Thermal insulation concrete and preparation method therefor and use thereof
By using a mixed formula of hydrophilic modified airgel and hydrophobic airgel in foam concrete, the problem of reduced mechanical properties of airgel in foam concrete is solved, achieving both thermal insulation and strength, and improving thermal insulation performance. and compressive strength, and simplifies the mixing process.
Patent Information
- Application Number
- PCT/CN2023/088648
- Authority / Receiving Office
- WO · WO
- Patent Type
- Applications
- Current Assignee / Owner
- Filing Date
- 2023-04-17
- Publication Date
- 2024-10-24
AI Technical Summary
When existing airgel is compounded with foam concrete, the hydrophobic properties of conventional airgel lead to reduced mechanical properties and uneven mixing, making it difficult to achieve both thermal insulation and strength properties.
Using a mixed formula of hydrophilic modified aerogel and hydrophobic aerogel, by adjusting their mass ratio and particle size, they are evenly dispersed in concrete to improve dispersion and strength while maintaining or improving thermal insulation performance.
The effective addition of airgel into foam concrete is achieved, which improves the thermal insulation performance and mechanical strength, especially the compressive strength, while simplifying the mixing process and reducing the mixing time.
Smart Images

Figure CN2023088648_24102024_PF_FP_ABST
Abstract
Description
Thermal insulation concrete and its preparation method and application Technical Field
[0001] The invention belongs to the technical field of building thermal insulation and relates to thermal insulation concrete and a preparation method and application thereof. Background Art
[0002] With the continuous development of the economy and construction technology, the demand for green, energy-saving, and environmentally friendly buildings continues to increase. In the construction industry, the use of effective thermal insulation materials can effectively reduce building energy consumption. Among insulating concretes, foamed concrete is widely used. It is a lightweight building insulation material with a large number of air holes. Compared with ordinary concrete, it has a lower density and better thermal insulation performance. It also has the advantages of simple processing and low cost. Optimizing the thermal insulation performance of foamed concrete meets the current demand for green and sustainable development.
[0003] Aerogel is a lightweight, solid material with a three-dimensional network structure and nanoscale pores. It boasts a large surface area, high porosity, low density, and extremely low thermal conductivity, enhancing the performance of traditional insulation materials.
[0004] However, when conventional aerogel is combined with foamed concrete, the hydrophobic nature of the aerogel results in reduced mechanical properties, such as compressive strength. Furthermore, the hydrophobic nature of the aerogel also leads to uneven mixing, resulting in poor mechanical properties. There is an urgent need to develop an aerogel formulation that effectively incorporates aerogel into foamed concrete, hoping to achieve a modified foamed concrete with both excellent thermal insulation and strength properties.
[0005] Summary of the Invention
[0006] In order to solve the above technical problems, the present invention provides the following technical solutions:
[0007] A thermal insulation concrete comprises aerogel and concrete; the aerogel is uniformly dispersed in the concrete; and the aerogel comprises hydrophilic modified aerogel and hydrophobic aerogel.
[0008] The inventors discovered that while using hydrophilic modified aerogel alone as a modifying material can effectively improve the mixing uniformity of aerogel and concrete, the introduction of the hydrophilic modified aerogel can significantly reduce the strength of the concrete. However, using a powder mixture of hydrophobic and hydrophilic modified aerogels as an additive to concrete not only improves the dispersibility of the concrete but also has a certain thickening effect, effectively maintaining or even increasing the strength of the concrete. It is based on this discovery that the present invention was proposed.
[0009] According to an embodiment of the present invention, in the aerogel, the mass ratio of the hydrophilic modified aerogel to the hydrophobic aerogel is 100:(0-200), and the content of the hydrophobic aerogel is not zero, preferably 100:(100-200), for example, 100:100, 100:110, 100:120, 100:130, 100:140, 100:160, 100:170, 100:180, 100:190. Studies have found that when the mass ratio of the hydrophobic aerogel to the hydrophilic modified aerogel is within the above range, the thermal insulation performance of the thermal insulation concrete can be guaranteed while maintaining the mechanical strength of the thermal insulation concrete.
