Method for preparing aerogel modified gypsum

Through the method of combining vacuum stirring and normal pressure stirring, combined with the use of hydrophilic modified aerogel and hydrophobic aerogel, the problem of difficulty in mixing aerogel and gypsum is solved, and the efficient insulation and strength improvement of gypsum are achieved.

WO2024216430A1PCT designated stage expired Publication Date: 2024-10-24ZHONGKE RUNZI (CHONGQING) AEROGEL RES INST CO LTD

Patent Information

Application Number
PCT/CN2023/088650
Authority / Receiving Office
WO · WO
Patent Type
Applications
Current Assignee / Owner
Filing Date
2023-04-17
Publication Date
2024-10-24

AI Technical Summary

Technical Problem

It is difficult to achieve effective mixing of airgel and gypsum with existing technology, resulting in insufficient thermal insulation performance and strength of gypsum.

Method used

Use vacuum stirring to mix the airgel and gypsum raw materials, then add air-entraining agent under normal pressure conditions, and combine the mixing of hydrophilic modified airgel and hydrophobic airgel to improve the mixing uniformity and thermal insulation performance.

Benefits of technology

It significantly improves the thermal insulation effect and strength of gypsum, overcomes the problem of reduced air-entraining agent effect, and maintains the mechanical strength of gypsum.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN2023088650_24102024_PF_FP_ABST
    Figure CN2023088650_24102024_PF_FP_ABST
Patent Text Reader

Abstract

Disclosed is a method for preparing aerogel modified gypsum. The preparation method of the present invention comprises: mixing aerogel with gypsum raw materials and auxiliary materials while vacuum stirring, then adding an air entraining agent under normal-pressure conditions, and uniformly mixing to obtain an aerogel modified gypsum. By first performing vacuum stirring and then adding the air entraining agent and stirring under normal pressure, the present invention effectively overcomes the problem in the prior art whereby the the effect of the air entraining agent is reduced due to introduction during vacuum stirring. The method of the present invention achieves a better mixing effect while maximizing the function of the air entraining agent, and prepares a gypsum having significantly improved thermal insulation and strength.
Need to check novelty before this filing date? Find Prior Art

Description

A method for preparing aerogel-modified gypsum Technical Field

[0001] The invention belongs to the technical field of building thermal insulation and relates to a method for preparing aerogel-modified gypsum. Background Art

[0002] As demand for green, energy-efficient, and environmentally friendly buildings continues to increase, building insulation materials are a major research area for building energy conservation. Gypsum is a widely used building insulation material, and optimizing its thermal insulation properties meets the current demands for green and sustainable development.

[0003] Aerogel is a lightweight, solid material with a three-dimensional network structure and nanoscale pores. It boasts a large surface area, high porosity, low density, and extremely low thermal conductivity, enhancing the performance of traditional insulation materials.

[0004] Some existing technologies attempt to improve the thermal insulation properties of gypsum by adding aerogel. However, aerogel powder is extremely light and floats above the gypsum slurry during mixing, making it difficult to mix. There is an urgent need to develop a method for effectively adding aerogel to produce a modified gypsum with both excellent thermal insulation and strength properties.

[0005] To solve the problem of aerogel powder and gypsum being difficult to mix, the main methods currently used include increasing the stirring time and changing the mixing ratio. However, most of the existing methods can only improve the mixing of aerogel powder particles in the gypsum slurry, and cannot effectively achieve uniform mixing.

[0006] Summary of the Invention

[0007] In order to solve the above technical problems, the present invention provides the following technical solutions:

[0008] A method for preparing aerogel-modified gypsum comprises: mixing aerogel with raw materials and auxiliary materials of gypsum under vacuum stirring conditions, and then adding an air entraining agent under normal pressure conditions and mixing them uniformly to obtain the aerogel-modified gypsum.

[0009] According to an embodiment of the present invention, the conditions for vacuum stirring specifically include: stirring under an absolute pressure of less than 1 KPa; stirring time of no more than 5 minutes; and stirring temperature of 8°C to 10°C.

[0010] According to an embodiment of the present invention, the aerogel is added into the raw materials of gypsum.

[0011] According to an embodiment of the present invention, the raw material of the gypsum is selected from plaster of Paris.

[0012] According to an embodiment of the present invention, in the aerogel-modified gypsum, the mass ratio of aerogel to gypsum is (0-30):100 and the content of the aerogel is not zero.

[0013] According to an embodiment of the present invention, in the aerogel-modified gypsum, the particle size of the aerogel is 1 nm to 50 nm.

[0014] According to an embodiment of the present invention, the aerogel is selected from hydrophilically modified aerogels and / or hydrophobic aerogels.

