Adhesive, rubber layer and waterproof leakage-repairing adhesive tape

By using a specific combination of adhesive and rubber layer materials, combined with the PVC film, the problem of the soft rubber layer and fragile aluminum foil lining of the existing waterproof leak-proofing tape is solved, achieving efficient waterproof sealing and UV resistance, and extending the service life of the tape and reduces replacement costs.

WO2024212427A1PCT designated stage expired Publication Date: 2024-10-17SHU GROUP CO LTD

Patent Information

Application Number
PCT/CN2023/116287
Authority / Receiving Office
WO · WO
Patent Type
Applications
Current Assignee / Owner
Priority Date
2023-04-10
Filing Date
2023-08-31
Publication Date
2024-10-17

AI Technical Summary

Technical Problem

The rubber layer of the existing aluminum foil butyl waterproof leak-proofing tape is too soft, and there is a hidden danger of the rubber layer flowing. The aluminum foil lining is thin and brittle, and it is easy to crack after being exposed to ultraviolet rays, resulting in a decrease in waterproofing effect and an increase in replacement costs.

Method used

Made of thermoplastic styrene-butadiene rubber SEBS An adhesive composed of YH502 and SIS1105, hydrogenated C5 petroleum resin LH100-1, terpene resin T90, naphthenic oil, antioxidant zinc dibutyl disulfate carbamate and titanium dioxide, combined with butyl rubber 1751, ternary The rubber layer of ethylene propylene rubber, C5 petroleum resin RT1102, stearic acid, zinc oxide, carbon black N330, ultrafine talc, accelerator M, accelerator ZDMC and antioxidant 1010 is combined with a PVC film to form a waterproof leak-proofing tape.

Benefits of technology

Improves the oxidation and UV aging resistance of the adhesive layer and rubber layer, enhances the mechanical strength and flexibility of the PVC film, avoids the flow of the adhesive layer and the cracking of the liner, ensures the waterproof sealing effect, and extends the use of the tape longevity and reduced replacement costs.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN2023116287_17102024_PF_FP_ABST
    Figure CN2023116287_17102024_PF_FP_ABST
Patent Text Reader

Abstract

Disclosed in the present invention are an adhesive, a rubber layer and a waterproof leakage-repairing adhesive tape. The waterproof leakage-repairing adhesive tape comprises a PVC film, an adhesive layer, a rubber layer and an adhesive layer which are sequentially arranged, wherein the PVC film comprises the following raw materials: SG3 resin, a polyester plasticizer, a filler, an aluminum paste, an ultraviolet light absorber, an antioxidant W, a stabilizer B, a flame retardant Sb2O3 and color chips; the adhesive layer comprises the following raw materials: thermoplastic styrene-butadiene rubber SEBS YH502, thermoplastic styrene-butadiene rubber SIS1105, C5 hydrogenated petroleum resin LH100-1, terpene resin T90, naphthenic oil, an anti-aging agent zinc dibutyldithiocarbamate and titanium dioxide; and the rubber layer comprises the following raw materials: butyl rubber 1751, an ethylene propylene diene monomer, C5 petroleum resin RT1102, stearic acid, zinc oxide, carbon black N330, ultrafine talcum powder, an accelerant M, an accelerant ZDMC and an antioxidant 1010. According to the present invention, a PVC film, adhesive layers and a rubber layer are organically combined, so that the obtained waterproof leakage-repairing adhesive tape has a good waterproof sealing effect and high mechanical strength and is resistant to ultraviolet irradiation.
Need to check novelty before this filing date? Find Prior Art

Description

Adhesive, rubber layer and waterproof leak-proof tape Technical Field

[0001] The invention relates to the field of adhesive tapes, in particular to an adhesive, a rubber layer and a waterproof leak-proof adhesive tape. Background Art

[0002] With the development of social economy, consumers have higher requirements for product quality and have also made more demands on its economy and durability. Enterprises need to improve or redevelop their products in a targeted manner.

[0003] The rubber layer of the aluminum foil butyl waterproof leak-proof tape currently used on the market is too soft, and there is a risk of the rubber layer flowing during use. At the same time, the aluminum foil lining is thin and brittle, and it is easy to crack after being exposed to ultraviolet rays outdoors, which greatly reduces the waterproof effect and increases the cost in disguise when replacing it.

[0004] To solve these problems, the aluminum foil lining needs to use a substrate with high mechanical strength and resistance to UV radiation to adapt to the outdoor thermal oxidative aging environment. The strength of the rubber layer needs to be improved and at the same time have good adhesion properties to ensure the sealing between the waterproof leak-proof tape and the bonding surface.

[0005] Summary of the Invention

[0006] The purpose of the present invention is to overcome the deficiencies of the prior art and provide an adhesive, a rubber layer and a waterproof leak-proof tape to solve the problems raised in the above technical background.

[0007] To achieve the above object, the present invention is implemented through the following technical solutions:

[0008] In a first aspect, the present invention provides an adhesive, wherein the adhesive raw materials include: thermoplastic styrene butadiene rubber SEBS YH502, thermoplastic styrene butadiene rubber SIS1105, hydrogenated C5 petroleum resin LH100-1, terpene resin T90, naphthenic oil, antioxidant dibutyl zinc disulfate carbamate and titanium dioxide.

[0009] Furthermore, the content of the adhesive raw materials includes, by weight: 50 parts of thermoplastic styrene-butadiene rubber SEBS YH502, 50 parts of thermoplastic styrene-butadiene rubber SIS1105, 80 to 120 parts in total of hydrogenated C5 petroleum resin LH100-1 and terpene resin T90, 20 parts of naphthenic oil, 5 parts of antioxidant dibutyl zinc disulfate carbamate and 5 parts of titanium dioxide; wherein the weight ratio of hydrogenated C5 petroleum resin LH100-1:terpene resin T90 is 4:1.

