Glass for vehicles and sensors, bent glass, and laminated glass
A glass with a specific composition and boron coordination achieves high fracture toughness and low viscosity, addressing the limitations of conventional glass in vehicle and sensor applications and reducing energy consumption.
Patent Information
- Application Number
- PCT/JP2024/014003
- Authority / Receiving Office
- WO · WO
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2023-04-10
- Filing Date
- 2024-04-04
- Publication Date
- 2024-10-17
AI Technical Summary
Conventional techniques fail to produce glass with excellent fracture toughness, low viscosity, and low density, making it unsuitable for vehicle and sensor applications that require bending and have high fuel and electricity consumption concerns.
A specific glass composition range is used, including SiO2, B2O3, Al2O3, and alkali metal oxides, with controlled boron coordination to achieve high Young's modulus and fracture toughness while reducing viscosity and density.
The glass exhibits improved fracture toughness, low viscosity, and reduced density, enhancing its suitability for vehicle and sensor applications while minimizing fuel and electricity consumption.
Smart Images

Figure JP2024014003_17102024_PF_FP_ABST
Abstract
Description
Vehicle and sensor glass, bent glass, laminated glass
[0001] The present invention relates to glass for vehicles and sensors, bent glass, and laminated glass.
[0002] In recent years, glass used in mobility, such as glass for vehicles and cover glass for sensors such as LiDAR (Light Detection and Ranging), has been required to have high strength in order to extend its life cycle from the perspective of carbon neutrality.
[0003] In order to improve the strength of glass, it is effective to increase the Young's modulus or fracture toughness of the glass (see, for example, Patent Documents 1 and 2).
[0004] International Publication No. 2012 / 086664 Japanese Patent Application Publication No. 2019-529298
[0005] However, glasses with high Young's modulus and fracture toughness tend to be viscous, making them unsuitable for applications requiring bending, such as vehicle window glass or cover glass for sensors such as LiDAR.
[0006] For example, the glass described in Patent Document 1 has a Young's modulus of 81 GPa or more and a fracture toughness value of 0.9 MPa m 1/2 Although the glass has a high Young's modulus of 85 GPa or more and a fracture toughness of 0.86 MPa m 1/2 Although the temperature is high at 800°C or higher, the annealing point is high at 800°C or higher.
[0007] Furthermore, glass with a high Young's modulus generally tends to have a high density, i.e., a high weight. Therefore, using such glass for mobility applications such as vehicles and sensors is undesirable from the viewpoint of fuel economy and electric power consumption. Thus, it has been difficult to achieve glass with excellent fracture toughness, low viscosity, and low density using conventional technology.
[0008] In view of the above problems, an object of the present invention is to provide glass for vehicles and sensors, bent glass, and laminated glass that have excellent fracture toughness, low viscosity, and low density.
[0009] The present inventors have found that the above problems can be solved by using glass having a specific composition range, and have completed the present invention.
[0010] That is, the present invention is as follows: [1] Li, expressed in mole percent on an oxide basis 2 Contains substantially no O, SiO 2 : 70-80% B 2 O 3 : 10 to 17% Al 2 O 3 :1.0~6.0% MgO:0.0~5.0% CaO:0.0~5.0% SrO:0.0~5.0% BaO:0.0~5.0% Na 2 O: 0.0-19% K 2 O: 0.0~10% R' 2 O: 6.0 to 19% RO: 0.0 to 5.0% (wherein RO is at least one selected from MgO, CaO, SrO, and BaO; R' 2 O is Na 2 O.K. 2 (R' is at least one selected from 2 O] + 1 / 2 [RO] - [Al 2 O 3 ])-[B 2 O 3 [2] A glass for vehicles and sensors in which the content of tricoordinated boron is B 2 O 3 [3] The glass for vehicles and sensors according to [1], wherein the content of SiO is 10 mol % or less in terms of mol % based on oxides. 2 : 70-80% B 2 O 3 : 10 to 17% Al 2 O 3:1.0~6.0% MgO:0.0~5.0% CaO:0.0~5.0% SrO:0.0~5.0% BaO:0.0~5.0% Li 2 O: More than 0 to 15% Na 2 O: 3.5-15% K 2 O: 0.0~10% R 2 O: 6.0 to 19% RO: 0.0 to 5.0% (wherein RO is at least one selected from MgO, CaO, SrO, and BaO; R 2 O is Li 2 O, Na 2 O.K. 2 O), and 2 O] + 1 / 2 [RO] - [Al 2 O 3 ])-[B 2 O 3 ]≧−10.0 (where [ ] means the content of each component in the brackets expressed in mole percent based on the oxide), [4] Glass for vehicles and sensors, wherein the content of tricoordinated boron is B 2 O 3 [5] The glass for vehicles and sensors according to [1] or [3], having a Young's modulus of 65 GPa or more. [6] The glass for vehicles and sensors according to [1] or [3], having a fracture toughness value K measured by the SEPB method. IC is 0.76 MPa m 1/2 [7] The glass for vehicles and sensors according to [5], wherein the glass viscosity is 10 11 Temperature T at which viscosity becomes dPa s 11 [8] The glass for vehicles and sensors according to [7], having a Young's modulus of 70 GPa or more. [9] The glass for vehicles and sensors according to [8], having a fracture toughness value K measured by the SEPB method. IC is 0.80 MPa m 1/2
[10] The glass for vehicles and sensors according to [9], wherein the critical impact fracture speed when a tungsten carbide alloy having a tip curvature radius of 200 μm, an apex angle of 120°, and a weight of 1.365 g is collided with the glass when the surface roughness Ra is 5.0 nm or less and the thickness is 2.5 mm is 35 km / h or more.
[11] The glass for vehicles and sensors according to [9], wherein the critical impact fracture speed when a tungsten carbide alloy having a tip curvature radius of 200 μm, an apex angle of 120°, and a weight of 1.365 g is collided with the glass when the surface roughness Ra is 5.0 nm or less and the thickness is 2.5 mm is 55 km / h or more.
[12] The glass for vehicles and sensors according to
[11] , wherein the thickness is 2.5 mm or more.
[13] A curved glass comprising the glass for vehicles and sensors according to [1] or [3].
[14] A laminated glass comprising a first glass plate, a second glass plate, and an interlayer sandwiched between the first glass plate and the second glass plate, wherein the first glass plate is the glass for vehicles and sensors described in [1] or [3].
[15] The laminated glass described in
[14] , wherein the first glass plate has a surface roughness Ra of 5.0 nm or less and a thickness of 2.5 mm, and wherein a critical impact fracture speed when a tungsten carbide alloy having a tip radius of curvature of 200 μm, an apex angle of 120°, and a weight of 1.365 g is collided with a surface of the first glass plate is 35 km / h or more.
[16] The laminated glass described in
[14] , wherein a critical impact fracture speed when a tungsten carbide alloy having a tip radius of curvature of 200 μm, an apex angle of 120°, and a weight of 1.365 g is collided with a surface of the first glass plate is 55 km / h or more.
[17] The laminated glass according to
[16] , wherein the total thickness of the first glass sheet, the second glass sheet, and the interlayer film is 4.5 mm or more.
[18] The thickness t 1 and the thickness t of the second glass plate 2 The ratio (t 1 / t 2) is 1.5 or more.
[19] Laminated glass having a first glass plate, a second glass plate, and an interlayer film sandwiched between the first glass plate and the second glass plate, wherein the first glass plate and the second glass plate are the glass for vehicles and sensors described in [1] or [3].
[20] Laminated glass according to
[14] , wherein the second glass plate is soda lime glass.
[21] Laminated glass according to
[14] , wherein the second glass plate is aluminosilicate glass.
[22] Laminated glass according to
[14] , wherein the second glass plate has been subjected to a chemical strengthening treatment.
[0011] According to the present disclosure, it is possible to provide glass for vehicles and sensors, bent glass, and laminated glass that have excellent fracture toughness, low viscosity, and low density.
[0012] Fig. 1 is a graph showing the relationship between the content of tri-coordinated boron or tetra-coordinated boron and Young's modulus. Fig. 2 is a graph showing the relationship between the content of tri-coordinated boron or tetra-coordinated boron and surface fracture energy. Fig. 3 is a graph showing the relationship between the content of tri-coordinated boron or tetra-coordinated boron and surface fracture energy. 2 O 3 ]-([RO]+[R' 2 O]-[Al 2 O 3 ]) and B 2 O 3 4 is a graph showing the relationship between the content of tricoordinated boron in terms of the amount of [B 2 O 3 ]-([RO]+[R 2 O]-[Al 2 O 3 ]) and B 2 O 3 Fig. 5 is a graph showing the relationship between the content of tricoordinated boron converted from SiO2 and the total amount of SiO2. Fig. 5 is a cross-sectional view of an example of laminated glass according to an embodiment of the present invention. Fig. 6 is a conceptual diagram showing a state in which laminated glass according to an embodiment of the present invention is used as a window glass for a vehicle. Fig. 7 is an enlarged view of part S in Fig. 6. Fig. 8 is a cross-sectional view taken along line Y-Y in Fig. 7.
[0013] The present invention will be described in detail below based on embodiments, but the present invention is not limited to these embodiments. Furthermore, in the following drawings, components and parts that perform the same function may be denoted by the same reference numerals, and redundant explanations may be omitted or simplified. Furthermore, the embodiments shown in the drawings are schematic to clearly explain the present invention, and do not necessarily accurately represent the size or scale of the actual product. Furthermore, in this specification, a numerical range indicated using "to" indicates a range that includes the numerical values before and after "to" as the minimum and maximum values, respectively.
[0014] <Glass Composition> In this embodiment, the glass composition is expressed in mole percent based on oxides, and contains Li 2 Contains substantially no O, SiO 2 : 70-80% B 2 O 3 : 10 to 17% Al 2 O 3 :1.0~6.0% MgO:0.0~5.0% CaO:0.0~5.0% SrO:0.0~5.0% BaO:0.0~5.0% Na 2 O: 0.0-19% K 2 O: 0.0~10% R' 2 O: 6.0 to 19% RO: 0.0 to 5.0% (wherein RO is at least one selected from MgO, CaO, SrO, and BaO; R' 2 O is Na 2 O.K. 2 (R' is at least one selected from 2 O] + 1 / 2 [RO] - [Al 2 O 3 ])-[B 2 O 3 ] ≧−6.5 (hereinafter referred to as “glass of the first embodiment”).
[0015] In this embodiment, the oxide-based mol % is: SiO 2 : 70-80% B 2 O 3 : 10 to 17% Al 2 O 3:1.0~6.0% MgO:0.0~5.0% CaO:0.0~5.0% SrO:0.0~5.0% BaO:0.0~5.0% Li 2 O: More than 0 to 15% Na 2 O: 3.5-15% K 2 O: 0.0~10% R 2 O: 6.0 to 19% RO: 0.0 to 5.0% (wherein RO is at least one selected from MgO, CaO, SrO, and BaO; R 2 O is Li 2 O, Na 2 O.K. 2 O), and 2 O] + 1 / 2 [RO] - [Al 2 O 3 ])-[B 2 O 3 ] ≧−10.0 (hereinafter referred to as “glass of the second embodiment”).
[0016] In this specification, the term "glass of the present embodiment" includes the glass of the first embodiment and the glass of the second embodiment.
[0017] The composition range of each component is expressed in mole percent based on the oxide unless otherwise specified. Furthermore, the phrase "substantially free of" each component means that the component is not contained except as an unavoidable impurity mixed in from raw materials, etc., that is, it is not intentionally contained.
[0018] Hereinafter, a glass of a first embodiment and a glass of a second embodiment will be described as specific embodiments of the glass for a vehicle and a glass for a sensor (hereinafter, sometimes simply referred to as "glass") according to the present embodiment.
[0019] [Glass of the First Embodiment] The glass of the first embodiment contains, in mole percent on an oxide basis, Li 2 Contains substantially no O, SiO 2 : 70-80% B 2 O 3 : 10 to 17% Al 2 O 3:1.0~6.0% MgO:0.0~5.0% CaO:0.0~5.0% SrO:0.0~5.0% BaO:0.0~5.0% Na 2 O: 0.0-19% K 2 O: 0.0~10% R' 2 O: 6.0 to 19% RO: 0.0 to 5.0% (wherein RO is at least one selected from MgO, CaO, SrO, and BaO; R' 2 O is Na 2 O.K. 2 (R' is at least one selected from 2 O] + 1 / 2 [RO] - [Al 2 O 3 ])-[B 2 O 3 ]≧−6.5, where [ ] is the content of each component in the brackets expressed in mole percent on an oxide basis.
[0020] SiO 2 is a component that constitutes the network structure of the glass and is an essential component of the glass of this embodiment. 2 In the glass of the first embodiment, the content of SiO 2 When the content of SiO is 70% or more, the structure of the glass becomes strong and the Young's modulus can be increased. In addition, the density of the glass can be easily reduced, and further, moisture resistance and chemical durability can be ensured. Furthermore, the viscosity of the glass can be reduced. Furthermore, an increase in the average linear expansion coefficient can be suppressed, and thermal cracking of the glass can be suppressed. 2 The content is more preferably 71% or more, even more preferably 72% or more, even more preferably 73% or more, particularly preferably 74% or more, and most preferably 75% or more.
[0021] In the glass of the first embodiment, SiO 2 By making the content of SiO 80% or less, an increase in viscosity during glass melting is suppressed, making glass production easier and improving the formability of glass for vehicles, particularly windshields and cover glasses for sensors. 2The content is preferably 79% or less, more preferably 78% or less, even more preferably 77% or less, and particularly preferably 76% or less.
[0022] In this embodiment, B 2 O 3 reduces the viscosity and density of the glass and contributes to improving the Young's modulus. It is also a component that controls the optical properties. 2 O 3 In the glass of the first embodiment, B 2 O 3 By adding 10% or more of B, the viscosity and density of the glass can be reduced. In addition, as will be described later, by controlling the coordination number, the Young's modulus can be increased. 2 O 3 The content is preferably 11% or more, more preferably 12% or more, and even more preferably 13% or more.
[0023] In the glass of the first embodiment, B 2 O 3 If the content of B is 17% or less, the alkali elements are less likely to volatilize during the melting and forming of the glass, and deterioration of the glass quality can be suppressed. In addition, acid resistance and alkali resistance can be improved. 2 O 3 The content is preferably 16% or less, more preferably 15% or less, and even more preferably 14% or less.
[0024] In the glass of the first embodiment, B 2 O 3 The converted tricoordinate boron content (B 3 as B 2 O 3 The present inventors have found that by adjusting the ratio of tricoordinated boron to tetracoordinated boron contained in the glass, it is possible to obtain a glass having a high Young's modulus and excellent fracture toughness.
