the grain boundary, making the crack more likely to propagate. On the other hand, as the crack propagation progresses, the amount of Cu remaining at the grain boundary increases. As a result, the amount of Cu present at the tip of the crack gradually decreases, and the crack propagation finally stops. At this time, the depth of the surface crack is about the width of one austenite grain.
[0047] Furthermore, when the amount of displacement due to tensile stress increases near the surface of the steel material 1, the depth of the surface crack increases in the initial stage of the displacement, but as the displacement progresses, the depth of the surface crack does not increase, but the width of the surface crack increases. Therefore, in red embrittlement cracking due to the Cu enrichment phenomenon, the propagation depth of the surface crack is at most several mm (e.g., 1 mm). Therefore, if several mm (e.g., 1 mm) of the surface layer of the steel material 1 is removed from the steel material 1 after rolling, quality defects on the surface of the steel material 1 can be suppressed.
[0048] Therefore, in the hot rolling equipment 10 according to this embodiment, the surface layer of the slab 1A is removed by a scarifying device 30. As shown in FIG. 3 as an example, the scarifying device 30 has two scarfer units 31 facing the surfaces on both sides (top and bottom) in the thickness direction of the steel material 1, and two scarfer units 31 facing the surfaces (side end faces) on both sides (left and right) in the width direction of the steel material 1. The four scarfer units 31 have the same configuration. Therefore, hereinafter, only the scarfer unit 31 facing one (upper) surface in the thickness direction of the steel material 1 will be described.
[0049] As shown in Figure 4, the scarfer unit 31 includes a preheating gas jetting section 34 and a fracturing-cutting oxygen jetting section 36. The preheating gas jetting section 34 jets preheating oxygen 32 and combustible gas 33. The fracturing-cutting oxygen jetting section 36 jets fracturing-cutting oxygen 37. From the bottom of the fracturing-cutting oxygen jetting section 36, a shielding gas 38 consisting of combustible gas is jetted together with the fracturing-cutting oxygen 37. The steel material 1 is configured to be transported in the direction of arrow Y in Figure 4.
[0050] As shown in Figure 4, the jet of cutting oxygen 37 jetted from the cutting oxygen jetting section 36 is jetted further forward in the conveying direction Y of the steel material 1 than the jets of preheating oxygen 32 and combustible gas 33 jetted from the preheating gas jetting section 34.
[0051] In the scalding device 30, first, a preheating step is carried out as shown on the left side of Fig. 4. In the preheating step, preheating oxygen 32 and combustible gas 33 are ejected from a preheating gas ejection portion 34 of the scarfer unit 31 toward the surface of the steel material 1, and the combustible gas 33 is burned. Then, a part of the surface of the steel material 1 is melted by the heat of the burning combustible gas 33, and a basin portion 1E is formed.
[0052] The length of the basin 1E formed on the surface of the steel material 1 along the conveying direction Y is set to, for example, a range of about 20 mm to 30 mm.
[0053] Next, as shown on the right side of Fig. 4, a laser cutting process is carried out. In the laser cutting process, laser cutting oxygen 37 is ejected from the laser cutting oxygen ejection portion 36 of the scarfer unit 31 toward the surface of the steel material 1, and the steel material 1 on which the basin portion 1E has been formed is transported in the transport direction Y. At this time, a shielding gas 38 is ejected from the laser cutting oxygen ejection portion 36 together with the laser cutting oxygen 37, and the laser cutting oxygen 37 is protected by the shielding gas 38. The laser cutting process is an example of a removal process.
[0054] Then, the jet of cutting oxygen 37 jetted from the cutting oxygen jetting portion 36 collides with the molten iron in the basin 1E of the transported steel material 1, causing an oxidation reaction between the molten iron and the cutting oxygen 37. The heat of this oxidation reaction melts the surface of the steel material 1 one after another, and the surface of the steel material 1 is laser-cut. That is, the surface of the steel material 1 is laser-cut by the heat of the oxidation reaction on the rear side of the basin 1E in the transport direction Y. In this way, the surface of the slab 1A after being heated in the heating furnace 20 is laser-cut by the laser-cutting device 30.
[0055] As an example, as shown in FIG. 5 , the laser cutting device 30 removes a target region T, which is a region including cracks C caused by a Cu-enriched layer R. Here, the target region T refers to a predetermined thickness region set from the surface of the steel material 1 toward the center in the thickness direction of the steel material 1 so as to include all of the Cu-enriched layer R, the cracks C caused by the Cu-enriched layer R, and the scale S. This target region T is a range of a predetermined distance from the surface of the steel material 1 (i.e., the surface of the scale S) in the thickness direction t of the steel material 1. The predetermined distance is, for example, greater than 0 mm and equal to or less than 3 mm (0 < distance ≦ 3 mm), preferably greater than 0 mm and equal to or less than 2 mm (0 < distance ≦ 2 mm), and more preferably greater than 0 mm and equal to or less than 1 mm (0 < distance ≦ 1 mm).
[0056] When the steel material 1 is a rough bar 1B, the thickness of the steel material 1 is, for example, about 25 to 50 mm. Therefore, by removing a region of 1 mm or less from the surface of the steel material 1 as the target region T in the thickness direction t of the slab 1A, the reduction in the thickness of the steel material 1 is reduced, and the yield of the slab 1A can be improved.