[0010] Furthermore, the content of the adhesive raw materials includes, by weight: 50 parts of thermoplastic styrene-butadiene rubber SEBS YH502, 50 parts of thermoplastic styrene-butadiene rubber SIS1105, 120 parts in total of hydrogenated C5 petroleum resin LH100-1 and terpene resin T90, 20 parts of cyclohexane oil, 5 parts of antioxidant dibutyl zinc disulfate carbamate and 5 parts of titanium dioxide; wherein the weight ratio of hydrogenated C5 petroleum resin LH100-1:terpene resin T90 is 4:1.

[0011] In a second aspect, the present invention provides a rubber layer, the raw materials of which include: butyl rubber 1751, EPDM rubber, C5 petroleum resin RT1102, stearic acid, zinc oxide, carbon black N330, ultrafine talc, accelerator M, accelerator ZDMC and antioxidant 1010.

[0012] Furthermore, the content of the rubber layer raw materials includes, by weight: 70-80 parts of butyl rubber 1751, 20-30 parts of EPDM rubber, 20 parts of C5 petroleum resin RT1102, 2 parts of stearic acid, 5 parts of zinc oxide, 10 parts of carbon black N330, 20 parts of ultrafine talc, 0.5 parts of accelerator M, 1 part of accelerator ZDMC and 1 part of antioxidant 1010.

[0013] Furthermore, the content of the rubber layer raw materials includes, by weight: 75 parts of butyl rubber 1751, 25 parts of EPDM rubber, 20 parts of C5 petroleum resin RT1102, 2 parts of stearic acid, 5 parts of zinc oxide, 10 parts of carbon black N330, 20 parts of ultrafine talc, 0.5 parts of accelerator M, 1 part of accelerator ZDMC and 1 part of antioxidant 1010.

[0014] In a third aspect, the present invention provides a waterproof leak-proof tape comprising a waterproof layer, an adhesive layer, a rubber layer, and an adhesive layer arranged in sequence, wherein the adhesive layer is made of the adhesive raw material described in the first aspect; and the rubber layer is made of the rubber layer raw material described in the second aspect.

[0015] Furthermore, the waterproof layer is a PVC film, which contains the following raw materials in parts by weight: 100 parts of SG3 resin, 50-60 parts of polyester plasticizer, 10 parts of filler, 0.5 parts of aluminum silver paste, 0.1-0.5 parts of ultraviolet absorber, 1 part of antioxidant W, 1 part of stabilizer B, 2 parts of flame retardant Sb2O3, and 0.5 parts of color chip.

[0016] Furthermore, the PVC film contains the following raw materials in parts by weight: 100 parts of SG3 resin, 55 parts of polyester plasticizer, 10 parts of filler, 0.5 parts of aluminum silver paste, 0.3 parts of ultraviolet absorber, 1 part of antioxidant W, 1 part of stabilizer B, 2 parts of flame retardant Sb2O3, and 0.5 parts of color flakes.

[0017] In a fourth aspect, the present invention provides a method for preparing a waterproof leak-proof tape, comprising the following steps:

[0018] Step 1: Preparation of PVC film, specifically:

[0019] 1.1 Prepare various raw materials according to the PVC film raw material formula, put them into a high-speed stirring tank, stir for 3 to 4 minutes, stir the mixed powder evenly, and control the temperature, which should not exceed 100°C;

[0020] 1.2 Discharge the mixed powder in the mixing tank into the internal mixer and stir under pressure. The temperature is controlled at around 140°C. The discharge frequency is determined according to the amount of rubber on the mill.

[0021] 1.3 Set the temperature of the rolling mill to 170℃ and the speed to about 1000rpm. Use the knife to turn the rubber material until it is evenly mixed and then convey it to the filter;

[0022] 1.4 Set the temperature of the rolling mill to 160℃, control the speed to about 1100rpm, and filter out impurities with a filter;

[0023] 1.5 Set the temperature of the rolling mill to 170℃, the temperature of the lower roller can be appropriately lowered, and adjust the thickness and width of the PVC film as needed to produce the required specifications;

[0024] Step 2: Preparation of adhesive layer, specifically:

[0025] 2.1 Raise the temperature of the reactor to 150℃~155℃, add naphthenic oil, thermoplastic styrene butadiene rubber SEBS YH502, and thermoplastic styrene butadiene rubber SIS1105 in sequence according to the adhesive raw material formula, fill with nitrogen for protection, and stir for 20~30 minutes to fully melt the rubber and oil;

[0026] 2.2 Add hydrogenated C5 petroleum resin LH100-1, terpene resin T90, antioxidant dibutyl disulfate zinc carbamate and titanium dioxide in sequence according to the adhesive raw material formula, fill with nitrogen for protection, and continue stirring for 15 to 20 minutes to fully melt the mixture;

[0027] 2.3 Place a light release film in the plastic container, inject the molten adhesive into the plastic container, and package it after it is fully cooled and solidified;

[0028] Step 3: Preparation of rubber layer, specifically:

[0029] 3.1 Adjust the roller distance of the open mill to 2mm, and according to the raw material formula of the rubber layer, pass butyl rubber 1751 and EPDM rubber on the open mill for 3 to 4 times, roll them into rubber tubes, and store them naturally for 8 to 24 hours;