[0010] According to an embodiment of the present invention, in the thermal insulation concrete, the particle size of the aerogel is 1 nm-50 nm, preferably 20 nm-50 nm, for example, 1 nm, 10 nm, 20 nm, 30 nm, 40 nm or 50 nm.
[0011] According to an embodiment of the present invention, in the thermal insulation concrete, the mass ratio of aerogel to concrete is (0-30):100 and the content of the aerogel is not 0, for example, 5:100, 10:100, 15:100, 20:100, 25:100, or 30:100.
[0012] According to an embodiment of the present invention, the hydrophilically modified aerogel is a hydrophilically modified aerogel particle.
[0013] According to an embodiment of the present invention, the contact angle between the hydrophilic modified aerogel and water is less than 90°. Preferably, the surface of the hydrophilic modified aerogel contains hydrophilic groups, which are selected from groups known in the art, such as hydroxyl groups (-OH).
[0014] According to an embodiment of the present invention, the contact angle of the hydrophobic aerogel with water is greater than 90°. Preferably, the surface of the hydrophobic aerogel contains hydrophobic groups, which are selected from groups known in the art, such as alkoxy groups (-OR, R represents an alkyl group).
[0015] According to an embodiment of the present invention, the raw material of the concrete is selected from cement, and cement includes silicate cement, aluminate cement, sulphoaluminate cement, and magnesium oxychloride cement.
[0016] According to an embodiment of the present invention, the raw materials of the concrete may further include auxiliary materials.
[0017] According to an embodiment of the present invention, the auxiliary material is at least one of water, a water reducing agent, a foaming agent, fly ash, glass microspheres and reinforcing fibers.
[0018] According to an embodiment of the present invention, in the raw materials of the concrete, the foaming agent is 0.1 to 10 parts by mass per 100 parts by mass of cement, for example, 0.1 part by weight, 0.5 part by weight, 1 part by weight, 2 parts by weight, 3 parts by weight, or 5 parts by weight.
[0019] According to an embodiment of the present invention, the auxiliary materials of the concrete also include a water reducer. Studies have found that the introduction of a water reducer can improve the fluidity of the product during molding and processing without affecting the performance of the product, and is non-toxic and reasonably priced.
[0020] According to an embodiment of the present invention, the water reducer is selected from at least one of calcium lignin sulfonate, sodium lignin sulfonate, magnesium lignin sulfonate, sulfonated melamine formaldehyde resin, aromatic aminosulfonate polymer, aliphatic hydroxysulfonate polymer, HSB aliphatic high-efficiency water reducer, casein, polyoxyethylene dioleate, tetraethylene glycol monostearate, tetraethylene glycol monooleate, polyoxypropylene mannitol dioleate, polyoxyethylene sorbitol lanolin oleic acid derivative, polyoxyethylene sorbitol lanolin derivative, polyoxypropylene stearate, polyoxyethylene (5EO) lanolin ether, anhydrous sorbitan laurate, polyoxyethylene fatty acid, polyoxyethylene oxypropylene oleate, triethylhexyl phosphoric acid, sodium lauryl sulfate, methyl amyl alcohol, cellulose derivatives, polyacrylamide, gur gum, fatty acid polyethylene glycol ester, etc., preferably polyoxypropylene stearate and / or polyoxyethylene dioleate.
[0021] According to an embodiment of the present invention, the water reducer is 0.01-20 parts by mass per 100 parts by mass of cement, for example, 0.1 parts by mass, 1 part by mass, 5 parts by mass, 10 parts by mass, 15 parts by mass, or 20 parts by mass.
[0022] According to an embodiment of the present invention, the foaming agent can be selected from foaming agents known in the art, for example, selected from rosin resin foaming agents, synthetic surfactant foaming agents, plant protein foaming agents, animal protein foaming agents, hydrogen peroxide foaming agents, ammonium bicarbonate foaming agents, azodicarbonamide foaming agents, aluminum powder foaming agents, alkylbenzene sulfonate foaming agents, and fatty alcohol sulfonate foaming agents.
