Electrophotographic belt and electrophotographic image-forming device
The electrophotographic belt with a PEEK base layer and treated carbon black maintains moisture content and cooling crystallization temperature to prevent conductivity increases and cracking, addressing the issues of conductivity and cracking in conventional belts, ensuring stable and high-quality image formation.
Patent Information
- Application Number
- PCT/JP2024/014634
- Authority / Receiving Office
- WO · WO
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2024-03-06
- Filing Date
- 2024-04-11
- Publication Date
- 2024-10-17
AI Technical Summary
Conventional electrophotographic belts experience increased conductivity and cracking issues over time due to carbonization of the binder resin between carbon black particles, leading to decreased electrical resistance and image quality in long-term use.
An electrophotographic belt with a base layer composed of polyetheretherketone (PEEK) and carbon black, where the carbon black content is between 18-30% by mass, and the moisture content is maintained at 0.50% or more, suppressing conductivity changes and crack formation through controlled cooling crystallization temperature and surface treatment of carbon black.
The solution effectively stabilizes conductivity and prevents cracking in the electrophotographic belt, ensuring high-quality image formation over a long period by maintaining moisture content and adjusting the cooling crystallization temperature, thereby enhancing the belt's durability and performance.
Smart Images

Figure JP2024014634_17102024_PF_FP_ABST
Abstract
Description
Electrophotographic belt and electrophotographic image forming apparatus
[0001] The present disclosure relates to an electrophotographic belt and an electrophotographic image forming apparatus having the electrophotographic belt.
[0002] Some electrophotographic image forming apparatuses (hereinafter also referred to as "electrophotographic apparatuses"), such as copiers and laser beam printers, use an intermediate transfer belt having an endless shape. Endless electrophotographic belts used as intermediate transfer belts include those with a single-layer structure consisting of only a base layer, and those with a two- or three-layer laminate structure. Examples of two-layer structures include those consisting of a base layer and an elastic layer on the outer circumferential surface of the base layer, while examples of three-layer structures include those consisting of a base layer, an elastic layer on the outer circumferential surface of the base layer, and a surface layer on the outer circumferential surface of the elastic layer.
[0003] It has been proposed to use polyether ether ketone and polyphenyl sulfide, which are super engineering plastics with excellent strength, as binders for inexpensive, easily recyclable thermoplastic resins in the base layer of such electrophotographic belts. Polyether ether ketone may be referred to as "PEEK" hereinafter. Polyphenyl sulfide may be referred to as "PPS" hereinafter. Because crystalline thermoplastic resins such as PEEK and PPS have high melting points, conductive fillers such as carbon black are used as conductivity-imparting agents for making the base layer conductive, as described in Patent Document 1.
[0004] Here, Patent Document 1 discloses an invention aimed at providing a sheet member for an image-forming apparatus that has excellent roller habit resistance and excellent crack resistance. The sheet member for an image-forming apparatus contains PEEK and less than 19 mass% of a conductive filler, and has a temperature-lowering crystallization peak temperature Tc of less than 299.0°C. Paragraph
[0038] of Patent Document 1 states that a low Tc results in low heat resistance, but contains a large amount of high-molecular-weight components, which is advantageous for crack resistance, and that a high Tc is thought to tend to increase the degree of crystallization by allowing low-molecular-weight components to act as crystal nuclei, resulting in high heat resistance and low crack resistance.
[0005] Patent Document 1 also describes how selecting PEEK with a low Tc, i.e., PEEK with excellent crack resistance, and then slowly cooling and crystallizing it during the film formation process improves roller habit resistance, thereby achieving both crack resistance and roller habit resistance. Furthermore, paragraph
[0050] of Patent Document 1 states that if the content of the conductive filler in the sheet member for an image-forming apparatus according to the invention described in Patent Document 1 exceeds 19% by weight, crack resistance decreases, which is undesirable. From the viewpoint of stably exhibiting conductivity, it is preferable to use as much carbon black as possible. However, the sheet member for an image-forming apparatus according to Patent Document 1 is premised on a carbon black content of less than 19% by weight, and in the examples, the carbon black content ratio based on the mass of the sheet member was at most 16% by weight.
[0006] On the other hand, Patent Document 2 discloses that when an electrophotographic belt that has been made conductive by using a conductive filler is used as, for example, an intermediate transfer belt for forming electrophotographic images over a long period of time, the electrical resistance of the electrophotographic belt may decrease. Patent Document 2 describes that such a decrease in electrical resistance occurs due to the following mechanism.
[0007] That is, discharge occurs at the location where the intermediate transfer belt is separated from the primary transfer roller and the secondary transfer roller, causing an excessive current to flow all at once inside the intermediate transfer belt. At this time, a high voltage is applied between the carbon black particles, which are conductive points, and the binder resin interposed between the carbon black particles is heated and carbonized. As a result, the carbon black particles, which are originally electrically insulating, become conductive, increasing the conductivity. Patent Document 2 discloses that the aforementioned decrease in electrical resistance can be solved by improving the dispersibility of the carbon black in the binder resin. To achieve this, the document describes repeatedly melt-kneading (2 to 6 times) the carbon black and PEEK.
[0008] JP 2021-009400 A JP 2012-177811 A
[0009] The repeated melt-kneading of binder resin and carbon black disclosed in Patent Document 2 can increase the manufacturing cost of electrophotographic belts. Furthermore, repeated kneading at high temperatures may cause thermal degradation of the binder resin (crosslinking due to thermal decomposition or oxidation), resulting in a decrease in the strength of the electrophotographic belt. Furthermore, even if the dispersibility of carbon black is highly improved, it is difficult to equalize the interparticle distances of all carbon black particles. Therefore, when excessive current flows through the intermediate transfer belt, a high voltage is applied between carbon black particles that are relatively close to each other. Therefore, it is difficult to completely prevent carbonization of the binder resin interposed between the carbon black particles.
[0010] Therefore, at least one aspect of the present disclosure is directed to providing an electrophotographic belt that can suppress an increase in electrical conductivity and prevent cracks from occurring over time due to long-term use at a higher level, and at least one aspect of the present disclosure is directed to providing an electrophotographic image forming apparatus that can stably form high-quality electrophotographic images over a long period of time.
[0011] According to at least one embodiment of the present disclosure, there is provided an electrophotographic belt, the electrophotographic belt having at least a base layer, the base layer containing polyether ether ketone, which is a thermoplastic resin, and carbon black, the content of the carbon black being 18 to 30% by mass based on the mass of the base layer, a sample cut out from the base layer is heated in a nitrogen atmosphere from 30°C to 100°C at a rate of 20°C per minute and held at 100°C for 30 minutes, the mass of the sample is defined as X1, and the sample is then cooled from 100°C to 30°C at a rate of 20°C per minute and further placed in an atmosphere at a temperature of 23°C and a relative humidity of 50% for 48 hours, the moisture content of the base layer calculated by the formula moisture content of base layer = ((X2 - X1) / X2) × 100 is 0.50% by mass or more, An electrophotographic belt is provided in which the base layer has a crystallization temperature upon cooling measured by differential scanning calorimetry of 288.0° C. or less.
[0012] According to at least one aspect of the present disclosure, there is also provided an electrophotographic image forming apparatus including the above-described electrophotographic belt.
[0013] According to at least one aspect of the present disclosure, it is possible to obtain an electrophotographic belt that can suppress the change (increase) in the electrical conductivity of the electrophotographic belt over time due to long-term use and prevent the occurrence of cracks at a higher level.Furthermore, according to at least one aspect of the present disclosure, it is possible to obtain an electrophotographic image forming apparatus that can stably form high-quality electrophotographic images over a long period of time.
[0014] 1 is a schematic cross-sectional view of an image forming apparatus used for image evaluation. 2 is an explanatory diagram of an example of the configuration of an electrophotographic belt.