[0015] According to a preferred embodiment of the present invention, the aerogel includes hydrophilic modified aerogel and hydrophobic aerogel, wherein the mass ratio of hydrophilic modified aerogel to hydrophobic aerogel is 100:(0-100) and the content of the hydrophobic aerogel is not zero.

[0016] Preferably, the mass ratio of the hydrophilic modified aerogel to the hydrophobic aerogel is 100:(20-50).

[0017] According to an embodiment of the present invention, the hydrophilically modified aerogel is a hydrophilically modified aerogel particle.

[0018] According to an embodiment of the present invention, the contact angle between the hydrophilic modified aerogel and water is less than 90°.

[0019] According to an embodiment of the present invention, the contact angle of the hydrophobic aerogel with water is greater than 90°.

[0020] According to an embodiment of the present invention, the auxiliary material includes water and at least one of the following substances: glass microspheres, a reinforcing agent, a dispersant, a reinforcing fiber, and a retarder.

[0021] According to an embodiment of the present invention, the amount of the auxiliary material added is 0.1 to 200 parts by mass per 100 parts by mass of the gypsum raw material.

[0022] According to an embodiment of the present invention, the amount of water is 100 to 120 parts by mass per 100 parts by mass of the gypsum raw material.

[0023] According to an embodiment of the present invention, the dispersant is present in an amount of 0.01 to 5 parts by mass per 100 parts by mass of the gypsum raw material.

[0024] According to an embodiment of the present invention, the dispersant is selected from polyoxyethylene dioleate, tetraethylene glycol monostearate, tetraethylene glycol monooleate, polyoxypropylene mannitol dioleate, polyoxyethylene sorbitol lanolin oleic acid derivatives, polyoxyethylene sorbitol lanolin derivatives, polyoxypropylene stearate, polyoxyethylene (5EO) lanolin ether, anhydrous sorbitan laurate, polyoxyethylene fatty acid, polyoxyethylene oxypropylene oleate, triethylhexyl phosphoric acid, sodium lauryl sulfate, methyl amyl alcohol, cellulose derivatives, polyacrylamide, gur gum, fatty acid polyethylene glycol esters.

[0025] According to an embodiment of the present invention, the amount of the vitrified microspheres is 5 to 40 parts by mass per 100 parts by mass of the gypsum raw material.

[0026] According to an embodiment of the present invention, the reinforcing fibers are selected from inorganic fibers and organic fibers. Preferably, the reinforcing fibers are short fibers, specifically fibers with a length of 3 mm to 60 mm.

[0027] According to an embodiment of the present invention, the reinforcing fiber is present in an amount of 0.5 to 5 parts by mass per 100 parts by mass of the gypsum raw material.

[0028] According to an embodiment of the present invention, the retarder is selected from organic acids and soluble salts thereof, alkaline phosphates, proteins and other retarders.

[0029] According to an embodiment of the present invention, the retarder is in an amount of 0.01-0.5 parts by mass per 100 parts by mass of the gypsum raw material.

[0030] According to an embodiment of the present invention, before the vacuum stirring, the gypsum raw materials, auxiliary materials and aerogel are premixed to obtain a uniform premix. Preferably, the temperature during premixing is controlled at 8°C to 10°C.

[0031] According to an embodiment of the present invention, the mass ratio of the air entraining agent to the gypsum raw materials is 0.1 to 1:100. Beneficial effects

[0032] 1. This invention provides a method for preparing aerogel-modified gypsum. This method first performs vacuum stirring, then adds an air-entraining agent and stirs under normal pressure. This method effectively overcomes the problem in the prior art where vacuum stirring reduces the effectiveness of the air-entraining agent. This method achieves excellent mixing while fully utilizing the function of the air-entraining agent, resulting in a gypsum with significantly improved thermal insulation and strength.

[0033] 2. The present invention further introduces hydrophilic modified aerogel, which is easier to mix with gypsum slurry. In addition, compared with untreated hydrophobic aerogel, the hydrophilic modified aerogel has better thermal insulation performance.

[0034] 3. In order to solve the problem that adding hydrophilic modified aerogel to gypsum will reduce the strength of gypsum, the present invention also proposes a solution of mixing hydrophilic modified aerogel with hydrophobic aerogel. Under the premise of maintaining thermal insulation performance, the strength is not reduced. That is, the mixed aerogel has better thermal insulation performance and the strength of gypsum is not greatly reduced. Moreover, after adding hydrophobic aerogel as an additive, the dispersibility of the gypsum slurry can also be improved. BRIEF DESCRIPTION OF THE DRAWINGS

[0035] FIG1 is a schematic diagram of a preparation process of an aerogel thermal insulation gypsum according to the present invention.

