Modified lithium ion sieve, preparation method and use of modified lithium ion sieve in electrochemical lithium extraction

The modified lithium ion sieve is prepared by alternately stacking MnO2 nanosheets and reduced graphene oxide nanosheets, and combined with electrochemical methods, solves the problems of structural instability and low lithium extraction efficiency of traditional MnO2-based ion sieves, achieving high efficiency and long life. The application of advanced lithium ion screen materials has improved the production efficiency of lithium extraction from salt lakes.

WO2024216574A1PCT designated stage expired Publication Date: 2024-10-24GUANGDONG BRUNP RECYCLING TECH CO LTD +1
View PDF 6 Cites 0 Cited by

Patent Information

Application Number
PCT/CN2023/089440
Authority / Receiving Office
WO · WO
Patent Type
Applications
Current Assignee / Owner
Filing Date
2023-04-20
Publication Date
2024-10-24

AI Technical Summary

Technical Problem

The structure of traditional MnO2-based ion sieves collapses quickly during the lithium extraction process from salt lakes, and their cycle life is not long. Moreover, the specific surface area of ​​a single MnO2-based ion sieve is small, and the lithium extraction efficiency is low, making it difficult to efficiently and selectively enrich lithium resources.

Method used

A modified lithium ion sieve is prepared by using alternately stacked MnO2 nanosheets and reduced graphene oxide nanosheets. The specific surface area and structural stability are increased through hydrothermal reaction and cationic modification, and the selective insertion and extraction of lithium ions is achieved by combining electrochemical methods.

Benefits of technology

The specific surface area and lithium ion insertion sites of the modified lithium ion screen are significantly increased, the service life is extended, the lithium extraction efficiency and production efficiency are improved, and the use cost is reduced.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN2023089440_24102024_PF_FP_ABST
    Figure CN2023089440_24102024_PF_FP_ABST
Patent Text Reader

Abstract

Disclosed in the present disclosure are a modified lithium ion sieve, a preparation method and the use of the modified lithium ion sieve in electrochemical lithium extraction. The modified lithium ion sieve comprises matrix material nanosheets and reduced graphene oxide nanosheets which are alternately stacked, the matrix material nanosheets being MnO2 nanosheets. The modified lithium ion sieve can be applied to salt lake electrochemical lithium extraction. The modified lithium ion sieve in the present disclosure can effectively increase the lithium extraction rate, greatly increases the use value of MnO2-based lithium ion sieves, and fully reduces the use cost, thereby improving production benefit.
Need to check novelty before this filing date? Find Prior Art

Description

Modified lithium ion sieve, preparation method and application in electrochemical lithium extraction Technical Field

[0001] The present disclosure relates to the field of metallurgy technology, and in particular to a modified lithium ion sieve, a preparation method thereof, and an application thereof in electrochemical lithium extraction. Background Art

[0002] Lithium resources are widely used in lithium-ion batteries and other related fields. With the rapid development of the lithium-ion battery industry, the demand for lithium resources in industrial production is increasing at an increasingly faster rate. In recent years, there has even been a situation where lithium raw materials are in short supply.

[0003] Lithium reserves are substantial in some plateau regions. For example, the salt lakes of China's Qinghai-Tibet Plateau are rich in lithium. Therefore, efficient and rapid extraction of lithium from salt lakes has long been a scientific challenge. Salt lakes contain low levels of lithium but high levels of other metals, such as magnesium. Due to the similar properties of magnesium and lithium, selective extraction of lithium from salt lakes is challenging. In the past, methods for extracting lithium from salt lakes included precipitation, calcination leaching, carbonization, nanofiltration membranes, solvent extraction, and adsorption. Adsorption, which uses lithium ion sieves to adsorb lithium ions, is considered a promising method for extracting lithium from salt lakes due to its high adsorption capacity and selectivity. MnO2-based ion sieves exhibit excellent lithium adsorption and industrial benefits, and have therefore been gradually adopted in the field of lithium extraction from salt lakes. However, traditional MnO2-based ion sieves require cyclic acid dissolution during use, resulting in rapid structural collapse and a short cycle life.

[0004] Typically, electrochemical methods can be combined to ensure cycle life without sacrificing the adsorption capacity of MnO2-based ion sieves. However, single MnO2-based ion sieves have a small specific surface area and low lithium extraction efficiency. Therefore, it is necessary to structurally modify MnO2-based ion sieves to efficiently and selectively enrich lithium resources from brine for use in industrial salt lake lithium extraction.

[0005] In view of this, the present disclosure is proposed.

[0006] Summary of the Invention

[0007] The purpose of the present disclosure is to provide a modified lithium ion sieve, a preparation method and its application in electrochemical lithium extraction.

