Electrostatic chuck device
The electrostatic chuck device addresses abnormal discharge near gas holes by using a gas hole member with specific resistivity and micropores, ensuring reliable semiconductor processing.
Patent Information
- Application Number
- PCT/JP2024/013090
- Authority / Receiving Office
- WO · WO
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2023-03-30
- Filing Date
- 2024-03-29
- Publication Date
- 2024-10-03
AI Technical Summary
In semiconductor manufacturing, electrostatic chuck devices face challenges in suppressing abnormal discharge near gas holes, which can lead to damage of semiconductor wafers, especially with the increasing power of plasma etching equipment for deep hole processing.
The electrostatic chuck device incorporates a gas hole member with a volume resistivity of 1.0×10³ Ω·cm or more, made from a composite material of insulating and conductive materials, and having micropores with diameters between 0.03 mm and 0.15 mm, to prevent abnormal discharge by maintaining equal potential across the gas hole member.
This configuration effectively suppresses abnormal discharge near the gas holes, ensuring the reliability and integrity of the electrostatic chuck device during semiconductor processing.
Smart Images

Figure JP2024013090_03102024_PF_FP_ABST
Abstract
Description
Electrostatic Chuck Device
[0001] This application claims priority to Japanese Patent Application No. 2023-055653, filed on March 30, 2023, the contents of which are incorporated herein by reference.
[0002] Electrostatic chuck devices are used in semiconductor manufacturing processes to hold semiconductor wafers in a vacuum environment. In the electrostatic chuck device, a plate-shaped sample, such as a semiconductor wafer, is placed on a mounting surface, and electrostatic force is generated between the plate-shaped sample and an internal electrode to attract and fix the plate-shaped sample. Furthermore, some electrostatic chuck devices are provided with through-holes for supplying gas to the mounting surface to cool the mounted semiconductor wafer (see, for example, Patent Document 1). In the following description, the "through-holes for supplying gas to the mounting surface" will be referred to as "gas holes."
[0003] The gas supply through-holes may become the starting point of discharges that can lead to damage to the semiconductor wafer. To suppress such discharges, Patent Document 2 proposes installing a gas plug containing silicon carbide as a main component in the gas hole.
[0004] JP 2017-157726 A International Publication No. 2020 / 203680
[0005] In recent years, plasma etching equipment for semiconductor manufacturing has become increasingly powerful in order to process deep holes in response to the increasing number of stacked devices such as DRAMs and 3D-NANDs. This has created a need for methods to suppress abnormal discharges that occur near gas holes.
[0006] The present invention has been made in view of the above circumstances, and has an object to provide an electrostatic chuck device that can suppress abnormal discharge near the gas holes.
[0007] In order to solve the above problems, one aspect of the present invention includes the following aspects.
[0008] [1] An electrostatic chuck plate including a dielectric substrate having a mounting surface on which a sample is mounted, and an electrostatic chuck plate having an attraction electrode located inside the dielectric substrate, and a base supporting the electrostatic chuck plate from the opposite side of the mounting surface, wherein the electrostatic chuck plate has a gas hole penetrating in a thickness direction of the electrostatic chuck plate, and the gas hole is provided with a gas hole member through which a gas for cooling the sample passes, and the volume resistivity of the material of the gas hole member is 1.0×10 3 Ω・cm or more 1.0×10 10 An electrostatic chuck device having a resistance of Ω·cm or less.
[0009] [2] The electrostatic chuck device according to [1], wherein the material of the gas hole member is a composite material of an insulating material and a conductive material.
[0010] [3] The electrostatic chuck device according to [2], wherein the dielectric substrate and the gas hole member are made of the same material.
[0011] [4] The electrostatic chuck device according to any one of [1] to [3], wherein the gas hole member is a porous body.
[0012] [5] An electrostatic chuck device according to any one of [1] to [4], wherein the gas hole member has one or more micropores that penetrate in the thickness direction and have a diameter of 0.03 mm or more and 0.15 mm or less.
[0013] [6] An electrostatic chuck plate including a dielectric substrate having a mounting surface on which a sample is mounted, and an electrostatic chuck plate having an attraction electrode located inside the dielectric substrate, and a base supporting the electrostatic chuck plate from the opposite side of the mounting surface, wherein the electrostatic chuck plate has a gas hole penetrating through the electrostatic chuck plate in a thickness direction, the dielectric substrate has a gas hole forming portion at a position overlapping with the gas hole in a plan view, the gas hole including a recess provided in a surface of the gas hole forming portion opposite to the mounting surface, and a microhole opening from the mounting surface to the recess, the diameter of the microhole being 0.03 mm or more and 0.15 mm or less, and the volume resistivity of a material of the gas hole forming portion being 1.0×10 3 Ω・cm or more 1.0×10 10 An electrostatic chuck device having a resistance of Ω·cm or less.
[0014] [7] The electrostatic chuck device according to [6], wherein the dielectric substrate and the gas hole forming portion are made of the same material.
[0015] According to the present invention, it is possible to provide an electrostatic chuck device capable of suppressing abnormal discharge near the gas holes.
[0016] Fig. 1 is a schematic cross-sectional view showing an example of an electrostatic chuck device 1A. Fig. 2 is a schematic cross-sectional view showing an example of an electrostatic chuck device 1B. Fig. 3 is a process diagram showing a method for manufacturing the electrostatic chuck device 1B. Fig. 4 is a process diagram showing a method for manufacturing the electrostatic chuck device 1B. Fig. 5 is a process diagram showing a method for manufacturing the electrostatic chuck device 1B. Fig. 6 is an explanatory diagram of an electrostatic chuck plate 2C.
[0017] Hereinafter, preferred examples of each embodiment of the electrostatic chuck device of the present invention will be described with reference to the drawings. In all of the following drawings, the dimensions and proportions of each component may be displayed differently as appropriate to make the drawings easier to understand.
[0018] Furthermore, the present embodiment is specifically described to provide a better understanding of the gist of the invention, and does not limit the present invention unless otherwise specified. For example, unless otherwise specified, conditions such as materials, amounts, types, numbers, sizes, shapes, ratios, and temperatures may be changed, added, or omitted as necessary. Preferred examples may be exchanged or shared among the embodiments described below.
[0019] 1 is a schematic cross-sectional view showing an electrostatic chuck device 1A according to a first embodiment. The electrostatic chuck device 1A includes an electrostatic chuck plate 2A having a mounting surface 2s on which a sample (wafer W) is mounted, and a base 3 that supports the electrostatic chuck plate 2A from the side opposite the mounting surface 2s (the back surface 2p side). A focus ring that surrounds the wafer W may be disposed on the outer periphery of the upper surface of the electrostatic chuck plate 2A. Each component will be described below in order.