[0023] Specifically, the foaming agent can be selected from at least one of sodium lauryl sulfate, sodium rosinate, triterpenoid saponin, sodium α-olefin sulfonate, and hydrolyzed waste animal hair.
[0024] According to an embodiment of the present invention, the fly ash is in an amount of 0.5-20 parts by mass per 100 parts by mass of cement.
[0025] According to an embodiment of the present invention, the amount of the vitrified microspheres is 5 to 40 parts by weight, for example, 10 parts by weight, 20 parts by weight, 30 parts by weight, or 40 parts by weight, per 100 parts by weight of cement.
[0026] According to an embodiment of the present invention, the fly ash and vitrified microspheres can be selected from materials known in the art and are not specifically limited in the present invention.
[0027] According to an embodiment of the present invention, among the raw materials of the concrete, water accounts for 20 to 100 parts by mass per 100 parts by mass of cement, for example, 20 parts by mass, 30 parts by mass, 40 parts by mass, 50 parts by mass, 60 parts by mass, 70 parts by mass, 80 parts by mass, 90 parts by mass, or 100 parts by mass.
[0028] According to an embodiment of the present invention, the reinforcing fibers are selected from inorganic fibers and organic fibers, such as polyester fibers, glass fibers, basalt fibers, etc. Preferably, the reinforcing fibers are short fibers, specifically fibers with a length of 3 mm to 60 mm, such as 10 mm, 20 mm, 30 mm, 40 mm, or 50 mm.
[0029] According to an embodiment of the present invention, the reinforcing fiber is present in an amount of 0.5-5 parts by weight, for example, 0.6 parts by weight, 0.7 parts by weight, 0.8 parts by weight, or 0.9 parts by weight, per 100 parts by weight of cement in the gypsum concrete. In the present invention, the reinforcing fiber is used as a skeleton filler to increase the strength of the aerogel-modified concrete.
[0030] According to an embodiment of the present invention, the thermal conductivity of the thermal insulation concrete is not higher than 0.40w / (mk), for example, 0.3w / (mk), 0.2w / (mk), 0.1w / (mk), 0.07w / (mk), or 0.05w / (mk).
[0031] According to an embodiment of the present invention, the compressive strength of the thermal insulation concrete is 1 to 10 MPa, for example, 2 MPa, 3 MPa, 4 MPa, 5 MPa, 6 MPa, 7 MPa, 8 MPa, or 9 MPa.
[0032] The present invention further provides a method for preparing the thermal insulation concrete, which comprises: mixing hydrophilic modified aerogel and hydrophobic aerogel, and then mixing the mixture with concrete raw materials to obtain the aerogel thermal insulation concrete.
[0033] According to an embodiment of the present invention, the preparation method specifically comprises:
[0034] A: Aerogel is obtained by mixing hydrophilic modified aerogel and hydrophobic aerogel in proportion;
[0035] B: Mixing the aerogel obtained in step A with the raw materials of concrete;
[0036] C: Add water to the dry powder mixture in step B and mix;
[0037] D: Mix the foaming agent with water to make foam;
[0038] E: The foam in step D is mixed with the slurry prepared in step C, and the mixture is stirred to obtain the thermal insulation concrete.
[0039] According to an embodiment of the present invention, in step A, the preparation method of the hydrophilic modified aerogel is as follows: taking a hydrophobic aerogel, treating it at a high temperature of 200 to 350° C. for 1 to 10 minutes to obtain a hydrophilic modified aerogel; or,
[0040] The hydrophilic modified aerogel is obtained by impregnation with a hydrophilic agent.
[0041] According to an embodiment of the present invention, the hydrophilic agent is selected from surfactants, low surface tension solvents or silicones.