[0036] FIG2 is a schematic diagram of the preparation process of another aerogel thermal insulation gypsum of the present invention. DETAILED DESCRIPTION

[0037] As mentioned above, the present invention provides a method for preparing aerogel-modified gypsum, which comprises: mixing aerogel with raw materials and auxiliary materials of gypsum under vacuum stirring conditions, and then adding an air entraining agent under normal pressure conditions and mixing them uniformly to obtain the aerogel-modified gypsum.

[0038] The inventors discovered that while vacuum stirring can reduce aerogel splashing, it also reduces the effectiveness of the air-entraining agent. Therefore, the present invention first performs vacuum stirring, then adds the air-entraining agent and stirs under normal pressure. This achieves better mixing while fully utilizing the air-entraining agent's function, resulting in a gypsum with significantly improved thermal insulation and strength.

[0039] According to an embodiment of the present invention, the conditions for vacuum stirring specifically include: stirring under an absolute pressure of less than 1 KPa; stirring time of no more than 5 minutes; and stirring temperature of 8°C to 10°C.

[0040] According to an embodiment of the present invention, the aerogel is added to the gypsum raw material. Preferably, the aerogel can be added in multiple times to shorten the vacuum stirring time. The number of additions can be selected based on actual conditions, for example, 2-10 times.

[0041] According to an embodiment of the present invention, the raw material of the gypsum is selected from gypsum powder (e.g., hemihydrate gypsum powder). Preferably, the purity of the gypsum powder is at least greater than 90%, for example, 95% or 98%. Preferably, the gypsum powder has a relatively high fineness, for example, 100-120 mesh.

[0042] According to an embodiment of the present invention, in the aerogel-modified gypsum, the mass ratio of aerogel to gypsum is (0-30):100 and the content of the aerogel is not 0, for example, 5:100, 10:100, 15:100, 20:100, 25:100, or 30:100.

[0043] According to an embodiment of the present invention, in the aerogel-modified gypsum, the particle size of the aerogel is 1 nm-50 nm, preferably 20 nm-50 nm, for example, 1 nm, 10 nm, 20 nm, 30 nm, 40 nm or 50 nm.

[0044] According to an embodiment of the present invention, the aerogel is selected from hydrophilically modified aerogels and / or hydrophobic aerogels.

[0045] The study found that when hydrophilic modified aerogel is added, it is easier to mix with gypsum slurry. In addition, compared with untreated hydrophobic aerogel, the hydrophilic modified aerogel has better thermal insulation performance.

[0046] According to a preferred embodiment of the present invention, the aerogel includes hydrophilic modified aerogel and hydrophobic aerogel, wherein the mass ratio of hydrophilic modified aerogel to hydrophobic aerogel is 100:(0-100) and the content of the hydrophobic aerogel is not zero.

[0047] The study found that if only hydrophilic modified aerogel is added to gypsum, the strength of the gypsum will be reduced. However, if hydrophobic aerogel is introduced at the same time as the hydrophilic modified aerogel, the strength can be maintained without reducing while maintaining the thermal insulation performance. That is, the mixed aerogel has better thermal insulation performance and the strength of the gypsum does not decrease much. Moreover, after adding hydrophobic powder as an additive, the dispersibility of the gypsum slurry can also be improved.

[0048] Preferably, the mass ratio of the hydrophilic modified aerogel to the hydrophobic aerogel is 100:(20-50), for example, 100:5, 100:10, 100:20, 100:30, 100:40, 100:60, 100:70, 100:80, or 100:90. Studies have found that when the mass ratio of the hydrophobic aerogel to the hydrophilic modified aerogel is within the above range, the thermal insulation performance of the thermal insulation gypsum can be guaranteed while maintaining the mechanical strength of the thermal insulation gypsum.

[0049] According to an embodiment of the present invention, the hydrophilically modified aerogel is a hydrophilically modified aerogel particle.

[0050] According to an embodiment of the present invention, the contact angle between the hydrophilic modified aerogel and water is less than 90°. Preferably, the surface of the hydrophilic modified aerogel contains hydrophilic groups, which are selected from groups known in the art, such as hydroxyl groups (-OH).

[0051] According to an embodiment of the present invention, the contact angle of the hydrophobic aerogel with water is greater than 90°. Preferably, the surface of the hydrophobic aerogel contains hydrophobic groups, which are selected from groups known in the art, such as alkoxy groups (-OR, R represents an alkyl group).