[0020] <Electrostatic Chuck Plate> The electrostatic chuck plate 2A includes a dielectric substrate 11 and an attraction electrode 13 located inside the dielectric substrate 11. The electrostatic chuck plate 2A attracts the wafer W onto a mounting surface 2s of the dielectric substrate 11.
[0021] In the following description, each part of the electrostatic chuck device 1A will be described with the side of the electrostatic chuck plate 2A on which the wafer W is mounted as the upper side and the side facing the base 3 as the lower side. That is, the thickness direction of the electrostatic chuck plate 2A is the up-down direction. Note that the up-down direction here is used merely for the sake of simplicity of description and does not limit the orientation of the electrostatic chuck device 1A during use.
[0022] (Dielectric Substrate) The dielectric substrate 11 has a circular plate shape in a plan view. In this embodiment, "plan view" refers to the thickness direction of the electrostatic chuck device 1A, i.e., the field of view seen from above. The dielectric substrate 11 has a mounting surface 2s on which the wafer W is mounted and a back surface 2p facing the opposite side to the mounting surface 2s. For example, a plurality of protrusions (not shown) are formed at predetermined intervals on the mounting surface 2s. The mounting surface 2s supports the wafer W at the tips of the plurality of protrusions.
[0023] The dielectric substrate 11 is made of a sintered body having sufficient mechanical strength and durability against corrosive gases and their plasma. As a dielectric material for the dielectric substrate 11, ceramics having sufficient mechanical strength and durability against corrosive gases and their plasma are preferably used.
[0024] The ceramics constituting the dielectric substrate 11 include, for example, aluminum oxide (Al 2 O 3 Insulating materials such as aluminum oxide (Al) sintered bodies, aluminum nitride (AlN) sintered bodies, and insulating materials such as aluminum oxide (Al 2 O 3 ) and silicon carbide (SiC), a conductive material, are sintered into a composite material (composite material). 2 O 3 In particular, from the viewpoint of dielectric properties at high temperatures, high corrosion resistance, plasma resistance, and heat resistance, the material constituting the dielectric substrate 11 is preferably Al.2 O 3 The volume resistivity of the material of the dielectric substrate 11 can be selected arbitrarily, but is preferably 1.0×10 13 It is preferable that the volume resistivity is 10 Ω·cm or more. 13 If the dielectric material has a volume resistivity of Ω·cm or more, when a voltage is applied to the dielectric material, a charge that exerts an adsorption force is generated on the surface, and the dielectric material functions as a Coulomb-type electrostatic chuck device. 17 Ω cm or less, 16 Ω cm or less, 15 It may be Ω·cm or less.
[0025] (Chuck Electrode) The chucking electrode 13 is disposed inside the dielectric substrate 11. The chucking electrode 13 extends in a plate shape along the mounting surface 2 s of the dielectric substrate 11. When a voltage is applied to the chucking electrode 13, it generates an electrostatic chucking force that holds the wafer W on the mounting surface 2 s of the dielectric substrate 11.
[0026] The chucking electrode 13 is made of a composite of an insulating material and a conductive material. The insulating material contained in the chucking electrode 13 is not particularly limited, but may be, for example, aluminum oxide (Al 2 O 3 ), aluminum nitride (AlN), silicon nitride (Si 3 N 4 ), yttrium (III) oxide (Y 2 O 3 ), yttrium aluminum garnet (YAG) and SmAlO 3 The conductive material contained in the attraction electrode 13 is preferably at least one selected from the group consisting of molybdenum carbide (Mo 2 It is preferable that the material is at least one selected from the group consisting of molybdenum (Mo), tungsten carbide (WC), tungsten (W), tantalum carbide (TaC), tantalum (Ta), silicon carbide (SiC), carbon black, carbon nanotubes, and carbon nanofibers.
[0027] The thickness of the electrostatic chuck plate 2A can be selected arbitrarily, but is preferably 0.5 mm or more and 6 mm or less. For example, it may be 1.0 mm or more and 5.5 mm or less, 1.5 mm or more and 5.0 mm or less, or 2.0 mm or more and 4.0 mm or less. When the thickness of the electrostatic chuck plate 2A is 0.5 mm or more, the withstand voltage of the electrostatic chuck plate 2A is high. Furthermore, when the thickness of the electrostatic chuck plate 2A is 6 mm or less, the heat capacity of the electrostatic chuck plate 2A is small, making it easier to maintain a uniform temperature of the plate-shaped sample being processed during plasma processing.
[0028] <<Base>> The base 3 supports the electrostatic chuck plate 2A from below. The base 3 has a support surface 3a facing upward and a lower surface 3b facing the opposite side to the support surface 3a. The support surface 3a faces the back surface 2p of the dielectric substrate 11 in the vertical direction. The support surface 3a is in contact with the back surface 2p. That is, the base 3 supports the back surface 2p of the dielectric substrate 11 on the support surface 3a.
[0029] The base 3 is a disk-shaped member in a plan view. The material constituting the base 3 is not particularly limited as long as it is a metal having excellent thermal conductivity, electrical conductivity, and processability, or a composite material containing such a metal, or a conductive ceramic, or a composite material of metal and ceramic (MMC: Metal Matrix Composition). Suitable materials for the base 3 include, for example, alloys containing aluminum (Al), copper (Cu), stainless steel (SUS), titanium (Ti), etc., and conductive ceramics. From the viewpoints of thermal conductivity, electrical conductivity, and processability, the material constituting the base 3 is preferably an aluminum alloy.
[0030] Of the surfaces of the base 3, the surface exposed to plasma is preferably anodized or resin-coated with a polyimide resin. It is more preferable that the entire surface of the base 3 is anodized or resin-coated. By anodizing or resin-coating the base 3, the plasma resistance of the base 3 is improved and abnormal discharge on the surface of the base 3 is suppressed. Therefore, the plasma resistance stability of the base 3 is improved and the occurrence of surface scratches on the base 3 can be prevented.
[0031] A flow path for circulating a coolant may be provided inside the base 3. The coolant flowing through the flow path may be water, He gas, N 2 A gas or the like is used. The flow path may be configured to extend along the support surface 3a. The coolant in the flow path cools the entire base 3 and also cools the electrostatic chuck plate 2A via the support surface 3a. The body of the base 3 also functions as an internal electrode for generating plasma. The body of the base 3 is connected to an external high-frequency power source 22 via a matching box (not shown).