[0030] 3.2 Add the butyl rubber 1751 and EPDM rubber masticated in step 3.1 into the internal mixing chamber in sequence, and then add C5 petroleum resin RT1102, carbon black N330, accelerator M, accelerator ZDMC and antioxidant 1010 in sequence according to the raw material formula of the rubber layer, and mix for 7 to 8 minutes;

[0031] 3.3 Add stearic acid, zinc oxide and 1 / 2 of the amount of ultra-fine talc powder into the mixing chamber according to the rubber layer raw material formula, and mix for 2 minutes;

[0032] 3.4 Add the remaining ultra-fine talcum powder into the mixer and mix for 2 minutes;

[0033] 3.5 Pour out the mixed material, pass it through the open mill 5-6 times, and stack it into 5-8mm thick films. Store it in a natural environment for 24 hours;

[0034] 3.6 Raise the temperature of the front roller and upper roller of the calender to 100-110°C, and the temperature of the middle roller and lower roller to 110-130°C;

[0035] 3.7 Thin the mixed rubber sheet prepared in 2.5 on an open mill until the temperature reaches 70°C and then press it onto a calender to a thickness of 1mm±0.05mm.

[0036] 3.8 The film is rolled into a semi-finished shaft with a light release film as the isolation layer for standby use;

[0037] Step 4: Preparation of waterproof sealing tape, specifically:

[0038] 4.1 Set up the coating machine so that the structure of the waterproof sealing tape obtained by coating is waterproof layer, adhesive layer, rubber layer, adhesive layer, and light release isolation film from top to bottom;

[0039] 4.2 Raise the coating machine's glue box temperature to about 160°C and the coating die head temperature to about 150°C. Apply and rewind according to the coating method in step 4.1. The coating amount is 80-120g / ㎡. Pay attention to cooling and controlling the tension.

[0040] 4.3 After the semi-finished shaft is stored for 24 hours, it should be cut. When cutting, the cutter should be fully lubricated to prevent the tape from sticking to the disc due to friction.

[0041] 4.4 When packaging, the two ends of the tape are separated by release paper or film, and then sealed with thermoplastic PE film.

[0042] In the present invention, the applicant has determined the ratio of PVC film plasticizer and UV absorber through years of work and research: polyester plasticizer provides flexibility to PVC film, and compared with ordinary plasticizers, its plastic products have better weather resistance and strength, but the cost is higher. A balance is sought between quality and cost. The required flexibility is achieved when the dosage is 55 parts, and 55 parts is finally determined. The UV absorber absorbs ultraviolet light for PVC film under sunlight, delaying the aging of the PVC film by sunlight. The recommended dosage is no more than 0.5 parts. Within this range, the greater the dosage, the better the effect. However, the price of this material is also relatively high. The performance improvement from 0.3 parts to 0.5 parts has been reduced. After comprehensive consideration, 0.3 parts was determined. A moderate ratio can achieve a higher cost-effectiveness.

[0043] In the present invention, the applicant has determined the types and proportions of adhesive rubbers through years of work and research: SIS1105 rubber has relatively poor resistance to heat and oxygen aging due to the presence of unsaturated bonds, while the glass transition temperature of the rubber segments is relatively low, resulting in better initial tack and lower cost than SEBS YH502 rubber; SEBS YH502 rubber has hydrogenated unsaturated bonds, which can be used to formulate an adhesive that is resistant to oxidation and UV aging and can still maintain good adhesion after heat, oxygen and light aging; however, due to the high glass transition temperature of the saturated rubber segments, the initial tack is poor and the material cost is high; after comprehensively weighing performance and economy, the two rubbers are mixed in a ratio of half and half, and the two rubbers cooperate with each other and work synergistically, resulting in a high cost-effectiveness. The types and ratios of adhesive resins were determined. Terpene resins, due to their natural properties, are affected by factors such as origin and climate, and have relatively poor resistance to natural aging. While their quality stability is inferior to that of petroleum resins, they exhibit excellent initial tack. Petroleum resins, on the other hand, are more stable and, once the process technology is finalized, ensure consistent product quality. Their cohesion is superior to that of terpene resins. To ensure excellent conformability of the adhesive layer, terpene resins are used at a ratio of 25% to petroleum resin, improving initial tack with minimal change in sustained tack. The goal of varying the ratio of rubber to resin in the adhesive is to achieve a balanced formulation with respect to initial tack, sustained tack, and peel strength. Within a certain range, a higher relative resin content improves initial tack and peel strength, but also reduces sustained tack, which can lead to adhesive runoff. Conversely, a lower relative resin content improves sustained tack, but reduces initial tack and peel strength, resulting in lower bonding efficiency during application. A moderate ratio achieves a well-balanced adhesive performance.

[0044] In the present invention, the applicant, through years of research and development, has determined the ratio of rubber to resin in the rubber layer: the rubber layer, which performs the sealing function of the present invention and works together with the adhesive layer as a whole, needs to have both sufficient strength to prevent flow and sufficient flexibility to adhere tightly to the adherend and maintain good sealing performance. Excessive rubber content results in a relatively high hardness of the rubber layer, making it difficult to adhere during construction, especially in cold weather. Excessive resin content results in excessive softness, which increases the fluidity of the rubber layer under external pressure or heat, leading to flow. A 20% resin content improves the flexibility and conformability of the rubber layer without significantly affecting its strength. The varying ratios of butyl rubber and EPDM rubber in the rubber layer are intended to achieve a formulation with a relatively balanced softness and mechanical properties: a greater relative amount of butyl rubber results in better softness and higher elongation, but lower tensile strength; a greater relative amount of EPDM rubber results in greater tensile strength, but lower softness and elongation. A moderate ratio can achieve relatively balanced properties in the rubber layer.