[0052] According to an embodiment of the present invention, the auxiliary material includes water and at least one of the following substances: glass microspheres, a reinforcing agent, a dispersant, a reinforcing fiber, and a retarder. Exemplarily, the auxiliary material includes water, glass microspheres, a reinforcing agent, a dispersant, a reinforcing fiber, and a retarder.

[0053] According to an embodiment of the present invention, the amount of the auxiliary material added is 0.1 to 200 parts by mass per 100 parts by mass of the gypsum raw material.

[0054] According to an embodiment of the present invention, the amount of water is 100 to 120 parts by mass, for example, 105 parts by mass, 110 parts by mass, 115 parts by mass, or 120 parts by mass, per 100 parts by mass of the gypsum raw material.

[0055] According to the embodiment of the present invention, the dispersant can improve the fluidity of the product during molding and processing; it does not affect the performance of the product, and is non-toxic and reasonably priced.

[0056] According to an embodiment of the present invention, the dispersant is 0.01-5 parts by mass per 100 parts by mass of the gypsum raw material, for example, 0.1 parts by mass, 0.5 parts by mass, 1 part by mass, 2 parts by mass, 3 parts by mass, or 4 parts by mass.

[0057] According to an embodiment of the present invention, the dispersant is selected from polyoxyethylene dioleate, tetraethylene glycol monostearate, tetraethylene glycol monooleate, polyoxypropylene mannitol dioleate, polyoxyethylene sorbitol lanolin oleic acid derivatives, polyoxyethylene sorbitol lanolin derivatives, polyoxypropylene stearate, polyoxyethylene (5EO) lanolin ether, anhydrous sorbitan laurate, polyoxyethylene fatty acid, polyoxyethylene oxypropylene oleate, triethylhexyl phosphoric acid, sodium lauryl sulfate, methyl amyl alcohol, cellulose derivatives, polyacrylamide, gur gum, fatty acid polyethylene glycol esters, preferably polyoxypropylene stearate and polyoxyethylene dioleate.

[0058] According to an embodiment of the present invention, the amount of the vitrified microspheres is 5 to 40 parts by weight, for example, 10 parts by weight, 20 parts by weight, 30 parts by weight, or 40 parts by weight, per 100 parts by weight of the gypsum raw material.

[0059] According to an embodiment of the present invention, the glass microspheres can be selected from materials known in the art and are not specifically limited in the present invention.

[0060] According to an embodiment of the present invention, the reinforcing fibers are selected from inorganic fibers and organic fibers, such as polyester fibers, glass fibers, basalt fibers, etc. Preferably, the reinforcing fibers are short fibers, specifically fibers with a length of 3 mm to 60 mm, such as 10 mm, 20 mm, 30 mm, 40 mm, or 50 mm.

[0061] According to an embodiment of the present invention, the reinforcing fiber is present in an amount of 0.5-5 parts by mass, for example, 0.6 parts by mass, 0.7 parts by mass, 0.8 parts by mass, or 0.9 parts by mass, per 100 parts by mass of the gypsum raw material. In the present invention, the reinforcing fiber is used as a skeleton filling material to increase the strength of the aerogel-modified gypsum.

[0062] According to an embodiment of the present invention, the retarder is selected from organic acids and their soluble salts, alkaline phosphates, and proteins. Exemplarily, the retarder is selected from citric acid, sodium citrate, tartaric acid, potassium tartrate, acrylic acid and sodium acrylate, sodium hexametaphosphate, sodium polyphosphate, borax, sodium borate, sodium tripolyphosphate, and sodium gluconate, with citric acid, tartaric acid, and sodium gluconate being preferred. In the present invention, the retarder can extend the mixing time, increase the paste-water ratio, and enhance the strength of the finished product.

[0063] According to an embodiment of the present invention, the retarder is 0.01-0.5 parts by mass, for example, 0.05 parts by mass, 0.1 parts by mass, 0.2 parts by mass, 0.3 parts by mass, or 0.4 parts by mass, per 100 parts by mass of the gypsum raw material.

[0064] According to an embodiment of the present invention, the gypsum raw materials, auxiliary materials, and aerogel may be premixed prior to vacuum stirring to obtain a uniform premix. Preferably, the temperature during premixing is controlled at 8°C to 10°C. This is to reduce the dissolution rate of hemihydrate gypsum in water, prolong the dissolution and crystal nucleation time of the gypsum raw materials in water, and thus slow the reaction rate between the gypsum raw materials and water.

[0065] According to an embodiment of the present invention, the mass ratio of the air entraining agent to the gypsum raw material is 0.1 to 1:100, for example 0.1:100 or 0.5:100. The inventors have found that adding the air entraining agent and stirring uniformly can improve the fluidity and cohesiveness of the mixture.