[0032] The base 3 is fixed to the electrostatic chuck plate 2A by an adhesive. That is, an adhesive layer 55 that bonds the electrostatic chuck plate 2A and the base 3 to each other is provided between the electrostatic chuck plate 2A and the base 3. The adhesive layer 55 is interposed between the back surface 2p of the electrostatic chuck plate 2A and the support surface 3a of the base 3, and bonds and integrates the electrostatic chuck plate 2A and the base 3. A heater that heats the electrostatic chuck plate 2A may be embedded inside the adhesive layer 55.
[0033] The adhesive used for the adhesive layer 55 preferably has heat resistance in the temperature range of -20°C to 150°C, and suitable examples include acrylic resins, silicone resins, and epoxy resins.
[0034] The electrostatic chuck plate 2A and the base 3, which are integrated by the adhesive layer 55, are provided with a terminal through-hole 17 that penetrates through a portion of the base 3 and the dielectric substrate 11 in the thickness direction. A power supply terminal 16 for applying a DC voltage to the chucking electrode 13 is inserted into the terminal through-hole 17 and is electrically connected to the chucking electrode 13. An insulating terminal insulator 23 is provided on the outer periphery of the power supply terminal 16. The terminal insulator 23 receives the power supply terminal 16 in a through-hole 15 provided in the terminal insulator 23, thereby insulating the base 3 from the power supply terminal 16.
[0035] The power supply terminal 16 is connected to an external power source 21. The power source 21 applies a voltage to the chucking electrode 13. The number, shape, etc. of the power supply terminals 16 are determined depending on the type of the chucking electrode 13, i.e., whether it is a monopolar type or a bipolar type.
[0036] <Gas Holes and Gas Hole Members> The electrostatic chuck plate 2A, the base 3, and the adhesive layer 55 are provided with a plurality of gas holes 30A that vertically penetrate these. The number and positions of the gas holes 30A can be selected arbitrarily. A gas hole member 40 is provided at the end of the gas hole 30A on the mounting surface 2s side. The gas holes 30A are connected to a gas supply device (not shown). The gas holes 30A are provided to supply a sample-cooling gas G, such as helium (He), to the mounting surface 2s of the electrostatic chuck plate 2A to cool the wafer W mounted on the mounting surface 2s.
[0037] (Gas Hole) The gas hole 30A has a first through hole 31 that penetrates the electrostatic chuck plate 2A and a second through hole 32 that penetrates the base 3. That is, the electrostatic chuck plate 2A is provided with the first through hole 31, and the base 3 is provided with the second through hole 32. The first through hole 31 and the second through hole 32 have the same central axis. The first through hole 31 and the second through hole 32 are connected to each other. The shape (internal shape) of the first through hole 31 may be a straight shape (e.g., cylindrical or truncated cone) having a smooth inner surface without any internal steps, or may have one or more steps and / or one or more inclined surfaces. The first through hole 31 may have a circular shape in a plan view. The first through hole 31 may have one or more vertical surfaces (curved surfaces), one or more steps, and / or one or more inclined surfaces on its inner surface. The inner diameter and the lateral cross-sectional shape of the first through hole 31 may be constant, or one or both may change continuously and / or stepwise in the thickness direction. For example, the inner diameter of the first through hole 31 may decrease or increase gradually or stepwise in the thickness direction, or any combination thereof may be used. The number of steps and the angle of the steps can be selected arbitrarily. For example, the number may be 1 to 10, 2 to 8, or 3 to 6, and the angle may be 10 to 150 degrees, 30 to 90 degrees, or 45 to 60 degrees. The inner shape of the first through hole 31 may match the outer shape of the gas hole member or gas hole forming portion described below.
[0038] The first through hole 31 penetrates the dielectric substrate 11 of the electrostatic chuck plate 2A in the thickness direction. In addition, a retraction hole 13h is provided between the chucking electrode 13 of the electrostatic chuck plate 2A and the first through hole 31, surrounding the periphery of the first through hole 31. A part of the dielectric substrate 11 is disposed inside the retraction hole 13h. Therefore, the chucking electrode 13 is not exposed from the inner circumferential surface of the first through hole 31.
[0039] The second through hole 32 is connected to the first through hole 31. A cylindrical insulator 24 may be inserted into the second through hole 32. The outer peripheral surface of the insulator 24 is fixed to the second through hole 32 by, for example, an adhesive. The inside of the insulator 24 functions as a passage for the gas G.
[0040] The insulator 24 is made of, for example, ceramic. That is, the insulator 24 is made of an insulating material. The insulator 24 has durability against plasma. Examples of ceramics that make up the insulator 24 include AlN, Al 2 O 3 , Si 3 N 4 , ZrO 2 , sialon, and boron nitride (BN).
[0041] (Gas hole member) The gas hole member 40 fits into the first through hole 31 and is in close contact with the inner wall of the first through hole 31. The shape of the gas hole member 40 is complementary to the shape of the first through hole 31. For example, if the first through hole 31 is circular in a plan view and has a uniform cross-sectional shape extending in the vertical direction, the gas hole member 40 has a cylindrical shape extending in the vertical direction.
[0042] 1 shows that the height of the gas hole member 40 is the same as the vertical length of the first through-hole 31, but this is not limited to this. The gas hole member 40 may be shorter than the vertical length of the first through-hole 31. In this case, the upper end of the gas hole member 40 is the same as the upper end of the first through-hole 31 and is at the same height as the mounting surface 2s.
[0043] The gas hole member 40 allows the gas G flowing through the gas holes 30A to pass through. The structure of the gas hole member 40 for allowing the gas G to pass through is not particularly limited.
[0044] For example, the gas hole member 40 may be a porous body. When the gas hole member 40 is a porous body, the pores in the porous body are connected to each other and are continuous in the vertical direction of the gas hole member 40, thereby forming a flow path for the gas G in the gas hole member 40.
[0045] The pore diameter of the porous body is not particularly limited as long as it can sufficiently supply the gas G to the mounting surface 2s and suppress abnormal discharge. The pore diameter of the porous body can be selected arbitrarily, and may be, for example, 30 μm to 150 μm, or 50 μm to 100 μm. If the pore diameter of the gas hole member 40 is too small, the gas G cannot be sufficiently supplied to the mounting surface 2s. If the pore diameter is too large, the potential change near the upper end of the first through hole 31 is large, and the generated electric field is also large, which may make it difficult to suppress abnormal discharge.