[0008] The present disclosure is achieved as follows:

[0009] In a first aspect, the present disclosure provides a modified lithium ion sieve comprising alternately stacked matrix material nanosheets and reduced graphene oxide nanosheets, wherein the matrix material nanosheets are MnO2 nanosheets.

[0010] In an optional embodiment, the matrix material nanosheets are MnO2 nanosheets with a three-dimensional layered skeleton structure.

[0011] In an optional embodiment, the reduced graphene oxide nanosheets are positively charged modified reduced graphene oxide nanosheets.

[0012] In an alternative embodiment, the positive charge is provided by ammonium and / or ammonium derivatives.

[0013] In an optional embodiment, the mass ratio of the matrix material nanosheets to the reduced graphene oxide nanosheets is (2-6):1.

[0014] In an optional embodiment, the gap between adjacent MnO2 nanosheets and reduced graphene oxide nanosheets is 2 to 6 nm.

[0015] In an optional embodiment, the specific surface area of ​​the modified lithium ion sieve is greater than 119m 2 / g.

[0016] In a second aspect, the present disclosure provides a method for preparing the modified lithium ion sieve described in any one of the aforementioned embodiments, comprising mixing the matrix material nanosheets and the reduced graphene oxide nanosheets in a solution system to obtain a lower layer of flocculent material, which is the modified lithium ion sieve.

[0017] In an optional embodiment, the preparation of the reduced graphene oxide nanosheets comprises mixing graphene oxide, a cationic modifier and a reducing agent and performing a hydrothermal reaction to obtain the reduced graphene oxide nanosheets.

[0018] In an optional embodiment, the cationic modifier is at least one of polydiallyl dimethyl ammonium chloride, polydivinyl propyl dimethyl ammonium chloride, polydimethyl diallyl ammonium chloride, and polyacrylamide.

[0019] In an optional embodiment, the reducing agent is at least one of hydrazine hydrate and sodium borohydride.

[0020] In an optional embodiment, in the hydrothermal reaction step, the initial concentration of graphene oxide is 0.01 to 10 g / L.

[0021] In an optional embodiment, the initial concentration of graphene oxide is 1 to 2.8 g / L.

[0022] In an optional embodiment, in the hydrothermal reaction step, the mass ratio of graphene oxide to the cationic modifier is 1:(0.01-100).

[0023] In an optional embodiment, the mass ratio of graphene oxide to the cationic modifier is 1:(0.5-5).

[0024] In an optional embodiment, in the hydrothermal reaction step, the mass ratio of graphene oxide to reducing agent is 1:(0.01-100).

[0025] In an optional embodiment, the mass ratio of graphene oxide to the reducing agent is 1:(0.1-1).

[0026] In an optional embodiment, the temperature of the hydrothermal reaction step is 30-100° C., and the time is 0.1-10 h.

[0027] In an optional embodiment, the temperature of the hydrothermal reaction step is 70-90° C., and the time is 3-8 hours.

[0028] In an optional embodiment, the mixing in the step of preparing reduced graphene oxide nanosheets is ultrasonic mixing or mechanical stirring.

[0029] In an optional embodiment, the mixing time in the step of preparing reduced graphene oxide nanosheets is 1 to 60 minutes.

[0030] In an optional embodiment, the mixing time in the reduced graphene oxide nanosheet preparation step is 6 to 20 minutes.

[0031] In an optional embodiment, in the reduced graphene oxide nanosheet preparation step, the lower layer of flocculants is separated by centrifugation after mixing, and the rotation speed of the centrifugation step is 6000 to 30000 rpm and the time is 1 to 60 minutes.

[0032] In an optional embodiment, in the step of preparing the reduced graphene oxide nanosheets, the lower layer of flocculants is separated by centrifugation after mixing, and the rotation speed of the centrifugation step is 10,000 to 20,000 rpm and the time is 8 to 20 minutes;

[0033] In an optional embodiment, in the reduced graphene oxide nanosheet preparation step, the separated lower layer flocculants are dried to obtain a dried modified lithium ion sieve, and the drying step is performed at a temperature of 65 to 85° C. for 1 to 18 hours.

[0034] In a third aspect, the present disclosure provides a modified lithium ion sieve electrode, which is obtained by coating a mixture of the modified lithium ion sieve described in any one of the aforementioned embodiments, a conductive agent, and a binder on a current collector and drying the mixture.

[0035] In an optional embodiment, the conductive agent is at least one of acetylene black, conductive carbon black, graphene and carbon nanotubes.

[0036] In an optional embodiment, the binder is at least one of polyvinylidene fluoride, carboxymethyl cellulose and polytetrafluoroethylene.

[0037] In an optional embodiment, the mass ratio of the modified lithium ion sieve, the conductive agent and the binder is 8: (0.5-1.5): (0.8-9).