[0042] Preferably, the surfactant is selected from one or more of anionic surfactants, cationic surfactants, amphoteric surfactants, and nonionic surfactants. Furthermore, the anionic surfactant is selected from one or more of fatty alcohol phosphates, fatty alcohol polyoxyethylene ether phosphates, alkyl sulfates, fatty alcohol polyoxyethylene ether sulfates, glycerol fatty acid ester sulfates, sulfated ricinoleates, cycloalkyl sulfates, fatty amide alkyl sulfates, alkylbenzene sulfonates, alkyl sulfonates, fatty acid methyl ester ethoxylate sulfonates, fatty acid methyl ester sulfonates, and fatty alcohol polyoxyethylene ether carboxylates. Furthermore, the cationic surfactant is selected from aliphatic ammonium salts. Furthermore, the amphoteric surfactant is selected from one or more of alkyl amino acids, carboxylic acid betaines, sulfobetaines, phosphate betaines, and alkyl hydroxyamine oxides. Furthermore, the nonionic surfactant is selected from one or more of aliphatic polyesters, alkylphenol polyoxyethylene ethers, high-carbon fatty alcohol polyoxyethylene ethers, fatty acid polyoxyethylene esters, fatty acid methyl ester ethoxylates, ethylene oxide adducts of polypropylene glycol, sorbitan esters, sucrose fatty acid esters, and alkyl ester amides.
[0043] Preferably, the low surface tension solvent is selected from one or more mixtures of acetone, n-hexane, n-pentane, n-heptane, ethanol, isopropanol, tert-butanol, propylene glycol, and glycerol.
[0044] Preferably, the organosilicon is selected from silane coupling agent ethyl orthosilicate, vinyl silane, aminosilane, methacryloxysilane, isobutyl triethoxysilane, propyl trimethoxysilane, triethoxysilane, and specifically KH-550 and KH-560.
[0045] According to an embodiment of the present invention, in step B, the raw materials of the concrete have the meanings as described above.
[0046] According to an embodiment of the present invention, in step E, the stirring is carried out at 5-30°C, preferably 8-10°C.
[0047] According to an embodiment of the present invention, in step E, after stirring, hardening and curing are further performed. Preferably, the curing conditions are: 20±2°C, relative humidity above 90%, and curing for more than 7 days.
[0048] The present invention further provides an application of the thermal insulation concrete, which is used in the fields of heat insulation, sound insulation, fire protection, thermal insulation, etc., and is preferably used for heat insulation, sound insulation, fire protection, and thermal insulation of buildings.
[0049] Exemplarily, the thermal insulation concrete is coated on a concrete wall, a building ceiling, a masonry wall, or a bottom layer of a concrete slab, or is poured into a mold and hardened to produce thermal insulation bricks or thermal insulation boards. Beneficial effects
[0050] 1. After adding hydrophilic modified aerogel particles, the present invention is easier to mix with concrete slurry. Compared with untreated hydrophobic aerogel particles, hydrophilic aerogel particles have better thermal insulation performance.
[0051] 2. In order to solve the problem that adding hydrophilic aerogel particles to concrete will reduce the strength of concrete, this application also introduces hydrophobic aerogel. Under the premise of maintaining thermal insulation performance, the strength is not reduced. That is, the mixed aerogel has better thermal insulation performance and the strength of concrete does not decrease much, especially the compressive strength. After adding hydrophobic powder as an additive, the dispersibility of the concrete slurry can be improved.
[0052] 3. After the hydrophilic modified aerogel particles are added to the present invention, the dust flying problem during the mixing process of aerogel powder and concrete is effectively solved.
[0053] 4. Hydrophilic modified aerogel particles are easier to mix with concrete. Compared with traditional mixing processes, the mixing time is shortened and the mixing process is simplified. BRIEF DESCRIPTION OF THE DRAWINGS
[0054] FIG1 is a schematic diagram of a preparation process of aerogel thermal insulation concrete according to the present invention.
[0055] FIG2 is a schematic diagram of the preparation process of another aerogel thermal insulation concrete of the present invention.
[0056] FIG3 is a line graph showing the compressive strength change of the thermal insulation concrete of the present invention with different aerogel addition amounts.
[0057] FIG4 is a line graph showing the change in thermal conductivity of the thermal insulation concrete of the present invention with different aerogel addition amounts. DETAILED DESCRIPTION
[0058] The technical solutions of the present invention will be described in further detail below with reference to specific embodiments. It should be understood that the following embodiments are merely illustrative and explanations of the present invention and should not be construed as limiting the scope of protection of the present invention. All technologies implemented based on the above content of the present invention are encompassed within the scope of protection that the present invention is intended to protect.