[0046] The porosity of the porous body is not particularly limited as long as it can supply a sufficient amount of gas G to the mounting surface 2s, and may be, for example, 30% to 70%, 35% to 65%, or 45% to 55%, etc.
[0047] Here, "porosity" refers to the ratio of the total volume of pores to a given unit volume of the porous body. The porosity may be a value determined from the ratio of the true density of the material forming the porous body to the apparent density of the porous body, or may be determined by actually measuring the volume of pores per unit volume. The higher the porosity of a porous body, the more pores there are, and the easier it is for gas G to flow out.
[0048] The gas hole member 40 may also have one or more micropores penetrating in the thickness direction. When the gas hole member 40 has micropores (through holes or parts of through holes), the diameter of the micropores is not particularly limited as long as the gas G can be sufficiently supplied to the mounting surface 2s. The diameter of the micropores can be selected arbitrarily, but is preferably 0.03 mm or more and 0.15 mm or less. For example, it may be 0.05 mm or more and 0.13 mm or less, or 0.07 mm or more and 0.10 mm or less. The diameter of the micropores may be constant in the thickness direction, but may not be constant as necessary.
[0049] The shape (internal shape) of the micropores is not particularly limited as long as the gas G can pass through it, and may be a rectangular parallelepiped, cubic, or cylindrical shape. The shape may be regular or irregular. The micropores may have a polygonal shape such as a circle or a square in a plan view.
[0050] The number of micropores may be adjusted appropriately to a number that satisfies both gas permeability and abnormal discharge suppression. The number of micropores can be selected arbitrarily, for example, 1 to 200, 5 to 180, 10 to 160, or 30 to 100. The micropores can be formed by various methods. For example, micropores may be formed in a molded body that does not have micropores by laser processing or mechanical processing. The gas hole member 40 may also be a porous body having one or more micropores penetrating in the thickness direction.
[0051] The volume resistivity of the material of the gas hole member 40 is 1.0×10 3 Ω・cm or more 1.0×10 10 Ω cm or less, and 1.0 × 10 4 Ω・cm or more 1.0×10 9 It may be Ω cm or less, and may be 1.0 × 10 5 Ω・cm or more 1.0×10 8 It may be Ω cm or less, and may be 1.0 × 10 6 Ω・cm or more 1.0×10 7 It may be Ω·cm or less.
[0052] The volume resistivity of the gas hole member 40 is 1.0×10 3 If the resistivity is less than Ω cm, electricity will flow more easily, which is undesirable because heat generation in the vicinity of the first through holes 31 will increase and the plasma resistance of the gas hole member 40 will tend to decrease. 10 If the electrical resistance exceeds Ω·cm, it is not preferable because there is a tendency that abnormal discharge occurring around the first through-hole 31 cannot be sufficiently suppressed.
[0053] Conventional gas hole members have generally been made of insulating materials, but with the recent trend toward higher power semiconductor manufacturing equipment, it has become difficult to suppress the occurrence of abnormal discharge using insulating gas hole members.
[0054] Therefore, the present inventors conducted various studies using simulations and surprisingly found that in a certain specific case, when the side portion of the gas hole member is conductive, an equipotential is maintained from the top end to the bottom end of the gas hole member even when the electrostatic chuck device is exposed to plasma, that is, the gas hole member does not become a starting point for abnormal discharge. 3 Ω・cm or more 1.0×10 10 The idea was to use materials with a resistivity of Ω·cm or less.
[0055] The method for measuring the volume resistivity of the gas hole member 40 is not particularly limited, but for example, it can be measured by a direct current three-terminal method.
[0056] The material of the gas hole member 40 is preferably a composite of an insulating material and a conductive material. The volume resistivity of such a composite can be adjusted to a desired value by adjusting the types of insulating material and conductive material and the mixing ratio of the insulating material and the conductive material.
[0057] In this specification, "insulating" means a material having a volume resistivity of 1×10 13 An "insulating" material has a volume resistivity of 1 x 10 13 In this specification, "electrically conductive" refers to a material having a volume resistivity of 1×10 13 A material that is "conductive" has a volume resistivity of less than 1 x 10 13 It is a material with a resistivity of less than Ω·cm.
[0058] Since the material of the gas hole member 40 is a composite material of an insulating material and a conductive material, it is easy to adjust the volume resistivity of the gas hole member 40 within a desired range. Therefore, it is possible to easily obtain a gas hole member 40 that can suppress abnormal discharge and has excellent plasma resistance.
[0059] The insulating material contained in the gas hole member 40 is not particularly limited, but may be, for example, Al 2 O 3 , AlN, silicon oxide (SiO 2 ), silicon nitride (Si3 N 4 ), yttrium (III) oxide (Y 2 O 3 ), calcium oxide (CaO), magnesium oxide (MgO), zirconium oxide (ZrO 2 ), yttrium aluminum garnet (YAG) and SmAlO 3 It is preferable that the polymer is at least one selected from the group consisting of:
[0060] The conductive material contained in the gas hole member 40 is molybdenum carbide (Mo 2 It is preferable that the material is at least one selected from the group consisting of silicon carbide (SiC), molybdenum (Mo), tungsten carbide (WC), tungsten (W), tantalum carbide (TaC), tantalum (Ta), SiC, carbon black, carbon nanotubes, and carbon nanofibers.
[0061] The gas hole member 40 is preferably made of the same material as the dielectric substrate 11. "Made of the same material" may mean that it is manufactured from the same material, or that it is formed using the same raw material (material). The material may be a composite or a mixture. The materials contained in the composite or mixture may be different in ratio (mixing ratio), shape, and / or size. The gas hole member 40 is made of Al 2 O 3 It is preferable to use SiC. 2 O 3 The gas hole member 40 made of -SiC can suppress abnormal discharge and has excellent plasma resistance.
[0062] The size of the gas hole member 40 is not particularly limited as long as it can be provided in the first through-hole 31. For example, the diameter of the gas hole member 40 may be 0.5 mm or more and 2.5 mm or less, 1.0 mm or more and 2.2 mm or less, or 1.5 mm or more and 2.0 mm or less. The thickness of the gas hole member 40 can be selected arbitrarily and may be, for example, 0.1 mm or more and 10 mm or less, 0.5 mm or more and 6 mm or less, or 1 mm or more and 5 mm or less. The thickness of the gas hole member 40 can be selected as needed and may be 5 to 100%, 10 to 90%, 20 to 80%, or 30 to 70% of the thickness of the dielectric substrate 11.
[0063] The gas hole member 40 can be manufactured, for example, by the following method.