[0015] In this disclosure, unless otherwise specified, the expressions "XX or more and YY or less" or "XX to YY" representing a numerical range mean a numerical range including the lower and upper limits, which are the endpoints. Furthermore, when a numerical range is described in stages, the upper and lower limits of each numerical range can be combined arbitrarily. Furthermore, in this disclosure, "Ω / □" means "Ω / square."
[0016] An electrophotographic belt according to the present disclosure will be described. FIG. 2A shows a perspective view of an electrophotographic belt 200 according to one embodiment of the present disclosure. The electrophotographic belt may have an endless shape. An example of a layer structure is a monolayer structure in which the cross section taken along line A-A in FIG. 2A is composed of only a base layer 201, as shown in FIG. 2B. In this case, the outer surface 200-1 of the base layer becomes the toner carrying surface (outer surface) of the electrophotographic belt. The electrophotographic belt 200 has at least a base layer. As described above, the electrophotographic belt 200 may have an elastic layer on the outer peripheral surface of the base layer 201, and may further have a surface layer on the outer peripheral surface of the elastic layer. Furthermore, a back surface layer covering the inner peripheral surface of the base layer 201 may be provided.
[0017] The base layer contains polyether ether ketone (hereinafter sometimes referred to as "PEEK"), a thermoplastic resin, and carbon black. PEEK can serve as a binder resin for the base layer. Carbon black can also serve as a conductivity imparting agent. The carbon black content is 18 to 30 mass % based on the mass of the base layer.
[0018] A sample cut out from the base layer is heated in a nitrogen atmosphere from 30°C to 100°C at a rate of 20°C per minute and held at 100°C for 30 minutes; the mass of the sample is designated X1. The sample is then cooled from 100°C to 30°C at a rate of 20°C per minute, and then placed in air at a temperature of 23°C and a relative humidity of 50% for 48 hours; the mass of the sample is designated X2. The value (moisture content) calculated by the formula "moisture content of the base layer = ((X2 - X1) / X2) x 100" is 0.50 mass% or more.
[0019] Here, X1 is the mass of a sample cut out from the base layer when the temperature is increased from 30°C to 100°C at a rate of 20°C per minute in a nitrogen atmosphere and then maintained at 100°C for 30 minutes. X1 is considered to be the mass of the sample in a state in which water has been removed (hereinafter also referred to as the "dry state"). X2 is the mass of the sample when the dried sample is cooled from 100°C to 30°C at a rate of 20°C per minute and then placed in an air environment at 23°C and 50% relative humidity for 48 hours. X2 is considered to be the mass of the sample when it has absorbed water after being dried (hereinafter also referred to as the "water-absorbed state").
[0020] Therefore, in the present disclosure, the value calculated by ((X2-X1) / X2) x 100 is referred to as the "water content of the base layer." The present inventors have found that an electrophotographic belt having a base layer with a water content of 0.50% by mass or more is less likely to experience a change in conductivity even with repeated use over a long period of time.
[0021] As described above, the increase in conductivity over time of a conventional electrophotographic belt having a base layer containing PEEK as a binder resin and carbon black as conductive particles dispersed in the binder resin is thought to be due to carbonization of the binder resin interposed between the carbon black particles when a high voltage is applied between the carbon black particles.
[0022] On the other hand, a base layer according to the present disclosure having a moisture content of 0.50% by mass or more measured by the above method stably contains a certain amount of moisture in a typical office environment, such as a temperature of 23°C and a relative humidity of 50% under atmospheric conditions. Even if a high voltage is applied between carbon black particles due to the above-mentioned discharge phenomenon, a base layer that stably contains moisture consumes the energy for evaporation and electrolysis of moisture. Therefore, carbonization of the binder resin present between carbon black particles is suppressed, and the insulation between the carbon black particles is thought to be better maintained. As a result, the conductivity of the base layer is thought to be less likely to change (increase) even with repeated use over a long period of time.
[0023] As described above, even if the base layer becomes dry, it can regain a certain amount of water by leaving it in an atmospheric environment at a temperature of 23°C and a relative humidity of 50% for 48 hours. Therefore, in the electrophotographic belt according to the present disclosure, even if the moisture in the base layer is consumed by evaporation or decomposition due to the application of a high voltage, the base layer can absorb moisture again. Therefore, carbonization of PEEK can be continuously suppressed even with long-term use. As a result, it is believed that changes in conductivity can be suppressed even with long-term use.
[0024] The glass transition point of the PEEK contained in the base layer is, for example, about 143° C. The heat absorption effect of moisture is manifested at a temperature sufficiently lower than the glass transition point of PEEK, and therefore, it is expected to have the effect of suppressing changes in electrical resistance due to the influence of resin contraction caused by heat generation.
[0025] X1 and X2 are measured using a thermogravimetric analyzer under the following conditions: A plurality of samples of 4 mm x 4 mm are cut out from the electrophotographic belt and loaded into a platinum sample pan with a capacity of 50 μL or 100 μL so that the total mass is 15 mg ± 4 mg.
[0026] The sample is heated from 30°C to 100°C at a rate of 20°C per minute in a nitrogen atmosphere and held at 100°C for 30 minutes; the mass of the sample is designated X1. The sample is then cooled from 100°C to 30°C at a rate of 20°C per minute, and then placed in an air environment at a temperature of 23°C and a relative humidity of 50% for 48 hours; the mass of the sample is designated X2. The moisture content of the base layer is determined by the mass change rate calculated by the formula: moisture content of base layer = ((X2 - X1) / X2) x 100. In the electrophotographic belt according to the present disclosure, the moisture content of the base layer is 0.50% by mass or more. When a similar evaluation is performed using PEEK alone, which does not contain any carbon black, the moisture content is less than 0.04%.
[0027] The water content of the base layer is preferably 0.70 to 1.00% by mass, and more preferably 0.70 to 0.90% by mass. Within this range, the effect of suppressing the change in the conductivity of the base layer over time is more easily exhibited.
[0028] A method for obtaining a base layer having a moisture content within the above range includes, for example, using carbon black, which easily adsorbs moisture, as a conductive filler in the base layer. From the viewpoint of achieving a desired moisture content and further a desired electrical resistivity, the content of carbon black is 18 to 30 mass% based on the mass of the base layer, as described above.
[0029] Thus, by incorporating 18% by mass or more of carbon black into the base layer, based on the mass of the base layer, it is possible to easily impart the desired electrical conductivity to the base layer. However, increasing the carbon black content in the base layer can lead to the occurrence of cracks in the base layer. As a result of further studies by the present inventors, it was found that even when the carbon black content in the base layer is set to 18 to 30% by mass as described above, the crack resistance can be improved by controlling the cooling crystallization temperature of the base layer within a specific range.
[0030] Specifically, the cooling crystallization temperature of the base layer measured by differential scanning calorimetry (DSC) must be 288.0°C or lower. The peak temperature detected in the DSC during cooling from a molten state is the cooling crystallization temperature. The cooling crystallization temperature is the peak temperature that appears when a sample is cut out from the base layer, set in the DSC, heated to 400°C at 10°C / min, and then cooled to room temperature (25°C) at 10°C / min.
[0031] The inventors believe that the reason why crack resistance improves when the temperature-decreasing crystallization temperature is 288.0°C or lower is as follows. The temperature-decreasing crystallization temperature of 288.0°C is even lower than the temperature-decreasing crystallization temperature (292.8°C) of PEEK achieved in Example 5 of Patent Document 2. The base layer containing PEEK and carbon black is formed, for example, by extrusion molding a melt of a resin composition for forming the base layer containing PEEK. During this process, the PEEK cools from a molten state and solidifies, with the carbon black acting as a nucleus to promote crystallization. Delaying this crystallization, i.e., lowering the temperature-decreasing crystallization temperature of the base layer, reduces the crystallinity of the PEEK in the base layer and allows for the presence of a large amount of amorphous portions. This is believed to result in improved crack resistance.