[0059] Unless otherwise specified, the raw materials and reagents used in the following examples are commercially available or can be prepared by known methods.
[0060] The reagents used in the following examples are as follows:
[0061] Cement: Commercially available Portland cement can be used, with grade 42.5 and above Portland cement being preferred.
[0062] Vitrified microbeads: particle size is 100μm~300μm.
[0063] Hydrophobic aerogel: Zhongke Runzi Technology Co., Ltd., brand RZF500 or RZF1000.
[0064] Water reducer: polyoxyethylene oleate, Polyshun Chemical.
[0065] Foaming agent: Sodium dodecylbenzenesulfonate, Shandong Tenghang New Material Technology Co., Ltd.
[0066] Preparation Example 1
[0067] Preparation of hydrophilic modified aerogel:
[0068] The hydrophobic aerogel (produced by Zhongke Runzi Technology Co., Ltd., brand RZF500 or RZF1000) is treated at a high temperature of 200-350° C. for 1-10 minutes to obtain a hydrophilic modified aerogel.
[0069] Preparation Example 2
[0070] Preparation of hydrophilic modified aerogel:
[0071] The hydrophobic aerogel (Zhongke Runzi Technology Co., Ltd., brand RZF500 or RZF1000) is impregnated with ethanol and dried to obtain a hydrophilic modified aerogel. Drying can be natural drying or heat drying. The heat drying conditions are: high temperature 90-110°C for 1-10 minutes.
[0072] The performance of the hydrophilic modified aerogel prepared in Preparation Example 2 is basically equivalent to that in Preparation Example 1. Both hydrophilic modification methods can achieve the hydrophilic modification effect.
[0073] Example 1
[0074] The preparation method of the hybrid aerogel thermal insulation concrete is as follows (the following parts are all by mass):
[0075] 1) Pretreatment: Take commercial cement and sieve it through a 100-150 mesh sieve to obtain cement powder with a particle size of 100-120 mesh;
[0076] 2) Mixing dry powder raw materials: 100 parts of cement powder and auxiliary materials from step 1) are mixed evenly to obtain a dry powder mixture, wherein the auxiliary materials include: 5 parts of water reducer and 12 parts of fly ash;
[0077] 3) Adding aerogel: Add 5 parts of mixed aerogel (which may be powder or aerogel premix paste) to the dry powder mixture of step 2) and mix evenly to obtain a mixture; wherein the mixed aerogel comprises the hydrophilic modified aerogel of Preparation Example 1 and commercially available hydrophobic aerogel in a mass ratio of 1:1, with the hydrophilic modified aerogel accounting for 2.5 parts;
[0078] 4) Stirring: Add 20-30 parts of water to the mixture of step 3) at a temperature of 5-30°C (preferably 8-10°C) to obtain slurry A;
[0079] 5) preparing foam: mixing 3 parts of a foaming agent, sodium lauryl sulfate, with 10 parts of water to form foam;
[0080] 6) Stirring: Add the foam prepared in step 5) to the slurry A obtained in step 4), and stir again for 3 minutes to obtain slurry B;
[0081] 7) Hardening: Harden and cure the slurry B prepared in step 6) to obtain aerogel thermal insulation concrete. Curing conditions are: temperature 20±2°C, relative humidity above 90%, and curing for at least 7 days.
[0082] The test shows that the compressive strength of the thermal insulation concrete of this embodiment is 8.78 MPa and the thermal conductivity is 0.277 W / (m·K), which are recorded in Table 1.
[0083] Example 1-1
[0084] The preparation method of the thermal insulation concrete of this embodiment is basically the same as that of Example 1, except that in step 3), the mixed aerogel is 5 parts, of which the hydrophilic modified aerogel is added in an amount of 1.67 parts, that is, the mass ratio of the hydrophilic modified aerogel to the hydrophobic aerogel is 1:2.