[0064] First, the above-mentioned insulating material and conductive material are mixed with a binder, a dispersant, a solvent, etc. as appropriate to prepare a slurry.
[0065] Next, a pore opening agent is further added to the resulting slurry.
[0066] Next, the slurry containing the pore-opening agent is placed in a mold of the desired shape and fired to obtain the gas hole member 40. The pore-opening agents come into contact with each other as the slurry dries and then disappear during firing. As a result, in the resulting gas hole member 40, continuous pores are formed in the vertical direction of the gas hole member 40 at the positions where the pore-opening agent was present. The amount of pore-opening agent is the amount that will form pores that communicate with each other in the resulting gas hole member 40. It is recommended that the specific amount used be confirmed in advance through a preliminary experiment.
[0067] Alternatively, the obtained slurry may be impregnated into a mold made of a porous material such as urethane sponge, temporarily dried to remove excess slurry, and then fired to obtain the gas hole member 40. Further processing may be performed after firing as necessary. The slurry may or may not contain a pore-opening agent.
[0068] The mold of the porous member disappears during firing, and as a result, continuous pores are formed in the vertical direction of the gas hole member 40 at the positions where the mold agent of the porous member was present.
[0069] Alternatively, a photosensitive material such as a photocurable resin can be further added to the slurry, and the resulting photosensitive material-containing slurry can be molded into a desired shape using a stereolithography device to form a temporary molded body, which can then be fired to obtain the gas hole member 40. The photosensitive material disappears during firing. By forming a plurality of through holes in the temporary molded body during stereolithography, micropores that penetrate the gas hole member 40 can be formed in the resulting gas hole member 40 at positions corresponding to the through holes.
[0070] The through-holes formed by stereolithography may pass straight through the temporary molded body, or may be curved or bent inside the temporary molded body.
[0071] Furthermore, a pore-forming agent may also be added to the slurry containing the photosensitive material to form pores in the resulting gas hole member.
[0072] The gas hole member 40 thus manufactured may have micropores formed therein by laser processing or machining.
[0073] Alternatively, the slurry may be formed into any shape, for example, a cylindrical shape, and fired. Micropores may be formed in the resulting cylindrical sintered body by laser processing or mechanical processing, thereby forming the gas hole member 40. That is, the gas hole member 40 may be formed without using a pore-opening agent, a porous member mold, or a photosensitive material. The micropores may penetrate the cylindrical sintered body from top to bottom. Alternatively, the sintered body may further have recesses. For example, recesses 33 and micropores 39 as shown in FIG. 2 may be formed in the resulting cylindrical sintered body. The shape of the recesses can be selected arbitrarily, and may be, for example, a cylindrical, prismatic, or other valley portion.
[0074] The gas hole member 40, in which the gas hole is formed before being fitted into the first through hole, can be inserted or press-fitted into the first through hole 31 provided in the dielectric substrate 11 and fired as necessary to be fixed in the gas hole. The firing temperature can be selected arbitrarily, for example, 1600 to 1850 degrees Celsius. The firing may be performed under pressure in the range of 1 to 50 MPa, for example. When inserting or press-fitting the gas hole member 40 into the first through hole 31, an adhesive may be applied in advance to at least a portion of the side or bottom surface of the gas hole member 40 before inserting or press-fitting.
[0075] In the electrostatic chuck device 1A as described above, the first through-holes 31 are blocked by the gas hole member 40. The gas hole member 40 has a volume resistivity of 1.0×10 3 Ω・cm or more 1.0×10 10 Since the resistance is Ω·cm or less, abnormal discharge of the electrostatic chuck device 1A is suppressed, thereby making it possible to provide a highly reliable electrostatic chuck device 1A.
[0076] 2 to 5 are explanatory views showing an example of an electrostatic chuck device 1B according to a second embodiment and a manufacturing method thereof. The electrostatic chuck device 1B of this embodiment differs from the electrostatic chuck device 1A of the first embodiment in the configuration of part of the electrostatic chuck plate and / or the manufacturing method thereof, but shares other configurations with the electrostatic chuck device 1A. Therefore, the following mainly describes the electrostatic chuck plate 2B, and a description of the configuration and conditions common to the electrostatic chuck device 1A will be omitted.
[0077] 2 is a schematic cross-sectional view of the electrostatic chuck device 1B. As shown in Fig. 2, the electrostatic chuck plate 2B of the electrostatic chuck device 1B has a dielectric substrate 11 and an attraction electrode 13 located inside the dielectric substrate 11. The electrostatic chuck plate 2B attracts the wafer W onto a mounting surface 2s of the dielectric substrate 11.
[0078] A plurality of gas holes 30B are provided in the electrostatic chuck plate 2B, the base 3, and the adhesive layer 50, penetrating them vertically. The gas holes 30B are configured by connecting the recesses 33 and the micropores 39 provided in the electrostatic chuck plate 2B with the second through holes 32 provided in the base 3. The gas holes 30B are connected to a gas supply device (not shown).
[0079] The recess 33 is provided in a gas hole forming portion 45 set in the dielectric substrate 11 of the electrostatic chuck plate 2B. The gas hole forming portion 45 is a part of the dielectric substrate 11. The gas hole forming portion 45 may be formed integrally with the dielectric substrate 11. In a plan view, the gas hole forming portion 45 overlaps with the gas hole 30B. Note that examples of the shape, size, and material of the gas hole forming portion 45, the recess 33, and the micropores 39 may be the same as those shown in the example of the gas hole member 40. The gas hole forming portion 45 may include the gas hole member 40, may be formed only from the gas hole member 40, or may be formed by combining the gas hole member 40 with the dielectric substrate 11. For example, the gas hole forming portion 45 may have an upper portion made of the gas hole member 40 and a lower portion made of a part of the dielectric substrate having a recess. In the electrostatic chuck plate 2B, the gas hole forming portion 45 may refer to a portion overlapping with the gas hole member 40 in a plan view, but is not limited to this example. For example, when the diameter of the recess 33 is smaller than the diameter of the gas hole member 40, the gas hole forming portion 45 may refer to the portion that overlaps with the gas hole member 40 in a plan view. When the diameter of the recess 33 is larger than the diameter of the gas hole member 40, the gas hole forming portion 45 may refer to the portion that overlaps with the recess 33 in a plan view.