[0025] In glass, boron can have an oxygen coordination number of either three or four. Tetracoordinated boron enters the glass framework and forms a tetrahedral structure. In this case, the tetrahedral structure is negatively charged, and the charge is compensated by alkali metal ions or alkaline earth metal ions. Therefore, tetracoordinated boron forms a three-dimensional glass structure with almost no non-bridging oxygen. On the other hand, tricoordinated boron has non-bridging oxygen in glass and is known to form a planar structure such as a ring structure (boroxol ring).
[0026] 1 is a diagram showing the relationship between the content of tricoordinated boron or tetracoordinated boron and Young's modulus. As shown in FIG. 1, the Young's modulus tends to decrease as the content of tricoordinated boron increases, and to increase as the content of tetracoordinated boron increases. The reason why the Young's modulus improves with an increase in the content of tetracoordinated boron is thought to be that a decrease in the proportion of tricoordinated boron and an increase in the proportion of tetracoordinated boron reduces non-bridging oxygen, resulting in a dense structure, and therefore increases the ion packing fraction and bond dissociation energy that contribute to the Young's modulus.
[0027] FIG. 2 shows the relationship between the content of tricoordinated boron or tetracoordinated boron and the surface breakdown energy. As shown in FIG. 2, the surface breakdown energy tends to increase as the content of tetracoordinated boron increases, and tends to decrease as the content of tricoordinated boron increases.
[0028] Next, the fracture toughness value K IC The relationship between the Young's modulus and the surface fracture energy is explained. IC is an index of glass strength, and the fracture toughness value K IC The larger the fracture toughness value K, the more the propagation of cracks that occur in the glass can be suppressed. IC (MPa m 1/2 ) can be calculated from Young's modulus E (GPa), surface fracture energy γ (KPa·m), and Poisson's ratio ν (unitless) using the following formula (1).
[0029]
[0030] As shown in the above formula (1), the fracture toughness value K ICThe value of γ increases as the Young's modulus E and the surface fracture energy γ increase.
[0031] As shown in Figures 1 and 2, the Young's modulus and surface fracture energy improve as the content of tetrahedral boron increases, and therefore, in this embodiment, the more boron present in the tetrahedral state, the higher the fracture toughness value of the glass obtained. 2 O 3 The converted tricoordinate boron content is more preferably 9.0% or less, even more preferably 8.0% or less, even more preferably 7.0% or less, particularly preferably 6.0% or less, and most preferably 5.0% or less.
[0032] In addition, from the viewpoint of suppressing the increase in viscosity due to the increase in glass network formation caused by tetracoordinated boron, B 2 O 3 The converted tricoordinate boron content is preferably 1.5% or more, more preferably 2.0% or more, and particularly preferably 2.5% or more.
[0033] In addition, the glass of this embodiment contains Fe 2 O 3 When the glass contains the above-mentioned element, the color tone of the glass can be adjusted by adjusting the ratio of tricoordinated boron to tetracoordinated boron. Specifically, the greater the ratio of tetracoordinated boron, the stronger the gray color of the glass, resulting in glass with excellent design. Since the glass has a gray color, it is more suitable for use as a window glass for a vehicle, and from this viewpoint, the content of tricoordinated boron in the glass of the first embodiment is preferably within the above-mentioned range.
[0034] The ratio of tricoordinated boron to tetracoordinated boron can be adjusted by the glass composition. 2 O 3 The amount of the compound can be adjusted by appropriately adjusting the content of the compound.
[0035] As described above, boron in glass exists in a tetrahedral structure (tetracoordinated boron) when its charge is assisted by alkali metal ions or alkaline earth metal ions. On the other hand, boron not coordinated with alkali metal ions exists as tricoordinated boron. Therefore, the ratio of tricoordinated boron to tetracoordinated boron can be adjusted by adjusting the content of alkali metal ions.
[0036] Also, at this time, Al 2 O 3 The content of must also be taken into consideration. It is known that Al in glass has a coordination number of 4 to 6 due to oxygen, and tetracoordinated Al forms a tetrahedral glass structure. Because tetracoordinated Al has a negative charge like tetracoordinated boron, the charge is compensated by alkali metal ions or alkaline earth metal ions. In this case, alkali metal ions tend to coordinate preferentially to Al over boron.
[0037] Specifically, Al 2 O 3 and alkali metal oxides and B 2 O 3 In the case of a glass in which the content ratio of Al is 1:1:1, almost all of the alkali metal oxide is consumed in the formation of tetracoordinated Al. Therefore, in the above case, almost all of the boron in the glass exists as tricoordinated boron.
[0038] Similarly to alkali metal oxides, alkaline earth metal oxides also affect the coordination number of boron. Ions with lower electronegativity tend to react with boron and increase the amount of tetrahedral boron. Therefore, the proportion of tetrahedral boron increases in the order of Ba, Sr, Ca, and Mg, which have lower electronegativity.
[0039] Therefore, the content of tricoordinated boron and tetracoordinated boron varies depending on the alkali metal oxide and alkaline earth metal oxide, Al 2 O 3 The contents of tricoordinated boron and tetracoordinated boron can also be adjusted by adjusting the average cooling rate, which will be described later.
[0040] The proportions of tricoordinated boron and tetracoordinated boron in the glass can be measured by nuclear magnetic resonance (NMR). More specifically, it can be measured by the method described in the examples below.
[0041] Al 2 O 3 is a component that constitutes the network structure of the glass and is an essential component of the glass of this embodiment. 2 O 3 The content is 1.0 to 6.0%. 2 O 3 By setting the Al content to 1.0% or more, the Young's modulus can be increased. In addition, the weather resistance, moisture resistance, and chemical durability are improved. Furthermore, the average linear expansion coefficient does not become too large, which can suppress thermal cracking of the glass, and also makes it possible to perform chemical strengthening treatment using ion exchange. 2 O 3 The content is preferably 1.5% or more, more preferably 1.8% or more, even more preferably 2.0% or more, particularly preferably 2.3% or more, and most preferably 2.5% or more.
[0042] In the glass of the first embodiment, Al 2 O 3 By making the content of Al 6.0% or less, an increase in viscosity during glass melting is suppressed, facilitating glass production, and the formability of vehicle glass, particularly windshields and cover glasses for sensors, etc. is improved. Furthermore, the content of alkali metals coordinated to boron increases, and the proportion of tricoordinated boron can be reduced. 2 O 3 The content is preferably 5.5% or less, more preferably 5.0% or less, even more preferably 4.5% or less, particularly preferably 4.0% or less, and most preferably 3.5% or less.
[0043] In this embodiment, MgO is a component that reduces the viscosity of the glass and contributes to improving the Young's modulus. Furthermore, as described above, MgO is a component that increases the proportion of three-coordinated boron due to its high electronegativity. The glass of the first embodiment contains 0.0 to 5.0% MgO. By including MgO in the glass of the first embodiment, the viscosity of the glass can be reduced and the melting of the glass raw materials can be promoted. Additionally, the Young's modulus and moisture resistance can be improved. When MgO is included in the glass of the first embodiment, the content is preferably 0.20% or more, more preferably 0.40% or more, even more preferably 0.60% or more, particularly preferably 0.80% or more, and most preferably 1.0% or more.
[0044] Furthermore, in the glass of the first embodiment, if the MgO content is 5.0% or less, the glass is less susceptible to devitrification and an excessive increase in viscosity during glass melting is suppressed, facilitating glass production and improving the formability of vehicle glass, particularly windshields and cover glass for sensors. In addition, the proportion of tricoordinated boron can be kept low. The MgO content is preferably 4.0% or less, more preferably 3.5% or less, even more preferably 3.0% or less, particularly preferably 2.5% or less, and most preferably 2.0% or less.
[0045] In this embodiment, CaO is a component that reduces the viscosity of the glass. Additionally, as described above, CaO is a component that increases the proportion of three-coordinated boron due to its high electronegativity. The glass of the first embodiment contains 0.0 to 5.0% CaO. By including CaO in the glass of the first embodiment, the meltability of the glass raw materials is improved, and the viscosity is further reduced, thereby improving the formability of vehicle glass, particularly windshields and cover glass for sensors. When CaO is included in the glass of the first embodiment, the content is preferably 0.20% or more, more preferably 0.40% or more, even more preferably 0.60% or more, particularly preferably 0.80% or more, and most preferably 1.0% or more.
[0046] Furthermore, in the glass of the first embodiment, by setting the CaO content to 5.0% or less, an increase in the density of the glass can be suppressed, and the average linear expansion coefficient can be reduced, thereby suppressing thermal cracking of the glass. Furthermore, the proportion of tricoordinated boron can be kept low. The CaO content in the glass of the first embodiment is preferably 4.0% or less, more preferably 3.5% or less, even more preferably 3.0% or less, particularly preferably 2.5% or less, and most preferably 2.0% or less.
[0047] In this embodiment, SrO is a component that reduces the viscosity of the glass. Furthermore, because Sr has a lower electronegativity than Mg and Ca, it can increase the proportion of tetrahedral boron. The glass of the first embodiment contains 0.0 to 5.0% SrO. In the glass of the first embodiment, by limiting the SrO content to 5.0% or less, an increase in the density of the glass can be suppressed. In the glass of the first embodiment, the SrO content is preferably 4.0% or less, more preferably 3.0% or less, even more preferably 2.0% or less, even more preferably 1.0% or less, particularly preferably 0.5% or less, and most preferably substantially free. In the glass of the first embodiment, "substantially free of SrO" means that the SrO content in the glass is 0.10 mol% or less.
[0048] In the glass of the first embodiment, when SrO is contained, the content of SrO may be 0.20% or more, 0.40% or more, 0.60% or more, 0.80% or more, or 1.0% or more. By containing SrO, the viscosity of the glass can be reduced and the proportion of tetrahedral boron can be increased.
[0049] In this embodiment, BaO is a component that reduces the viscosity of the glass. Furthermore, because Ba has a lower electronegativity than Mg and Ca, it can increase the proportion of tetrahedral boron. The glass of the first embodiment contains 0.0 to 5.0% BaO. In the glass of the first embodiment, by limiting the BaO content to 5.0% or less, an increase in the density of the glass can be suppressed. In the glass of the first embodiment, the BaO content is preferably 4.0% or less, more preferably 3.0% or less, even more preferably 2.0% or less, even more preferably 1.0% or less, particularly preferably 0.5% or less, and most preferably substantially free. In the glass of the first embodiment, "substantially free of BaO" means that the BaO content in the glass is 0.10 mol% or less.
[0050] When BaO is contained in the glass of the first embodiment, the content of BaO may be 0.20% or more, 0.40% or more, 0.60% or more, 0.80% or more, or 1.0% or more. By containing BaO, the viscosity of the glass can be reduced and the proportion of tetrahedral boron can be increased.
[0051] In this embodiment, Na 2 O is a component that improves the melting property of glass and reduces its viscosity. It also increases the Young's modulus and contributes to the average linear expansion coefficient of glass. Furthermore, chemical strengthening treatment by ion exchange with K ions can increase the strength of glass. In addition, Na ions can be coordinated to boron to increase the proportion of tetrahedral boron.
[0052] In the glass of the first embodiment, Na 2 The content of O is 0.0 to 19%. 2 By including O, the viscosity of the glass can be reduced, and further, the proportion of tetrahedral boron can be increased. In addition, the Young's modulus and the average linear expansion coefficient can be increased. 2When O is contained, the content is preferably 2.0% or more, more preferably 3.0% or more, even more preferably 4.0% or more, still more preferably 5.0% or more, particularly preferably 5.5% or more, particularly preferably 6.0% or more, and most preferably 6.5% or more.
[0053] Also, Na 2 By keeping the O content at 19% or less, thermal cracking of the glass due to an excessively large average linear expansion coefficient can be suppressed. In addition, the moisture resistance of the glass is improved, making it suitable for use as glass exposed to the atmosphere for long periods of time, such as vehicle window glass. 2 The O content is preferably 17% or less, more preferably 15% or less, even more preferably 13% or less, even more preferably 12% or less, particularly preferably 11% or less, and most preferably 10% or less.
[0054] K 2 O is a component that improves the meltability of the glass and reduces the viscosity, and also makes it easier to increase the Young's modulus and contributes to the average linear expansion coefficient of the glass. 2 The O content is 0.0 to 10%.
[0055] In the glass of the first embodiment, K 2 By incorporating O, the viscosity of the glass can be reduced. In addition, the Young's modulus and the average linear expansion coefficient can be increased. Furthermore, O can be coordinated to boron to increase the proportion of tetrahedral boron. 2 When O is contained, the content is preferably 0.10% or more, more preferably 0.20% or more, even more preferably 0.30% or more, particularly preferably 0.40% or more, and most preferably 0.50% or more.
[0056] On the other hand, K 2 O is Li 2 O and Na 2 Compared to O, it has the effect of increasing the average linear expansion coefficient and density. 2 By keeping the O content at 10% or less, thermal cracking of the glass due to an excessively large average linear expansion coefficient can be suppressed. 2The O content is preferably 8.0% or less, more preferably 6.0% or less, even more preferably 5.0% or less, even more preferably 4.0% or less, particularly preferably 3.0% or less, and most preferably 2.0% or less.
[0057] In the glass of the first embodiment, Na 2 O and K 2 The total content of O (hereinafter referred to as R' 2 R' is 6.0% or more and 19% or less. 2 When O is 6.0% or more, the Young's modulus is increased and the viscosity of the glass is reduced, thereby improving the formability of vehicle glass, particularly windshields and cover glass for sensors. 2 The O content is preferably 6.5% or more, more preferably 7.0% or more, even more preferably 7.5% or more, particularly preferably 8.0% or more, and most preferably 8.5% or more.
[0058] Also, R' 2 If the O content is 19% or less, an increase in density can be suppressed and the moisture resistance of the glass can be improved. 2 O is preferably 17% or less, more preferably 15% or less, even more preferably 14% or less, even more preferably 13% or less, particularly preferably 12% or less, and most preferably 11% or less.
[0059] In the glass of the first embodiment, the total content of MgO, CaO, SrO, and BaO (hereinafter sometimes referred to as RO) is 0.0% or more and 5.0% or less. By containing at least one selected from MgO, CaO, SrO, and BaO, the Young's modulus can be improved. When RO is contained, the RO content is preferably 0.20% or more, more preferably 0.40% or more, even more preferably 0.60% or more, particularly preferably 0.80% or more, and most preferably 1.0% or more.