[0085] The test shows that the compressive strength of the thermal insulation concrete of this embodiment is 8.91 MPa and the thermal conductivity is 0.295 W / (m·K), which are recorded in Table 1.
[0086] Example 2
[0087] The preparation method of the thermal insulation concrete of this embodiment is basically the same as that of Example 1, except that in step 3), the mixed aerogel is 10 parts, of which the hydrophilic modified aerogel is added in an amount of 5 parts, and the mass ratio of the hydrophilic modified aerogel to the hydrophobic aerogel is 1:1.
[0088] The test shows that the compressive strength of the thermal insulation concrete of this embodiment is 7.83 MPa and the thermal conductivity is 0.184 W / (m·K), which are recorded in Table 1.
[0089] Example 2-1
[0090] The preparation method of the thermal insulation concrete of this embodiment is basically the same as that of Example 2, except that in step 3), the mixed aerogel is 10 parts, of which the hydrophilic modified aerogel is added in an amount of 3.33 parts, and the mass ratio of the hydrophilic modified aerogel to the hydrophobic aerogel is 1:2.
[0091] The test shows that the compressive strength of the thermal insulation concrete of this embodiment is 8.03 MPa and the thermal conductivity is 0.203 W / (m·K), which are recorded in Table 1.
[0092] Example 3
[0093] The preparation method of the thermal insulation concrete of this embodiment is basically the same as that of Example 1, except that in step 3), the mixed aerogel is 20 parts, of which the hydrophilic modified aerogel is added in an amount of 10 parts, and the mass ratio of the hydrophilic modified aerogel to the hydrophobic aerogel is 1:1.
[0094] The test shows that the compressive strength of the thermal insulation concrete of this embodiment is 4.65 MPa and the thermal conductivity is 0.133 W / (m·K), which are recorded in Table 1.
[0095] Example 3-1
[0096] The preparation method of the thermal insulation concrete of this embodiment is basically the same as that of Example 3, except that in step 3), the mixed aerogel is 20 parts, of which the hydrophilic modified aerogel is added in an amount of 6.67 parts, and the mass ratio of the hydrophilic modified aerogel to the hydrophobic aerogel is 1:2.
[0097] The test shows that the compressive strength of the thermal insulation concrete of this embodiment is 4.89 MPa and the thermal conductivity is 0.147 W / (m·K), which are recorded in Table 1.
[0098] Example 4
[0099] The preparation method of the thermal insulation concrete of this embodiment is basically the same as that of Example 1, except that in step 3), the mixed aerogel is 15 parts, of which the hydrophilic modified aerogel is added in an amount of 7.5 parts, and the mass ratio of the hydrophilic modified aerogel to the hydrophobic aerogel is 1:1.
[0100] The test shows that the compressive strength of the thermal insulation concrete of this embodiment is 5.93 MPa and the thermal conductivity is 0.152 W / (m·K), which are recorded in Table 1.
[0101] Example 4-1
[0102] The preparation method of the thermal insulation concrete of this embodiment is basically the same as that of Example 4, except that in step 3), the mixed aerogel is 15 parts, of which the hydrophilic modified aerogel is added in an amount of 5 parts, and the mass ratio of the hydrophilic modified aerogel to the hydrophobic aerogel is 1:2.
[0103] The test shows that the compressive strength of the thermal insulation concrete of this embodiment is 6.14 MPa and the thermal conductivity is 0.166 W / (m·K), which are recorded in Table 1.
[0104] Example 5
[0105] The preparation method of the thermal insulation concrete of this embodiment is basically the same as that of Example 1, except that in step 3), the mixed aerogel is 25 parts, of which the hydrophilic modified aerogel is added in an amount of 12.5 parts, and the mass ratio of the hydrophilic modified aerogel to the hydrophobic aerogel is 1:1.
[0106] The test shows that the compressive strength of the thermal insulation concrete of this embodiment is 3.82 MPa and the thermal conductivity is 0.125 W / (m·K), which are recorded in Table 1.