[0057] Here, the relationship between the maximum conveying speed of the slab 1A at which the surface of the slab 1A can be continuously and uninterruptedly scarified and the scarified thickness of the slab 1A at that time is expressed by the following formula (1): h = 6 × Vs -0.6 ... (1) h (mm): Thickness of slab 1A to be cut, Vs (m / min): Maximum conveying speed of slab 1A that can be cut continuously without interruption
[0058] As shown in the above formula (1), the thickness of the slab 1A being scrubbed decreases as the conveying speed of the slab 1A increases. In other words, the faster the conveying speed of the slab 1A, the thinner the scrubbed thickness of the slab 1A. As described above, the depth of surface cracks in the steel material 1 is considered to be several millimeters (e.g., 1 mm). Therefore, to keep the scrubbed thickness of the slab 1A at approximately 1 to 2 mm, it is preferable to set the conveying speed of the slab 1A to 20 m / min or more. Furthermore, by setting the conveying speed of the slab 1A to 20 m / min or more, partial interruptions in scrubbed thickness of the slab 1A are suppressed even when the scrubbed thickness of the slab 1A is as thin as 1 mm. The upper limit of the conveying speed of the slab 1A during scrubbed cutting is appropriately set based on the operating conditions of the scrubbed cutting device 30 and the thickness of the steel material 1 to be scrubbed, and is set to, for example, 80 m / min or less.
[0059] In the example shown in Figure 5, one surface in the thickness direction of the steel material 1 is laser-cut, but the laser-cutting device 30 of this embodiment also laser-cuts other surfaces in the thickness direction of the steel material 1 and both surfaces (side end faces) in the width direction of the steel material 1.
[0060] The target region T including the Cu-enriched layer R is removed by being spalled (removed) from the steel material 1, thereby removing the cracks C present at the grain boundaries GB. As a result, red embrittlement cracking on the surface of the steel material 1 is suppressed.
[0061] Next, a hot rolling method according to this embodiment will be described with reference to Fig. 6. Fig. 6 is a flowchart for explaining a part of the manufacturing process of a hot-rolled steel sheet according to this embodiment. As shown in Fig. 6, first, in the heating process of step ST10, the continuously cast slab 1A is heated to a predetermined temperature (for example, about 1300°C) by a heating furnace 20. After the heating process of step ST10 is performed, the manufacturing process proceeds to step ST12.
[0062] In the descaling process of step ST12, the slab 1A heated in step ST10 is descaled by the descaling device 40 using cooling water W. As a result of the descaling, the surface temperature of the slab 1A is reduced to, for example, less than 1100°C. After the descaling process of step ST12 is performed, the manufacturing process proceeds to step ST14.
[0063] In the rough rolling step of step ST14, the slab 1A descaled in step ST12 is rough rolled by the rough rolling device 50. As a result, the slab 1A is formed into a rough bar 1B having a predetermined thickness. After the rough rolling step of step ST14 is performed, the manufacturing process proceeds to step ST16.
[0064] In the laser cutting process (removal process) of step ST16, the slab 1A rough-rolled in step ST14 is laser-cut by the laser cutting device 30, thereby removing the target region T including the Cu-enriched layer from the slab 1A. The laser cutting of the slab 1A by the laser cutting device 30 is performed after the first rough rolling of the slab 1A, which is performed multiple times (e.g., four times) by the rough rolling device 50. At the stage where the slab 1A is laser-cut by the laser cutting device 30, the temperature of the surface of the slab 1A becomes 1000°C or less. After the laser cutting process of step ST16 is performed, the manufacturing process proceeds to step ST18.
[0065] In the rough rolling process of step ST18, the slab 1A that was spall-cut in step ST16 is subjected to the remaining rough rolling by the rough rolling device 50. As a result, the slab 1A is formed into a rough bar 1B, and the rough rolling process ends. After the rough rolling process of step ST18 is performed, the manufacturing process proceeds to step ST20.
[0066] In the finish rolling process of step ST20, the rough bar 1B obtained in step ST18 is finish rolled by the finish rolling mill 60. As a result, the rough bar 1B is formed into a steel strip 1C having a predetermined thickness. After the finish rolling process of step ST20 is performed, the manufacturing process proceeds to step ST22.
[0067] In the winding process of step ST22, the steel strip 1C obtained in step ST20 is formed into a hot-rolled coil 1D by being wound by a winding device 80. After the winding process of step ST22 is performed, part of the manufacturing process of the hot-rolled steel sheet according to this embodiment is completed.
[0068] As described above, in the hot rolling equipment 10 according to the first embodiment, the rough rolling device 50 includes a plurality of rolling mills 51-54. The rough rolling device 30 is located downstream of the rolling mill 51, which is located furthest upstream in the conveying direction of the steel material 1, and upstream of the finishing rolling device 60. When the steel material 1 is heated to a predetermined temperature (e.g., 1300°C) in the heating furnace 20, liquid-phase Cu is concentrated at the grain boundaries GB near the surface of the steel material 1. The Cu-concentrated portion of the steel material 1 has poor ductility compared to the base metal portion of the steel material 1. Therefore, the occurrence of a Cu-concentrated layer contributes to red embrittlement cracking. In this embodiment, the rough rolling device 30 is provided to remove surface cracks due to the Cu-concentrated layer from the steel material 1 that is being rough rolled after heating in the heating furnace 20. This allows cracks that have occurred on the surface of the steel material 1 to be removed during or after rough rolling. Therefore, according to this embodiment, the occurrence of red embrittlement cracking in the steel material 1 is suppressed.