[0032] The cooling-down crystallization temperature is preferably 280.0 to 288.0° C., and more preferably 285.0 to 287.8° C. There are no particular limitations on the means for setting the cooling-down crystallization temperature to 288.0° C. or less, but examples include using furnace black that has been subjected to a surface treatment described below.
[0033] Therefore, it is preferable that the carbon black contains furnace black. Compared with acetylene black, which is highly graphitized, furnace black is less likely to interact with PEEK molecules and is therefore less likely to form PEEK crystal nuclei. Furthermore, furnace black that has been treated (at least one of surface treatment and nitrogen treatment) as described below is less likely to form PEEK crystal nuclei, and can lower the temperature-lowering crystallization temperature of the base layer. The reason that surface-treated carbon black is less likely to form crystal nuclei is thought to be that fine irregularities are formed on the surface of the surface-treated carbon black, which significantly increases its surface area.
[0034] The method for manufacturing the electrophotographic belt is specifically described below. <Binder Resin> The electrophotographic belt is required to have sufficient strength to withstand prolonged tensile loads in an electrophotographic image forming apparatus. Therefore, the thermoplastic resin used as the binder resin in the base layer is preferably one that is classified as a super engineering plastic. The base layer according to the present disclosure contains PEEK as the binder resin.
[0035] PEEK is commercially available in various grades, but in the present disclosure, a single grade may be used, or two or more grades may be used in combination. Commercially available PEEK products include the "Victrex PEEK" series manufactured by Victrex. Examples of grades include PEEK "450G," "381G," and "151G."
[0036] <Carbon Black> The base layer contains carbon black. The carbon black may be a conductivity imparting agent. The carbon black is preferably, for example, commercially available carbon black that has been subjected to a treatment described below to form fine convex portions derived from an organic compound on its surface. In other words, the carbon black preferably has convex portions derived from an organic compound on its surface.
[0037] In this specification, carbon black before treatment may be referred to as "raw carbon black." Furthermore, carbon black after treatment that has fine protrusions on its surface may be referred to as "treated carbon black" or simply as "carbon black."
[0038] The melting point of PEEK, which is used as a binder resin, is, for example, approximately 330°C. Therefore, when manufacturing an endless conductive base layer using these resins, it is difficult to use an ionic conductivity imparting agent, and carbon black is instead used. To achieve the above-mentioned surface resistivity using carbon black, the carbon black content in the base layer is set to 18 to 30 mass% based on the mass of the base layer. The carbon black content in the base layer is preferably 19 to 30 mass%, more preferably 19 to 25 mass%, and even more preferably 20 to 24 mass%. The PEEK content in the base layer is preferably 70 to 81 mass%, more preferably 75 to 81 mass%, and even more preferably 76 to 80 mass%.
[0039] In this case, the carbon black preferably has a moisture absorption rate (hereinafter also referred to as CB moisture absorption rate) of 0.70% by mass or more, calculated by the following formula (1): By using such carbon black, it becomes easier to achieve a moisture content of the base layer of 0.50% by mass or more.
[0040] After storing carbon black at a temperature of 23°C and a relative humidity of 50% for 48 hours, the mass is measured using a thermogravimetric analyzer (TGA) and designated as W0. The carbon black for which W0 has been measured is then heated from 30°C to 120°C at a rate of 20°C per minute in a nitrogen atmosphere and held at 120°C for 15 minutes. The mass is then similarly measured using a thermogravimetric analyzer (TGA) and designated as W1. CB moisture absorption rate = [(W0 - W1) / W0] x 100 (1).
[0041] The CB moisture absorption rate is more preferably 1.00 to 2.00% by mass, and even more preferably 1.10 to 1.50% by mass. The CB moisture absorption rate can be controlled by increasing the specific surface area of the carbon black used, thereby increasing the amount of moisture per unit mass. As described above, furnace black is preferred as the carbon black from the perspective of suppressing crystallization during molding, and the crystallization temperature can be further reduced by increasing the BET specific surface area using the treatment method described below.
[0042] <Surface Treatment Method of Carbon Black> A surface treatment method for forming fine protrusions on the surface of raw carbon black to produce treated carbon black will be described. The treatment for forming fine protrusions on the surface of raw carbon black includes a first step of adhering an organic substance to the surface of the raw carbon black, and a second step of calcining the adhering organic substance. The formation of such fine protrusions facilitates an increase in the BET specific surface area.
[0043] First, the first step of adhering an organic substance to the surface of raw carbon black will be described. In the step of adhering an organic substance to the surface of raw carbon black, the raw carbon black may be mixed with the organic substance while still in a solid powder state. From the viewpoint of evenly adhering the organic substance to the surface, it is preferable to mix the raw carbon black with the organic substance in a liquid. Here, the step of adhering an organic substance to the surface of raw carbon black in a liquid will be described.
[0044] The first step involves dissolving an organic substance in a solvent to form an organic solution, and then adding raw carbon black to the organic solution and stirring to form a raw carbon black dispersion. Water or an organic solvent can be used as the solvent, but water is preferred in view of ease of handling and environmental impact. A common dispersant may also be used to improve the dispersion state of the raw carbon black.
[0045] The organic substance to be adhered to the raw carbon black preferably has a high affinity for the surface of the raw carbon black and also for the solvent. Specific examples include organic compounds known as cationic surfactants, anionic surfactants, and nonionic surfactants. Among these, nonionic surfactants are preferred because they tend to prevent coarsening due to aggregation when the carbon black with the adhered organic substance is removed in a subsequent process.
[0046] Nonionic surfactants include, for example, ester and ether types. Examples of ester types include glycerin fatty acid esters, sorbitan fatty acid esters, and sucrose fatty acid esters, which have a structure in which polyhydric alcohols such as glycerin and sorbitan, and sucrose are ester-bonded to fatty acids. Examples of ether types include polyoxyethylene alkyl ethers, polyoxyethylene alkyl allyl ethers, and polyoxyethylene propylene glycol, which are mainly obtained by addition polymerization of ethylene oxide with higher alcohols, alkylphenols, propylene glycol, and the like. Among these, polyoxyethylene alkyl ethers are preferred because they have good affinity with solvents and the surface of conductive carbon. One type of dispersant may be used, or multiple dispersants may be used in combination.
[0047] The amount of organic substance added to and dissolved in the solvent is preferably adjusted so that it is equal to or less than the saturated solubility relative to 100 parts by mass of the solvent, and the mass ratio "A / B," where A is the parts by mass of raw carbon black and B is the parts by mass of the organic substance relative to 100 parts by mass of the solvent, is 0.1 or more and 20.0 or less. A / B is more preferably 0.5 or more and 3.0 or less. By adjusting the amount of organic substance added to be equal to or less than the saturated solubility, precipitation of the organic substance can be suppressed, making it easier to process the raw carbon black.
[0048] Furthermore, by setting the mass ratio A / B of carbon black to organic matter at 0.1 or more, the amount of organic matter relative to carbon black becomes appropriate, thereby suppressing the amount of organic matter that fails to adhere to the surface of the raw carbon black and floats away. Furthermore, by setting the mass ratio A / B at 20 or less, the raw carbon black can be treated more efficiently.
[0049] The dissolution of the organic substance in the solvent can be promoted by appropriately selecting a means for promoting dissolution of the organic substance, such as agitation with an agitating blade, or a combination of means such as ultrasonic vibration, a homogenizer, or heat treatment. Since foaming may occur during agitation, an antifoaming agent or the like can also be appropriately selected. The amount of raw carbon black added to the organic substance-dissolved solution is preferably 1 part by mass or more and 50 parts by mass or less, and more preferably 5 parts by mass or more and 30 parts by mass or less, per 100 parts by mass of the solvent.