[0107] Example 5-1
[0108] The preparation method of the thermal insulation concrete of this embodiment is basically the same as that of Example 5, except that in step 3), the mixed aerogel is 25 parts, of which the hydrophilic modified aerogel is added in an amount of 8.3 parts, and the mass ratio of the hydrophilic modified aerogel to the hydrophobic aerogel is 1:2.
[0109] The test shows that the compressive strength of the thermal insulation concrete of this embodiment is 4.02 MPa and the thermal conductivity is 0.134 W / (m·K), which are recorded in Table 1.
[0110] Comparative Example 1
[0111] This embodiment is basically the same as embodiment 2, except that in step 3), only hydrophilic modified aerogel is used, and the addition amount thereof is 10 parts.
[0112] The test shows that the compressive strength of the thermal insulation concrete of this comparative example is 7.61 MPa and the thermal conductivity is 0.158 W / (m·K), which are recorded in Table 1.
[0113] Comparative Example 2
[0114] This embodiment is basically the same as embodiment 2, except that only hydrophobic aerogel is used in step 3), and the amount of hydrophobic aerogel added is 10 parts.
[0115] The test shows that the compressive strength of the thermal insulation concrete of this comparative example is 8.16 MPa and the thermal conductivity is 0.211 W / (m·K), which are recorded in Table 1.
[0116] Table 1
[0117] The above describes exemplary embodiments of the present invention. However, the scope of protection of this application is not limited to the above embodiments. Any modifications, equivalent substitutions, improvements, etc. made by those skilled in the art within the spirit and principles of the present invention should be included in the scope of protection of the present invention.
Claims
1. A thermal insulation concrete, comprising aerogel and concrete; characterized in that: The aerogel is uniformly dispersed in the concrete; the aerogel includes hydrophilic modified aerogel and hydrophobic aerogel; The thermal insulation concrete according to claim 2 is characterized in that, in the thermal insulation concrete, the mass ratio of aerogel to concrete is (0-30):100 and the content of aerogel is not 0.
2. The thermal insulation concrete according to claim 1, characterized in that: In the aerogel, the mass ratio of the hydrophilic aerogel to the hydrophobic aerogel is 100:(0-200) and the content of the hydrophobically modified aerogel is not zero.
3. The thermal insulation concrete according to claim 2, characterized in that: The hydrophilic modified aerogel is a hydrophilic modified aerogel particle.
4. The thermal insulation concrete according to claim 3, characterized in that: The raw materials of the concrete include cement.
5. The thermal insulation concrete according to claim 4, characterized in that: The raw materials of the concrete further include auxiliary materials.
6. The thermal insulation concrete according to claim 5, characterized in that: The auxiliary materials also include a foaming agent.
7. The thermal insulation concrete according to claim 6, characterized in that: The foaming agent is added in an amount of 0.1 to 5 parts by mass per 100 parts by mass of cement.
8. The thermal insulation concrete according to claim 6, characterized in that: The auxiliary material is selected from at least one of a water reducing agent, fly ash, vitrified microspheres, water and reinforcing fibers.
9. The thermal insulation concrete according to any one of claims 1 to 8, characterized in that: The thermal conductivity of the thermal insulation concrete is not higher than 0.3w / (mk); And / or, the compressive strength of the thermal insulation concrete is 1 to 10 MPa.
10. The method for preparing the thermal insulation concrete according to any one of claims 1 to 8, characterized in that: The preparation method comprises: mixing hydrophilic modified aerogel and hydrophobic aerogel, and then mixing the mixture with raw materials of concrete to obtain the aerogel thermal insulation concrete.
11. Use of the thermal insulation concrete according to any one of claims 1 to 8 in the fields of heat insulation, sound insulation, fire protection or thermal insulation.
Citation Information
Patent Citations
Super-thermal-insulation aerogel foamed concrete and preparation method thereof
CN107265962A
Super-thermal-insulation aerogel foamed concrete and preparation method thereof
CN107265963A
Aerogel foam concrete and preparation method and application thereof
CN110803938A
Foam concrete and preparation method thereof
CN113603423A
Carbon sequestration thermal insulation concrete and preparation method thereof
CN115304398A