[0045] Compared with the prior art, the present invention has the following beneficial effects:

[0046] 1. Due to the use of polyester plasticizer, the mechanical strength and flexibility of the PVC film reach a good balance, providing good mechanical protection for the leak-proof tape; the addition of aluminum silver paste can reflect sunlight and prevent the tape from overheating and causing the adhesive layer to flow; the addition of ultraviolet absorber absorbs ultraviolet rays in sunlight, greatly slowing the aging rate of the PVC film and extending the service life of the tape.

[0047] 2. The introduction of SEBS YH502 rubber in the adhesive layer improves the adhesive layer's resistance to oxidation and UV aging, ensuring that the tape can maintain reliable bonding performance after a long period of use and extending the effectiveness of the tape's waterproofing ability.

[0048] 3. The use of EPDM rubber in the rubber layer contributes to good mechanical strength for the rubber layer, avoiding deformation of the tape during construction that affects its use and flow of the rubber layer in high temperature seasons that causes functional failure, while providing the tape with better waterproof ability and service life.

[0049] 4. Using PVC film instead of aluminum foil avoids the problem that the aluminum foil lining is thin and brittle, and is easy to crack after being exposed to ultraviolet rays outdoors, which greatly reduces the waterproof effect. It greatly extends the service life of the product and reduces the cost of replacing the waterproof tape. The adhesive layer with good adhesion performance and the rubber layer with both rigidity and flexibility avoid the hidden danger of the adhesive layer flowing during the use of the tape, ensuring the sealing between the waterproof leak-proof tape and the bonding surface, and playing a good waterproof sealing role.

[0050] The present invention adopts the organic combination of PVC film, adhesive layer, adhesive layer and rubber layer, and the obtained waterproof leak-proof adhesive tape has good waterproof sealing effect, high mechanical strength and can withstand ultraviolet radiation. BRIEF DESCRIPTION OF THE DRAWINGS

[0051] FIG1 is a schematic structural diagram of the waterproof leak-proof tape of the present invention;

[0052] FIG2 is a schematic diagram of the coating of the waterproof leak-proof tape of the present invention;

[0053] In the figure, 1. waterproof layer; 2. adhesive layer; 3. rubber layer; 4. light release isolation film. DETAILED DESCRIPTION

[0054] The following describes the embodiments of the present invention through specific examples. Those skilled in the art can easily understand other advantages and effects of the present invention from the content disclosed in this specification. The present invention can also be implemented or applied through other different specific embodiments. The details in this specification can also be modified or changed based on different viewpoints and applications without departing from the spirit of the present invention. It should be noted that the following embodiments and features in the embodiments can be combined with each other unless they conflict.

[0055] Example 1

[0056] This embodiment provides a waterproof leak-proof tape, which includes a waterproof layer, an adhesive layer, a rubber layer, and an adhesive layer arranged in sequence. The adhesive layer is made of adhesive raw materials; the rubber layer is made of rubber layer raw materials.

[0057] The waterproof layer is a PVC film, which contains the following raw materials in parts by weight: 100 parts of SG3 resin, 55 parts of polyester plasticizer, 10 parts of filler, 0.5 parts of aluminum silver paste, 0.3 parts of ultraviolet absorber, 1 part of antioxidant W, 1 part of stabilizer B, 2 parts of flame retardant Sb2O3, and 0.5 parts of color chip.

[0058] The adhesive comprises the following raw materials in parts by weight: 50 parts of thermoplastic styrene-butadiene rubber SEBS YH502, 50 parts of thermoplastic styrene-butadiene rubber SIS1105, 120 parts in total of hydrogenated C5 petroleum resin LH100-1 and terpene resin T90, 20 parts of naphthenic oil, 5 parts of antioxidant dibutyl zinc disulfate carbamate, and 5 parts of titanium dioxide; wherein the weight ratio of hydrogenated C5 petroleum resin LH100-1 to terpene resin T90 is 4:1.

[0059] The rubber layer comprises the following raw materials in parts by weight: 75 parts of butyl rubber 1751, 25 parts of EPDM rubber, 20 parts of C5 petroleum resin RT1102, 2 parts of stearic acid, 5 parts of zinc oxide, 10 parts of carbon black N330, 20 parts of ultrafine talc, 0.5 parts of accelerator M, 1 part of accelerator ZDMC and 1 part of antioxidant 1010.

[0060] Some of the raw materials of the present invention come from:

[0061] Thermoplastic styrene butadiene rubber SEBS YH502, thermoplastic styrene butadiene rubber SIS1105: Baling Petrochemical;

[0062] Hydrogenated C5 petroleum resin LH100-1: Lanzhou Petrochemical;

[0063] Naphthenic oil: Karamay, Xinjiang;

[0064] Butyl rubber 1751: Yanjing Petrochemical;

[0065] EPDM rubber: imported from Japan;

[0066] C5 petroleum resin RT1102: Shanghai Sansi;

[0067] Accelerator M, Accelerator ZDMC: Tianjin Maofeng Chemical Technology Co., Ltd.;

[0068] Antioxidant 1010, Antioxidant W: Tianjin Li'anlong Chemical Co., Ltd.

[0069] SG3 resin: Qilu Petrochemical;

[0070] Aluminum paste: Xuyang Aluminum Silver Material Co., Ltd.

[0071] UV absorber: imported from the United States.