[0066] According to an embodiment of the present invention, the air entraining agent can be selected from air entraining agents known in the art, for example, rosin resin air entraining agents, alkylbenzene sulfonate air entraining agents, and fatty alcohol sulfonate air entraining agents.

[0067] Specifically, the air entraining agent can be selected from at least one of sodium lauryl sulfate, sodium rosinate, triterpenoid saponin, and sodium α-olefin sulfonate.

[0068] According to an embodiment of the present invention, the vacuum stirring and stirring are respectively carried out in a high-speed stirring device. Specifically, the high-speed stirring device can be a high-speed magnetic stirrer, a free-fall stirrer or a forced stirrer.

[0069] According to an embodiment of the present invention, after the air entraining agent is added and mixed evenly, hardening and curing can be further performed. Preferably, the curing can be performed using methods known in the art.

[0070] Exemplarily, the curing process includes natural curing followed by enhanced curing. Furthermore, the natural curing process includes curing at 0-40°C for 12-36 hours. Furthermore, the enhanced curing process includes an ambient temperature of 30-50°C (preferably 40°C), a humidity of no more than 90% (preferably 10%, 20%, 50%, 70%, or 80%), and a curing time of 48-72 hours.

[0071] The present invention also provides aerogel-modified gypsum obtained by the above preparation method.

[0072] According to an embodiment of the present invention, the thermal conductivity of the aerogel-modified gypsum is not higher than 0.25w / (mk), for example, 0.2w / (mk), 0.1w / (mk), 0.07w / (mk), or 0.05w / (mk).

[0073] According to an embodiment of the present invention, the compressive strength of the aerogel-modified gypsum is 1 to 10 MPa, for example, 2 MPa, 3 MPa, 4 MPa, 5 MPa, 6 MPa, 7 MPa, 8 MPa, or 9 MPa.

[0074] The technical solutions of the present invention will be described in further detail below with reference to specific embodiments. It should be understood that the following embodiments are merely illustrative and explanations of the present invention and should not be construed as limiting the scope of protection of the present invention. All technologies implemented based on the above content of the present invention are encompassed within the scope of protection that the present invention is intended to protect.

[0075] Unless otherwise specified, the raw materials and reagents used in the following examples are commercially available or can be prepared by known methods.

[0076] The reagents used in the following examples are as follows:

[0077] Plaster of Paris: Commercially available gypsum powder (calcium sulfate hemihydrate) may be used, with a CaSO4·0.5H2O content (purity) greater than 90%, preferably greater than 98%.

[0078] The reinforcing fibers include at least one of glass fibers, polypropylene fibers, and polyester fibers. The reinforcing fibers can improve the anti-cracking performance of the thermal insulation gypsum and increase the tensile strength.

[0079] Vitrified microbeads: particle size is 100μm~300μm.

[0080] Hydrophobic aerogel: Zhongke Runzi Technology Co., Ltd., brand RZF500 or RZF1000.

[0081] Dispersant: polyoxyethylene oleate, Polyshun Chemical.

[0082] Preparation Example 1

[0083] Preparation of hydrophilic modified aerogel:

[0084] Hydrophilic modification method 1: Take the above-mentioned hydrophobic aerogel (Zhongke Runzi Technology Co., Ltd., brand RZF500 or RZF1000) and treat it at a high temperature of 200-350° C. for 1-10 minutes to obtain a hydrophilic modified aerogel.

[0085] Preparation Example 2

[0086] Preparation of hydrophilic modified aerogel:

[0087] Hydrophilic Modification Method 2: Take the hydrophobic aerogel (Zhongke Runzi Technology Co., Ltd., brand RZF500 or RZF1000), impregnate it with ethanol, and then dry it to obtain a hydrophilic modified aerogel. This can be done naturally or by heating. The heating and drying conditions are: high temperature (90-110°C) for 1-10 minutes.

[0088] The performance of the hydrophilic modified aerogel prepared in Preparation Example 2 is basically equivalent to that in Preparation Example 1. Both hydrophilic modification methods can achieve the hydrophilic modification effect.