[0080] The material of the gas hole forming portion 45 may be the same as or different from the material of the dielectric substrate 11. The dielectric substrate 11 and the gas hole forming portion 45 may be made of the same material, but the ratio of materials (raw materials), shape, and / or size may be different. The volume resistivity of the material of the gas hole forming portion 45 may be in the same numerical range as that of the gas hole member 40 described above. The vertical length of the gas hole forming portion 45 is preferably the same as the thickness of the dielectric substrate 11, but may be shorter than the thickness of the dielectric substrate 11 if necessary. When the gas hole member 40 is included, if the vertical length of the gas hole member 40 is shorter than the thickness of the dielectric substrate 11, the upper end of the gas hole forming portion 45 is aligned with the upper end of the first through hole 31 and is at the same height as the mounting surface 2s.
[0081] The recess 33 is formed from the rear surface 2p of the dielectric substrate 11 toward the mounting surface 2s. The recess 33 does not penetrate the dielectric substrate 11.
[0082] The width (inner diameter) of the recess 33 may be the same as, narrower than, or wider than the widths of the gas hole forming portion 45 and the gas hole member 40. The inner wall of the recess 33 is formed from the material of the gas hole forming portion 45 or the dielectric substrate 11. For example, the recess 33 may be formed only in the gas hole member 40, or only in the dielectric substrate other than the gas hole member, or may be formed continuously in both the gas hole member and the dielectric substrate.
[0083] The fine holes 39 penetrate the gas hole forming portion 45 in the thickness direction and open into the recess 33. The gas hole forming portion 45 in which the fine holes 39 are formed performs the same function as the gas hole member 40 described above.
[0084] 3 to 5 are process diagrams showing an example of a method for manufacturing the electrostatic chuck device 1B and an example of a method for manufacturing the electrostatic chuck plate 2B.
[0085] First, as shown in FIG. 3, a dielectric substrate 11 was filled with a through-hole 11x having a volume resistivity of 1.0×10 3 Ω・cm or more 1.0×10 10A material with a resistivity of Ω·cm or less is placed in the through-hole 11x and sintered to form an integrated structure, thereby forming the gas hole forming portion 451. The material to be sintered can be the same as the material of the gas hole member 40 described above, for example, a composite material of an insulating material and a conductive material. The sintering temperature can be selected arbitrarily from temperatures that allow integration by sintering, and examples include 1600°C to 1850°C. The firing may be performed under pressure in the range of 1 MPa to 50 MPa, for example. Note that the through-hole 11x provided at the position overlapping the gas hole has a volume resistivity of 1.0×10 3 Ω・cm or more 1.0×10 10 A dielectric substrate 11 containing a material with a resistivity of Ω·cm or less and a dielectric substrate 11 without a through hole 11x may be stacked, sintered, and integrated, and the gas hole forming portion 451 may be formed only on the mounting surface 2s side.
[0086] 4, the gas hole forming portion 451 is countersunk from the rear surface 2p toward the mounting surface 2s to form the gas hole forming portion 452 having the recess 33. The depth of the recess 33 is arbitrary and may be, for example, 10 to 30%, 30 to 50%, 50 to 70%, or 70 to 90% of the thickness of the dielectric substrate 11.
[0087] Next, the dielectric substrate 11 is bonded to a base (not shown) (see FIG. 2), and the mounting surface 2s is subjected to surface grinding. Thereafter, one or more micropores 39 are formed therein, as shown in FIG. 5. This results in an electrostatic chuck plate 2B having a gas hole forming portion 45 and an electrostatic chuck device 1B having the electrostatic chuck plate 2B. Note that the order of the above steps may be changed as necessary.
[0088] For example, bonding to the base may be performed after the micropores 39 are formed. Specifically, after the mounting surface 2s of the dielectric substrate 11 is subjected to flat grinding, one or more micropores 39 communicating with the recess 33 are formed therein, as shown in Fig. 5, to obtain the electrostatic chuck plate 2B. Next, the electrostatic chuck plate 2B is bonded to a base (not shown) (see Fig. 2) to obtain an electrostatic chuck device 1B having the electrostatic chuck plate 2B.
[0089] As in the electrostatic chuck plate 2C shown in FIG. 6, a member similar to the gas hole member 40 of the first embodiment may be machined and fitted into the recess 33 as necessary.
[0090] Even with the electrostatic chuck device 1B configured as described above, abnormal discharge can be suppressed, and the electrostatic chuck device can be made highly reliable.
[0091] Although various embodiments of the present invention have been described above, the configurations and combinations thereof in each embodiment are merely examples, and additions, omissions, substitutions, and other modifications of the configurations are possible without departing from the spirit of the present invention. Furthermore, the present invention is not limited to the embodiments.
[0092] The present invention will be described in more detail below with reference to examples and comparative examples, but the present invention is not limited to the following examples. In the following examples, the symbols used in the above-mentioned embodiments will be used as appropriate for explanation.
[0093] [Example 1] "Preparation of slurry" As starting materials, silicon carbide (SiC) particles having an average particle size of 0.03 μm and aluminum oxide (Al) particles having an average particle size of 0.1 μm were mixed. 2 O 3 ) particles were used.
[0094] SiC particles and Al 2 O 3 The SiC particles were weighed so that the SiC particles accounted for 18 mass% of the total amount of the particles. Next, the particles were placed in distilled water containing a polycarboxylic acid-based dispersant. 2 O 3 The dispersion liquid containing the SiC particles is dispersed using an ultrasonic dispersion device, and then crushed and mixed using a two-flow particle collision type crushing and mixing device. 2 O 3 A particle-containing slurry was obtained.
[0095] "Preparation of gas hole member" The obtained slurry was impregnated into a urethane sponge (a mold for forming a porous member) and dried. The obtained dried body was then fired at 1800°C for 48 hours in an Ar atmosphere to obtain a molded body. The urethane sponge portion disappeared due to firing. The obtained molded body was ground to obtain the gas hole member of Example 1.
[0096] "Evaluation of gas hole member" (measurement of volume resistivity) A test piece with a diameter of 28 mm and a thickness of 1 mm was obtained from the obtained molded body, and the resistivity of the gas hole member of Example 1 was measured using the test piece by the DC three-terminal method using a resistivity measuring device and a digital ultra-high resistance / microcurrent meter (model 5450, manufactured by ADC Corporation). The main electrode, counter electrode, and guard electrode were formed by screen-printing silver paste (US-202A, manufactured by Daiken Chemical Manufacturing and Sales Co., Ltd.) on the upper and lower surfaces of the test piece using a screen printer (manufactured by Mitani Micronics, MODEL MEC-2400) and drying in air at 150 ° C. for 12 hours. The diameter of the main electrode was 1.45 cm, and the inner diameter of the guard electrode was 1.60 cm.