[0072] The present invention provides a method for preparing a waterproof leak-proof tape, comprising the following steps:

[0073] Step 1: Preparation of PVC film, specifically:

[0074] 1.1 Prepare various raw materials according to the PVC film raw material formula, put them into a high-speed stirring tank, stir for 3 to 4 minutes, stir the mixed powder evenly, and control the temperature, which should not exceed 100°C;

[0075] 1.2 Discharge the mixed powder in the mixing tank into the internal mixer and stir under pressure. The temperature is controlled at around 140°C. The discharge frequency is determined according to the amount of rubber on the mill.

[0076] 1.3 Set the temperature of the rolling mill to 170℃ and the speed to about 1000rpm. Use the knife to turn the rubber material until it is evenly mixed and then convey it to the filter;

[0077] 1.4 Set the temperature of the rolling mill to 160℃, control the speed to about 1100rpm, and filter out impurities with a filter;

[0078] 1.5 Set the temperature of the rolling mill to 170℃, the temperature of the lower roller can be appropriately lowered, and adjust the thickness and width of the PVC film as needed to produce the required specifications;

[0079] Step 2: Preparation of adhesive layer, specifically:

[0080] 2.1 Raise the temperature of the reactor to 150℃~155℃, add naphthenic oil, thermoplastic styrene butadiene rubber SEBS YH502, and thermoplastic styrene butadiene rubber SIS1105 in sequence according to the adhesive raw material formula, fill with nitrogen for protection, and stir for 20~30 minutes to fully melt the rubber and oil;

[0081] 2.2 Add hydrogenated C5 petroleum resin LH100-1, terpene resin T90, antioxidant dibutyl disulfate zinc carbamate and titanium dioxide in sequence according to the adhesive raw material formula, fill with nitrogen for protection, and continue stirring for 15 to 20 minutes to fully melt the mixture;

[0082] 2.3 Place a light release film in the plastic container, inject the molten adhesive into the plastic container, and package it after it is fully cooled and solidified;

[0083] Step 3: Preparation of rubber layer, specifically:

[0084] 3.1 Adjust the roller distance of the open mill to 2mm, and according to the raw material formula of the rubber layer, pass butyl rubber 1751 and EPDM rubber on the open mill for 3 to 4 times, roll them into rubber tubes, and store them naturally for 8 to 24 hours;

[0085] 3.2 Add the butyl rubber 1751 and EPDM rubber masticated in step 3.1 into the internal mixing chamber in sequence, and then add C5 petroleum resin RT1102, carbon black N330, accelerator M, accelerator ZDMC and antioxidant 1010 in sequence according to the raw material formula of the rubber layer, and mix for 7 to 8 minutes;

[0086] 3.3 Add stearic acid, zinc oxide and 1 / 2 of the amount of ultra-fine talc powder into the mixing chamber according to the rubber layer raw material formula, and mix for 2 minutes;

[0087] 3.4 Add the remaining ultra-fine talcum powder into the mixer and mix for 2 minutes;

[0088] 3.5 Pour out the mixed material, pass it through the open mill 5-6 times, and stack it into 5-8mm thick films. Store it in a natural environment for 24 hours;

[0089] 3.6 Raise the temperature of the front roller and upper roller of the calender to 100-110°C, and the temperature of the middle roller and lower roller to 110-130°C;

[0090] 3.7 Thin the mixed rubber sheet prepared in 2.5 on an open mill until the temperature reaches 70°C and then press it onto a calender to a thickness of 1mm±0.05mm.

[0091] 3.8 The film is rolled into a semi-finished shaft with a light release film as the isolation layer for standby use;

[0092] Step 4: Preparation of waterproof sealing tape, specifically:

[0093] 4.1 Set up a coating machine. The specific coating method is shown in Figure 2. The structure of the waterproof sealing tape obtained by coating (see Figure 1) is waterproof layer 1, adhesive layer 2, rubber layer 3, adhesive layer 2, and light release isolation film 4 from top to bottom.

[0094] In Figure 2, the film shaft is rolling up the rubber layer and the light release isolation film;

[0095] 4.2 Raise the coating machine's glue box temperature to about 160°C and the coating die head temperature to about 150°C. Apply and rewind according to the coating method in step 4.1. The coating amount is 115±5g / ㎡. Pay attention to cooling and controlling the tension.

[0096] 4.3 After the semi-finished shaft is stored for 24 hours, it should be cut. When cutting, the cutter should be fully lubricated to prevent the tape from sticking to the disc due to friction.

[0097] 4.4 When packaging, the two ends of the tape are separated by release paper or film, and then sealed with thermoplastic PE film.

[0098] Examples 2 and 3 are similar to Example 1, and the contents of the components contained in the PVC film, adhesive layer, and rubber layer remain unchanged. The PVC film contains the following raw materials in parts by weight: 100 parts of SG3 resin, 55 parts of polyester plasticizer, 10 parts of filler, 0.5 parts of aluminum paste, 0.3 parts of ultraviolet absorber, 1 part of antioxidant W, 1 part of stabilizer B, 2 parts of flame retardant Sb2O3, and 0.5 parts of color flakes; the adhesive layer contains the following raw materials in parts by weight: 50 parts of thermoplastic styrene-butadiene rubber SEBS YH502, 50 parts of thermoplastic styrene-butadiene rubber SIS1105, 120 parts in total of hydrogenated C5 petroleum resin LH100-1 and terpene resin T90, 20 parts of cyclohexane oil, 5 parts of antioxidant dibutyl disulfate zinc carbamate, and 5 parts of titanium dioxide; the weight ratio of hydrogenated C5 petroleum resin LH100-1 to terpene resin T90 is 4:1.