[0089] Example 1

[0090] The preparation method of aerogel modified gypsum is as follows:

[0091] A. Preparation of a hybrid aerogel: mixing a hydrophilic modified aerogel and a hydrophobic modified aerogel in proportion to obtain an aerogel; wherein the hybrid aerogel comprises the hydrophilic modified aerogel of Preparation Example 1 and a commercially available hydrophobic aerogel, and the mass ratio of the two is 1:1;

[0092] B. The aerogel obtained in step A is pre-mixed with gypsum powder, water, auxiliary materials and aerogel, and then stirred in a blender to obtain gypsum slurry. The specific preparation method is as follows (the following parts are all by mass):

[0093] 1) Pretreatment of gypsum powder: sieve commercially available gypsum powder through a 100-150 mesh sieve to obtain gypsum powder with a particle size of 100-120 mesh;

[0094] 2) Mixing dry powder raw materials: 100 parts of the gypsum powder prepared in step 1) are mixed uniformly with 5 parts of mixed aerogel (including 2.5 parts of hydrophilic modified aerogel) and auxiliary materials at 2-8° C. to obtain a dry powder mixture, wherein the auxiliary materials include: 0.2 parts of citric acid as a retarder, 1 part of a dispersant, 10 parts of vitrified microspheres, and 1 part of reinforcing fiber glass fiber;

[0095] 3) Vacuum stirring: add 100-120 parts of water to the dry powder mixture in step 2), with the water temperature at 8-10°C, and evacuate to an absolute pressure of less than 1 kPa. Maintain vacuum stirring for 2 minutes to obtain slurry A;

[0096] 4) Stirring at normal pressure: 0.2 parts of an air-entraining agent, sodium lauryl sulfate, was added to the slurry A obtained in step 3), and the mixture was stirred at normal pressure again (i.e., the stirring environment was at normal pressure) for 3 minutes to obtain slurry B;

[0097] C: Pour slurry B into the mold or apply it to the target substrate surface, and harden and cure it, including:

[0098] 1) Natural curing: Pour slurry B into a mold or apply it on the substrate and place it at room temperature for 12-36 hours;

[0099] 2) Enhanced curing: The mold containing slurry B or the substrate coated with slurry B after natural curing is subjected to enhanced curing, wherein the ambient temperature for enhanced curing is 40° C., the humidity is not greater than 70%, and the curing time is 48 h to 72 h to obtain the aerogel-modified gypsum.

[0100] The test shows that the compressive strength of the thermal insulation gypsum of this embodiment is 7.36 MPa and the thermal conductivity is 0.160 W / (m·K), which are recorded in Table 1.

[0101] Example 1-1

[0102] The preparation method of the thermal insulation gypsum of this embodiment is basically the same as that of Example 1, except that in step 2), the mixed aerogel is 5 parts, of which the hydrophilic modified aerogel is added in an amount of 3.33 parts, that is, the mass ratio of the hydrophilic modified aerogel to the hydrophobic aerogel is 2:1.

[0103] The test shows that the compressive strength of the thermal insulation gypsum of this embodiment is 7.40 MPa and the thermal conductivity is 0.157 W / (m·K), which are recorded in Table 1.

[0104] Example 2

[0105] The preparation method of the thermal insulation gypsum of this embodiment is basically the same as that of Example 1, except that in step 2), the mixed aerogel is 10 parts, of which the hydrophilic modified aerogel is added in an amount of 5 parts, and the mass ratio of the hydrophilic modified aerogel to the hydrophobic aerogel is 1:1.

[0106] The test shows that the compressive strength of the thermal insulation gypsum of this embodiment is 6.19 MPa and the thermal conductivity is 0.111 W / (m·K), which are recorded in Table 1.

[0107] Example 2-1

[0108] The preparation method of the thermal insulation gypsum of this embodiment is basically the same as that of Example 2, except that in step 2), the mixed aerogel is 10 parts, of which the hydrophilic modified aerogel is added in an amount of 6.67 parts, and the mass ratio of the hydrophilic modified aerogel to the hydrophobic aerogel is 2:1.

[0109] The test shows that the compressive strength of the thermal insulation gypsum of this embodiment is 5.97 MPa and the thermal conductivity is 0.109 W / (m·K), which are recorded in Table 1.

[0110] Example 3

[0111] The preparation method of the thermal insulation gypsum of this embodiment is basically the same as that of Example 1, except that in step 2), the mixed aerogel is 20 parts, of which the hydrophilic modified aerogel is added in an amount of 10 parts, and the mass ratio of the hydrophilic modified aerogel to the hydrophobic aerogel is 1:1.

[0112] The test shows that the compressive strength of the thermal insulation gypsum of this embodiment is 2.76 MPa and the thermal conductivity is 0.091 W / (m·K), which are recorded in Table 1.

[0113] Example 3-1

[0114] The preparation method of the thermal insulation gypsum of this embodiment is basically the same as that of Example 3, except that in step 2), the mixed aerogel is 20 parts, of which the hydrophilic modified aerogel is added in an amount of 13.33 parts, and the mass ratio of the hydrophilic modified aerogel to the hydrophobic aerogel is 2:1.

[0115] The test shows that the compressive strength of the thermal insulation gypsum of this embodiment is 2.45 MPa and the thermal conductivity is 0.082 W / (m·K), which are recorded in Table 1.