[0060] Furthermore, if RO is 5.0% or less, an increase in the density of the glass can be suppressed and the crack resistance of the glass can be improved. RO is preferably 4.5% or less, more preferably 4.0% or less, even more preferably 3.5% or less, still more preferably 3.0% or less, particularly preferably 2.5% or less, and most preferably 2.0% or less.
[0061] In addition, the glass of the first embodiment contains Li 2 In the glass of the first embodiment, Li is not contained. 2 By substantially not containing O, the formation of a crystalline phase containing Li can be suppressed during the production of the glass, thereby improving manufacturability. 2 The term "substantially free of O" means that the glass contains Li. 2 This means that the O content is 0.10 mol % or less.
[0062] In the glass of the first embodiment, ([R' 2 O] + 1 / 2 [RO] - [Al 2 O 3 ])-[B 2 O 3 ] is -6.5 or more. Here, [ ] is the content of each component in the brackets expressed in mole percent on an oxide basis. ([R' 2 O] + 1 / 2 [RO] - [Al 2 O 3 ])-[B 2 O 3 When the value of [Ratio of Coordinated Boron to 3] is -6.5 or more, the proportion of tricoordinated boron in the glass is reduced, and the Young's modulus and surface fracture energy are improved, resulting in an improved fracture toughness value.
[0063] As mentioned above, the ratio of tricoordinated boron to tetracoordinated boron in the glass varies depending on the alkali metal oxide, alkaline earth metal oxide, Al 2 O 3 As shown in FIG. 3, the amount of ([R' 2 O] + 1 / 2 [RO] - [Al 2 O 3 ])-[B 2 O 3 ] tends to decrease the content of tricoordinated boron.
[0064] In the glass of the first embodiment, ([R' 2 O] + 1 / 2 [RO] - [Al 2 O 3 ])-[B 2 O 3If [R'] is -6.5 or more, the content of tricoordinated boron can be sufficiently reduced, and the fracture toughness value of the glass can be increased. 2 O] + 1 / 2 [RO] - [Al 2 O 3 ])-[B 2 O 3 is preferably −6.2 or more, more preferably −6.0 or more, even more preferably −5.8 or more, even more preferably −5.6 or more, particularly preferably −5.4 or more, and most preferably −5.2 or more.
[0065] In addition, from the viewpoint of suppressing the increase in viscosity of the glass and the deterioration of bending formability due to an excessively high proportion of tetrahedral boron, ([R' 2 O] + 1 / 2 [RO] - [Al 2 O 3 ])-[B 2 O 3 is preferably 0.0 or less, more preferably −1.0 or less, even more preferably −1.5 or less, even more preferably −2.0 or less, particularly preferably −2.5 or less, and most preferably −3.0 or less.
[0066] [Glass of Second Embodiment] The glass of the second embodiment contains, in mole percent on an oxide basis, SiO 2 : 70-80% B 2 O 3 : 10 to 17% Al 2 O 3 :1.0~6.0% MgO:0.0~5.0% CaO:0.0~5.0% SrO:0.0~5.0% BaO:0.0~5.0% Li 2 O: More than 0 to 15% Na 2 O: 3.5-15% K 2 O: 0.0~10% R 2 O: 6.0 to 19% RO: 0.0 to 5.0% (wherein RO is at least one selected from MgO, CaO, SrO, and BaO; R 2 O is Li 2 O, Na 2 O.K. 2 O), and 2 O] + 1 / 2 [RO] - [Al 2 O3 ])-[B 2 O 3 ]≧−10.0.
[0067] In the glass of the second embodiment, SiO 2 , B 2 O 3 , Al 2 O 3 , MgO, CaO, SrO, BaO, K 2 The properties of O and RO are the same as those of the glass of the first embodiment.
[0068] In the glass of the second embodiment, Li 2 O is a component that improves the melting property of glass and reduces its viscosity. In addition, O is a component that increases the Young's modulus and contributes to the average linear expansion coefficient of glass. Furthermore, the strength of glass can be increased by performing a chemical strengthening treatment by ion exchange with Na ions. Furthermore, the proportion of tetrahedral boron can be increased by coordinating Li ions to boron. The glass of the second embodiment is made of Li 2 Contains more than 0 to 15% O.
[0069] In the glass of the second embodiment, Li 2 By containing O, Na 2 O and K 2 Compared to O, it can reduce the viscosity of the glass and increase the Young's modulus. Furthermore, it can increase the proportion of tetrahedral boron, so Na 2 O and K 2 Compared with O, it can increase Young's modulus and fracture toughness. 2 The O content is preferably 0.50% or more, more preferably 1.0% or more, even more preferably 1.5% or more, even more preferably 2.0% or more, particularly preferably 2.5% or more, and most preferably 3.0% or more.
[0070] In the glass of the second embodiment, Li 2 By setting the O content to 15% or less, it is possible to suppress thermal cracking of the glass due to an excessively large average linear expansion coefficient. Furthermore, it is possible to suppress the formation of a crystalline phase containing Li during the production of the glass, thereby improving the manufacturability of the glass. 2The O content is preferably 12% or less, more preferably 10% or less, even more preferably 8.0% or less, particularly preferably 6.0% or less, and most preferably 5.0% or less.
[0071] In the glass of the second embodiment, Na 2 Contains 3.5 to 15% O. 2 When the O content is 3.5% or more, the viscosity of the glass decreases, so that Li 2 The O content can be reduced, and the formation of a crystalline phase containing Li can be suppressed during glass production. Furthermore, the viscosity of the glass is reduced, improving the formability of vehicle glass, particularly windshields and cover glass for sensors. Furthermore, the proportion of tetrahedral boron can be increased, improving the Young's modulus and surface fracture energy. 2 The O content is preferably 4.0% or more, more preferably 4.5% or more, even more preferably 5.0% or more, still more preferably 5.5% or more, particularly preferably 6.0% or more, particularly preferably 6.5% or more, and most preferably 7.0% or more.
[0072] In the glass of the second embodiment, Na 2 By keeping the O content at 15% or less, the average linear expansion coefficient can be reduced, and thermal cracking of the glass can be suppressed. In addition, the moisture resistance of the glass is improved, making it suitable for use as glass that is exposed to the atmosphere for long periods of time, such as vehicle glass and sensor glass. 2 The O content is preferably 13% or less, more preferably 12% or less, even more preferably 11% or less, particularly preferably 10% or less, and most preferably 9.0% or less.
[0073] In the glass of the second embodiment, Li 2 O, Na 2 O and K 2 The total content of O (hereinafter referred to as R 2 O) is 6.0 to 19%. 2 When the O content is 6.0% or more, the Young's modulus is increased and the viscosity of the glass is reduced, improving the formability of vehicle glass, particularly windshields and sensor cover glass. 2O is preferably 6.5% or more, more preferably 7.0% or more, even more preferably 7.5% or more, even more preferably 8.0% or more, particularly preferably 8.5% or more, and most preferably 9.0% or more.
[0074] R 2 From the viewpoint of improving moisture resistance and suppressing an increase in density, O is 19% or less, preferably 17% or less, more preferably 15% or less, even more preferably 14% or less, still more preferably 13% or less, particularly preferably 12% or less, and most preferably 11% or less.
[0075] In the glass of the second embodiment, ([R 2 O] + 1 / 2 [RO] - [Al 2 O 3 ])-[B 2 O 3 ] is -10.0 or more. Here, [ ] is the content of each component in the brackets expressed in mole percent on an oxide basis. In the glass of the second embodiment, ([R 2 O] + 1 / 2 [RO] - [Al 2 O 3 ])-[B 2 O 3 When the value of [Ratio of Coordinated Boron to 3] is -10.0 or more, the proportion of tricoordinated boron in the glass is reduced, and the Young's modulus and surface fracture energy are improved, resulting in an improved fracture toughness value.
[0076] As mentioned above, the ratio of tricoordinated boron to tetracoordinated boron in the glass varies depending on the alkali metal oxide, alkaline earth metal oxide, Al 2 O 3 As shown in FIG. 2 O] + 1 / 2 [RO] - [Al 2 O 3 ])-[B 2 O 3 ] tends to decrease the content of tricoordinated boron.
[0077] In the glass of the second embodiment, ([R 2 O] + 1 / 2 [RO] - [Al 2 O 3 ])-[B 2 O 3If [R 2 O] + 1 / 2 [RO] - [Al 2 O 3 ])-[B 2 O 3 is preferably −9.0 or more, more preferably −8.0 or more, even more preferably −7.5 or more, even more preferably −7.0 or more, particularly preferably −6.5 or more, and most preferably −6.0 or more.
[0078] In addition, in order to prevent the proportion of tetrahedral boron from becoming too high, which increases the viscosity of the glass and deteriorates the bending formability, ([R 2 O] + 1 / 2 [RO] - [Al 2 O 3 ])-[B 2 O 3 ] is preferably −0.5 or less, more preferably −1.0 or less, even more preferably −1.5 or less, and most preferably −2.0 or less.
[0079] In the glass of the second embodiment, B 2 O 3 The converted tricoordinate boron content (B 3 as B 2 O 3 As described above, in the glass of this embodiment, the Young's modulus and surface fracture energy improve as the content of tetrahedral boron increases, and therefore, the more boron is present in a tetrahedral state, the higher the fracture toughness value obtained. Therefore, in the glass of the second embodiment, B 2 O 3 The converted tricoordinate boron content is more preferably 9.0% or less, even more preferably 8.0% or less, even more preferably 7.0% or less, particularly preferably 6.5% or less, and most preferably 6.0% or less.
[0080] In the glass of the second embodiment, from the viewpoint of suppressing an increase in viscosity due to an increase in glass network formation caused by tetracoordinated boron, B 2 O 3The converted tricoordinate boron content is preferably 1.0% or more, more preferably 1.5% or more, particularly preferably 2.0% or more, and most preferably 2.5% or more.
[0081] Other components and properties of the glass of the present embodiment, including the first and second embodiments, will be described below.
[0082] [Other Components] Fe 2 O 3 is a component that improves the heat insulating properties of the glass and also contributes to the color of the glass, and therefore may be contained in the glass of the present embodiment. 2 O 3 The total iron content converted to iron is preferably 0.0025 to 1.2%. 2 O 3 The total iron content converted to ferrous iron is the total iron content of FeO, which is an oxide of divalent iron, and Fe, which is an oxide of trivalent iron. 2 O 3 This refers to the total amount of iron, including Fe. 2 O 3 Furthermore, the load on the melting furnace caused by heat radiation reaching the bottom surface of the melting furnace during glass melting can be suppressed.
[0083] When the glass of this embodiment is used for vehicle glass, Fe in the glass of this embodiment is preferably used in order to improve heat insulation, provide design, and facilitate heat transfer to the glass during bending. 2 O 3 The total iron content, calculated as % iron, is preferably 0.0025% or more, more preferably 0.0040% or more, even more preferably 0.039% or more, still more preferably 0.097% or more, particularly preferably 0.11% or more, particularly preferably 0.15% or more, and most preferably 0.17% or more.
[0084] In addition, from the viewpoint of suppressing the decrease in light transmittance in the visible range, Fe 2 O 3 The total iron content, calculated as iron content, is preferably 1.0% or less, more preferably 0.80% or less, even more preferably 0.60% or less, particularly preferably 0.50% or less, and most preferably 0.40% or less.
[0085] On the other hand, when the glass of this embodiment is used for the cover glass of LiDAR or a camera, from the viewpoint of facilitating melting of raw materials during glass production and reducing the amount of expensive high-purity raw materials used, Fe 2 O 3 The total iron content converted into % is preferably 0.0030% or more, more preferably 0.0032% or more, even more preferably 0.0034% or more, still more preferably 0.0036% or more, particularly preferably 0.0038% or more, particularly preferably 0.0040% or more, and most preferably 0.0042% or more.
[0086] In addition, from the viewpoint of suppressing the decrease in light transmittance in the visible and near-infrared regions, Fe 2 O 3 The total iron content, calculated as iron content, is preferably 0.020% or less, more preferably 0.010% or less, even more preferably 0.0080% or less, particularly preferably 0.0070% or less, and most preferably 0.0060% or less.
[0087] The glass of this embodiment contains Fe 2 O 3 Fe in total iron converted to 2 O 3 It is preferable that the mass percentage (%) of divalent iron converted to Fe (hereinafter referred to as Fe-Redox) is 15% or more. 2 O 3 Fe relative to the total iron content converted 2 O 3 Conversion Fe 2+ The percentage of content.
[0088] The glass of this embodiment has an Fe-Redox content of 15% or more, and therefore has an absorption in the near-infrared region. 2+ Since the content of [beta] can be increased, heat is more easily transferred to the molten glass during glass production, improving manufacturability. In addition, the transmittance in the near-infrared region is reduced, improving heat insulation, making the glass suitable for applications requiring heat insulation, such as vehicle glass.
[0089] When the glass of this embodiment is used for a vehicle glass, the Fe-Redox is more preferably 20% or more, further preferably 22% or more, and particularly preferably 24% or more. Furthermore, the Fe-Redox is preferably 50% or less. By having the Fe-Redox content of 50% or less, deterioration of the melting equipment can be suppressed, and the amount of SO in the fining agent can be reduced. 3 When Fe-Redox is used, amber coloring can be suppressed and a decrease in visible light transmittance can be suppressed. Fe-Redox is more preferably 45% or less, further preferably 40% or less, and particularly preferably 38% or less.
[0090] On the other hand, when the glass of this embodiment is used as a cover glass for LiDAR, Fe-Redox is more preferably 16% or more, even more preferably 17% or more, and particularly preferably 18% or more. Furthermore, Fe-Redox is preferably 35% or less. By having Fe-Redox 35% or less, a decrease in transmittance in the near-infrared region can be suppressed. Fe-Redox is more preferably 32% or less, even more preferably 30% or less, and particularly preferably 28% or less.
[0091] Fe-Redox can be adjusted by the raw material composition, melting temperature, and melting atmosphere. Fe-Redox can also be adjusted by using a reducing agent such as coke or ammonium chloride as a raw material to control the degree of oxidation-reduction of the glass melt.
[0092] The glass of the present embodiment may contain components other than the above components (hereinafter also referred to as "other components").
[0093] Other components include, for example, TiO 2 , ZrO 2 , Y 2 O 3 , CeO 2 , Nd 2 O 5 , GaO 2 , GeO 2 , MnO 2 , NiO, Cr 2 O 3 , V 2 O 5 , Au 2 O 3 , Ag 2O, CuO, CdO, MoO 3 , S.O. 3 , Cl, F, SnO 2 , Sb 2 O 3 and the like, which may be metal ions or oxides. Other components may be contained in a total amount of 3.0% or less for various purposes (e.g., clarification and coloring, imparting chemical durability, etc.). If the total content of other components is 3.0% or less, the necessary properties for vehicle glass and cover glass for sensors such as LiDAR can be maintained. The total content of other components is preferably 2.5% or less, more preferably 2.0% or less, even more preferably 1.5% or less, even more preferably 1.0% or less, particularly preferably 0.80% or less, and most preferably 0.50% or less.