[0099] The rubber layer comprises the following raw materials in parts by weight: 75 parts of butyl rubber 1751, 25 parts of EPDM rubber, 20 parts of C5 petroleum resin RT1102, 2 parts of stearic acid, 5 parts of zinc oxide, 10 parts of carbon black N330, 20 parts of ultrafine talc, 0.5 parts of accelerator M, 1 part of accelerator ZDMC and 1 part of antioxidant 1010.

[0100] The difference lies in the different amounts of glue applied. The differences between Examples 1-3 are shown in Table 1.

[0101] Table 1

[0102] The waterproof leak-proof adhesive tapes obtained in Examples 1-3 were tested using an electronic peel tester, a tack tester, a constant temperature drying oven, etc. The test results are shown in Table 2.

[0103] Table 2 Note 1: Laboratory Method 1—Use a clean square glass plate with a side length of 15-20 cm and a thickness of 2-4 mm as the carrier. Clean the glass plate surface with the cleaning solvent specified in GB / T2792-2014. Remove the separator from a 20 mm wide waterproof sealing tape sample and adhere it parallel to the edge of the glass plate. Roll the tape as described in the peel test sample. Place the glass plate vertically in a constant temperature drying oven at 80 ± 2°C for 2 hours, with the long side of the tape sample perpendicular to the oven chassis. Remove the sample and cool it to room temperature. Observe the adhesive layer for any signs of flow, cracking, or deformation. Note 2: Laboratory Method 2—Use a 20 cm long, 5 cm wide, 6-8 mm thick soft silicone sheet as the carrier. Clean the glass plate surface with the cleaning solvent specified in GB / T 2792-2014. Remove the separator from a 20 mm wide waterproof sealant tape sample and adhere it to the silicone sheet parallel to the plate edge. Prepare a peel test specimen and roll it. Place the silicone sheet horizontally in a -20°C freezer for 72 hours, with the long edge of the tape sample facing upward. After this temperature, bend the sheet 180° around a 20 mm diameter steel rod. Immediately unbend the sheet after the first bend, then bend it in the opposite direction a second time, immediately unbend it, and then bend it in the opposite direction a third time. Remove the sheet and return it to room temperature. Observe the surface of the tape for cracks. Note 3: Laboratory Method 3 - Using two flat, 15cm long and 5cm wide color-coated steel sheets as carriers, place the long sides of the two sheets parallel to each other, overlapping them by approximately 5mm. Place a 10cm long, 2cm wide napkin flat on the seam between the two sheets. Remove the barrier film from a 5cm wide piece of waterproof sealing tape and tape it around the seam, ensuring the napkin is fully enclosed within the adhesive layer. Roll the tape once with a standard roller. Place the steel sheet in tap water for 96 hours. Remove and allow the surface moisture to air dry. Carefully cut the adhesive layer with a plywood knife and observe whether the napkin absorbs water. The less water absorbed, the better the seal.

[0104] It can be seen from Table 2 that the adhesive tape has the best performance when the coating amount is 100±5g / ㎡.

[0105] The present invention will be further described below with reference to the formula ratio of the PVC film, adhesive and rubber layer.

[0106] Example 4: PVC film

[0107] This embodiment provides a PVC film. The preparation method of the PVC film is similar to that of Example 1. This embodiment prepares four types of PVC films according to different PVC film raw material formulas. The specific PVC film formula raw materials are shown in Table 3.

[0108] Table 3

[0109] The PVC film samples obtained from the four formulations in Table 3 were subjected to comparative tests using a tensile testing machine, an ultraviolet aging testing machine, and a spotlight. The test results are shown in Table 4.

[0110] Table 4 Note 4: Laboratory Method 4 - Cut a film 10 cm long and 10 cm wide, and irradiate the film surface with a 200 W incandescent lamp 20 cm above the center of the film for 20 minutes. During irradiation, use a rectangular box 40 cm high and 20 cm long and wide at the bottom to cover the incandescent lamp and the film sample. After irradiation, use an infrared thermometer at a distance of 20 cm to measure the film surface temperature.

[0111] As shown in Table 4, the conventional PVC film formula (Formula 1-0) has significantly lower tensile strength compared to the other three formulas due to the lack of a polyester plasticizer. Without a UV absorber, the mechanical properties after UV aging are only 50% of the initial value, while after UV aging, they reach 65% to 93% of the initial value. Without aluminum-silver paste, the reflective effect is poor, heat absorption is rapid, and the temperature is higher. Therefore, the use of these three materials significantly improves performance. Furthermore, the overall performance of Formula 1-1 is significantly worse than that of Formulas 1-2 and 1-3. While Formula 1-3 has advantages over Formula 1-2, the advantages are not significant, the performance improvement is not significant, and Formula 1-3 is more expensive. Taking all factors into consideration, Formula 1-2 is the optimal choice.

[0112] Example 5, Adhesive

[0113] This embodiment provides an adhesive. The preparation method of the adhesive is similar to that of Example 1. In this embodiment, four adhesives are prepared according to different adhesive raw material formulas. The specific adhesive formula raw materials are shown in Table 5.

[0114] Table 5

[0115] The adhesives obtained from the four recipes in Table 5 were coated on both sides of the same rubber sheet (Recipe 3-2 in Example 6) with a coating amount of 100 g / m2, one side of which was covered with the above-mentioned UV-resistant PVC film (Recipe 1-2 in Example 4) to obtain a waterproof leak-proof film; then, the test was carried out using an electronic peel tester, a stickiness tester, and a constant temperature drying oven. The test results are shown in Table 6.