[0050] The raw carbon black is preferably added to the organic solution in small amounts at a time. The raw carbon black can be dispersed in the organic solution by, for example, screw stirring, shear flow (homogenizer, nanomizer), high-pressure liquid collision, or media dispersion (ball mill, bead mill).
[0051] Next, the second step of calcining the organic matter adhered to the surface of the raw carbon black will be described. The second step is a step of removing the solvent from the raw carbon black dispersion in which the organic matter adheres to the surface of the raw carbon black obtained in the first step, and calcining the resulting solid content.
[0052] Any known method can be used to remove the solvent from the raw carbon black dispersion and extract the solids. Examples of such methods include heat drying, vacuum drying, centrifugation, and reduced-pressure filtration. Heat drying is preferred, considering the throughput required for one run. Examples of heat drying include static drying, in which the dispersion is left standing in a heated atmosphere; agitation drying, in which the raw carbon black dispersion is exposed to a heated airflow to promote drying; and spray drying, in which the raw carbon black dispersion is sprayed in a mist form in a heated atmosphere to promote drying. However, spray drying is preferred, considering the throughput and solvent removal efficiency.
[0053] Known methods can be used to calcinate the extracted solid content. Calcination devices include direct heating and indirect heating methods. However, since directly heating the object with a flame such as a burner makes temperature control difficult and may result in the object being burned, indirect heating is preferred. Specific examples include electric furnaces, hot air circulation furnaces, and high-frequency induction heating furnaces. Hot air circulation furnaces are preferred because they provide excellent heating temperature uniformity. Furthermore, heating furnaces include batch-type and continuous-type furnaces. Although continuous-type furnaces have a loading and unloading mechanism, they are not suitable for long-term heating, so batch-type furnaces are preferred. In this case, the atmosphere in the heating furnace may be replaced with, for example, nitrogen to prevent excessive calcination.
[0054] The firing temperature is preferably equal to or higher than the thermal decomposition onset temperature of the organic matter and lower than the decomposition temperature of the raw carbon black. By setting the firing temperature at or higher than the thermal decomposition onset temperature of the organic matter, the organic matter adhering to the surface of the raw carbon black is decomposed, making it easier to form treated carbon black having convex shapes on the surface. Furthermore, by setting the firing temperature lower than the decomposition temperature of the raw carbon black, it is possible to prevent the raw carbon black from being burned during the treatment process. Specifically, the firing temperature is preferably, for example, 300°C or higher and 600°C or lower, and particularly preferably 350°C or higher and 500°C or lower.
[0055] The BET specific surface area of the obtained carbon black (treated carbon black) was 240 m 2 / g or more. 2 / g, and 250 to 300m 2 / g, and more preferably 250 to 270m 2 / g is even more preferable. Within this range, the crystallization temperature can be easily controlled within the aforementioned range. The BET specific surface area can be determined by immersing degassed carbon black in liquid nitrogen and determining the amount of nitrogen adsorbed on the particle surface of the carbon black when equilibrium is reached (Japanese Industrial Standards (JIS) K6217-2:2017). Furthermore, the DBP (dibutyl phthalate) absorption of the carbon black is preferably 100 to 200 mL / 100 g, more preferably 130 to 160 mL / 100 g.
[0056] <CB Moisture Absorption Rate> As mentioned above, carbonization of the binder resin is thought to occur mainly due to the application of high voltage between carbon black particles. Therefore, it is preferable to use carbon black with a high moisture adsorption capacity to ensure that the moisture content of the base layer is 0.50% by mass or more. Here, a base layer containing PEEK as a binder resin must be kneaded at approximately 300 to 400°C during its manufacturing process. Therefore, it is preferable that the carbon black contained in the base layer be able to maintain a certain amount of moisture adsorption capacity even after exposure to such temperatures. Specifically, the treated carbon black is preferably carbon black that satisfies the above-mentioned CB moisture absorption rate.
[0057] Water adsorption to carbon black is due to functional groups present on the surface of the carbon black and to the structure of the carbon black. It is believed that the functional groups on the surface of the carbon black are lost during the process of kneading the carbon black at temperatures above the melting point of PEEK. Therefore, the water adsorption ability of these functional groups is lost after kneading with PEEK. On the other hand, the structure of the carbon black is hardly lost even after the process of kneading with PEEK. Therefore, water adsorption by the structure is reversible.
[0058] This is because, if carbon black with a well-developed structure is present in the base layer, even if the water adsorbed by the carbon black is lost through evaporation or electrolysis when a high voltage is applied between the carbon black particles, moisture from the surrounding environment is absorbed into the carbon black structure, and as a result, the base layer is thought to be able to stably retain a certain amount of water.
[0059] <CB Moisture Content> Here, regardless of whether the surface treatment is performed or not, the amount of water contained in carbon black (hereinafter also referred to as "CB moisture content") can be measured and calculated by the following steps (iv) to (v). Step (iv): The carbon black to be evaluated is left at a temperature of 23°C and a relative humidity of 50% for 48 hours, and then its mass (W2) is measured using TGA. Step (v): The carbon black whose mass (W2) has been measured is heated from 30°C to 120°C at a rate of 20°C per minute in a nitrogen atmosphere, and then held at 120°C for 15 minutes, and its mass (W3) is measured using TGA.
[0060] The CB moisture content (mass%) is calculated by the following calculation formula (2): CB moisture content=((W2-W3) / W2)×100 (2) The CB moisture content is preferably 1.00 to 4.00 mass%, more preferably 2.00 to 3.00 mass%, and even more preferably 2.50 to 2.80 mass%.
[0061] The CB moisture content (%) calculated by the above formula (2) and the CB moisture absorption rate calculated by the above formula (1) for the following commercially available carbon blacks, "#3230B" and "Printex L," are shown in Table 1 below: "#3230B" (trade name, manufactured by Mitsubishi Chemical Corporation) "Printex L" (trade name, manufactured by Orion Engineered Carbons Co., Ltd.)
[0062] Although "Printex L" has a relatively high CB moisture content, its CB moisture absorption rate is extremely low. From this, it can be inferred that a large proportion of the moisture content of "Printex L" affects the functional groups on the surface of the carbon black. On the other hand, "#3230B" is able to adsorb more moisture than "Printex L" even after being baked at high temperatures. From this, it can be inferred that "#3230B" has a developed structure and is capable of reversibly adsorbing moisture.
[0063] Therefore, "#3230B" can be suitably used as the carbon black to be contained in the base layer. In addition to "#3230B," another commercially available carbon black having a CB moisture absorption rate of 0.70% by mass or more is, for example, "#44B" (trade name, manufactured by Mitsubishi Chemical Corporation; moisture absorption rate = 0.95%). However, the carbon black that can be used to obtain the base layer is not limited to these.
[0064] The CB moisture absorption rate can also be measured and calculated using the carbon black extracted from the base layer according to the above-mentioned procedure. Specifically, for example, when the binder resin is PEEK, a sample taken from the base layer is heated at 600°C for 1 hour in a nitrogen gas atmosphere, whereby the PEEK in the sample is decomposed and the carbon black in the base layer can be extracted. The carbon black extracted in this way can also be used to calculate the carbon black content in the base layer.
[0065] The number-average particle size of the primary particles of the carbon black is preferably 15 nm or more but less than 35 nm, and more preferably 20 to 30 nm. By setting the particle size within this range, deterioration of the carbon black due to heat applied during the base layer manufacturing process can be more reliably prevented. Furthermore, the carbon black can be more easily dispersed uniformly in PEEK.