[0069] For example, consider a case where the laser cutting device 30 is provided upstream of the rough rolling device 50 (e.g., upstream of the heating furnace 20) in the conveying direction of the steel material 1. In this case, if the temperature of the steel material 1 remains high (e.g., 1100°C or higher), a Cu-enriched layer will form again in the steel material 1, causing red embrittlement cracking. For this reason, it is difficult to suppress red embrittlement cracking of the steel material 1. In this embodiment, cracks that have occurred on the surface of the steel material 1 are removed during or after rough rolling, so the occurrence of red embrittlement cracking in the steel material 1 is suppressed.
[0070] On the other hand, consider the case where the laser cutting device 30 is provided downstream of the finish rolling device 60 in the conveying direction of the steel material 1. In this case, the temperature of the steel material 1 is sufficiently reduced, so Cu enrichment is unlikely to occur. However, the thickness of the steel material 1 (steel strip 1C) at the finish rolling stage is reduced compared to the thickness of the steel material 1 (slab 1A) up to the rough rolling stage. Therefore, if the surface cracks of the steel material 1 are removed at the finish rolling stage, the thickness of the steel material 1 will be further reduced, resulting in a decrease in the yield of the steel material 1. In this embodiment, the cracks generated on the surface of the steel material 1 are removed during or after rough rolling, so the decrease in the yield of the steel material 1 in the hot rolling process is suppressed.
[0071] Furthermore, in the hot rolling equipment 10 according to the first embodiment, of the plurality of rolling mills 51 to 54 in the roughing rolling device 50, the scalding device 30 is provided between the rolling mill 51 and the rolling mill 52 adjacent to the rolling mill 51. In other words, the scalding device 30 is provided between the rolling mill 51 and the rolling mill 52 adjacent to the rolling mill 51 among the plurality of rolling mills 51 to 54. This allows cracks that have occurred on the surface of the steel material 1 to be removed during the rough rolling process. Therefore, according to this embodiment, the occurrence of red embrittlement cracking in the steel material 1 is suppressed.
[0072] Furthermore, in the hot rolling equipment 10 according to the first embodiment, the rake cutting device 30 is provided after the rolling mill 51, which is located most upstream in the conveying direction of the steel material 1, among the multiple rolling mills 51 to 54. In other words, the rake cutting device 30 is provided on the roll exit side of the rolling mill 51, which is located most upstream in the conveying direction of the steel material 1. This allows cracks that have occurred on the surface of the steel material 1 to be removed during rough rolling. Furthermore, in the rough rolling process, surface cracks of the steel material 1 are removed when the thickness of the steel material 1 is at its thickest. Therefore, according to this embodiment, the occurrence of red embrittlement cracking in the steel material 1 is suppressed, and a decrease in the yield of the steel material 1 in the hot rolling process is suppressed.
[0073] Furthermore, in the hot rolling equipment 10 according to the first embodiment, the steel material 1 is subjected to laser cutting by the laser cutting device 30, thereby removing the target region T including the Cu-enriched layer from the steel material 1. Laser cutting has higher productivity than removal by cutting. Therefore, according to the present embodiment, a decrease in productivity in the hot rolling equipment 10 can be suppressed.
[0074] Furthermore, in the hot rolling equipment 10 according to the first embodiment, when the steel material 1 is laser-cut by the laser-cutting device 30, the conveying speed of the steel material 1 is set to 20 m / min or more. By setting the conveying speed of the steel material 1 to 20 m / min or more in this manner, the laser-cutting thickness of the steel material 1 becomes about 1 mm. This removes surface cracks in the steel material 1. Therefore, according to this embodiment, the occurrence of red embrittlement cracking in the steel material 1 is suppressed.
[0075] Furthermore, in the hot rolling equipment 10 according to the first embodiment, a region of 1 mm or less from the surface of the steel material 1 is removed in the thickness direction t of the steel material 1. Cracks caused by the Cu-enriched layer mainly occur in a region of 1 mm or less from the surface of the steel material 1 in the thickness direction t of the steel material 1. As described above, in red embrittlement due to Cu, the propagation depth of surface cracks in the steel material 1 is at most several mm (for example, 1 mm). Therefore, removing a region of up to 1 mm from the surface of the steel material 1 in the thickness direction t of the steel material 1 contributes to the removal of cracks. Therefore, according to this embodiment, the occurrence of red embrittlement cracks in the steel material 1 is suppressed.