[0116] Table 6

[0117] Table 6 shows that the standard adhesive layer formulation (Formula 2-0) exhibits significantly lower peel strength and adhesion compared to the other three formulations due to the absence of thermoplastic styrene-butadiene rubber (SEBS YH502). Furthermore, the adhesive layer exhibits flow after heat treatment, making it unsuitable for use as a waterproof sealant tape. However, performance improves significantly after heat treatment. Furthermore, Formulation 2-3 exhibits significantly better conformability than Formulations 2-1 and 2-2, and achieves the best sealing performance, a crucial property.

[0118] Example 6, rubber layer

[0119] This embodiment provides a rubber sheet including a rubber layer. The preparation method of the rubber layer is similar to that of Example 1. In this embodiment, four types of rubber layers are prepared according to different rubber layer raw material formulas. The specific rubber layer formula raw materials are shown in Table 7.

[0120] Table 7

[0121] The rubber sheets obtained from the four recipes in Table 7 were cut into 25 mm widths and tested for tensile strength and elongation using a tensile testing machine; the rubber sheets obtained from the four recipes in Table 7 were coated with the same adhesive (Recipes 2-3 in Example 5) on both sides with a coating amount of 100 g / m2, and one side was covered with the above-mentioned UV-resistant PVC film (Recipes 1-2 in Example 4) to obtain a waterproof leak-proof film; then, other indicators were tested using an electronic peel tester, a viscosity tester, and a constant temperature drying oven. The test results are shown in Table 8.

[0122] As shown in Table 8, the standard rubber layer formulation (Formula 3-0) lacks EPDM rubber, resulting in significantly lower tensile strength, tape peel strength, and adhesive retention compared to the other three formulations. The adhesive layer also exhibits flow after heat treatment, failing to meet the requirements for waterproofing and leak-proofing tapes. However, performance improves significantly after use. Furthermore, Formulation 3-2 exhibits moderate performance across all indicators, taking into account key properties such as sealing, ease of application, and heat resistance, while ensuring sufficient mechanical strength. Formulation 3-2 exhibits moderate softness, ease of application, excellent heat resistance, and excellent sealing, resulting in optimal overall performance.

[0123] The above-described embodiments merely represent specific implementations of the present invention. While the descriptions are relatively specific and detailed, they should not be construed as limiting the scope of the present invention. It should be noted that a person skilled in the art would be able to make numerous variations and improvements without departing from the spirit of the present invention, and all such variations and improvements fall within the scope of protection of the present invention.

Claims

1. An adhesive, characterized in that: The adhesive raw materials include: thermoplastic styrene butadiene rubber SEBS YH502, thermoplastic styrene butadiene rubber SIS1105, hydrogenated C5 petroleum resin LH100-1, terpene resin T90, cyclohexane oil, antioxidant dibutyl zinc disulfate carbamate and titanium dioxide.

2. An adhesive according to claim 1, characterized in that: The adhesive raw material comprises, by weight, 50 parts of thermoplastic styrene butadiene rubber SEBS YH502, 50 parts of thermoplastic styrene butadiene rubber SIS1105, 80 to 120 parts in total of hydrogenated C5 petroleum resin LH100-1 and terpene resin T90, 20 parts of cyclohexane oil, 5 parts of antioxidant dibutyl zinc disulfate carbamate and 5 parts of titanium dioxide; wherein the weight ratio of hydrogenated C5 petroleum resin LH100-1:terpene resin T90 is 4:

1.

3. An adhesive according to claim 2, characterized in that: In parts by weight, the content of the adhesive raw material includes: 50 parts of thermoplastic styrene butadiene rubber SEBS YH502, 50 parts of thermoplastic styrene butadiene rubber SIS1105, 120 parts in total of hydrogenated C5 petroleum resin LH100-1 and terpene resin T90, 20 parts of cyclohexane oil, 5 parts of antioxidant dibutyl zinc disulfate carbamate and 5 parts of titanium dioxide; wherein the weight ratio of hydrogenated C5 petroleum resin LH100-1:terpene resin T90 is 4:

1.

4. A rubber layer, characterized in that: The raw materials of the rubber layer include: butyl rubber 1751, ethylene propylene diene monomer rubber, C5 petroleum resin RT1102, stearic acid, zinc oxide, carbon black N330, ultrafine talcum powder, accelerator M, accelerator ZDMC and antioxidant 1010.

5. A rubber layer according to claim 4, characterized in that: The rubber layer raw materials include, by weight, 70 to 80 parts of butyl rubber 1751, 20 to 30 parts of EPDM rubber, 20 parts of C5 petroleum resin RT1102, 2 parts of stearic acid, 5 parts of zinc oxide, 10 parts of carbon black N330, 20 parts of ultrafine talc, 0.5 parts of accelerator M, 1 part of accelerator ZDMC and 1 part of antioxidant 1010.

6. A rubber layer according to claim 5, characterized in that: In parts by weight, the content of the rubber layer raw materials includes: the content of the rubber layer raw materials includes: 75 parts of butyl rubber 1751, 25 parts of EPDM rubber, 20 parts of C5 petroleum resin RT1102, 2 parts of stearic acid, 5 parts of zinc oxide, 10 parts of carbon black N330, 20 parts of ultrafine talc, 0.5 parts of accelerator M, 1 part of accelerator ZDMC and 1 part of antioxidant 1010.

7. A waterproof leak-proof tape, characterized in that: The invention comprises a waterproof layer, an adhesive layer, a rubber layer and an adhesive layer which are arranged in sequence, wherein the adhesive layer is made of the adhesive raw material according to claim 2; and the rubber layer is made of the rubber layer raw material according to claim 5.