[0066] <Method for Manufacturing Electrophotographic Belt> An electrophotographic belt can be manufactured by a method including the following steps: a step of melting and kneading a thermoplastic resin, PEEK, and carbon black to prepare a pellet-shaped conductive resin composition, and a step of melting the pellet-shaped conductive resin composition in a single-screw extruder, extruding the molten material from a cylindrical slit disposed at the tip of the extruder, cooling the extruded resin composition with a cylindrical cooling mandrel, and cutting it to a predetermined length.
[0067] The process of melt-kneading a conductive filler and a thermoplastic resin to prepare a pellet-shaped conductive resin composition will be described. The melt-kneading of the conductive filler and the thermoplastic resin can be performed by a known method. For example, a single-screw extruder, a twin-screw kneading extruder, a Banbury mixer, a roll, a Brabender mixer, a plastograph, a kneader, or the like can be used. Among these, a single-screw extruder or a twin-screw kneading extruder is preferred, considering that the materials can be continuously supplied and melt-kneaded, and the melt-kneaded resin composition is molded into pellets. Furthermore, necessary additives may be blended at this time to improve dispersion of the carbon black in the thermoplastic resin or to impart specific functions. When the carbon black contains a large amount of moisture, it is preferable to knead the carbon black while degassing under reduced pressure during heating.
[0068] The temperature during melt-kneading with the thermoplastic resin is equal to or higher than the glass transition temperature of the thermoplastic resin, and is within a temperature range in which the thermoplastic resin does not decompose. For example, when PEEK is used, the melt-kneading temperature is preferably 250°C or higher and 400°C or lower, and more preferably 300°C or higher and 400°C or lower. If the melt-kneading temperature is equal to or higher than the glass transition temperature, the viscosity of the resin is low, and large shear is not applied during melt-kneading, making it difficult for the molecular structure of the resin to be broken. Furthermore, if the melt-kneading temperature is 400°C or lower, oxidation and crosslinking of the resin do not proceed easily, making it difficult to form a strong structure.
[0069] The process of molding a pellet-shaped conductive resin composition into an electrophotographic belt will now be described. The resulting pellet-shaped conductive resin composition is melted in a single-screw extruder and extruded into a tube from a cylindrical slit at the tip of the extruder. The resin composition extruded into a tube is then cut to a predetermined length while controlling the temperature using a cylindrical cooling mandrel, thereby obtaining the base layer of the electrophotographic belt. The temperature during extrusion is preferably from the melting point of the resin to 400°C.
[0070] The conductivity of the base layer is not particularly limited, but considering the primary transferability and secondary transferability when used as an intermediate transfer belt, the surface resistivity is preferably 1.0×10 3 Ω / □ or more, 1.0×10 14 It is preferably in the range of 1.0×10 5 Ω / □ or more, 1.0×10 13 Ω / □ or less, and more preferably 1.0 × 10 9 Ω / □ or more, 1.0×10 13 The thickness of the base layer is preferably, for example, 25 to 100 μm, and more preferably 40 to 80 μm.
[0071] The obtained base layer may be further subjected to a heating and cooling treatment. The mechanical strength of PEEK varies greatly depending on its crystallinity. Therefore, by performing a heating and cooling treatment according to the usage conditions, the crystallinity can be adjusted to obtain an electrophotographic belt with the desired mechanical strength.
[0072] Furthermore, the base layer obtained through the above process may have a temporary low moisture content immediately after production due to the heating step, but the moisture content of the base layer can be controlled to the above range by storing it in an environment of 23°C and 50% relative humidity for 48 hours or more.
[0073] The base layer obtained as described above can then be provided with a surface layer to cover its outer peripheral surface and a back surface layer to cover its inner peripheral surface, as needed. Examples of surface layers include a layer with excellent abrasion resistance containing a cured product of an active energy ray-curable resin such as an acrylic resin. In this case, the surface layer can be provided, for example, by applying a composition containing an active energy ray-curable resin such as a photocurable resin to the outer peripheral surface of the base layer and curing it. The thickness of the surface layer is not particularly limited, but is preferably, for example, 1 to 5 μm. Examples of back surface layers include a resin layer for reinforcing the base layer and a conductive layer for making the inner peripheral surface of the electrophotographic belt conductive. The thickness of the back surface layer is not particularly limited, but is preferably, for example, 0.05 to 10 μm.
[0074] [Electrophotographic Image Forming Apparatus] An embodiment of an image forming apparatus equipped with an electrophotographic belt according to the present disclosure as an intermediate transfer belt will be described. Fig. 1 is a schematic cross-sectional view of an image forming apparatus 100 of this embodiment. The image forming apparatus 100 of this embodiment is a tandem color laser printer that employs an intermediate transfer system and is capable of forming full-color images using an electrophotographic system.
[0075] The image forming apparatus 100 has a plurality of image forming units, namely, first, second, third, and fourth image forming units Py, Pm, Pc, and Pk. These first, second, third, and fourth image forming units Py, Pm, Pc, and Pk are arranged in this order along the direction of movement of a flat portion (image transfer surface) of an intermediate transfer belt 7 (described later). Elements having the same or corresponding functions or configurations in the first, second, third, and fourth image forming units Py, Pm, Pc, and Pk may be generally described by omitting the Y, M, C, or K suffixes to reference numerals indicating elements for a particular color. In this embodiment, the image forming unit P includes a photosensitive drum 1, a charging roller 2, an exposure device 3, a developing device 4, and a primary transfer roller 5 (described later).
[0076] The image forming station P has a photosensitive drum 1, which is a drum-shaped (cylindrical) photosensitive member (electrophotographic photosensitive member) serving as an image carrier. The photosensitive drum 1 is formed, for example, by sequentially laminating a charge generating layer, a charge transport layer, and a surface protective layer on an aluminum cylinder serving as a base. The photosensitive drum 1 is rotated in the direction of arrow R1 (counterclockwise) in the figure. The surface of the rotating photosensitive drum 1 is uniformly charged to a predetermined potential of a predetermined polarity (negative in this embodiment) by a charging roller 2, which is a roller-shaped charging member serving as a charging means. During the charging process, a predetermined charging bias (charging voltage) containing a negative DC component is applied to the charging roller 2. The charged surface of the photosensitive drum 1 is scanned and exposed by an exposure device (laser scanner) 3 serving as an exposure means in accordance with image information, forming an electrostatic image (electrostatic latent image) on the photosensitive drum 1.
[0077] The electrostatic image formed on the photosensitive drum 1 is developed (visualized) by the developing device 4 as a developing means, which supplies toner as a developer, and a toner image (developer image) is formed on the photosensitive drum 1. During the development process, a predetermined development bias (developing voltage) including a negative DC component is applied to the developing roller 4a as a developer carrier provided in the developing device 4. In this embodiment, toner charged with the same polarity as the charging polarity of the photosensitive drum 1 (negative polarity in this embodiment) adheres to the exposed portion (image portion) on the photosensitive drum 1, which has been uniformly charged and then exposed to light, thereby reducing the absolute value of the potential.
[0078] An intermediate transfer belt 7, which is an endless belt serving as an intermediate transfer body, is disposed opposite the four photosensitive drums 1. The intermediate transfer belt 7 is stretched around a plurality of tension rollers, namely a drive roller 71, a tension roller 72, and a secondary transfer opposing roller 73, and is stretched with a predetermined tension. When the drive roller 71 is driven to rotate, the intermediate transfer belt 7 comes into contact with the photosensitive drums 1 and rotates (moves around) in the direction of arrow R2 (clockwise) in the figure. On the inner circumferential surface of the intermediate transfer belt 7, primary transfer rollers 5, which are roller-shaped primary transfer members serving as primary transfer means, are disposed corresponding to each photosensitive drum 1.
[0079] The primary transfer roller 5 is pressed against the photosensitive drum 1 via the intermediate transfer belt 7, forming a primary transfer portion (primary transfer nip) T1 where the photosensitive drum 1 and the intermediate transfer belt 7 come into contact with each other. The toner image formed on the photosensitive drum 1 as described above is primarily transferred onto the rotating intermediate transfer belt 7 at the primary transfer portion T1 by the action of the primary transfer roller 5.