[0116] Example 4

[0117] The preparation method of the thermal insulation gypsum of this embodiment is basically the same as that of Example 1, except that in step 2), the mixed aerogel is 15 parts, of which the hydrophilic modified aerogel is added in an amount of 7.5 parts, and the mass ratio of the hydrophilic modified aerogel to the hydrophobic aerogel is 1:1.

[0118] The test shows that the compressive strength of the thermal insulation gypsum of this embodiment is 4.14 MPa and the thermal conductivity is 0.098 W / (m·K), which are recorded in Table 1.

[0119] Example 4-1

[0120] The preparation method of the thermal insulation gypsum of this embodiment is basically the same as that of Example 4, except that in step 2), the mixed aerogel is 15 parts, of which the hydrophilic modified aerogel is added in an amount of 10 parts, and the mass ratio of the hydrophilic modified aerogel to the hydrophobic aerogel is 2:1.

[0121] The test shows that the compressive strength of the thermal insulation gypsum of this embodiment is 3.64 MPa and the thermal conductivity is 0.089 W / (m·K), which are recorded in Table 1.

[0122] Example 5

[0123] The preparation method of the thermal insulation gypsum of this embodiment is basically the same as that of Example 1, except that in step 2), the mixed aerogel is 25 parts, of which the hydrophilic modified aerogel is added in an amount of 12.5 parts, and the mass ratio of the hydrophilic modified aerogel to the hydrophobic aerogel is 1:1.

[0124] The test shows that the compressive strength of the thermal insulation gypsum of this embodiment is 1.93 MPa and the thermal conductivity is 0.085 W / (m·K), which are recorded in Table 1.

[0125] Example 5-1

[0126] The preparation method of the thermal insulation gypsum of this embodiment is basically the same as that of Example 5, except that in step 2), the mixed aerogel is 25 parts, of which the hydrophilic modified aerogel is added in an amount of 16.7 parts, and the mass ratio of the hydrophilic modified aerogel to the hydrophobic aerogel is 2:1.

[0127] The test shows that the compressive strength of the thermal insulation gypsum of this embodiment is 1.71 MPa and the thermal conductivity is 0.077 W / (m·K), which are recorded in Table 1.

[0128] Example 6

[0129] The preparation method of the thermal insulation gypsum of this embodiment is basically the same as that of Example 1, except that only the hydrophilic modified aerogel of Preparation Example 1 is used in step A;

[0130] In step B, step 2) uses the hydrophilic modified aerogel of Preparation Example 1.

[0131] The test shows that the compressive strength of the thermal insulation gypsum of this embodiment is 7.18 MPa and the thermal conductivity is 0.154 W / (m·K), which are recorded in Table 1.

[0132] Example 7

[0133] The preparation method of the thermal insulation gypsum of this embodiment is basically the same as that of Example 1, except that only commercially available hydrophobic aerogel is used in step A;

[0134] In step B, step 2) uses commercially available hydrophobic aerogel.

[0135] The test shows that the compressive strength of the thermal insulation gypsum of this embodiment is 8.45 MPa and the thermal conductivity is 0.171 W / (m·K), which are recorded in Table 1.

[0136] Comparative Example 1

[0137] This comparative example is basically the same as Example 2, except that:

[0138] In step 3), 0.2 parts of an air-entraining agent, sodium lauryl sulfate, was further added, and no vacuum operation was performed. The mixture was directly stirred at normal pressure for 5 minutes to obtain slurry B.

[0139] The test shows that the compressive strength of the thermal insulation gypsum of this comparative example is 5.63 MPa and the thermal conductivity is 0.118 W / (m·K), which are recorded in Table 1.

[0140] Comparative Example 2

[0141] This comparative example is basically the same as Example 2-1, except that:

[0142] In step 3), 0.2 parts of an air-entraining agent, sodium lauryl sulfate, was further added, and no vacuum operation was performed. The mixture was directly stirred at normal pressure for 5 minutes to obtain slurry B.

[0143] The test shows that the compressive strength of the thermal insulation gypsum of this comparative example is 5.43 MPa and the thermal conductivity is 0.116 W / (m·K), which are recorded in Table 1.

[0144] Comparative Example 3

[0145] This comparative example is basically the same as Example 2, except that only hydrophilic modified aerogel is used in step 2), and the addition amount thereof is 10 parts.

[0146] In step 3), 0.2 parts of an air-entraining agent, sodium lauryl sulfate, was further added, and no vacuum operation was performed. The mixture was directly stirred at normal pressure for 5 minutes to obtain slurry B.