[0094] In addition, to prevent environmental impact, 2 O 3 The content of each of PbO is preferably less than 0.0010%, and more preferably substantially none is contained.
[0095] The glass of this embodiment is ZrO 2 ZrO 2 is a component that improves chemical durability. 2 When ZrO is contained, its content is preferably 0.010% or more, more preferably 0.050% or more, further preferably 0.10% or more, and particularly preferably 0.20% or more. 2 The content is preferably 2.0% or less, more preferably 1.5% or less, even more preferably 1.0% or less, and particularly preferably 0.50% or less.
[0096] The glass of this embodiment is Y 2 O 3 Y 2 O 3 is a component that improves Young's modulus. 2 O 3When Y is contained, its content is preferably 0.10% or more, more preferably 0.20% or more, further preferably 0.30% or more, and particularly preferably 0.40% or more. 2 O 3 The content is preferably 2.0% or less, more preferably 1.5% or less, further preferably 1.0% or less, particularly preferably 0.80% or less.
[0097] In the glass of this embodiment, if NiO is contained, NiS may be generated, which may cause glass breakage, so the NiO content is preferably 0.0080% or less, more preferably 0.0040% or less, even more preferably 0.0020% or less, and particularly preferably substantially zero.
[0098] The glass of this embodiment contains CeO 2 It may contain CeO 2 Since CeO absorbs light in the ultraviolet region, it reduces the ultraviolet transmittance Tuv and improves UV blocking performance. It also acts as an oxidizing agent and can control Fe-Redox. 2 When CeO is contained, its content is preferably 0.010% or more, more preferably 0.020% or more, further preferably 0.040% or more, and particularly preferably 0.070% or more. 2 may absorb ultraviolet light, causing solarization and reducing transmittance in the visible range. 2 The content is preferably 0.25% or less, more preferably 0.18% or less, further preferably 0.14% or less, particularly preferably 0.10% or less.
[0099] The glass of this embodiment is Cr 2 O 3 Cr 2 O 3 acts as an oxidizing agent and can control Fe-Redox. 2 O 3 When Cr is contained, its content is preferably 0.0020% or more, and more preferably 0.0040% or more. 2 O 3Since Fe has coloration in the visible range, there is a risk of a decrease in visible light transmittance. 2+ Therefore, the glass of the present embodiment is preferably made of Cr. 2 O 3 When it is contained, the content is preferably 0.020% or less, more preferably 0.016% or less, further preferably 0.012% or less, and particularly preferably 0.0080% or less.
[0100] The glass of this embodiment is SnO 2 It may contain SnO 2 acts as a reducing agent and can control Fe-Redox. 2 When SnO is contained, its content is preferably 0.010% or more, more preferably 0.040% or more, further preferably 0.060% or more, and particularly preferably 0.080% or more. 2 In order to suppress defects caused by SnO in the glass of this embodiment, 2 The content of is preferably 0.40% or less, more preferably 0.30% or less, further preferably 0.20% or less, particularly preferably 0.15% or less.
[0101] The glass of this embodiment is SO 3 SO 3 acts as a fining agent to improve the bubble quality of the glass. 3 When SO is contained, its content is preferably 0.0010% or more, more preferably 0.0040% or more, further preferably 0.0070% or more, and particularly preferably 0.015% or more. 3 If the Fe-Redox is high, amber coloring occurs, turning the glass brown, and there is a risk of a decrease in visible light transmittance. 3 When it is contained, the content is preferably 0.070% or less, more preferably 0.060% or less, further preferably 0.050% or less, and particularly preferably 0.040% or less.
[0102] The glass of this embodiment may contain Cl. Cl acts as a fining agent and improves the bubble quality of the glass. When the glass of this embodiment contains Cl, the Cl content is preferably 0.080% or more, more preferably 0.15% or more, even more preferably 0.20% or more, particularly preferably 0.25% or more, and most preferably 0.30% or more. If the Cl content is high, Cl volatilized from the glass melt may be easily dissolved. 2 The gas may corrode surrounding members. When the glass of the present embodiment contains Cl, the Cl content is preferably 1.0% or less, more preferably 0.80% or less, even more preferably 0.60% or less, and particularly preferably 0.50% or less.
[0103] [Characteristics] (Fracture toughness value K IC The glass of this embodiment has a fracture toughness value K measured by the SEPB method. IC is 0.76 MPa m 1/2 The fracture toughness value K is preferably equal to or greater than the above. IC is an index of glass strength, and the fracture toughness value K IC The larger the fracture toughness value K, the more difficult it is for cracks to progress and the higher the resistance to cracking. IC is 0.76 MPa m 1/2 If the fracture toughness value K is 1.0 or more, sufficient resistance to cracking can be obtained, making the glass suitable for use as a cover glass for vehicles or sensors. IC is 0.78 MPa m 1/2 More preferably, 0.80 MPa m 1/2 More preferably, 0.82 MPa m 1/2 More preferably, 0.84 MPa m 1/2 More preferably, 0.86 MPa m 1/2 More than 0.88 MPa m is particularly preferred. 1/2 More preferably, 0.90 MPa m 1/2 The above is most preferable.
[0104] Fracture toughness value K ICis measured using a pre-crack introduction fracture test method (SEPB method: Single-Edge-Precracked-Beam method) based on JIS R1607:2015 "Fracture toughness test method for fine ceramics".
[0105] In order to set the fracture toughness value within the above range, SiO 2 Increase the content of R', increase the proportion of tetracoordinated boron, increase the proportion of alkaline earth metal components with small atomic numbers among RO, 2 O or R 2 In particular, the proportion of alkali metal components with small atomic numbers in the O range can be increased. 2 Or B 2 O 3 Since R' (especially tetrahedral boron) is a component that forms a network structure, increasing its content strengthens the glass structure, thereby improving the fracture toughness value. Furthermore, the smaller the atomic number of the alkaline earth metal component in RO, the higher the Young's modulus, and as a result, the higher the fracture toughness value. 2 O, R 2 Regarding O, the smaller the atomic number of the alkali metal component, the more the tendency similar to that of RO is shown.
[0106] (Young's modulus) The Young's modulus of the glass of this embodiment is preferably 65 GPa or more. A Young's modulus of 65 GPa or more gives the glass high rigidity and improved fracture toughness, making it more suitable for use as a window glass for vehicles or a cover glass for sensors such as LiDAR. The Young's modulus of the glass of this embodiment is more preferably 68 GPa or more, even more preferably 70 GPa or more, even more preferably 72 GPa or more, particularly preferably 73 GPa or more, and most preferably 74 GPa or more.
[0107] Furthermore, from the viewpoint of suppressing deformation and cracking when the glass is subjected to an external force, the Young's modulus is preferably 85 GPa or less, more preferably 83 GPa or less, even more preferably 82 GPa or less, particularly preferably 81 GPa or less, and most preferably 80 GPa or less.
[0108] In order to set the Young's modulus within the above range, the proportion of tetracoordinated boron is increased, and RO and R' are2 O and R 2 Examples of methods include adjusting the type and amount of O. Young's modulus can be measured by an ultrasonic pulse method based on JIS R1602:1995 "Testing method for elastic modulus of fine ceramics."
[0109] (Rigidity Modulus) The rigidity modulus of the glass of this embodiment is preferably 27 GPa or more. If the rigidity modulus is 27 GPa or more, the glass is less likely to deform when subjected to an external force. The rigidity modulus of the glass is more preferably 28 GPa or more, even more preferably 29 GPa or more, particularly preferably 30 GPa or more, and most preferably 31 GPa or more.
[0110] Furthermore, when the glass is subjected to an external force, deformation occurs, consuming energy and thereby suppressing cracking, so the modulus of rigidity is preferably 38 GPa or less, more preferably 37 GPa or less, even more preferably 36 GPa or less, and particularly preferably 35 GPa or less. The modulus of rigidity can be measured by an ultrasonic pulse method based on JIS R1602:1995 "Testing method for elastic modulus of fine ceramics."
[0111] (Poisson's ratio) The Poisson's ratio of the glass of this embodiment is preferably 0.26 or less. The smaller the Poisson's ratio, the smaller the stress generated when an external force is applied to the glass. The fracture toughness value also improves. The Poisson's ratio is more preferably 0.25 or less, even more preferably 0.24 or less, particularly preferably 0.23 or less, particularly preferably 0.22 or less, particularly preferably 0.21 or less, and most preferably 0.20 or less. The Poisson's ratio can be measured by an ultrasonic pulse method based on JIS R1602:1995 "Testing method for elastic modulus of fine ceramics."
[0112] (Surface fracture energy) The surface fracture energy of the glass of this embodiment is preferably 0.0045 KPa m or more. The larger the surface fracture energy, the more improved the fracture toughness value, which is preferable. The surface fracture energy is more preferably 0.0046 KPa m or more, even more preferably 0.0048 KPa m or more, particularly preferably 0.0049 KPa m or more, and most preferably 0.0050 KPa m or more. The surface fracture energy can be determined by measuring the fracture toughness value, Young's modulus, and Poisson's ratio and calculating from the relational expression (1) above.
[0113] (T 2 In the glass of this embodiment, the glass viscosity η, which is a criterion for the meltability of glass, is 10 2 [dPa s] Temperature T 2 It is preferable that T is 1700°C or less. 2 By keeping the temperature at 1700°C or less, the consumption of fuel used in melting the glass raw materials can be reduced, and the life of the brick members used in the melting furnace can be extended.
[0114] T 2 As a method for lowering the temperature to 1700° C. or less, for example, the R′ of the glass component 2 O or R 2 The content of O and RO was increased, and Al 2 O 3 A method for reducing the content of R 2 Among O, Li 2 Method for incorporating O, SiO 2 A method for reducing the content of 2 O 3 The method for adjusting the content of T is as follows. 2 is more preferably 1675°C or less, further preferably 1650°C or less, even more preferably 1640°C or less, particularly preferably 1630°C or less, and most preferably 1620°C or less. From the viewpoint of maintaining the fracture toughness of the glass and preventing the average linear expansion coefficient of the glass from becoming too large, T 2 The temperature is preferably 1450°C or higher, more preferably 1475°C or higher, even more preferably 1500°C or higher, particularly preferably 1525°C or higher, and most preferably 1550°C or higher.
[0115] (T 4 In the glass of this embodiment, the glass viscosity η, which is the standard for formability during float forming, is 10 4 [dPa s] Temperature T 4 It is preferable that T is 1200°C or less. 4 Since the temperature is 1200°C or less, it is suitable for forming into a plate by the float method.
[0116] T 4 As a method for lowering the temperature to 1200° C. or less, for example, the R′ of the glass component 2 O, R 2 Increased O and RO content, Al 2 O 3 A method for reducing the content of R 2 Among O, Li 2 Method for incorporating O, SiO 2 A method for reducing the content of 2 O 3 The method for adjusting the content of
[0117] T 4 is more preferably 1180°C or less, further preferably 1170°C or less, even more preferably 1160°C or less, particularly preferably 1150°C or less, and most preferably 1140°C or less. From the viewpoint of maintaining the fracture toughness of the glass and preventing the average linear expansion coefficient of the glass from becoming too large, T 4 The heating temperature is preferably 1000°C or higher, more preferably 1025°C or higher, even more preferably 1050°C or higher, and particularly preferably 1070°C or higher.
[0118] (T 11 In the glass of this embodiment, the glass viscosity η, which is the standard for bending workability, is 10 11 [dPa s] Temperature T 11 It is preferable that T is 640°C or less. 11 By keeping the temperature at 640°C or less, bending forming can be performed at a low temperature.
[0119] T 11 As a method for lowering the temperature to 640° C. or less, for example, the R′ of the glass component 2 O, R 2Increased O and RO content, Al 2 O 3 A method for reducing the content of R 2 Among O, Li 2 Method for incorporating O, SiO 2 A method for reducing the content of 2 O 3 The amount of boron and the coordination number of boron can be adjusted.
[0120] In the glass of this embodiment, T 11 The temperature is more preferably 635°C or lower, even more preferably 630°C or lower, even more preferably 625°C or lower, particularly preferably 620°C or lower, particularly preferably 615°C or lower, and most preferably 610°C or lower.
[0121] In addition, from the viewpoint of maintaining the fracture toughness of the glass, preventing the average linear expansion coefficient of the glass from becoming too large, and the firing temperature of the black ceramic printed on the windshield, T 11 The temperature is preferably 570°C or higher, more preferably 575°C or higher, even more preferably 580°C or higher, particularly preferably 585°C or higher, and most preferably 590°C or higher.
[0122] (T 12 In the glass of this embodiment, the glass viscosity η, which is the standard for bending workability, is 10 12 [dPa s] Temperature T 12 It is preferable that T is 610°C or less. 12 By keeping the temperature at 610°C or less, bending forming can be performed at a low temperature.
[0123] T 12 As a method for lowering the temperature to 610° C. or less, for example, the R′ of the glass component 2 O, R 2 Increased O and RO content, Al 2 O 3 A method for reducing the content of R 2 Among O, Li 2 Method for incorporating O, SiO 2 A method for reducing the content of 2 O 3 The method for adjusting the content and the coordination number of boron is mentioned.
[0124] T 12 is more preferably 605°C or less, even more preferably 600°C or less, even more preferably 595°C or less, particularly preferably 590°C or less, particularly preferably 585°C or less, and most preferably 580°C or less. From the viewpoint of maintaining the fracture toughness of the glass, preventing the average linear expansion coefficient of the glass from becoming too large, and from the viewpoint of the firing temperature of the black ceramic printed on the windshield, T 12 The temperature is preferably 540°C or higher, more preferably 545°C or higher, even more preferably 550°C or higher, particularly preferably 555°C or higher, and most preferably 560°C or higher.
[0125] (Density) The density of the glass of this embodiment is 2.50 g / cm 3 It is preferable that the density is 2.50 g / cm or less. 3 Generally, glass having a high Young's modulus and fracture toughness value tends to have a high density. 2 O, R 2 The composition and content of O and RO, and B 2 O 3 By adjusting the content of and the coordination number of boron, it is possible to achieve a low density and a high Young's modulus and fracture toughness.