8. The waterproof leak-proof tape according to claim 7, characterized in that: The waterproof layer is a PVC film, which contains the following raw materials in parts by weight: 100 parts of SG3 resin, 50-60 parts of polyester plasticizer, 10 parts of filler, 0.5 parts of aluminum silver paste, 0.1-0.5 parts of ultraviolet absorber, 1 part of antioxidant W, 1 part of stabilizer B, 2 parts of flame retardant Sb2O3, and 0.5 parts of color chip.

9. The waterproof leak-proof tape according to claim 7, characterized in that: The PVC film comprises the following raw materials in parts by weight: 100 parts of SG3 resin, 55 parts of polyester plasticizer, 10 parts of filler, 0.5 parts of aluminum paste, 0.3 parts of ultraviolet absorber, 1 part of antioxidant W, 1 part of stabilizer B, 2 parts of flame retardant Sb2O3, and 0.5 parts of color flakes.

10. The method for preparing a waterproof leak-proof tape according to claim 8, characterized in that: The following steps are involved: Step 1: Preparation of PVC film, specifically: 1.1 Prepare various raw materials according to the raw material formula of PVC film, put them into a high-speed stirring tank, stir for 3 to 4 minutes, stir the mixed powder evenly, and control the temperature, which should not exceed 100°C; 1.2 Discharge the mixed powder in the mixing tank into the internal mixer for pressure mixing. The temperature is controlled at 140℃. The discharge frequency is determined according to the amount of rubber on the rolling mill. 1.3 Set the temperature of the rolling mill to 170℃, the speed to 1000rpm, use the knife to turn the rubber until it is evenly mixed, and then transport it to the filter; 1.4 Set the temperature of the rolling mill to 160℃, the speed to 1100rpm, and filter out impurities with a filter; 1.5 Set the temperature of the rolling mill to 170℃, and adjust the thickness and width of the PVC film as needed to produce the required specifications; Step 2: Preparation of adhesive layer, specifically: 2.1 Raise the temperature of the reactor to 150℃~155℃, add naphthenic oil, thermoplastic styrene butadiene rubber SEBS YH502, and thermoplastic styrene butadiene rubber SIS1105 in sequence according to the adhesive raw material formula, fill with nitrogen for protection, and stir for 20~30 minutes to fully melt the rubber and oil; 2.2 Add hydrogenated C5 petroleum resin LH100-1, terpene resin T90, antioxidant dibutyl zinc disulfate carbamate and titanium dioxide in sequence according to the adhesive raw material formula, fill with nitrogen for protection, and continue stirring for 15 to 20 minutes to fully melt the mixture; 2.3 Place a light release film in the plastic container, inject the molten adhesive into the plastic container, and package it for later use after it is fully cooled and solidified; Step 3: Preparation of rubber layer, specifically: 3.1 Adjust the roller distance of the open mill to 2mm, and according to the raw material formula of the rubber layer, pass butyl rubber 1751 and EPDM rubber on the open mill for 3 to 4 times, roll them into rubber tubes, and store them naturally for 8 to 24 hours; 3.2 Put the butyl rubber 1751 and EPDM rubber masticated in step 3.1 into the internal mixing chamber in turn, and then put C5 petroleum resin RT1102, carbon black N330, accelerator M, accelerator ZDMC and antioxidant 1010 in turn according to the raw material formula of the rubber layer, and mix for 7 to 8 minutes; 3.3 Add stearic acid, zinc oxide and 1 / 2 amount of ultra-fine talcum powder into the internal mixing chamber according to the raw material formula of the rubber layer, and mix for 2 minutes; 3.4 Add the remaining ultra-fine talcum powder into the mixing chamber of the mixer in turn and mix for 2 minutes; 3.5 Pour out the mixed material, pass it through the open mixer for 5 to 6 times, and stack it into a film with a thickness of 5 to 8 mm. Store it in a natural environment for 24 hours; 3.6 Raise the temperature of the front roller and upper roller of the calender to 100-110°C, and the temperature of the middle roller and lower roller to 110-130°C; 3.7 Thin the mixed rubber sheet in 2.5 on the open mill, and when the temperature reaches 70℃, put it on the calender to press the sheet with a thickness of 1mm±0.05mm; 3.8 The film is rolled into a semi-finished shaft with a light release film as the isolation layer for standby use; Step 4: Preparation of waterproof sealing tape, specifically: 4.1 Set up the coating machine so that the structure of the waterproof leak-proof tape obtained by coating is waterproof layer, adhesive layer, rubber layer, adhesive layer, and light release isolation film from top to bottom; 4.2 Raise the temperature of the coating machine's glue box to about 160°C and the coating die head temperature to about 150°C, and apply and reel in the same manner as in step 4.1, with the coating amount being 80-120 g / ㎡; 4.3 After the semi-finished shaft is stored for 24 hours, it should be cut. When cutting, the cutter should be fully lubricated to prevent the disc from sticking due to friction with the tape surface. 4.4 When packaging, the two ends of the tape are separated by release paper or film, and then packaged with thermoplastic PE film.

Citation Information

Patent Citations

  • PVC (Poly Vinyl Chloride) composite material

    CN102582185A

  • Removable hot-melt pressure-sensitive adhesive tape for temporary fixation

    CN102702990A

  • Hot-melt pressure-sensitive adhesive for PVC electrical adhesive tape and preparation method

    CN105754526A

  • Hot-melt pressure-sensitive adhesive composition for automobile floor leather and preparation method thereof

    CN106085309A

  • Fireproof rubber and production method thereof

    CN108329605A

Cited By

  • Special repairing adhesive sticker for salt pond covering film, preparation method and application thereof