[0147] The test shows that the compressive strength of the thermal insulation gypsum of this comparative example is 5.23 MPa and the thermal conductivity is 0.111 W / (m·K), which are recorded in Table 1.

[0148] Comparative Example 4

[0149] This comparative example is basically the same as Example 2, except that only hydrophobic aerogel is used in step 2), and the amount of hydrophobic aerogel added is 10 parts.

[0150] In step 3), 0.2 parts of an air-entraining agent, sodium lauryl sulfate, was further added, and no vacuum operation was performed. The mixture was directly stirred at normal pressure for 5 minutes to obtain slurry B.

[0151] The test shows that the compressive strength of the thermal insulation gypsum of this comparative example is 6.16 MPa and the thermal conductivity is 0.130 W / (m·K), which are recorded in Table 1.

[0152] Table 1

[0153] The above describes exemplary embodiments of the present invention. However, the scope of protection of this application is not limited to the above embodiments. Any modifications, equivalent substitutions, improvements, etc. made by those skilled in the art within the spirit and principles of the present invention should be included in the scope of protection of the present invention.

Claims

1. A method for preparing aerogel-modified gypsum, characterized in that: The preparation method comprises: mixing raw materials and auxiliary materials of aerogel and gypsum under vacuum stirring conditions, and then adding an air entraining agent under normal pressure conditions to mix them evenly to obtain the aerogel modified gypsum.

2. The preparation method according to claim 1, characterized in that: The conditions for vacuum stirring specifically include: stirring at an absolute pressure of less than 1 KPa; stirring time of no more than 5 minutes; stirring temperature of 8°C to 10°C; And / or, the aerogel is added into the raw materials of gypsum.

3. The preparation method according to claim 1, characterized in that: The raw material of the gypsum is selected from plaster of Paris powder; In the aerogel-modified gypsum, the mass ratio of aerogel to gypsum is (0-30):100 and the content of the aerogel is not 0; In the aerogel-modified gypsum, the particle size of the aerogel is 1nm-50nm; The aerogel is selected from hydrophilically modified aerogels and / or hydrophobic aerogels.

4. The preparation method according to claim 3, characterized in that: The aerogel includes hydrophilic modified aerogel and hydrophobic aerogel, wherein the mass ratio of the hydrophilic modified aerogel to the hydrophobic aerogel is 100:(0-100) and the content of the hydrophobic aerogel is not zero.

5. The preparation method according to claim 3, characterized in that: The hydrophilic modified aerogel is a hydrophilic modified aerogel particle; The contact angle between the hydrophilic modified aerogel and water is less than 90°; The contact angle between the hydrophobic aerogel and water is greater than 90°.

6. The preparation method according to claim 1, characterized in that: The auxiliary materials include water and at least one of the following substances: vitrified microspheres, reinforcing agent, dispersant, reinforcing fiber and retarder; And / or, the amount of the auxiliary material added is 0.1 to 200 parts by mass per 100 parts by mass of the gypsum raw material.

7. The preparation method according to claim 6, characterized in that: The water is 100 to 120 parts by mass per 100 parts by mass of the gypsum raw material; and / or, the dispersant is 0.01-5 parts by mass per 100 parts by mass of the gypsum raw material; And / or, the vitrified microspheres are 5 to 40 parts by mass per 100 parts by mass of the gypsum raw material; And / or, the reinforcing fiber is 0.5-5 parts by mass per 100 parts by mass of the gypsum raw material; And / or, the retarder is 0.01-0.5 parts by mass per 100 parts by mass of the gypsum raw material.

8. The preparation method according to claim 6, characterized in that: The reinforcing fibers are selected from inorganic fibers and organic fibers; And / or, the retarder is selected from organic acids and soluble salts thereof, alkaline phosphates, proteins and other retarders.

9. The preparation method according to claim 1, characterized in that: Before the vacuum stirring, the raw materials, auxiliary materials and aerogel of gypsum are premixed to obtain a uniform premix.

10. The preparation method according to claim 1, characterized in that: The mass ratio of the air entraining agent to the gypsum raw materials is 0.1 to 1:100.

Citation Information

Patent Citations

  • Vacuum stirrer

    CN104369269A

  • Aerogel-containing gypsum material and preparation method thereof

    CN106747189A

  • Fiber-enhanced aerogel-polymer composite material and preparation method thereof

    CN107099117A

  • Super-thermal-insulation aerogel foamed concrete and preparation method thereof

    CN107265963A

  • Super-thermal-insulation aerogel foamed concrete and preparation method thereof

    CN107265964A

Cited By

  • Surface hydrophobically modified gypsum-aerogel composite thermal insulation material as well as preparation method and application thereof

    CN119462053A