[0080] During the primary transfer process, a primary transfer bias (primary transfer voltage), which is a DC voltage of opposite polarity (positive polarity in this embodiment) to the normal charging polarity of the toner (charging polarity during the development process), is applied to the primary transfer roller 5. The primary transfer roller 5 is often configured with a metal rotating shaft and an elastic layer formed on the outer surface of the rotating shaft, and is adjusted to a desired resistance value. However, in recent years, with the trend toward smaller devices and lower costs, an increasing number of devices are configured with a metal roller that is straight in the thrust direction and made of materials such as SUM (sulfur and sulfur composite free-cutting steel) or SUS (stainless steel).
[0081] In such primary transfer, a transfer voltage of several kV is usually applied to ensure a sufficient transfer rate, and at that time, discharge may occur near the transfer nip. This discharge is one of the causes of deterioration of the surface characteristics of the intermediate transfer member. When the primary transfer roller is made of a metal roller, the transfer nip becomes narrower than when the primary transfer roller has an elastic layer, and discharge is more likely to occur. Therefore, the effects of the electrophotographic belt according to the present disclosure are more pronounced in devices in which the primary transfer roller 5 is made of a metal roller.
[0082] A secondary transfer roller 8, which is a roller-shaped secondary transfer member serving as secondary transfer means, is disposed on the outer peripheral surface of the intermediate transfer belt 7 at a position facing the secondary transfer opposing roller 73. The secondary transfer roller 8 is pressed against the secondary transfer opposing roller 73 via the intermediate transfer belt 7, forming a secondary transfer portion (secondary transfer nip) T2 where the intermediate transfer belt 7 and the secondary transfer roller 8 come into contact. The toner image formed on the intermediate transfer belt 7 as described above is secondarily transferred, by the action of the secondary transfer roller 8, at the secondary transfer portion T2 onto a recording material (sheet, transfer material) S such as paper (form) being nipped and transported between the intermediate transfer belt 7 and the secondary transfer roller 8.
[0083] During the secondary transfer process, a secondary transfer bias (secondary transfer voltage), which is a DC voltage of opposite polarity to the normal charging polarity of the toner, is applied to the secondary transfer roller 8. In the secondary transfer, a transfer voltage of several kV is typically applied to ensure sufficient transfer efficiency. Similarly, the above image formation operation is performed in each of the magenta (M), cyan (C), and black (K) units Pm, Pc, and Pk as the intermediate transfer belt 7 moves, and toner images of four colors, yellow, magenta, cyan, and black, are layered on the intermediate transfer belt 7.
[0084] The four color toner layers are transported along the movement of the intermediate transfer belt 7, and at the secondary transfer section T2, they are transferred together by a secondary transfer roller 8, which serves as a secondary transfer means, onto a recording medium S (hereinafter also referred to as a "second image carrier") that is transported at a predetermined timing. In such secondary transfer, a transfer voltage of several kV is usually applied to ensure a sufficient transfer rate, and during this process, discharge may occur near the transfer nip. This discharge is one of the causes of a decrease in the electrical resistance of the intermediate transfer belt.
[0085] The recording material S is supplied to a conveying path by a pickup roller 13 from a cassette 12 in which the recording material S is stored. The recording material S supplied to the conveying path is conveyed to a secondary transfer portion T2 by a conveying roller pair 14 and a registration roller pair 15 in synchronization with the toner image on the intermediate transfer belt 7.
[0086] The recording material S onto which the toner image has been transferred is conveyed to a fixing device 9 serving as a fixing means. The fixing device 9 heats and presses the recording material S carrying the unfixed toner image with fixing members 91 and 92, thereby fixing (melting and adhering) the toner image onto the recording material S. The recording material S onto which the toner image has been fixed is discharged (output) to the outside of the main body of the image forming apparatus 100 by a pair of conveying rollers 16, a pair of discharging rollers 17, etc.
[0087] Toner remaining on the surface of the photosensitive drum 1 without being transferred to the intermediate transfer belt 7 in the primary transfer process (primary transfer residual toner) is simultaneously developed and collected by the developing device 4, which also serves as a photosensitive member cleaning means. Furthermore, toner remaining on the surface of the intermediate transfer belt 7 without being transferred to the recording material S in the secondary transfer process (secondary transfer residual toner) is removed from the surface of the intermediate transfer belt 7 and collected by a belt cleaning device 11, which serves as an intermediate transfer belt cleaning means. The belt cleaning device 11 is disposed downstream of the secondary transfer portion T2 and upstream of the most upstream primary transfer portion T1y in the rotation direction of the intermediate transfer belt 7 (in this embodiment, it faces the drive roller 71). The belt cleaning device 11 scrapes the secondary transfer residual toner from the surface of the rotating intermediate transfer belt 7 using a cleaning blade, which serves as a cleaning member disposed in contact with the surface of the intermediate transfer belt 7, and collects the scraped toner in a collection container 11b.
[0088] In this way, in the image forming operation, the process of electrically transferring the toner image from the photosensitive drum 1 to the intermediate transfer belt 7 and from the intermediate transfer belt 7 to the recording material S is repeated. Furthermore, by repeating image formation on a large number of recording materials S, the electrical transfer process is further repeated.
[0089] By using the electrophotographic belt as an intermediate transfer belt in the electrophotographic image forming apparatus, it becomes possible to repeatedly form high-quality electrophotographic images for a long period of time.
[0090] Examples of electrophotographic belts according to this embodiment are shown below. Note that, although the steps for producing electrophotographic belts in this embodiment were all carried out using a common device, this embodiment is not limited to the following examples.
[0091] The present disclosure will be specifically described below using examples. In the examples and comparative examples, the number of parts is by mass unless otherwise specified.
[0092] Commercially available carbon blacks shown in Table 2 below were prepared as conductive fillers for use in producing intermediate transfer belts according to Examples and Comparative Examples, and the carbon blacks were subjected to the surface treatment or nitrogen treatment described above. The nitrogen treatment was carried out as follows: The carbon blacks to be treated were baked (heat treated) in a nitrogen atmosphere at a temperature of 430°C for 6 hours.
[0093] The surface treatment was carried out as follows. 10 parts by mass of a nonionic surfactant (polyoxyethylene alkyl ether) (manufactured by Sanyo Chemical Industries, Ltd., product name: "Naroacty") was added to 100 parts by mass of water, and after dissolution, 15 parts by mass of raw carbon black (manufactured by Mitsubishi Chemical Corporation, product name: "#3230B") was added. The ratio "A / B," where A represents the mass of the raw carbon black and B represents the mass of the surfactant, was 1.5 per 100 parts by mass of water. The mixture was stirred in a bead mill (product name: "Alpha Mill," manufactured by Imex Co., Ltd.) to obtain a raw carbon black dispersion. Water was removed from this raw carbon black dispersion using a spray dryer (product name: "Spray Dryer L-8i," manufactured by Yamato Scientific Co., Ltd.) to obtain a solid content. The obtained solid content was baked at 400°C for 5 hours in a high-temperature furnace (product name: "Constant Temperature Dryer DR200," manufactured by Yamato Scientific Co., Ltd.).
[0094] The physical properties of the treated carbon black (DBP absorption amount, number average particle size of primary particles, BET specific surface area, CB water content, and CB water absorption amount) are shown in Table 2.
[0095] DBP absorption: DBP (dibutyl phthalate) was added dropwise to 100 g of carbon black while stirring, and the amount of dibutyl phthalate added at the point where the torque reached its maximum was determined (Japanese Industrial Standards (JIS) K6217-4:2017). The measurement was performed using an absorption meter (S-500, Asahi Research Institute).