[0076] (First Modification) In the above-described first embodiment, an example in which the rake cutting device 30 is provided between the rolling mill 51 provided at the most upstream side of the roughing rolling device 50 and the rolling mill 52 provided at the second stage in the conveying direction of the steel material 1 has been described. However, the present disclosure is not limited to this example. As shown in FIG. 7 as an example, in the first modification, the rake cutting device 30 is provided between the rolling mill 52 provided at the second stage (hereinafter also referred to as the "second rolling mill 52") and the rolling mill 53 provided at the third stage (hereinafter also referred to as the "third rolling mill 53") in the roughing rolling device 50 in the conveying direction of the steel material 1. In other words, the rake cutting device 30 is provided between the second rolling mill 52 and the third rolling mill 53, which are adjacent to each other. In this way, in the first modification, the rake cutting device 30 is provided between the second rolling mill 52 and the third rolling mill 53 in the roughing rolling device 50. As a result, cracks occurring on the surface of the steel material 1 are removed during rough rolling. Therefore, according to this modification, the occurrence of red embrittlement cracking in the steel material 1 is suppressed.
[0077] Although an example embodiment in which the rake-cutting device 30 is provided between the second rolling mill 52 and the third rolling mill 53 has been described here, the present disclosure is not limited to this example embodiment. The rake-cutting device 30 may be provided between the third rolling mill 53 and the final stage rolling mill 54. Furthermore, although an example embodiment in which the roughing rolling device 50 includes four rolling mills has been described here, the present disclosure is not limited to this example embodiment. The roughing rolling device 50 may include five or more rolling mills, or three or less rolling mills.
[0078] (Second Modification) In the above-described first embodiment, an example embodiment in which the roughing mill 50 includes non-reverse rolling mills 51 to 54 has been described, but the present disclosure is not limited to this example embodiment. As an example, as shown in FIG. 8 , in the second modification, the roughing mill 50A includes a reversing rolling mill 51A. Furthermore, the scalding device 30 is provided downstream of the reversing rolling mill 51A in the conveying direction of the steel material 1. In this case, after the first rolling of the steel material 1 is performed in the reversing rolling mill 51A, the steel material 1 is scalded by the scalding device 30. Thereafter, the steel material 1 is moved in the direction opposite to the conveying direction, and the steel material 1 is rolled multiple times in the reversing rolling mill 51A.
[0079] As an example, as shown in Figure 9, the roughing rolling device 50B includes a reversing rolling mill 51B, a non-reversing rolling mill 52B, and a tandem rolling mill 53B. In the example shown in Figure 9, the slag-cutting device 30 is provided downstream of the reversing rolling mill 51B in the conveying direction of the steel material 1. That is, the slag-cutting device 30 is provided between the reversing rolling mill 51B and the non-reversing rolling mill 52B. After the first rolling of the steel material 1 is performed in the reversing rolling mill 51B, the steel material 1 is slag-cut by the slag-cutting device 30. Then, after the steel material 1 is rolled multiple times in the reversing rolling mill 51B, the steel material 1 is rolled in the non-reversing rolling mill 52B and the tandem rolling mill 53B. Although the description has been given here of an example in which the scalloping device 30 is provided downstream of the reversing rolling mill 51B in the conveying direction of the steel material 1, the present disclosure is not limited to this example. The scalloping device 30 may be provided between the non-reversing rolling mill 52B and the tandem rolling mill 53B.
[0080] In the second modified example, the laser cutting device 30 is provided after the rolling mill (reverse rolling mill 51B) located most upstream of the roughing rolling devices 50 in the conveying direction of the steel material 1. As a result, cracks that have occurred on the surface of the steel material 1 are removed during rough rolling. Furthermore, in the rough rolling process, surface cracks of the steel material 1 are removed when the thickness of the steel material 1 is at its thickest. Therefore, according to this modified example, the occurrence of red embrittlement cracking in the steel material 1 is suppressed, and a decrease in the yield of the steel material 1 in the hot rolling process is suppressed.
[0081] (Third Modification) In the above-described first embodiment, an example in which the laser cutting of the steel material 1 by the laser cutting device 30 is performed during rough rolling has been described, but the present disclosure is not limited to this example. In the third modification, the laser cutting of the steel material 1 by the laser cutting device 30 is performed after rough rolling and before finish rolling.
[0082] As an example, as shown in FIG. 10 , the rake-cutting device 30 is provided downstream of the roughing rolling device 50 in the conveying direction of the steel material 1. Furthermore, the rake-cutting device 30 is provided upstream of the finish rolling device 60 in the conveying direction of the steel material 1. Specifically, the rake-cutting device 30 is provided between the exit side of the roughing rolling device 50 and the entry side of the finish rolling device 60. As such, in the third modified example, the rake-cutting device 30 is provided after the roughing rolling device 50 and before the finish rolling device 60 in the conveying direction of the steel material 1. This allows cracks that have occurred on the surface of the steel material 1 to be removed after the rough rolling process. Since the temperature of the steel material 1 after the rough rolling process is sufficiently reduced (for example, 1000°C or less), a Cu-enriched layer is unlikely to form, and the re-occurrence of surface cracks in the steel material 1 is suppressed. Therefore, according to this modified example, the occurrence of red embrittlement cracking in the steel material 1 is suppressed.
[0083] Furthermore, in the third variant, the steel material 1 is laser-cut before finish rolling, which improves the yield in the hot rolling process compared to when laser-cutting the steel material 1 whose plate thickness has been reduced by finish rolling.