[0126] The density of the glass of this embodiment is 2.46 g / cm 3 More preferably, 2.44 g / cm 3 More preferably, 2.42 g / cm 3 Even more preferably, 2.40 g / cm 3 The following is particularly preferred: 3 The following is particularly preferred: 2.36 g / cm 3 From the viewpoint of improving sound insulation, the density of the glass of this embodiment is most preferably 2.25 g / cm 3 More than 2.27 g / cm 3 More preferably, 2.28 g / cm 3 More than 2.29 g / cm is particularly preferred. 3The above is most preferable.
[0127] (T g ) the glass transition temperature (T g ) is preferably in the range of 460 to 590°C. g If the temperature is within this predetermined range, the glass can be bent within the range of normal manufacturing conditions. g By ensuring that the temperature is 460°C or higher, the alkali metal content or alkaline earth metal content does not become too large, and the average linear expansion coefficient of the glass can be prevented from increasing. In addition, moisture resistance and devitrification of the glass are suppressed, and formability is improved. g is more preferably 480° C. or higher, further preferably 490° C. or higher, and particularly preferably 500° C. or higher. From the viewpoint of preventing the bending temperature of the glass from becoming excessive and facilitating production, T g is preferably 590°C or lower, more preferably 585°C or lower, even more preferably 580°C or lower, particularly preferably 575°C or lower, and most preferably 570°C or lower.
[0128] (Average Coefficient of Linear Expansion) The average coefficient of linear expansion (CTE) of the glass of this embodiment at 50 to 350°C is 80 × 10 -7 / °C or less. The average linear expansion coefficient is preferably 80 x 10 -7 / °C or less, cracking due to heat shock can be suppressed when the glass is used as glass for vehicles or sensors. Furthermore, when the glass of this embodiment is made into bent glass, the difference in thermal expansion due to differences in in-plane thermal history can be suppressed, and bent glass with good dimensional and surface accuracy can be obtained.
[0129] The average linear expansion coefficient of the glass of this embodiment at 50 to 350°C is 75 × 10 -7 / °C or less is more preferable, and 70 x 10 -7 / °C or less is more preferable, and 68 x 10 -7 / °C or less is even more preferable, and 66 x 10 -7 / °C or less is particularly preferred, and 64 x 10 -7 / °C or less is most preferred.
[0130] In addition, the glass of this embodiment has an average linear expansion coefficient of 40×10 from the viewpoint of suppressing cracking of the black ceramic due to the difference in thermal expansion with the black ceramic printed on the windshield. -7 / °C or more. -7 / °C or more, the difference in thermal expansion with the black ceramic is small, and cracking of the black ceramic can be suppressed. -7 / °C or more is more preferable, and 44 x 10 -7 / °C or more is more preferable, and 46 x 10 -7 / °C or more is particularly preferred, and 48 x 10 -7 / °C or more is particularly preferred, and 50 x 10 -7 / °C or more is particularly preferred, and 52 x 10 -7 / °C or more is most preferred.
[0131] In order to set the average linear expansion coefficient within the above range, the SiO 2 Increase the content of R 2 O or R' 2 O, RO and Al 2 O 3 The content of B 2 O 3 The method for adjusting the content and the coordination number of boron is mentioned.
[0132] (Solar transmittance: Te) When the glass of this embodiment is used for vehicle glass, the solar transmittance Te of the glass of this embodiment, when converted to a thickness of 2.0 mm, according to ISO-9050:2003 is preferably 90% or less. If Te is 90% or less, excellent heat shielding properties can be obtained. Te is preferably 88% or less, more preferably 86% or less, even more preferably 84% or less, particularly preferably 82% or less, and most preferably 80% or less. There is no particular restriction on the lower limit of Te, but it is usually 30% or more, preferably 32% or more, more preferably 34% or more, and particularly preferably 36% or more.
[0133] To set Te in the above range, Fe 2 O 3 This can be achieved by adjusting the amount to 0.030% or more.
[0134] (Visible Light Transmittance: Tv) When the glass of this embodiment is used for vehicle glass, the glass of this embodiment preferably has a visible light transmittance Tv of 75% or more, calculated by measuring the transmittance with a spectrophotometer using a D65 light source in accordance with the specifications of ISO-9050:2003 when converted to a thickness of 2.00 mm. A Tv of 75% or more provides excellent transparency, making the glass more suitable for vehicle glass, particularly windshields and door glass. Tv is more preferably 78% or more, even more preferably 80% or more, and even more preferably 82% or more. 84% or more is particularly preferred, and 86% or more is most preferred. The upper limit of Tv is not particularly limited, but is, for example, 92% or less.
[0135] In order to set Tv within the above range, the glass composition, particularly SiO 2 and Fe 2 O 3 The content of B 2 O 3 This can be achieved by adjusting the content and the coordination number of boron.
[0136] (Ultraviolet Transmittance: Tuv) When the glass of this embodiment is used for vehicle glass, it is preferable that the glass of this embodiment has low ultraviolet transmittance, and when converted to a thickness of 2.00 mm, the ultraviolet transmittance Tuv defined in ISO-9050:2003 is preferably 70% or less. A Tuv of 70% or less can suppress deterioration of components such as interlayers and seats inside the vehicle cabin when the glass of this embodiment is used for laminated glass. Tuv is more preferably 68% or less, even more preferably 66% or less, even more preferably 64% or less, particularly preferably 62% or less, and most preferably 60% or less. The lower limit of Tuv is, for example, 10% or more.
[0137] To set Tuv within the above range, the glass composition, particularly SiO 2 and Fe 2 O 3 , TiO 2 and CeO 2 Alternatively, this can be achieved by adjusting Fe-Redox.
[0138] (Dominant Wavelength: Dw) When the glass of this embodiment is used for vehicle glass, the dominant wavelength Dw of the glass of this embodiment, measured using a standard C light source specified in JIS Z 8701:1999, is preferably 520 nm or more and 574 nm or less. Dw is more preferably 525 nm or more, even more preferably 530 nm or more, particularly preferably 535 nm or more, and most preferably 540 nm or more. Furthermore, Dw is more preferably 573 nm or less, even more preferably 570 nm or less, particularly preferably 567 nm or less, and most preferably 565 nm or less.
[0139] (Excitation Purity: Pe) When the glass of this embodiment is used for vehicle glass, the glass of this embodiment preferably has an excitation purity Pe of 4.0% or less, as measured using the standard C illuminant specified in JIS Z 8701:1999. Pe is more preferably 3.5% or less, even more preferably 3.0% or less, even more preferably 2.5% or less, particularly preferably 2.0% or less, and most preferably 1.5% or less. The lower limit of Pe is not particularly limited, but is generally 0.1% or more. When Dw and Pe are within the above ranges, the glass is gray and exhibits excellent design properties.
[0140] In order to adjust Dw and Pe, the glass of this embodiment contains Fe. 2 O 3 This can be achieved by adjusting the ratio of tricoordinated boron to tetracoordinated boron while containing the above.
[0141] When the glass of this embodiment is used for a vehicle glass, the shape of the glass of this embodiment is not particularly limited, but the area of the main surface is 0.25 m 2 More than 0.45m is preferable. 2 More preferably, 0.90 m or more 2 The above is even more preferable. When the area of the glass is within the above range, it can be adapted to various vehicle models. Furthermore, if the area of the glass is too large, it becomes difficult to handle, the temperature distribution during heating becomes uneven, the dimensional accuracy after bending becomes poor, and so on, making bending more difficult. Therefore, the glass of this embodiment is designed so that the area of the main surface is within 10 m 2 Preferably less than 7m 2 Less than 5m is more preferable. 2 The following is even more preferred:
[0142] When the glass of this embodiment is used as a cover glass for LiDAR, it is preferable that the glass of this embodiment has high transmittance at wavelengths of 905 nm or 1550 nm, which are used in LiDAR. Therefore, the transmittance of the glass of this embodiment at a wavelength of 905 nm or 1550 nm when converted to a thickness of 4.0 mm is preferably 86% or more, more preferably 87% or more, even more preferably 88% or more, even more preferably 89% or more, particularly preferably 90% or more, and most preferably 91% or more.
[0143] When the glass of this embodiment is used as a cover glass for a sensor, the shape of the glass of this embodiment is not particularly limited, but the area of the main surface is preferably 0.00010 m 2 More than 0.010 m is preferable. 2 More preferably, 0.020 m or more 2 More preferably, 0.040 m or more 2 More than 0.090 m is particularly preferable. 2 The above is most preferable. When the glass area is within the above range, it can be used as a cover glass for various LiDARs. Furthermore, if the glass area is too large, the temperature distribution during heating becomes uneven, the dimensional accuracy after bending becomes poor, and so on, making bending more difficult. Therefore, the glass of this embodiment has a main surface area of 1.0 m 2 Preferably less than 0.90 m 2 Less than 0.80 m is more preferable. 2 The following is even more preferred:
[0144] Furthermore, the glass of this embodiment preferably has a surface roughness Ra of 5.0 nm or less, a thickness of 2.5 mm, and a critical impact fracture speed of 35 km / h or more when impacted with a tungsten carbide alloy having a tip curvature radius of 200 μm, an apex angle of 120°, and a weight of 1.365 g. A critical impact fracture speed of 35 km / h or more can improve resistance to flying stones. The critical impact fracture speed is more preferably 40 km / h or more, even more preferably 45 km / h or more, particularly preferably 50 km / h or more, and most preferably 55 km / h or more. The upper limit of the critical impact fracture speed is, for example, 120 km / h or less. The surface roughness Ra can be measured according to JIS B0601:2001.
[0145] Furthermore, the glass of this embodiment preferably has a critical impact fracture speed of 55 km / h or more when a tungsten carbide alloy having a tip curvature radius of 200 μm, an apex angle of 120°, and a weight of 1.365 g is collided with the glass. A critical impact fracture speed of 55 km / h or more can further improve resistance to flying stones. The critical impact fracture speed is more preferably 57 km / h or more, even more preferably 60 km / h or more, even more preferably 62 km / h or more, particularly preferably 64 km / h or more, particularly preferably 66 km / h or more, particularly preferably 68 km / h or more, and most preferably 70 km / h or more. The upper limit of the critical impact fracture speed is, for example, 120 km / h or less. The critical impact fracture speed can be measured by the method described in the Examples below.
[0146] The glass of this embodiment preferably has a thickness of 2.5 mm or more. In particular, when the glass of this embodiment has the above properties, the thickness of the glass is preferably 2.5 mm or more. A glass thickness of 2.5 mm or more can improve the critical impact fracture speed of glass with a high fracture toughness value. The thickness of the glass is more preferably 2.8 mm or more, even more preferably 2.9 mm or more, even more preferably 3.0 mm or more, particularly preferably 3.1 mm or more, even more preferably 3.2 mm or more, even more preferably 3.3 mm or more, particularly preferably 3.4 mm or more, and most preferably 3.5 mm or more.
[0147] Furthermore, from the viewpoint of suppressing increases in fuel consumption and electricity consumption due to an increase in the weight of the glass, the thickness of the glass of this embodiment is preferably 5.0 mm or less, more preferably 4.8 mm or less, even more preferably 4.5 mm or less, particularly preferably 4.2 mm or less, and most preferably 4.0 mm or less. Examples of methods for adjusting the thickness of the glass include adjusting the thickness of the glass using the float method or down-draw method described below, and polishing the glass in the thickness direction with a grinding stone and then polishing it to a mirror finish using an abrasive such as cerium oxide. The surface roughness Ra after molding or polishing is preferably 5.0 nm or less, more preferably 2.0 nm or less, even more preferably 1.5 nm or less, particularly preferably 1.0 nm or less, and most preferably 0.50 nm or less.
[0148] The glass of this embodiment can be obtained, for example, by melting glass raw materials and forming and cooling the molten glass. At this time, the ratio of tricoordinated boron to tetracoordinated boron can be adjusted by adjusting the average cooling rate of the glass. Here, the average cooling rate refers to the average cooling rate when the formed glass is slowly cooled. A slower average cooling rate reduces the content of tricoordinated boron, thereby improving fracture toughness. Specifically, the cooling rate is preferably 400°C / min or less, more preferably 300°C / min or less, even more preferably 250°C / min or less, even more preferably 200°C / min or less, particularly preferably 150°C / min or less, and most preferably 100°C / min or less.
[0149] The average cooling rate can be calculated as follows: The composition of the glass for which the average cooling rate is to be calculated is analyzed, and multiple glasses with the same composition are prepared at different average cooling rates. The refractive indices of the multiple glasses prepared are measured, and a calibration curve of the average cooling rate and the refractive index is created. By determining the refractive index of the glass for which the average cooling rate is to be calculated, the average cooling rate can be calculated from the calibration curve. The refractive index can be measured, for example, by the V-block method.
[0150] The glass of the present embodiment is preferably float glass formed by, for example, the well-known float method, in which a molten glass base is floated on a molten metal such as tin, and strict temperature control is used to form glass with uniform thickness and width, as well as large area glass.
[0151] The glass of the present embodiment may be glass formed by a known roll-out method or down-draw method, or may be glass with a polished surface and a uniform thickness. Here, the down-draw method is broadly divided into a slot down-draw method and an overflow down-draw method (fusion method), both of which are techniques for continuously letting molten glass flow down from a forming body to form a band-shaped glass ribbon.
[0152] The glass of this embodiment may be glass that has been subjected to tempering treatment such as air-cooling tempering or chemical tempering. By performing the above treatment, the strength of the glass can be increased.
[0153] Here, air-cooling tempering is a process in which a compressive stress layer is formed on the surface of glass by thermal tempering. Specifically, uniformly heated glass is rapidly cooled from a temperature near its softening point, and compressive stress is formed on the surface of the glass due to the temperature difference between the surface and the interior of the glass. The compressive stress is generated uniformly over the entire surface of the glass, and a compressive stress layer of uniform depth is formed over the entire surface of the glass. Thermal tempering is more suitable for tempering thick glass than chemical tempering.
[0154] Chemical strengthening is a process in which alkali metal ions with a small ionic radius (typically Li ions or Na ions) on the surface of glass are exchanged with alkali metal ions with a larger ionic radius (typically Na ions or K ions) by ion exchange at a temperature below the glass transition temperature, thereby forming a compressive stress layer on the surface of the glass. Chemical strengthening can be performed by known methods, such as ion exchange. In the ion exchange process, a glass plate is immersed in a treatment solution (e.g., potassium nitrate molten salt) and ions with a small ionic radius (e.g., Na ions) contained in the glass are exchanged with ions with a large ionic radius (e.g., K ions), thereby generating compressive stress on the surface of the glass.
[0155] The magnitude of the compressive stress on the surface of the glass (hereinafter also referred to as surface compressive stress CS) and the depth DOL of the compressive stress layer formed on the surface of the glass can be adjusted by the glass composition, chemical strengthening treatment time, and chemical strengthening treatment temperature, respectively.