[0096] Primary particle size: Carbon black typically exists as multiple primary particles connected three-dimensionally like a bunch of grapes. The number-average particle size of primary particles (hereinafter also referred to as "primary particle size") refers to the number-average particle size of the smallest unit of carbon black (primary particle) that forms a single pigment particle. The primary particle size of carbon black was determined by observing the cross section of the base layer. Measurements were performed using a transmission electron microscope (TEM). Thinned samples prior to observation can be prepared using an ion beam, diamond knife, or the like. In this disclosure, a 40-nm-thick cut specimen for observation, which shows the cross section of the base layer in the full thickness direction, was obtained using an "ULTRACUT-S" (trade name, manufactured by Leica). TEM images were then obtained using a transmission electron microscope (TEM) (trade name: H-7100FA, manufactured by Hitachi, Ltd.) under measurement conditions of TE mode and an accelerating voltage of 100 kV. The obtained TEM images can be analyzed using known image analysis software such as "WinROOF" (product name, manufactured by Mitani Shoji Co., Ltd.) or "ImagePro" (product name, manufactured by Nippon Roper Co., Ltd.). In the present disclosure, "WinROOF" was used. The area-equivalent diameters of 50 primary particles of carbon black were then measured, and the average value was taken as the number-average particle diameter of the primary particles.
[0097] BET specific surface area: Degassed carbon black is immersed in liquid nitrogen, and the amount of nitrogen adsorbed on the particle surface of the carbon black at equilibrium is determined (Japanese Industrial Standards (JIS) K6217-2:2017). Specifically, the measurement was performed using a fully automatic specific surface area measuring device (Macsorb, Mountech Co., Ltd.). The measurement was performed under pre-degassing conditions at 150°C for 3 minutes.
[0098] Example 1 <Production of Electrophotographic Belt> <Pre-mixing> PEEK (product name: 381G, manufactured by Victrex Corporation) and treated carbon black shown in Table 2 were weighed out to the blending ratios shown in Table 3, and mixed using a Henschel mixer (Nippon Coke and Engineering Co., Ltd., FM-150L / I). The operating conditions and treatment conditions for the Henschel mixer were a blade rotation speed of 1500 rpm, a treatment amount of 30 kg, a treatment time of 5 minutes, and a treatment temperature of 50°C.
[0099] <Melt-Kneading> The mixture obtained by the above pre-mixing was charged into a twin-screw kneader (PCM43, Ikegai Corporation) and melt-kneaded under conditions of an extrusion rate of 6 kg / h, a screw rotation speed of 100 rpm, and a barrel control temperature of 360° C. to obtain a resin composition. During kneading, degassing was performed under reduced pressure through an upstream vent hole to remove vaporized materials.
[0100] <Melt Extrusion> The resin composition obtained through the melt-kneading step was pelletized, and then the pellets were extruded using a single-screw extruder (Plastic Engineering Research Institute Co., Ltd.) equipped with a spiral cylindrical die at the tip at an extrusion rate of 6 kg / h and a die temperature of 380°C to obtain an endless electrophotographic belt composed of a cylindrical film base layer having a thickness of 60 μm.
[0101] <Evaluation of Electrophotographic Belt> The electrophotographic belt thus produced was left for 48 hours in an environment of a temperature of 23° C. and a relative humidity of 50%, and then various evaluations were carried out.
[0102] (Evaluation 1: Measurement of Temperature-Down Crystallization Temperature) The peak temperature detected in a differential scanning calorimeter (DSC) during the temperature-down process from a molten state is taken as the temperature-down crystallization temperature. The temperature-down crystallization temperature is the peak temperature that appears when a sample is cut out from the base layer, set in the DSC, heated to 400°C at 10°C / min, and then cooled to room temperature (25°C) at 10°C / min. A differential scanning calorimeter (DSC Q2000, TA Instruments Inc.) was used as the measuring device. Samples were cut out at three points from the center of the base layer in a direction perpendicular to the circumferential direction of the electrophotographic belt, and the arithmetic average of the measured values was used.
[0103] (Evaluation 2: Calculation of Moisture Content of Base Layer) Samples were cut from the base layer of the fabricated electrophotographic belt, and the moisture content of the base layer was measured. In this example, a thermogravimetric analyzer (Q500 manufactured by TA Instruments) was used. Multiple samples, each measuring 4 mm x 4 mm, were cut from the base layer of the electrophotographic belt and loaded into a 100 μL platinum sample pan so that the total mass was 15 mg ± 4 mg. The sample was heated from 30°C to 100°C at a rate of 20°C per minute in a nitrogen atmosphere and held at 100°C for 30 minutes. The mass of the sample was designated X1. The sample was then cooled from 100°C to 30°C at a rate of 20°C per minute, and then placed in an air atmosphere at 23°C and 50% relative humidity for 48 hours. The mass of the sample was designated X2. The moisture content of the base layer was calculated using the formula: moisture content of base layer = ((X2 - X1) / X2) × 100. As a result, the moisture content of the base layer according to this example was 0.72% by mass.
[0104] (Evaluation 3: Mechanical Strength, Bending Resistance) A portion of the electrophotographic belt was cut out, and a bending resistance test was conducted to measure mechanical strength. In the present disclosure, the MIT test specified in Japanese Industrial Standards (JIS) P8115:2001 was applied as a folding endurance test (flexural fatigue test), except that the bending radius R was changed to 2.5 mm, and the number of times until breakage was taken as the bending strength and evaluated as follows: Rank "A": Did not break even after 1 million or more cycles Rank "B": Broken after 100,000 or more cycles but less than 1 million cycles Rank "C": Broken after 10,000 or more cycles but less than 100,000 cycles Rank "D": Broken after less than 10,000 cycles The electrophotographic belt evaluated in this example did not break even after 1 million or more cycles, and its mechanical strength was ranked as "A."
[0105] (Evaluation 4: Measurement of Surface Resistivity) The electrical resistance value of the electrophotographic belt was measured. The electrical resistance was measured using a Hiresta manufactured by Mitsubishi Chemical Corporation at a total of 40 points, 5 points in the width direction and 8 points in the circumferential direction, under the condition that the surface resistivity was measured after 10 seconds with an applied voltage of 100 V. The surface resistivity of the obtained electrophotographic belt was 3.00×10 10 It was Ω / □.
[0106] (Evaluation 5: Image Evaluation) The produced electrophotographic belt was attached as an intermediate transfer belt to an intermediate transfer unit of a copying machine (manufactured by Canon Inc., product name: "IR-ADVANCE C5051"), and an image quality test was carried out. The printing test was carried out in an environment of a temperature of 15°C and a relative humidity of 10%, using A4 size paper (manufactured by Canon Inc., product name: "GF-600" (basis weight 60 g / m 2 )) was used to print 600,000 full-color images, and a paper feed durability test was conducted. After the paper feed durability test, 20 magenta solid images were output to check the printed images on the entire circumferential surface of the intermediate transfer belt. The 20 output images were visually inspected for the presence of density unevenness, which is a defect in image quality, and evaluated according to the following criteria: Rank "A": No image defects were observed in any of the printed images. Rank "B": Image defects were observed in 1 to 3 printed images. Rank "C": Image defects were observed in 4 or more printed images. In the printed images after the paper feed durability test in this example, no image defects were observed. Therefore, the image quality evaluation was given an "A".
[0107] (Resistance Decrease) After printing 600,000 sheets, the surface resistivity of the electrophotographic belt was measured under the same conditions as before the paper feed durability test. The amount of change in resistance before and after the durability test was calculated from the initial resistance value (electrical resistance value before the paper feed durability test) and the electrical resistance value after the paper feed durability test. The Δ digits were calculated using the following formula. Here, the initial resistance value is ρ0, and the resistance value after durability is ρ. Δ digits = Log(ρ0) - Log(ρ) (3) The surface resistivity of the electrophotographic belt of Example 1 after the paper feed durability test was 2.74 × 10 10 The resistivity was Ω / □, and the change in resistivity before and after the durability test was in the order of 0.03.