[0084] (Fourth Modification) In the first embodiment, an example in which the descaling process is not performed before or after the laser cutting process (removal process) has been described, but the present disclosure is not limited to this example. In the fourth modification, a pre-removal descaling process is performed before the laser cutting process (removal process), and a post-removal descaling process is performed after the laser cutting process (removal process).
[0085] 11 , the laser cutting device 30 is provided downstream of the roughing rolling device 50 and upstream of the finish rolling device 60 in the conveying direction of the steel material 1. Furthermore, a pre-removal descaling device 40A is provided downstream of the roughing rolling device 50 and upstream of the laser cutting device 30 in the conveying direction of the steel material 1. In other words, the pre-removal descaling device 40A is provided between the most downstream rolling mill 54 of the multiple rolling mills 51 to 54 in the roughing rolling device 50 in the conveying direction of the steel material 1 and the laser cutting device 30. The basic configuration of this pre-removal descaling device 40A is the same as that of the descaling device 40.
[0086] The pre-removal descaling device 40A removes scale formed on the surface of the steel material 1 before (just before) the steel material 1 is subjected to thermal cutting by the thermal cutting device 30. That is, in the fourth modified example, the pre-removal descaling process is performed after the rough rolling process and before the thermal cutting process (removal process).
[0087] Here, when the steel material 1 is laser-cut by the laser-cutting device 30, if scale or the like is attached to the surface of the steel material 1, the combustion reaction between the laser-cutting oxygen 37 (see FIG. 4 ) sprayed from the laser-cutting device 30 and the steel material 1 is inhibited, and there is a possibility that the laser-cutting of the steel material 1 will be interrupted. In particular, when the laser-cutting thickness of the steel material 1 by the laser-cutting device 30 is kept to about 1 mm to 2 mm, the laser-cutting of the steel material 1 by the laser-cutting device 30 will be easily interrupted.
[0088] In contrast to this, in the fourth modified example, as described above, before the steel material 1 is laser-cut by the laser-cutting device 30, the pre-removal descaling device 40A removes scale adhering to the surface of the steel material 1. This makes it easier to stabilize the combustion reaction between the laser-cutting oxygen 37 (see FIG. 4 ) and the like sprayed from the laser-cutting device 30 and the steel material 1. Therefore, interruptions in the laser-cutting of the steel material 1 by the laser-cutting device 30 can be suppressed.
[0089] Furthermore, the pre-removal descaling device 40A removes scale adhering to the surface of the steel material 1 by spraying cooling water W onto the surface of the steel material 1. At this time, the surface of the steel material 1 is cooled by the cooling water W, which further suppresses the re-generation of a Cu-enriched layer in the steel material 1. Therefore, the occurrence of red embrittlement cracking in the steel material 1 is suppressed. Furthermore, in the fourth modified example, the pre-removal descaling device 40A cools the surface of the steel material 1 to less than 1100°C. Therefore, the re-generation of a Cu-enriched layer in the steel material 1 is further suppressed.
[0090] In addition, a post-removal descaling device 40B is provided downstream of the laser cutting device 30 and upstream of the finish rolling device 60 in the conveying direction of the steel material 1. The basic configuration of this post-removal descaling device 40B is the same as that of the descaling device 40.
[0091] The post-removal descaling device 40B removes scale and the like adhering to the surface of the steel material 1 after the surface of the steel material 1 has been laser-cut by the laser-cutting device 30. That is, in the fourth modified example, the post-removal descaling process is performed after the laser-cutting process (removal process) and before the finish rolling process.
[0092] By removing scales and the like adhering to the surface of the steel material 1 using the post-removal descaling device 40B in this manner, the quality of the hot finish rolling of the steel material 1 by the finish rolling device 60 can be improved.
[0093] Furthermore, when the steel material 1 is laser-cut by the laser-cutting device 30, the temperature of the surface of the steel material 1 rises (for example, to about 50°C). In response to this, the post-removal descaling device 40B removes scale adhering to the surface of the steel material 1 by spraying cooling water W onto the surface of the steel material 1. At this time, the surface of the steel material 1 is cooled by the cooling water W, which further suppresses the re-generation of a Cu-enriched layer in the steel material 1. Furthermore, in the fourth modified example, the post-removal descaling device 40B cools the surface of the steel material 1 to less than 1100°C. Therefore, the re-generation of a Cu-enriched layer in the steel material 1 is further suppressed. As a result, the occurrence of red embrittlement cracking in the steel material 1 is suppressed.
[0094] In the fourth modification, the pre-removal descaling process, the laser cutting process, and the post-removal descaling process are performed after the rough rolling process. However, the pre-removal descaling process, the laser cutting process, and the post-removal descaling process may be performed during the rough rolling process. In this case, for example, in the rough rolling device 50, a pre-removal descaling device 40A, a laser cutting device 30, and a post-removal descaling device 40B are provided between adjacent rolling mills 51, 52, 53, and 54.
[0095] Specifically, the pre-removal descaling device 40A, the laser cutting device 30, and the post-removal descaling device 40B are provided between the rolling mills 51 and 52, between the rolling mills 52 and 53, or between the rolling mills 53 and .