[0156] [Bent Glass] The bent glass according to this embodiment is made of the above-described glass. That is, it is formed by bending the glass of this embodiment. The bent glass according to this embodiment may be bent glass obtained by forming the flat glass of this embodiment into a curved shape by gravity forming, press forming, or the like.
[0157] The curved glass of this embodiment is glass that curves at a predetermined curvature, and may be single-curved glass that curves in only one direction, either up and down or left and right, or double-curved glass that curves in both up and down and left and right directions.
[0158] The minimum radius of curvature of the bent glass of this embodiment is preferably 50 mm or more and 100,000 mm or less. The radius of curvature of the bent glass is calculated by performing a shape simulation on a sample using a laser displacement meter (Dyvoce manufactured by Kohzu Seiki Co., Ltd.) based on the amount of warp inherent to the sample determined by weight deflection correction in a double-sided differential mode, and the radius of curvature is determined from the shape obtained by the simulation.
[0159] [Method for Manufacturing Curved Glass] In the method for manufacturing bent glass according to this embodiment, the glass is heated and bent to form bent glass. Examples of methods for forming bent glass include a method in which flat glass is heated, placed on a forming mold, and pressed from above by a press to bend it. Another example is a method in which flat glass is placed on a forming mold having a bending surface corresponding to the desired curved surface, and the forming mold is then carried into a heating furnace in this state, where the glass is heated to near the glass softening point temperature. According to this forming method, the glass is softened and curved along the bending surface of the forming mold due to its own weight, thereby producing bent glass having the desired curved surface.
[0160] In this embodiment, bending by the press means is preferred from the viewpoint of improving productivity and improving surface accuracy after forming. The bending method by the press means is not particularly limited, and for example, the method described in International Publication No. 2016 / 093031 can be appropriately adopted. Hereinafter, the bending method by the press means will be described as an example.
[0161] First, the glass of this embodiment is transported to a press area by a transport conveyor or the like. Then, in the press area, the glass is heated to a temperature at which it can be bent and softened. Here, the bendable temperature is, for example, a temperature at which the glass viscosity is 10 12 [dPa s] Temperature T 12 The heating may be performed by a heater in a heating furnace during the process of transporting the material to the pressing area on a transport conveyor or the like. 12 The bending time under the condition of maintaining the above condition can be set to, for example, 1 second or more.
[0162] A lower press mold (female mold) and an upper press mold (male mold) are arranged at predetermined positions in the press area, and the upper surface shape of the female mold and the lower surface shape of the male mold correspond to the curved shape of the glass to be bent in the conveying direction and the perpendicular direction. The female mold can be raised and lowered between a standby position below the conveyor and a press position above it, and after the glass is transferred from the conveyor, the female mold, with the glass placed on it, is raised from a predetermined raised position to a press position above the conveyor, thereby press-forming the glass.
[0163] Next, the press-formed glass is transported to a cooling area by a transport shuttle, etc. In the cooling area, the glass is cooled by blowing cooled air onto it, etc.
[0164] The above steps result in the formation of a curved glass. Although the above has been described with respect to the bending of glass according to this embodiment, the bending may also be carried out in the form of laminated glass, which will be described later.
[0165] [Laminated Glass] The laminated glass according to this embodiment includes a first glass plate, a second glass plate, and an interlayer film sandwiched between the first glass plate and the second glass plate, and the first glass plate is the glass according to this embodiment or the bent glass according to this embodiment.
[0166] FIG. 5 is a diagram showing an example of a laminated glass 10 according to this embodiment. The laminated glass 10 includes a first glass sheet 11, a second glass sheet 12, and an interlayer film 13 sandwiched between the first glass sheet 11 and the second glass sheet 12. The laminated glass 10 according to this embodiment is not limited to the configuration shown in FIG. 5 and can be modified without departing from the spirit of this embodiment. For example, the interlayer film 13 may be formed of a single layer as shown in FIG. 5 or may be formed of two or more layers. The laminated glass 10 according to this embodiment may also include three or more glass sheets, in which case an organic resin or the like may be interposed between adjacent glass sheets. Hereinafter, the laminated glass 10 according to this embodiment will be described as having only two glass sheets, a first glass sheet 11 and a second glass sheet 12, sandwiching the interlayer film 13.
[0167] In the laminated glass of the present embodiment, from the viewpoint of bend formability, the second glass sheet 12 is preferably the glass of the present embodiment or the bent glass of the present embodiment. When the first glass sheet 11 and the second glass sheet 12 are the glass of the present embodiment or the bent glass of the present embodiment, the first glass sheet 11 and the second glass sheet 12 may be glass sheets having the same composition or glass sheets having different compositions.
[0168] When the second glass plate 12 is not the glass of this embodiment, the type of the glass plate is not particularly limited, and any conventionally known glass plate used for vehicle window glass, etc., can be used. Specific examples include alkali aluminosilicate glass, alkali aluminoborosilicate glass, and soda-lime glass. These glass plates may or may not be colored to the extent that their transparency is not impaired.
[0169] In this embodiment, the second glass plate 12 is made of Al 2 O 3Alkali aluminosilicate glass containing 1.0% or more of Al 2 O 3 Contains 1.0% or more of B 2 O 3 By using the alkali aluminosilicate glass or alkali aluminoborosilicate glass for the second glass plate 12, chemical strengthening becomes possible as described below, and strength can be increased.
[0170] The alkali aluminosilicate glass and alkali aluminoborosilicate glass are made of Al, from the viewpoint of improving weather resistance, moisture resistance, and chemical strengthening properties. 2 O 3 The content of Al is more preferably 5.0% or more, further preferably 8.0% or more, and particularly preferably 10% or more. 2 O 3 The content is preferably 18% or less, more preferably 15% or less.
[0171] The alkali aluminosilicate glass and alkali aluminoborosilicate glass are R 2 The content of O is preferably 10% or more, more preferably 12% or more, and even more preferably 13% or more. 2 The O content is preferably 22% or less, more preferably 20% or less, and even more preferably 18% or less.
[0172] The alkali aluminoborosilicate glass is made of B to increase its strength when it comes into contact with flying stones, car keys, etc. 2 O 3 The content of B is preferably 2.0% or more, more preferably 3.0% or more, and even more preferably 4.0% or more. In alkali aluminoborosilicate glass, from the viewpoint of improving chemical durability and weather resistance, B 2 O 3 The content is preferably 9.0% or less, more preferably 8.0% or less, and even more preferably 7.0% or less.
[0173] Specific examples of the alkali aluminosilicate glass include glasses having the following compositions, where each component is expressed as a mole percentage based on oxide: 61%≦SiO 2 ≦75% 1.0%≦Al 2 O 3 ≦20% 0.0%≦MgO≦15% 0.0%≦CaO≦10% 0.0%≦SrO≦1.0% 0.0%≦BaO≦1.0% 0.0%≦Li 2 O≦15% 2.0%≦Na 2 O≦15% 0.0%≦K 2 O≦6.0% 0.0%≦ZrO 2 ≦4.0% 0.0%≦TiO 2 ≦1.0% 0.0%≦Y 2 O 3 ≦2.0% 10%≦R 2 O≦25% 0.0%≦RO≦20% (R 2 O is Li 2 O, Na 2 O and K 2 RO represents the total content of MgO, CaO, SrO, and BaO.
[0174] Specific examples of the alkali aluminoborosilicate glass include glasses having the following compositions, where each component is expressed as a mole percentage based on oxide: 61%≦SiO 2 ≦75% 1.0%≦Al 2 O 3 ≦20% 1.0%≦B 2 O 3 ≦10% 0.0%≦MgO≦15% 0.0%≦CaO≦10% 0.0%≦SrO≦1.0% 0.0%≦BaO≦1.0% 0.0%≦Li 2 O≦15% 2.0%≦Na 2 O≦15% 0.0%≦K 2 O≦6.0% 0.0%≦ZrO 2 ≦4.0% 0.0%≦TiO 2 ≦1.0% 0.0%≦Y 2 O 3 ≦2.0% 10%≦R 2 O≦25% 0.0%≦RO≦20% (R2 O is Li 2 O, Na 2 O and K 2 RO represents the total content of MgO, CaO, SrO, and BaO.
[0175] In the laminated glass of this embodiment, the second glass sheet 12 may be soda lime glass. 2 O 3 The soda-lime glass may contain 3.5% or less, preferably less than 1.0% of SiO. Specifically, examples of the glass include the following compositions. Each component is expressed in mole percentage based on oxide. 60%≦SiO 2 ≦75% 0.0%≦Al 2 O 3 ≦3.5% 2.0%≦MgO≦11% 2.0%≦CaO≦10% 0.0%≦SrO≦3.0% 0.0%≦BaO≦3.0% 10%≦Na 2 O≦18% 0.0%≦K 2 O≦8.0% 0.0%≦ZrO 2 ≦4.0% 0.0010%≦Fe 2 O 3 ≦5.0%
[0176] The thickness of the first glass plate 11 is preferably 2.5 mm or more. By making the thickness of the first glass plate 11 2.5 mm or more, the critical impact fracture speed of glass having a high fracture toughness value can be improved. The thickness of the first glass plate 11 is more preferably 2.8 mm or more, even more preferably 2.9 mm or more, even more preferably 3.0 mm or more, particularly preferably 3.1 mm or more, even more preferably 3.2 mm or more, even more preferably 3.3 mm or more, particularly preferably 3.4 mm or more, and most preferably 3.5 mm or more.
[0177] Furthermore, from the viewpoint of suppressing increases in fuel consumption and electricity consumption due to an increase in the weight of the glass, the thickness of the first glass plate 11 is preferably 5.0 mm or less, more preferably 4.8 mm or less, even more preferably 4.5 mm or less, particularly preferably 4.2 mm or less, and most preferably 4.0 mm or less.
[0178] The thickness of the second glass plate 12 is preferably 0.50 mm or more, more preferably 0.60 mm or more, even more preferably 0.70 mm or more, particularly preferably 0.80 mm or more, particularly preferably 0.90 mm or more, and most preferably 1.0 mm or more. A thickness of 0.50 mm or more is preferable from the viewpoint of impact resistance.
[0179] The thickness of the second glass sheet 12 is preferably 2.0 mm or less, more preferably 1.9 mm or less, even more preferably 1.8 mm or less, particularly preferably 1.7 mm or less, particularly preferably 1.6 mm or less, and most preferably 1.5 mm or less. A thickness of 2.0 mm or less for the second glass sheet 12 prevents the weight of the laminated glass 10 from becoming too large, which is preferable in terms of improving fuel efficiency when used in a vehicle.
[0180] The thicknesses of the first glass plate 11 and the second glass plate 12 may be the same or different, but it is preferable that the first glass plate 11 is thicker than the second glass plate 12. Methods for adjusting the thickness of the first glass plate 11 and the second glass plate 12 include adjusting the glass thickness using a float method or a down-draw method, or polishing the glass in the thickness direction with a grinding stone and then polishing it to a mirror finish using an abrasive such as cerium oxide. The surface roughness Ra after molding or polishing is preferably 5.0 nm or less, more preferably 2.0 nm or less, even more preferably 1.5 nm or less, particularly preferably 1.0 nm or less, and most preferably 0.50 nm or less.
[0181] In the laminated glass 10 of this embodiment, the thickness of the first glass sheet 11 and the second glass sheet 12 may be constant over the entire surface, or may vary from location to location as needed, such as forming a wedge shape in which the thickness of one or both of the first glass sheet 11 and the second glass sheet 12 gradually decreases.
[0182] At least one of the first glass plate 11 and the second glass plate 12 may be chemically strengthened glass that has been tempered to improve its strength. The chemical strengthening method is the same as the chemical strengthening method for glass described above. Examples of chemically strengthened glass include the alkali aluminosilicate glass and the alkali aluminoborosilicate glass that have been chemically strengthened.
[0183] The first glass sheet 11 and the second glass sheet 12 may have a flat shape or a curved shape having a curvature entirely or partially. If the first glass sheet 11 and the second glass sheet 12 are curved, they may have a single-curve shape, i.e., a curved shape in only one of the vertical or horizontal directions, or a complex-curve shape, i.e., a curved shape in both the vertical and horizontal directions. If the first glass sheet 11 and the second glass sheet 12 are curved, the radius of curvature in the vertical and horizontal directions may be the same or different. If the first glass sheet 11 and the second glass sheet 12 are curved, the radius of curvature in the vertical and / or horizontal directions is preferably 1000 mm or more. The shapes of the main surfaces of the first glass sheet 11 and the second glass sheet 12 are adapted to fit the window opening of the vehicle in which they are installed.
[0184] The interlayer film 13 is sandwiched between the first glass sheet 11 and the second glass sheet 12. By including the interlayer film 13, the laminated glass 10 of this embodiment can firmly bond the first glass sheet 11 and the second glass sheet 12 together and can also absorb the impact force when flying fragments collide with the glass sheets.
[0185] Various organic resins that are commonly used in laminated glass for conventional vehicles can be used as the interlayer film 13. Examples of organic resins include polyethylene (PE), ethylene vinyl acetate copolymer (EVA), polypropylene (PP), polystyrene (PS), methacrylic resin (PMA), polyvinyl chloride (PVC), polyethylene terephthalate (PET), polybutylene terephthalate (PBT), cellulose acetate (CA), diallyl phthalate resin (DAP), urea resin (UP), melamine resin (MF), unsaturated polyester (UP), polyvinyl butyral (PVB), and polyvinyl hol. Examples of materials that can be used include marl (PVF), polyvinyl alcohol (PVAL), vinyl acetate resin (PVAc), ionomer (IO), polymethylpentene (TPX), vinylidene chloride (PVDC), polysulfone (PSF), polyvinylidene fluoride (PVDF), methacrylic-styrene copolymer resin (MS), polyarate (PAR), polyallylsulfone (PASF), polybutadiene (BR), polyethersulfone (PESF), and polyetheretherketone (PEEK). Among these, EVA and PVB are preferred from the viewpoints of transparency and adhesion, and PVB is particularly preferred because it can impart sound insulation properties.
[0186] From the viewpoints of impact force absorption and sound insulation, the thickness of the interlayer film 13 is preferably 0.300 mm or more, more preferably 0.500 mm or more, and even more preferably 0.700 mm or more. From the viewpoint of suppressing a decrease in visible light transmittance, the thickness of the interlayer film 13 is preferably 1.00 mm or less, more preferably 0.900 mm or less, and even more preferably 0.800 mm or less. The thickness of the interlayer film 13 is preferably in the range of 0.300 mm to 1.00 mm, and more preferably in the range of 0.700 mm to 0.800 mm.
[0187] The thickness of the intermediate film 13 may be constant over the entire surface, or may vary from place to place as required.