[0097] The measurement was carried out at room temperature (24°C) in the atmosphere by applying a DC voltage of 100 V and measuring the current after charging for 1 minute to determine the volume resistance (Rv) of the test piece. Next, the volume resistivity (ρv) was calculated using the thickness of the test piece and the electrode area according to the following formula (1): ρv = S / t × Rv = S / t × V / I ... (1) (S: effective area of the electrode (cm2), t: thickness of the sintered body (cm), Rv: volume resistance (Ω), V: DC voltage (V), I: current (A)). As a result, the volume resistivity of the test piece, i.e., the gas hole member of Example 1, was 1.1 × 10 5 The value was Ω·cm.
[0098] "Fabrication of Electrostatic Chuck Device" In an electrostatic chuck device having the configuration shown in FIG. 1, the gas hole member of Example 1 was inserted into the first through hole 31 to obtain the electrostatic chuck device of Example 1.
[0099] (Discharge Test) The electrostatic chuck device 1 of Example 1 was operated, and plasma was applied to the semiconductor wafer while the semiconductor wafer was attracted to the electrostatic chuck device 1. As a result, no discharge marks or the like were found on the semiconductor wafer. In other words, no abnormal discharge was observed, and it was confirmed that discharge was suppressed.
[0100] [Example 2] A gas hole member, a dielectric substrate, and an electrostatic chuck plate and an electrostatic chuck device using these were manufactured by the following method. "Manufacturing of gas hole member" The slurry obtained in Example 1 was spray-dried using a spray dryer to separate SiC and Al. 2 O 3 The obtained mixed particles were subjected to uniaxial press molding at a pressure of 8 MPa to obtain a molded body having a diameter of 320 mm and a thickness of 15 mm.
[0101] The obtained molded body was then heat-treated in a nitrogen atmosphere by raising the temperature to 385°C at a temperature increase rate of 0.5°C / min without applying pressure, to remove moisture and dispersant (impurities) contained in the molded body.
[0102] The obtained compact was set in a graphite mold and subjected to pressure sintering. Specifically, the compact was heated to 1100°C under a vacuum atmosphere at a pressing pressure of 5 MPa, and then heated to 1800°C under an argon atmosphere at a pressing pressure of 40 MPa to obtain a sintered body.
[0103] A portion of the obtained sintered body was ground to prepare 15 cylindrical sintered bodies (gas hole members) having a diameter of 1.8 mm and a thickness of 2.8 mm. The volume resistivity of the cylindrical sintered bodies was measured in the same manner as in Example 1. As a result, the volume resistivity of the sintered body of Example 2 was found to be 1.1 × 10 5 The electrical resistance was Ω·cm. Micropores were formed in these sintered bodies by the method described below.
[0104] "Fabrication of Dielectric Substrate" As starting materials, silicon carbide (SiC) particles having an average particle size of 0.03 μm and aluminum oxide (Al) particles having an average particle size of 0.1 μm were used. 2 O 3) particles were used. Aluminum oxide particles and silicon carbide particles were weighed out so that the mass ratio was 95:5, and the mixture was added to distilled water containing a polycarboxylic acid-based dispersant to obtain a mixed solution. This mixed solution was dispersed using an ultrasonic dispersion device. After that, the mixture was pulverized and mixed using a two-stream particle collision type pulverization and mixing device to obtain a slurry. Nitric acid was added to the obtained slurry, and the pH of the slurry was adjusted to 6.5. Next, the slurry with the pH adjusted to 6.5 was spray-dried using a spray dryer to obtain mixed particles containing silicon carbide and aluminum oxide.
[0105] The resulting mixed particles were then uniaxially press-molded at a pressure of 8 MPa to form a molded body having a diameter of 320 mm and a thickness of 15 mm.
[0106] The compact was then heat-treated in a nitrogen atmosphere by raising the temperature to 385° C. at a rate of 0.5° C. / min without applying pressure to remove moisture and dispersant (impurities).
[0107] The obtained compact was set in a graphite mold and subjected to pressure sintering. The sintering conditions were a vacuum atmosphere and a press pressure of 5 MPa up to 1100°C, followed by heating to 1800°C under an argon atmosphere and a press pressure of 40 MPa.
[0108] The obtained sintered body was processed to produce two compacts (compacts A and B) measuring 310 mm in diameter and 3 mm in thickness. Fifteen through-holes, each 2 mm in diameter, were formed at predetermined positions in compact A for inserting gas hole members. The gas hole members of Example 2 were inserted into each of the 15 through-holes.
[0109] In compact B, a through-hole with a diameter of 3 mm was formed in the center. A cylinder of aluminum oxide-tantalum carbide sintered body (tantalum carbide 30% by volume) machined to fit the shape of the through-hole was inserted and fixed into the formed through-hole to form a power supply terminal. Note that compact B did not have a hole for inserting a gas hole member.
[0110] "Fabrication of Adsorption Electrode" Aluminum oxide particles, acicular carbon (0.1 μm in the transverse direction, 2 μm in the longitudinal direction), and screen oil (terephthalic acid) were mixed to prepare a conductive dispersion liquid, in which the acicular carbon accounted for 5% by volume of the total amount of the aluminum oxide particles and the acicular carbon.
[0111] Also, an insulating dispersant was prepared by mixing aluminum oxide with screen oil.
[0112] Using a screen printing device, a conductive dispersion liquid was printed in the shape of a desired adsorption electrode on the surface of the molded body B. Furthermore, on the surface of the molded body B, an insulating dispersant was printed near each of the positions where the recesses 33 of the second embodiment were to be formed and the positions surrounding the printed conductive dispersion liquid.
[0113] The molded body A with the gas hole member inserted was placed on the printed side of the molded body B, and heat was applied using a hot press device to pressure bond them (40 MPa, 1800°C), thereby obtaining an electrostatic chuck plate. In this way, the gas hole member (gas hole forming portion) was formed.
[0114] The obtained electrostatic chuck plate was processed to a thickness of 0.5 mm for compact A, a thickness of 4.0 mm for compact B, and an outer diameter of 293 mm. Next, a recess (corresponding to recess 33 in the second embodiment) having a diameter of 1 mm and a depth of 4 mm was formed by boring the back surface of the electrostatic chuck plate in a region corresponding to the region where the gas hole member was formed. Furthermore, a lift pin insertion hole was formed in the electrostatic chuck plate.