[0108] [Examples 2 to 3, Comparative Examples 1 to 4] Using the material configurations and blending ratios shown in Table 3 below, electrophotographic belts of Examples 2 to 3 and Comparative Examples 1 to 4 were produced by the same production method as in Example 1. Each of the obtained electrophotographic belts was subjected to various evaluations by the same methods as in Example 1.
[0109] Example 2 An electrophotographic belt was produced in the same manner as in Example 1, except that the compounding ratio of PEEK to carbon black (CB) was adjusted as shown in Table 3.
[0110] Example 3 An electrophotographic belt was produced in the same manner as in Example 1, except that the compounding ratio of PEEK to carbon black (CB) was adjusted as shown in Table 3.
[0111] Comparative Example 1 An electrophotographic belt was produced in the same manner as in Example 1, except that the type of carbon black was selected and the compounding ratio was adjusted as shown in Table 3.
[0112] Comparative Example 2 An electrophotographic belt was produced in the same manner as in Example 1, except that the type of carbon black was selected and the compounding ratio was adjusted as shown in Table 3.
[0113] Comparative Example 3 An electrophotographic belt was produced in the same manner as in Example 1, except that the type of carbon black was selected and the compounding ratio was adjusted as shown in Table 3.
[0114] Comparative Example 4 An electrophotographic belt was produced in the same manner as in Example 1, except that the type of carbon black was selected and the compounding ratio was adjusted as shown in Table 3. The evaluation results of the electrophotographic belts produced in Examples 1 and 2 and Comparative Examples 1 to 4 are shown in Table 3.
[0115] In Example 1, the image evaluation after the paper feed durability test showed good results. The change in resistance value before and after the paper feed durability test was also small, suggesting that resistance value change was unlikely to occur due to discharge occurring in the gap between the inner peripheral surface of the intermediate transfer body and the primary transfer roller in the primary transfer section, or between the outer peripheral surface of the intermediate transfer body and the paper in the secondary transfer section. As a result, it is thought that no image defects occurred after the paper feed durability test. Furthermore, in Example 2, no decrease in crack resistance was observed even when the amount of carbon black was increased. In Example 3, no decrease in resistance due to the moisture content of the belt was observed even when the amount of carbon black was small.
[0116] In the electrophotographic belt according to Comparative Example 1, a decrease in crack resistance was confirmed due to a high crystallization temperature upon cooling. It is believed that the carbon black used in Comparative Example 1 has a small BET specific surface area due to a small number of fine protrusions on the surface, which resulted in a high crystallization temperature upon cooling. In the electrophotographic belt according to Comparative Example 2, a decrease in crack resistance was also confirmed due to a high crystallization temperature upon cooling.
[0117] The electrophotographic belt according to Comparative Example 3 also had a high crystallization temperature upon cooling, and therefore a decrease in crack resistance was confirmed. Furthermore, in Comparative Example 3, the moisture content of the base layer was low, which caused the conductivity to change over time, resulting in poor images. The moisture content of the base layer was low in the electrophotographic belt according to Comparative Example 4, which caused the conductivity to change significantly over time, resulting in poor images. The electrophotographic belt according to Comparative Example 4 had a high crystallization temperature upon cooling, but was excellent in mechanical strength. This is thought to be due to the low content of carbon black in the base layer. The high crystallization temperature upon cooling of the base layer of the electrophotographic belt according to Comparative Example 4 is thought to be due to the use of acetylene black, which is likely to become a crystal nucleus for PEEK, as the carbon black.
[0118] The number of flexing times indicates the number of flexing times at which the electrophotographic belt breaks. "1 million or more flexing times" indicates that the electrophotographic belt did not break even after flexing 1 million times.
[0119] As described above, by increasing the moisture content of the base layer of the electrophotographic belt, it is possible to suppress the decrease in resistance, and by lowering the crystallization temperature during cooling, it is possible to improve the crack resistance, thereby making it possible to obtain an electrophotographic belt that can achieve both suppression of the decrease in electrical resistance and high crack resistance even after long-term use.
[0120] The present disclosure is not limited to the above-described embodiments, and various modifications and variations are possible without departing from the spirit and scope of the present disclosure. Therefore, the following claims are appended to clarify the scope of the present disclosure. This application claims priority based on Japanese Patent Application No. 2023-065502 filed on April 13, 2023, and Japanese Patent Application No. 2024-033578 filed on March 6, 2024, the entire contents of which are incorporated herein by reference.
Claims
1. An electrophotographic belt comprising at least a base layer, the base layer containing polyether ether ketone, a thermoplastic resin, and carbon black, the carbon black content being 18-30% by mass based on the mass of the base layer, a sample cut out from the base layer is heated in a nitrogen atmosphere from 30°C to 100°C at a rate of 20°C per minute and held at 100°C for 30 minutes, the mass of the sample being X1, and then cooled from 100°C to 30°C at a rate of 20°C per minute and then placed in an atmosphere at a temperature of 23°C and a relative humidity of 50% for 48 hours, the moisture content of the base layer calculated by the formula moisture content of base layer = ((X2 - X1) / X2) x 100 is 0.50% by mass or more, and the cooling crystallization temperature of the base layer measured by differential scanning calorimetry is 288.0°C or less.
2. The electrophotographic belt according to claim 1, wherein the content of said carbon black is 19 to 30% by weight based on the weight of said base layer.
3. The electrophotographic belt according to claim 1 or 2, wherein the number average particle size of the primary particles of said carbon black is 15 nm or more and less than 35 nm.
4. The electrophotographic belt according to any one of claims 1 to 3, wherein the carbon black has a moisture absorption rate of 0.70% by mass or more, calculated by the following formula (1): The carbon black is left for 48 hours under conditions of a temperature of 23°C and a relative humidity of 50%, and its mass is measured using a thermogravimetric analyzer and designated as W0. The carbon black after measuring W0 is then heated from 30°C to 120°C at a rate of 20°C per minute in a nitrogen atmosphere and held at a temperature of 120°C for 15 minutes, and its mass is similarly measured using a thermogravimetric analyzer and designated as W1. Moisture absorption rate = [(W0 - W1) / W0] x 100 ... (1).
5. The BET specific surface area of the carbon black is 240 m 2 5. The electrophotographic belt according to claim 1, wherein the surface roughness is 1 / g or more.
6. The electrophotographic belt according to any one of claims 1 to 5, wherein said carbon black comprises furnace black.
7. The electrophotographic belt according to any one of claims 1 to 6, wherein said carbon black has protrusions on the surface thereof derived from an organic compound.
8. The electrophotographic belt according to claim 1, wherein the moisture content of the base layer is 0.70 to 1.00% by weight.
9. The surface resistivity of the base layer is 1.0 x 10 3 Ω / □ or more, 1.0×10 14 9. The electrophotographic belt according to claim 1, wherein the surface roughness is Ω / □ or less.
10. The electrophotographic belt according to claim 1, wherein the thickness of said base layer is from 25 to 100 μm.
11. The electrophotographic belt according to any one of claims 1 to 10, wherein the electrophotographic belt is an intermediate transfer belt.
12. An electrophotographic image forming apparatus comprising the electrophotographic belt according to any one of claims 1 to 11.
13. The electrophotographic image forming apparatus according to claim 12, wherein said electrophotographic belt is provided as an intermediate transfer belt.
Citation Information
Patent Citations
Sheet-like member for image forming apparatus and extrusion molding method of the same
JP2017129846A
Belt for electrophotography and electrophotographic image forming apparatus
JP2023075032A
Resin member and image forming apparatus
JP2023172549A