[0188] If the difference in linear expansion coefficient between the interlayer film 13 and the first glass sheet 11 or the second glass sheet 12 is large, cracks or warping may occur in the laminated glass 10 when the laminated glass 10 is produced through the heating step described below, which may result in poor appearance. Therefore, it is preferable that the difference in linear expansion coefficient between the interlayer film 13 and the first glass sheet 11 or the second glass sheet 12 is as small as possible. The difference in linear expansion coefficient between the interlayer film 13 and the first glass sheet 11 or the second glass sheet 12 may be expressed as the difference between the average linear expansion coefficients within a predetermined temperature range.
[0189] In particular, since the resin constituting the interlayer film 13 has a low glass transition temperature, a predetermined difference in the average linear expansion coefficient may be set within a temperature range below the glass transition temperature of the resin material. The difference in the linear expansion coefficient between the first glass sheet 11 or the second glass sheet 12 and the resin material may be set at a predetermined temperature below the glass transition temperature of the resin material.
[0190] Alternatively, an adhesive layer containing an adhesive may be used for interlayer film 13. The adhesive is not particularly limited, but examples thereof include an acrylic adhesive, a silicone adhesive, etc. When interlayer film 13 is an adhesive layer, a heating step is not required in the process of joining first glass plate 11 and second glass plate 12, and therefore the risk of the above-mentioned cracking or warping occurring is reduced.
[0191] [Other Layers] The laminated glass 10 of the present embodiment may include layers (hereinafter also referred to as "other layers") other than the first glass sheet 11, the second glass sheet 12, and the interlayer film 13, provided that the effects of the present embodiment are not impaired. For example, the laminated glass 10 may include a coating layer that imparts water-repellent properties, hydrophilic properties, anti-fogging properties, or the like, an infrared reflective film, or the like.
[0192] The positions at which the other layers are provided are not particularly limited, and the other layers may be provided on the surface of the laminated glass 10, or may be sandwiched between the first glass sheet 11, the second glass sheet 12, or the interlayer film 13. The laminated glass 10 of this embodiment may also include a black ceramic layer or the like arranged in a strip shape along part or all of the peripheral edge for the purpose of concealing the attachment portion to the frame or the wiring conductors.
[0193] In the laminated glass 10 of this embodiment, the first glass sheet 11 has a surface roughness Ra of 5.0 nm or less and a thickness of 2.5 mm. When a tungsten carbide alloy having a tip curvature radius of 200 μm, an apex angle of 120°, and a weight of 1.365 g is collided with the surface of the first glass sheet 11, the critical impact fracture speed is preferably 35 km / h or more. A critical impact fracture speed of 35 km / h or more can improve resistance to flying stones. The critical impact fracture speed is more preferably 40 km / h or more, even more preferably 45 km / h or more, particularly preferably 50 km / h or more, and most preferably 60 km / h or more. The upper limit of the critical impact fracture speed is, for example, 120 km / h or less.
[0194] Furthermore, the laminated glass of this embodiment preferably has a critical impact fracture speed of 55 km / h or more when a tungsten carbide alloy having a tip curvature radius of 200 μm, an apex angle of 120°, and a weight of 1.365 g is struck against the surface of the first glass sheet 11. A critical impact fracture speed of 55 km / h or more can further improve resistance to flying stones. The critical impact fracture speed is more preferably 57 km / h or more, even more preferably 60 km / h or more, even more preferably 62 km / h or more, particularly preferably 64 km / h or more, particularly preferably 66 km / h or more, particularly preferably 68 km / h or more, and most preferably 70 km / h or more. The upper limit of the critical impact fracture speed is, for example, 120 km / h or less.
[0195] The total thickness of the first glass plate 11, the second glass plate 12, and the interlayer film 13 is preferably 4.5 mm or more. In particular, when the laminated glass of this embodiment has the above-mentioned properties, the total thickness of the first glass plate 11, the second glass plate 12, and the interlayer film 13 is preferably 4.5 mm or more. A total thickness of 4.5 mm or more can improve sound insulation. The total thickness is more preferably 4.6 mm or more, even more preferably 4.7 mm or more, even more preferably 4.8 mm or more, particularly preferably 4.9 mm or more, and most preferably 5.0 mm or more. Furthermore, from the viewpoint of weight reduction, the total thickness is preferably 8.0 mm or less, more preferably 7.8 mm or less, even more preferably 7.6 mm or less, particularly preferably 7.4 mm or less, particularly preferably 7.2 mm or less, and most preferably 7.0 mm or less. When the total thickness of the first glass plate 11, the second glass plate 12, and the interlayer film 13 varies depending on the location, it is preferable that the total thickness at the thinnest location be 4.5 mm or more.
[0196] In addition, the laminated glass of this embodiment has a thickness t 1 and the thickness t of the second glass plate 2 The ratio (t 1 / t 2 It is preferable that the ratio (t 1 / t 2 When the ratio (t) is 1.5 or more, a high critical impact destruction speed can be achieved. 1 / t 2 ) is more preferably 2.0 or more, even more preferably 2.5 or more, even more preferably 3.0 or more, particularly preferably 3.5 or more, and most preferably 4.0 or more. In addition, in order to approximate the curvature when the glass after bending is made into laminated glass, the ratio (t 1 / t 2 ) is preferably 6.0 or less, more preferably 5.5 or less, and even more preferably 5.0 or less.
[0197] When the laminated glass 10 of this embodiment is used as a vehicle glass, the visible light transmittance Tv as defined in ISO-9050:2003 using a D65 light source is preferably 70% or more, more preferably 71% or more, and even more preferably 72% or more. Furthermore, Tv is, for example, 90% or less.
[0198] When used as vehicle glass, the laminated glass 10 of this embodiment preferably has a total solar transmittance (Tts) of 70% or less, as defined in ISO-13837:2008 Convention A and measured at a wind speed of 4 m / s. When the total solar transmittance (Tts) of the laminated glass 10 of this embodiment is 70% or less, sufficient heat-shielding properties are obtained. Tts is more preferably 68% or less, and even more preferably 66% or less. Furthermore, Tts is, for example, 55% or more.
[0199] The laminated glass 10 of this embodiment can be manufactured by a method similar to that of conventionally known laminated glass. For example, by laminating a first glass sheet 11, an interlayer film 13, and a second glass sheet 12 in this order and then subjecting them to a heating and pressurizing process, a laminated glass 10 is obtained in which the first glass sheet 11 and the second glass sheet 12 are bonded together via the interlayer film 13.
[0200] The method for manufacturing the laminated glass 10 of this embodiment may, for example, include a step of heating and shaping the first glass sheet 11 and the second glass sheet 12, followed by a step of inserting the interlayer film 13 between the first glass sheet 11 and the second glass sheet 12 and applying heat and pressure. By performing these steps, the laminated glass 10 may be configured such that the first glass sheet 11 and the second glass sheet 12 are joined together via the interlayer film 13.
[0201] [Uses] The glass of this embodiment can be suitably used for both vehicles and sensors, and more specifically, can be suitably used as window glass or cover glass for sensors in vehicles. In particular, the glass of this embodiment has excellent fracture toughness, low viscosity, and low density, and is therefore suitable for components such as window glass in vehicles, specifically windshields, side windows, rear windows, and roof windows. From the same perspective, the glass can be suitably used as cover glass for sensors such as LiDAR, cameras, and millimeter-wave radar mounted on vehicles and unmanned or manned eVTOLs (Electric Vertical Take-Off and Landing aircraft) such as drones.
[0202] An example of a specific application in which the glass of this embodiment is used as a window glass for a vehicle will be described below with reference to the drawings. Fig. 6 is a conceptual diagram showing a state in which a laminated glass 10 including the glass of this embodiment is installed in an opening 110 formed in the front of an automobile 100 and used as the window glass of the automobile. The laminated glass 10 used as the window glass of an automobile may have a housing (case) 120, which houses an information device or the like, attached to its surface on the interior side of the vehicle to ensure the driving safety of the vehicle.
[0203] The information device housed in the housing is a device that uses a camera, radar, etc. to prevent rear-end collisions with vehicles ahead, pedestrians, obstacles, etc., and to alert the driver to danger. For example, it is an information receiving device and / or information transmitting device, etc., and includes millimeter-wave radar, stereo cameras, infrared lasers, etc., which send and receive signals. The "signal" refers to electromagnetic waves including millimeter waves, visible light, infrared light, etc.
[0204] 7 is an enlarged view of the portion S in FIG. 6 and is a perspective view showing the portion of the laminated glass 10 of this embodiment where the housing 120 is attached. The housing 120 houses a millimeter-wave radar 201 and a stereo camera 202 as information devices. The housing 120 housing the information devices is usually attached on the outer side of the vehicle relative to the rearview mirror 150 and on the inner side of the vehicle relative to the laminated glass 10, but may also be attached to other portions.
[0205] 8 is a cross-sectional view taken along line Y-Y in FIG. 7 and perpendicular to the horizontal line. It is preferable that the first glass sheet 11 of the laminated glass 10 be disposed on the exterior side of the vehicle. This configuration makes it possible to realize a lightweight windshield with excellent fracture toughness. Furthermore, because the glass of this embodiment has low viscosity, it can be easily bent when manufacturing the windshield.
[0206] As described above, the present specification discloses the following configurations: <1> Li, expressed in mole percent on an oxide basis, 2 Substantially does not contain O, SiO 2 : 70-80% B 2 O 3 : 10 to 17% Al 2 O 3 :1.0~6.0% MgO:0.0~5.0% CaO:0.0~5.0% SrO:0.0~5.0% BaO:0.0~5.0% Na 2 O: 0.0-19% K 2 O: 0.0~10% R' 2 O: 6.0 to 19% RO: 0.0 to 5.0% (wherein RO is at least one selected from MgO, CaO, SrO, and BaO; R' 2 O is Na 2 O.K. 2 (R' is at least one selected from 2 O] + 1 / 2 [RO] - [Al 2 O 3 ])-[B 2 O 3]≧−6.5 (where [ ] means the content of each component in the brackets expressed in mole percent based on the oxide), and <2> the content of tricoordinated boron is B 2 O 3 <3> The glass for vehicles and sensors according to <1>, wherein the content of SiO is 10 mol % or less in terms of mol % based on oxides. 2 : 70-80% B 2 O 3 : 10 to 17% Al 2 O 3 :1.0~6.0% MgO:0.0~5.0% CaO:0.0~5.0% SrO:0.0~5.0% BaO:0.0~5.0% Li 2 O: More than 0 to 15% Na 2 O: 3.5-15% K 2 O: 0.0~10% R 2 O: 6.0 to 19% RO: 0.0 to 5.0% (wherein RO is at least one selected from MgO, CaO, SrO, and BaO; R 2 O is Li 2 O, Na 2 O.K. 2 O), and 2 O] + 1 / 2 [RO] - [Al 2 O 3 ])-[B 2 O 3 ]≧−10.0 (where [ ] means the content of each component in the brackets expressed in mole percent based on the oxide), and <4> the content of tricoordinated boron is B 2 O 3 <5> The glass for vehicles and sensors according to any one of <1> to <4>, having a Young's modulus of 65 GPa or more. <6> The glass for vehicles and sensors according to <5>, having a fracture toughness value K measured by the SEPB method. IC is 0.76 MPa m 1/2 <7> The glass for vehicles and sensors according to any one of <1> to <5>, wherein the glass viscosity is 10 or more. 11 Temperature T at which viscosity becomes dPa s 11<8> The glass for vehicles and sensors according to any one of <1> to <6>, having a Young's modulus of 70 GPa or more, <9> a fracture toughness value K measured by the SEPB method, IC is 0.80 MPa m 1/2 The glass for vehicles and sensors according to <8>, which has a surface roughness Ra of 5.0 nm or less and a thickness of 2.5 mm, and when a tungsten carbide cemented carbide having a tip curvature radius of 200 μm, an apex angle of 120°, and a weight of 1.365 g is collided with the glass for vehicles and sensors according to any one of <1> to <9>, the critical impact fracture speed is 35 km / h or more when the glass is collided with a tungsten carbide cemented carbide having a tip curvature radius of 200 μm, an apex angle of 120°, and a weight of 1.365 g. <11> The glass for vehicles and sensors according to any one of <1> to <9>, which has a critical impact fracture speed of 55 km / h or more when the glass is collided with a tungsten carbide cemented carbide having a tip curvature radius of 200 μm, an apex angle of 120°, and a weight of 1.365 g. <12> The glass for vehicles and sensors according to any one of <1> to <11>, which has a thickness of 2.5 mm or more. <13> A curved glass comprising the glass for vehicles and sensors according to any one of <1> to <12>. <14> A laminated glass comprising a first glass plate, a second glass plate, and an interlayer film sandwiched between the first glass plate and the second glass plate, wherein the first glass plate is the glass for vehicles and sensors described in any one of <1> to <12>. <15> The laminated glass described in <14>, wherein the first glass plate has a surface roughness Ra of 5.0 nm or less and a thickness of 2.5 mm, and wherein a critical impact fracture speed when a tungsten carbide alloy having a tip curvature radius of 200 μm, an apex angle of 120°, and a weight of 1.365 g is collided with a surface of the first glass plate is 35 km / h or more. <16> The laminated glass described in <14>, wherein a critical impact fracture speed when a tungsten carbide alloy having a tip curvature radius of 200 μm, an apex angle of 120°, and a weight of 1.365 g is collided with a surface of the first glass plate is 55 km / h or more. <17> The laminated glass according to <14> or <16>, wherein the total thickness of the first glass plate, the second glass plate, and the interlayer film is 4.5 mm or more. <18> The thickness t of the first glass plate 1 and the thickness t of the second glass plate2 The ratio (t 1 / t 2 <19> The laminated glass according to any one of <14> to <18>, wherein the second glass sheet is the glass for a vehicle or a sensor according to any one of <1> to <12>. <20> The laminated glass according to any one of <14> to <18>, wherein the second glass sheet is soda lime glass. <21> The laminated glass according to any one of <14> to <18>, wherein the second glass sheet is aluminosilicate glass. <22> The laminated glass according to any one of <14> to <18>, wherein the second glass sheet has been subjected to a chemical strengthening treatment.
[0207] The present invention will be specifically described below with reference to examples, but the present invention is not limited thereto.
[0208] <Preparation of Glass Plates of Examples 1 to 30> Raw materials were placed in a platinum crucible and melted at a temperature of 1600°C to 1650°C for 3 hours to obtain molten glass so as to obtain the glass compositions (unit: mol%) shown in Tables 1 and 2. The molten glass was poured onto a carbon plate and heated to a temperature above the glass transition temperature, T 11 The glass was maintained at the following temperature for 3 hours and then slowly cooled at an average cooling rate of 1°C / min. Both surfaces of the obtained glass plate were polished to obtain glass plates with thicknesses of 2.0 mm and 4.0 mm. Examples 1 to 21 are working examples, and Examples 22 to 30 are comparative examples.