[0096] In addition, in the fourth modified example, a pre-removal descaling step is performed before the laser cutting step (removal step), and a post-removal descaling step is performed after the laser cutting step (removal step). However, at least one of the pre-removal descaling step and the post-removal descaling step can be omitted.
[0097] Second Embodiment In the above-described first embodiment, an example has been described in which the target region T including the Cu-enriched layer is removed from the steel material 1 by the laser cutting device 30, but the present disclosure is not limited to this example. In a second embodiment, the target region T is removed from the steel material 1 by a cutting device 90 instead of the laser cutting device 30. The cutting device 90 is an example of a removal device.
[0098] As an example, as shown in FIG. 12 , the hot rolling equipment 10 is provided with a cutting device 90 instead of the slag-cutting device 30. The cutting device 90 cuts the steel material 1 discharged from the heating furnace 20 to remove a surface portion of the steel material 1. Details of the cutting device 90 will be described later. The cutting device 90 is provided downstream of the rolling mill 51 located most upstream in the conveying direction of the steel material 1 among the multiple rolling mills 51 to 54 in the roughing rolling device 50. Furthermore, the cutting device 90 is provided upstream of the finish rolling device 60 in the conveying direction of the steel material 1. More specifically, the cutting device 90 is provided between the rolling mill 51 located most upstream in the roughing rolling device 50 and the rolling mill 52 located on the second stage in the conveying direction of the steel material 1. In other words, the cutting device 90 is provided between the rolling mill 51 and the rolling mill 52 adjacent to the rolling mill 51.
[0099] As an example, as shown in Figure 13, the cutting device 90 includes a rotary cutting tool 92. The rotary cutting tool 92 has a holder 94 and a number of cutting blades 96 attached to the outer periphery of the holder 94. The rotary cutting tool 92 receives power from a power source (not shown) and rotates. The rotating cutting blades 96 come into contact with the surface of the steel material 1, thereby cutting the surface of the steel material 1. In this way, the cutting device 90 cuts the surface of the steel material 1, thereby removing a target area T on the surface of the steel material 1 after it has been heated in the heating furnace 20.
[0100] Although an example in which the cutting device 90 has one rotary cutting tool 92 has been given here, the present disclosure is not limited to this example. For example, one surface of the steel material 1 may be cut by a plurality of rotary cutting tools 92. Furthermore, the cutting device 90 may be provided with rotary cutting tools 92 at positions facing both surfaces of the steel material 1 in the thickness direction and both surfaces (side end faces) of the steel material 1 in the width direction.
[0101] As described above, in the hot rolling equipment 10 according to the second embodiment, the target region T including the Cu-enriched layer is removed from the steel material 1 by the cutting device 90. Mechanical removal such as cutting is less likely to cause deterioration in the surface quality of the steel material 1 (e.g., surface roughness) compared to removal by surface cutting. Therefore, according to this embodiment, deterioration in the surface quality of the steel material 1 in the hot rolling process can be suppressed.
[0102] In the second embodiment, an example in which the steel material 1 is cut by the cutting device 90 has been described, but the present disclosure is not limited to this example. The removal device is not limited to the cutting device 90, and may be, for example, a mechanical removal method such as grinding using a grinding wheel device.
[0103] <Third embodiment> In the above-described first embodiment, an example has been described in which the heating furnace 20 is provided separately from the production line of the continuous casting machine 11 that continuously casts the steel material 1. However, the present disclosure is not limited to this example. In a third embodiment, a heating furnace 102 is provided on the production line of the continuous casting machine that continuously casts the steel material 1.
[0104] As an example, as shown in Figure 14, a continuous casting machine 11 continuously casts a slab 1A that is thinner (e.g., 50 mm to 100 mm) than the continuous casting machine 11 in the first embodiment. A hot rolling facility 100 is provided on the production line of this continuous casting machine 11. In other words, the production line of the hot rolling facility 100 is continuous with the production line of the continuous casting machine 11. This hot rolling facility 100 includes a heating furnace 102, a descaling device 40, a roughing rolling device 50, a pre-removal descaling device 40A, a laser cutting device 30, a post-removal descaling device 40B, a rough bar heating furnace 104, and a finish rolling device 60. Note that the roughing rolling device 50 of the third embodiment includes, as an example, two rolling mills 51 and 52.
[0105] The heating furnace 102 is, for example, a table heating furnace. The heating furnace 102 is provided upstream of the roughing rolling device 50 in the conveying direction of the steel material 1. The heating furnace 102 heats the steel material 1 (for example, a slab 1A) obtained by cutting the steel material 1 discharged from the continuous casting machine 11 to a predetermined length, to a predetermined temperature (1100°C or higher).
[0106] The rough bar heating furnace 104 is, for example, a table heating furnace. The rough bar heating furnace 104 is provided downstream of the rough rolling device 50 and upstream of the finish rolling device 60 in the conveying direction of the steel material 1. The rough bar heating furnace 104 heats the steel material 1 rough rolled by the rough rolling device 50 to a predetermined temperature (less than 1100°C).