[0115] Both the front surface (the side of molded body A) and the back surface (the side of molded body B) of the electrostatic chuck plate were subjected to surface grinding. Next, a plurality of microholes (corresponding to the microholes 39 in the second embodiment) having a diameter of 0.1 mm were formed in each gas hole member by laser processing from the front surface side of the electrostatic chuck plate. In this manner, an electrostatic chuck plate of Example 2 having gas hole members was obtained.
[0116] The electrostatic chuck plate of Example 2 and an aluminum base were bonded together using a silicone adhesive to obtain an electrostatic chuck device of Example 2. The base had a thermally sprayed aluminum oxide film formed on its top and side surfaces.
[0117] As in Example 1, a discharge test was carried out on the electrostatic chuck device 1 of Example 2. As a result, no discharge marks were found on the wafer, and it was confirmed that abnormal discharge was suppressed.
[0118] An electrostatic chuck plate and an electrostatic chuck device of Example 3 were obtained in the same manner as in Example 2, except that the gas hole member of Example 1 was processed and inserted into the recess of the electrostatic chuck plate of Example 2. Example 3 has a structure similar to that shown in FIG.
[0119] As a result of conducting a discharge test in the same manner as in Example 1, no discharge traces were found on the semiconductor wafer, and it was confirmed that abnormal discharge was suppressed.
[0120] [Comparative Example 1] As a starting material, aluminum oxide (Al 2 O 3 A gas hole member and an electrostatic chuck device of Comparative Example 1 were obtained in the same manner as in Example 1, except that only the ) particles were used.
[0121] The volume resistivity was measured in the same manner as in Example 1. As a result, the volume resistivity of the gas hole member of Comparative Example 1 was 1.0×10 11 It was bigger.
[0122] As a result of conducting a discharge test in the same manner as in Example 1, discharge marks were observed on the semiconductor wafer, and it was confirmed that abnormal discharge was not suppressed.
[0123] Comparative Example 2 A gas hole member and an electrostatic chuck device of Comparative Example 2 were obtained in the same manner as in Example 1, except that only silicon carbide (SiC) particles having an average particle size of 0.03 μm were used as the starting material.
[0124] The volume resistivity was measured in the same manner as in Example 1. As a result, the volume resistivity of the gas hole member of Comparative Example 2 was 1.0×10 3 It was smaller than Ω·cm.
[0125] As a result of carrying out a discharge test in the same manner as in Example 1, it was confirmed that the heat rose near the gas hole member and that the plasma resistance was poor.
[0126] [Comparative Example 3] Al 2 O 3The volume resistivity was adjusted to 1.0 × 10 by changing the mixing ratio of SiC particles and SiC particles. 11 An electrostatic chuck device of Comparative Example 3 was obtained in the same manner as in Example 1, except that the gas hole member had a resistivity of Ω·cm.
[0127] As a result of conducting a discharge test in the same manner as in Example 1, discharge marks were observed on the semiconductor wafer, and it was confirmed that abnormal discharge was not suppressed.
[0128] By comparing Examples 1 to 3 with Comparative Examples 1 to 3, it was found that the volume resistivity was 10 3 Ω・cm or more 10 10 It was confirmed that an electrostatic chuck device having a member with a resistivity of Ω·cm or less in a gas hole can suppress abnormal discharge.
[0129] The present invention provides an electrostatic chuck device capable of suppressing abnormal discharge near a gas hole.
[0130] From the above results, it was confirmed that the present invention is useful.
[0131] DESCRIPTION OF SYMBOLS 1A, 1B... Electrostatic chuck device 2A, 2B, 2C... Electrostatic chuck plate 2s... Mounting surface 2p... Back surface 3... Base 3a... Support surface 3b... Lower surface 11... Dielectric substrate 11x... Lower surface 13... Attraction electrode 13h... Retraction hole 15... Through hole 16... Power supply terminal 17... Terminal through hole 21... Power supply 23... Terminal insulator 24... Insulator 30, 30A, 30B... Gas hole 31... First through hole 32... Second through hole 33... Recess 39... Microhole 40... Gas hole member 45, 451, 452... Gas hole forming portion 50, 55... Adhesion layer G... Gas W... Wafer (sample)
Claims
1. An electrostatic chuck plate having a dielectric substrate having a mounting surface on which a sample is mounted, and an adsorption electrode located inside the dielectric substrate; and a base supporting the electrostatic chuck plate from the opposite side of the mounting surface, wherein the electrostatic chuck plate has a gas hole penetrating in a thickness direction of the electrostatic chuck plate, and a gas hole member is provided in the gas hole to pass a gas for cooling the sample, and the volume resistivity of the material of the gas hole member is 1.0×10 3 Ω・cm or more 1.0×10 10 The electrostatic chuck device has a resistivity of Ω·cm or less.
2. An electrostatic chuck device according to claim 1, wherein the material of said gas hole member is a composite material of an insulating material and a conductive material.
3. An electrostatic chuck device according to claim 2, wherein said dielectric substrate and said gas hole member are made of the same material.
4. An electrostatic chuck device according to claim 1 or 2, wherein the gas hole member is a porous body.
5. An electrostatic chuck device according to claim 1 or 2, wherein the gas hole member has one or more micropores penetrating in the thickness direction and having a diameter of 0.03 mm or more and 0.15 mm or less.
6. An electrostatic chuck plate having a dielectric substrate having a mounting surface for mounting a sample, and an adsorption electrode located inside the dielectric substrate; and a base supporting the electrostatic chuck plate from the opposite side of the mounting surface, wherein the electrostatic chuck plate has a gas hole penetrating in a thickness direction of the electrostatic chuck plate, the dielectric substrate has a gas hole forming portion at a position overlapping with the gas hole in a plan view, the gas hole including a recess provided in a surface of the gas hole forming portion opposite the mounting surface, and a microhole opening from the mounting surface to the recess, the diameter of the microhole being 0.03 mm or more and 0.15 mm or less, and the volume resistivity of a material of the gas hole forming portion being 1.0×10 3 Ω・cm or more 1.0×10 10 The electrostatic chuck device has a resistivity of Ω·cm or less.
7. An electrostatic chuck device as set forth in claim 6, wherein the dielectric substrate and the gas hole forming portion are made of the same material.
Citation Information
Patent Citations
Production of structural body for mitigating electrification and the structural body
JP1996035051A
Electrostatic chuck and manufacturing method of the same
JP2013235879A
High power electrostatic chuck with aperture-reducing plug in gas hole
JP2020174180A
Substrate fixing device
JP2021048243A
Electrostatic chuck, substrate fixing device, and method for manufacturing electrostatic chuck
JP2023018840A