[0209] The glass plates obtained above were subjected to the following evaluations, and the results are shown in Tables 1 and 2. In the tables, blank spaces indicate that no measurement was performed, and "-" indicates that the glass plates were not B. 2 O 3 Indicates that measurement is not possible because the substance is not contained.
[0210] (1) Boron Coordination Number: The proportion of the coordination number of boron atoms in the glass was analyzed by NMR. The NMR measurement conditions are as follows: Measurement apparatus: JEOL ECZ700 nuclear magnetic resonance apparatus; Resonance frequency: 156.38 MHz; Rotation speed: 15 kHz; Probe: 3.2 mm for solids; Flip angle: 90°; Pulse repetition waiting time: 16 sec. Measurement was performed using the single pulse method, with adamantane as the external standard (C 28.46 ppm and 37.85 ppm). The measurement results were subjected to phase correction and baseline correction using JEOL NMR software Delta, followed by fitting using a Gaussian function to calculate the proportions of three- and four-coordination, and the average coordination number was determined. Phase correction and baseline correction were appropriately processed by subtracting the spectrum of an empty cell containing no sample. Regarding peak fitting, the peak top was set at 20-8 ppm for tricoordinated boron and 5-5 ppm for tetracoordinated boron, and good fitting was obtained by appropriately setting the peak width (so that the ratio between each coordination number was 1.5 times or less at most). In addition, from the ratio of tricoordinated boron and tetracoordinated boron obtained above, B 2 O 3 The converted tricoordinate boron content (B 3 as B 2 O 3 [mol%]) and B 2 O 3 The converted tetracoordinate boron content (B 4 as B 2 O 3 [mol %]) were calculated and are shown in Tables 1 and 2.
[0211] (2) Temperature T 2 , temperature T 4 : The glass viscosity η, which is the standard for the melting property of glass, is 10 2 Temperature T when viscosity becomes dPa s 2 and the glass viscosity η is 10 4 Temperature T at which viscosity becomes dPa s 4 was measured using a rotational viscometer.
[0212] (3) Glass transition temperature (T g): Values measured using TMA and determined in accordance with JIS R3103-3 (2001).
[0213] (4) Temperature T 11 , temperature T 12 Viscosity η, which is the standard for glass bending workability, is 10 11 Temperature T when viscosity becomes dPa s 12 and the viscosity η, which is the standard for bending workability, is 10 12 Temperature T when viscosity becomes dPa s 12 and were measured using the beam bending method.
[0214] (5) Average coefficient of linear expansion (CTE) from 50 to 350 °C 50-350 ): Measured using a differential thermal dilatometer (TMA) and determined in accordance with JIS R3102 (1995).
[0215] (6) Density: A glass block of about 20 g containing no bubbles cut out from a glass plate was measured by Archimedes' method.
[0216] (7) Young's modulus: Measured at 25° C. by an ultrasonic pulse method (Olympus, DL35) based on JIS R1602:1995 "Testing method for elastic modulus of fine ceramics."
[0217] (8) Rigidity Modulus: Measured at 25°C by an ultrasonic pulse method (Olympus, DL35) based on JIS R1602:1995 "Testing Method for Elastic Modulus of Fine Ceramics".
[0218] (9) Poisson's ratio: Measured at 25° C. by an ultrasonic pulse method (Olympus, DL35) based on JIS R1602:1995 "Testing method for elastic modulus of fine ceramics."
[0219] (10) Fracture toughness value @ SEPB method The fracture toughness of the glass plate obtained above was measured using a pre-crack introduction fracture test method (SEPB method: Single-Edge-Precracked-Beam method) based on JIS R1607:2015 “Fracture toughness test method for fine ceramics”.
[0220] (11) Surface Fracture Energy: Calculated using the Young's modulus and fracture toughness values obtained above according to the above formula (1).
[0221]
[0222]
[0223] The glasses of Examples 1 to 21 have high fracture toughness or Young's modulus, low density, and a high fracture toughness at temperature T 11 On the other hand, Example 22, which is a comparative example, had a low SiO 2 is less than 70%, and B 2 O 3 Does not contain Al 2 O 3 was less than 1.0%, MgO was more than 5.0%, CaO was more than 5.0%, and RO was more than 5.0%, so the fracture toughness was poor and the density was high.
[0224] In addition, Example 23 is excellent in Young's modulus, but SiO 2 is less than 70%, and B 2 O 3 is less than 10%, and Al 2 O 3 is more than 6.0%, MgO is more than 5.0%, and RO is more than 5.0%, so T g and T 12 was high.
[0225] Also, Example 24 is SiO 2 is more than 80%, and R' 2 Since the content of O is less than 6.0%, the fracture toughness value and Young's modulus are small, and further, the temperature T 11 In addition, Example 25 had a low density, but 2 O] + 1 / 2 [RO]) - [Al 2 O 3 ]-[B 2 O 3 ] was less than −6.5, the fracture toughness and Young's modulus were smaller than those of the examples.
[0226] In addition, Example 26 has a low density, but Al 2 O 3 is more than 6.0%, ([R' 2O] + 1 / 2 [RO]) - [Al 2 O 3 ]-[B 2 O 3 ] was less than −6.5, so the Young's modulus was low. 2 is less than 70%, and Al 2 O 3 is more than 6.0%, ([R' 2 O] + 1 / 2 [RO]) - [Al 2 O 3 ]-[B 2 O 3 ] was less than −6.5, so that the Young's modulus was low.
[0227] In addition, although Examples 28 and 29 have low density, ([R' 2 O] + 1 / 2 [RO]) - [Al 2 O 3 ]-[B 2 O 3 ] was less than −6.5, so that the Young's modulus was low. 2 O 3 is less than 10%, and Al 2 O 3 is more than 6.0%, ([R' 2 O] + 1 / 2 [RO]) - [Al 2 O 3 ]-[B 2 O 3 ] was less than −6.5, so that the Young's modulus was low.
[0228] <Preparation of Laminated Glass> Laminated glasses of Test Examples 1 to 7 were prepared according to the following procedure. Test Examples 1 to 4 are comparative examples, and Test Examples 5 to 7 are working examples.
[0229] (Test Example 1) As the first glass plate, glass having a thickness of 2.0 mm, a surface roughness Ra of 2.0 nm or less, and a composition shown in Example 22 in Table 2 was used. As the interlayer film, polyvinyl butyral (PVB) having a thickness of 0.78 mm was used. As the second glass plate, glass having a thickness of 2.0 mm and a composition shown in Example 22 in Table 2 was used. The first glass plate, the interlayer film, and the second glass plate were laminated in this order, and preliminary bonding was performed at 120°C for 15 minutes, followed by pressure bonding under conditions of 130°C and 1 MPa. The laminated glass of Test Example 1 was then produced by returning to room temperature and atmospheric pressure over 90 minutes. The laminated glass of Test Example 1 had a total thickness of 4.8 mm for the first glass plate, the second glass plate, and the interlayer film, and a thickness of 1.0 mm for the first glass plate. 1 and the thickness t of the second glass plate 2 The ratio (t 1 / t 2 ) was 1.0.
[0230] Test Example 2 A laminated glass was produced in the same manner as in Test Example 1, except that the thicknesses of the first glass plate and the second glass plate were changed to the values shown in Table 3.
[0231] Test Example 3 A laminated glass was produced in the same manner as in Test Example 1, except that the thickness of the first glass plate was changed to the value shown in Table 3 and a soda-lime glass (manufactured by AGC, model number: AS2) having a thickness of 0.7 mm was used as the second glass plate.
[0232] Test Examples 4 to 7 Laminated glasses were produced in the same manner as in Test Example 3, except that the type of the first glass plate was changed to one shown in Table 3 (all of which had a surface roughness Ra of 2.0 nm or less).
[0233] The critical impact fracture velocity Vcrt of the laminated glass sheet obtained above was measured using the following procedure. <Procedure> A tungsten carbide cemented carbide with a tip curvature radius of 200 μm, an apex angle of 120°, and a weight of 1.365 g was injected at a speed of 20 km / h or more and allowed to impact the surface of the first glass sheet. During this impact, the propagation process of a crack generated by the impact of the tungsten carbide cemented carbide was observed from the cross section of the laminated glass using a high-speed camera. The test was carried out while changing the injection velocity, and a crack generated on the surface of the first glass sheet was judged to have occurred when it propagated and reached the surface of the first glass sheet opposite the surface against which the tungsten carbide cemented carbide was impacted. The impact velocity at this time was taken as the critical impact fracture velocity Vcrt.
[0234]
[0235] The laminated glasses of Test Examples 5 to 7, which are working examples, had higher critical impact fracture speeds than the comparative examples.
[0236] This application is based on Japanese Patent Application No. 2023-063642 filed on April 10, 2023, the contents of which are incorporated herein by reference.
[0237] REFERENCE SIGNS LIST 10 Laminated glass 11 First glass sheet 12 Second glass sheet 13 Interlayer 100 Automobile 110 Opening 120 Housing 150 Rearview mirror 201 Millimeter wave radar 202 Stereo camera 300 Radio wave
Claims
1. In mole percent based on oxide, Li 2 Contains substantially no O, SiO 2 : 70-80% B 2 O 3 : 10 to 17% Al 2 O 3 :1.0~6.0% MgO:0.0~5.0% CaO:0.0~5.0% SrO:0.0~5.0% BaO:0.0~5.0% Na 2 O: 0.0-19% K 2 O: 0.0~10% R' 2 O: 6.0 to 19% RO: 0.0 to 5.0% (wherein RO is at least one selected from MgO, CaO, SrO, and BaO; R' 2 O is Na 2 O.K. 2 O), 2 O] + 1 / 2 [RO] - [Al 2 O 3 ])-[B 2 O 3 ]≧−6.5 (where [ ] means the content of each component in the brackets expressed in mol % on the oxide basis), 2. The content of tricoordinate boron is B 2 O 3 The glass for vehicles and sensors according to claim 1, wherein the total amount of the glass is 10 mol % or less in terms of the total amount of the glass.
3. In terms of oxide mole percent, SiO 2 : 70-80% B 2 O 3 : 10 to 17% Al 2 O 3 :1.0~6.0% MgO:0.0~5.0% CaO:0.0~5.0% SrO:0.0~5.0% BaO:0.0~5.0% Li 2 O: More than 0 to 15% Na 2 O: 3.5-15% K 2 O: 0.0~10% R 2 O: 6.0-19% RO: 0.0-5.0% (wherein RO is at least one selected from MgO, CaO, SrO, and BaO; R 2 O is Li 2 O, Na 2 O.K. 2 O), 2 O] + 1 / 2 [RO] - [Al 2 O 3 ])-[B 2 O 3 ]≧−10.0 (where [ ] means the content of each component in the brackets expressed in mol % on the oxide basis), 4. The content of tricoordinate boron is B 2 O 3 The glass for vehicles and sensors according to claim 3, wherein the total amount of the oxides is 10 mol % or less in terms of the total amount of the oxides.
5. The glass for vehicles and sensors according to claim 1 or 3, having a Young's modulus of 65 GPa or more.
6. Fracture toughness value K measured by the SEPB method IC is 0.76MPa·m 1/2 The glass for vehicles and sensors according to claim 5 .
7. Glass viscosity is 10 11 Temperature T at which viscosity becomes dPa·s 11 7. The glass for vehicles and sensors according to claim 6, wherein the glass has a melting point of 640° C. or less.
8. The glass for vehicles and sensors according to claim 7, having a Young's modulus of 70 GPa or more.
9. Fracture toughness value K measured by the SEPB method IC is 0.80MPa·m 1/2 The glass for vehicles and sensors according to claim 8 .
10. The glass for vehicles and sensors according to claim 9, which has a critical impact fracture speed of 35 km / h or more when collided with a tungsten carbide alloy having a tip curvature radius of 200 μm, an apex angle of 120° and a weight of 1.365 g, when the glass has a surface roughness Ra of 5.0 nm or less and a thickness of 2.5 mm.
11. The glass for vehicles and sensors according to claim 9, which has a critical impact fracture speed of 55 km / h or more when collided with a tungsten carbide hard alloy having a tip curvature radius of 200 μm, an apex angle of 120° and a weight of 1.365 g.
12. The glass for vehicles and sensors according to claim 11, having a thickness of 2.5 mm or more.
13. Bent glass comprising glass for vehicles and sensors according to claim 1 or 3.
14. A laminated glass comprising a first glass plate, a second glass plate, and an intermediate film sandwiched between the first glass plate and the second glass plate, wherein the first glass plate is the glass for vehicles and sensors according to claim 1 or 3.
15. The laminated glass according to claim 14, wherein the first glass plate has a surface roughness Ra of 5.0 nm or less, a thickness of 2.5 mm, and a critical impact fracture speed of 35 km / h or more when a tungsten carbide cemented carbide having a tip radius of curvature of 200 μm, an apex angle of 120° and a weight of 1.365 g is collided with a surface of the first glass plate.
16. The laminated glass according to claim 14, wherein the critical impact fracture speed when a tungsten carbide cemented carbide having a tip curvature radius of 200 μm, an apex angle of 120° and a weight of 1.365 g is collided with a surface of the first glass sheet is 55 km / h or more.
17. The laminated glass according to claim 16, wherein the total thickness of the first glass sheet, the second glass sheet, and the interlayer film is 4.5 mm or more.
18. Thickness t of the first glass plate 1 and the thickness t of the second glass plate 2 Ratio to (t 1 / t 2 15. The laminated glass according to claim 14, wherein the coefficient of friction coefficient is 1.5 or more.
19. A laminated glass comprising a first glass plate, a second glass plate, and an intermediate film sandwiched between the first glass plate and the second glass plate, wherein the first glass plate and the second glass plate are the glass for vehicles and sensors as defined in claim 1 or 3.
20. The laminated glass of claim 14, wherein the second glass sheet is soda-lime glass.
21. The laminated glass of claim 14, wherein the second glass sheet is an aluminosilicate glass.
22. The laminated glass according to claim 14, wherein the second glass sheet has been subjected to a chemical strengthening treatment.
Citation Information
Patent Citations
Cover glass for solid-state image pickup element
JP1994211538A
Cover glass for semiconductor package
JP2002249340A
Borosilicate glass, laminated glass, and window glass for vehicle
WO2022131274A1
Cited By
Glass plate and laminated glass
WO2026075247A1