[0107] Fig. 15 shows an example of the thermal history of the steel material 1 in a series of processes of continuous casting, hot rolling, and cold rolling in the third embodiment. As shown in Fig. 15, the temperature of the steel material 1 is about 1500°C at the start of continuous casting. Therefore, scale is generated on the surface of the steel material 1. On the other hand, after leaving the heating furnace 20, the steel material 1 is cooled to 1000°C or less during the rough rolling process, and is not heated to 1100°C or more thereafter. Therefore, the third embodiment can achieve the same effects as the first embodiment.
[0108] In order to evaluate the performance of the hot rolling equipment 10 and the hot rolling method according to the present disclosure, an evaluation was made of the relationship between the depth of surface cracks in the steel plate (steel material 1) and the Cu concentration in the steel plate.
[0109] Specifically, as an example, multiple steel plates (steel material 1) with different Cu contents were prepared. The multiple steel plates had a common composition of 0.2 wt% C, 0.01-0.25 wt% Si, 0.5 wt% Mn, 0.03% T-Al, and the balance Fe, with Cu contents of 0.2 wt%, 0.5 wt%, 1 wt%, and 1.5 wt%, respectively. Each steel plate was heated and held at 1100°C or higher (1200°C), and then elongated at a strain rate of 5 / s to a cross-sectional area reduction of 33%, causing cracks to form in each steel plate. Then, 1 mm of the surface of each steel plate was removed by surface machining. The multiple steel plates according to the comparative example were similar to the multiple steel plates according to the example, except that the surface was not machined. Each steel plate according to the example and comparative example was cut, and the depth of the surface cracks in each steel plate was measured within the field of view by observing the cut surface. Then, for each steel plate according to the examples and comparative examples, the average depth of the measured surface cracks was calculated.
[0110] As an example, as shown in FIG. 16 , cracks occurred on the surface of each steel plate according to the comparative example. That is, red embrittlement cracks occurred in each steel plate in a temperature range near the rough rolling start temperature (e.g., 1100°C). As the Cu concentration in the steel plate increased, the depth of the surface cracks increased, and the Cu concentration phenomenon became more pronounced. However, even when the Cu concentration in the steel plate was high (e.g., 1 wt% or higher), the depth of the surface cracks in the steel plate was 1 mm or less. In each steel plate according to the example, the surface cracks were removed by 1 mm of surface abrasion, and the depth of the surface cracks became almost zero. In this way, it was confirmed that red embrittlement cracks can be removed by abrading the surface of the steel plate.
[0111] Although the preferred embodiments of the present disclosure have been described in detail above with reference to the accompanying drawings, the present disclosure is not limited to these examples. It is clear that a person skilled in the art of the present disclosure can conceive of various modifications or applications within the scope of the technical ideas described in the claims, and it is understood that these also naturally fall within the technical scope of the present disclosure.
[0112] The disclosure of Japanese Patent Application No. 2023-054365, filed on March 29, 2023, is incorporated herein by reference in its entirety. All documents, patent applications, and technical standards described herein are incorporated herein by reference to the same extent as if each individual document, patent application, and technical standard was specifically and individually indicated to be incorporated by reference.
[0113] In addition to the above-described embodiment, the following supplementary notes are also disclosed.
[0114] (Supplementary Note 1) A hot rolling facility for hot rolling a steel material containing Cu, comprising: a heating furnace that heats the steel material after continuous casting to a predetermined temperature; a roughing rolling device including a plurality of rolling mills that perform rough rolling on the steel material heated in the heating furnace; a finish rolling device that performs finish rolling on the steel material that has been rough rolled by the roughing rolling device; and a removal device that removes a target area that is present on the surface side of the steel material that is being rough rolled or has been rough rolled and that includes cracks caused by a Cu-enriched layer having a higher Cu concentration than in the base material, the removal device being provided downstream of a rolling mill that is located most upstream in a conveying direction among the plurality of rolling mills in the roughing rolling device and upstream of the finish rolling device. (Supplementary Note 2) The hot rolling facility according to Supplementary Note 1, wherein the removal device is provided between one of the plurality of rolling mills in the roughing rolling device and another rolling mill adjacent to the one rolling mill. (Supplementary Note 3) The hot rolling facility according to Supplementary Note 2, wherein the removal device is provided after the rolling mill that is located most upstream in the conveying direction among the plurality of rolling mills in the roughing rolling device. (Supplementary Note 4) The hot rolling facility according to Supplementary Note 1, wherein the removal device is provided downstream in the conveying direction of the roughing rolling device and upstream in the conveying direction of a finishing rolling device. (Supplementary Note 5) The hot rolling facility according to any one of Supplementary Notes 1 to 4, wherein the removal device removes the target area by scarifying. (Supplementary Note 6) The hot rolling facility according to any one of Supplementary Notes 1 to 4, wherein the removal device removes the target area by mechanical removal.(Appendix 7) A hot rolling method for hot rolling a steel material containing Cu, comprising: a heating step of heating the steel material after continuous casting to a predetermined temperature; a rough rolling step of performing rough rolling multiple times on the steel material heated in the heating step; a finish rolling step of performing finish rolling on the steel material rough rolled in the rough rolling step; and a removal step of removing a target region that is present on the surface side of the steel material during or after rough rolling and includes cracks caused by a Cu-enriched layer having a higher Cu concentration than in the base material, the removal step being performed after a first of the multiple rough rolling steps and before the finish rolling step. (Appendix 8) The hot rolling method according to Appendix 7, wherein the removal step is performed at a surface temperature of the steel material during or after rough rolling is 1000°C or lower. (Supplementary Note 9) The hot rolling method according to Supplementary Note 7 or Supplementary Note 8, wherein, in the removing step, when the target region is removed by laser cutting, the conveying speed of the steel material during or after rough rolling is 20 m / min or more. (Supplementary Note 10) The hot rolling method according to any one of Supplementary Note 7 to Supplementary Note 9, wherein the target region is a region of 1 mm or less in the thickness direction from the surface of the steel material during or after rough rolling.
Claims
1. A hot rolling facility for hot rolling a steel material containing Cu, comprising: a heating furnace for heating the steel material after casting to a predetermined temperature; a rough rolling device including a plurality of rolling mills for rough rolling the steel material heated in the heating furnace; a finish rolling device for finish rolling the steel material rough rolled by the rough rolling device; and a removal device for removing a target area including cracks caused by a Cu-enriched layer that is present on the surface side of the steel material during or after the rough rolling and has a higher concentration of Cu components than in the base material of the steel material, wherein the removal device is provided downstream of the rolling mill that is located most upstream of the plurality of rolling mills in the rough rolling device and upstream of the finish rolling device in the conveying direction of the steel material.
2. The hot rolling equipment according to claim 1, further comprising a post-removal descaling device that is provided downstream of the removal device and upstream of the finishing rolling device in the conveying direction of the steel material and that removes scale from the steel material using cooling water.
3. A hot rolling facility as described in claim 1 or claim 2, comprising: among the multiple rolling mills in the rough rolling device, a rolling mill that is located upstream of the removal device in the transport direction of the steel material and adjacent to the removal device; and a pre-removal descaling device that is provided between the removal device and removes scales from the steel material using cooling water.
4. A hot rolling facility according to any one of claims 1 to 3, wherein the removal device is provided between one of the plurality of rolling mills in the rough rolling device and another rolling mill adjacent to the one rolling mill.
5. The hot rolling facility according to claim 4, wherein the removal device is provided behind a rolling mill that is located most upstream of the plurality of rolling mills in the rough rolling device in the conveying direction of the steel material.
6. A hot rolling facility according to any one of claims 1 to 3, wherein the removal device is provided downstream of the rough rolling device and upstream of the finish rolling device in the transport direction of the steel material.
7. The hot rolling facility according to any one of claims 1 to 6, wherein the removal device removes the target area from the steel material by dry cutting, or removes the target area from the steel material by mechanical removal.
8. The hot rolling facility according to any one of claims 1 to 7, wherein the heating furnace is provided separately from a production line of a casting machine that casts the steel material.
9. The hot rolling facility according to any one of claims 1 to 7, wherein the heating furnace is provided on a production line of a casting machine that casts the steel material.
10. A hot rolling method for hot rolling a steel material containing Cu, comprising: a heating step for heating the steel material after casting to a predetermined temperature; a rough rolling step for performing rough rolling multiple times on the steel material heated in the heating step; a finish rolling step for performing finish rolling on the steel material rough rolled in the rough rolling step; and a removal step for removing a target area that is present on the surface side of the steel material during or after the rough rolling and includes cracks caused by a Cu-enriched layer having a higher concentration of Cu component than in the base material of the steel material, wherein the removal step is performed after a first rough rolling of the multiple rough rolling steps and before the finish rolling step.
11. The hot rolling method according to claim 10, further comprising a post-removal descaling step of removing scale from the steel material using cooling water after the removing step and before the finish rolling step.
12. The hot rolling method according to claim 10 or 11, further comprising a pre-removal descaling step of removing scale from the steel material using cooling water after a rolling step immediately preceding the removing step among the multiple rough rolling steps and before the removing step.
13. A hot rolling method according to any one of claims 10 to 12, wherein the removing step is carried out when the surface temperature of the steel material during or after the rough rolling is 1000°C or lower.
14. A hot rolling method according to any one of claims 10 to 13, wherein, in the removing step, when the removal of the target area is carried out by laser cutting, the conveying speed of the steel material during or after the rough rolling is 20 m / min or more.
15. A hot rolling method according to any one of claims 10 to 14, wherein the target area is an area of 1 mm or less in a thickness direction from a surface of the steel material being rough rolled or having been rough rolled.
Citation Information
Patent Citations
Method for preventing hot crack of cu-and sn-containing steel
JP1994297026A
Production of hot rolled steel sheet excellent in workability
JP1995242938A
Cu-CONTAINING STEEL
JP2005029886A
Heteroaromatic and heterobicyclic aromatic derivatives for the treatment of ferroptosis-associated disorders
JP2023054365A
Hot rolling container steel without punctiform surface defect and manufacturing method thereof
CN102644031A
Cited By
Preparation method of high-weather-resistance refined steel anti-corrosion steel-plastic plate
CN121019100A
Preparation method of high-weather-resistance fine steel anticorrosion steel-plastic plate
CN121019100B