[0038] In an optional embodiment, the modified lithium ion sieve is dried at a temperature of 50 to 100° C. for a time of 1 to 12 hours.

[0039] In an optional embodiment, a modified lithium ion sieve electrode is placed in a brine chamber, and an inert electrode is placed in a lithium salt chamber as a counter electrode. Then, an external potential is driven to embed lithium ions in the brine chamber into the ion sieve to obtain a modified lithium ion sieve electrode in a lithium-intercalated state.

[0040] In a fourth aspect, the present disclosure provides an application of the modified lithium ion sieve described in any one of the aforementioned embodiments in extracting lithium elements.

[0041] In a fifth aspect, the present disclosure provides a device for electrochemically extracting lithium from a salt lake using the modified lithium ion sieve electrode according to any one of the aforementioned embodiments, comprising:

[0042] Electrodes, including a modified lithium ion sieve electrode as a cathode electrode and a modified lithium ion sieve electrode in a lithium-intercalated state as an anode electrode;

[0043] A lithium salt chamber, wherein the anode electrode is disposed in the lithium salt chamber;

[0044] A brine chamber, wherein the cathode electrode is disposed in the brine chamber;

[0045] Anion membrane: used to separate the lithium salt chamber and the brine chamber.

[0046] In a sixth aspect, the present disclosure provides a method for electrochemically extracting lithium from a salt lake using the device described in any one of the aforementioned embodiments, wherein an external potential is applied between the cathode electrode and the anode electrode to drive the Li + The lithium-ion sieve is embedded in the ion sieve to form a lithium-ion sieve, and the lithium-ion sieve embedded in the lithium salt chamber is formed. + Take it out to the lithium salt chamber to obtain lithium salt.

[0047] The modified lithium ion sieve disclosed in the present invention is composed of alternating stacks of MnO2 nanosheets and graphene, and has an increased specific surface area, more lithium embedding sites and a stable skeleton structure, which effectively improves the specific surface area compared to the unmodified lithium ion sieve.

[0048] Electrochemical lithium extraction uses an external electric field to achieve the embedding and extraction of lithium ions in brine into the ion sieve, without involving acid dissolution and lithium removal, so the ion sieve has a long life. Combined with electrochemical devices for lithium extraction, the present disclosure can effectively increase the lithium extraction rate, greatly improve the use value of MnO2-based lithium ion sieves and fully reduce the cost of use, thereby improving production efficiency. BRIEF DESCRIPTION OF THE DRAWINGS

[0049] In order to more clearly illustrate the technical solutions of the embodiments of the present disclosure, the following briefly introduces the drawings required for use in the embodiments. It should be understood that the following drawings only illustrate certain embodiments of the present disclosure and therefore should not be regarded as limiting the scope. For ordinary technicians in this field, other relevant drawings can be obtained based on these drawings without creative work.

[0050] FIG1 is a schematic diagram of an electrochemical lithium extraction device according to the present disclosure;

[0051] FIG2 is a SEM image of the modified lithium ion sieve synthesized in Example 1;

[0052] FIG3 is a SEM image of the lithium ion sieve synthesized in Comparative Example 1. DETAILED DESCRIPTION

[0053] To make the purpose, technical solutions, and advantages of the embodiments of the present disclosure more clear, the technical solutions in the embodiments of the present disclosure are described clearly and completely below. Where specific conditions are not specified in the embodiments, conventional conditions or conditions recommended by the manufacturer were followed. Reagents or instruments used where the manufacturer is not specified are conventional products that can be purchased commercially.

[0054] This embodiment provides a modified lithium ion sieve, comprising alternately stacked matrix material nanosheets and reduced graphene oxide nanosheets, wherein the matrix material nanosheets are MnO2 nanosheets.

[0055] The modified lithium ion sieve is composed of alternating stacks of MnO2 nanosheets and graphene, and has a larger specific surface area and more lithium embedding sites. The specific surface area is increased by more than 40% compared with the unmodified lithium ion sieve; the stable skeleton structure is conducive to extending the service life of the modified lithium ion sieve.

[0056] In some optional embodiments, the matrix material nanosheets are MnO2 nanosheets with a three-dimensional layered skeleton structure. For reference, MnO2 nanosheets disclosed in the prior art can be selected, for example, the three-dimensional layered skeleton structure MnO2 nanosheets disclosed in patent CN115594223A can be selected (unless otherwise specified in the following embodiments, the preparation method of MnO2 nanosheets shall refer to patent CN115594223A), which has a large specific surface area, and after the introduction of reduced graphene oxide nanosheets, its specific surface area can be further increased.

[0057] In some optional embodiments, the mass ratio of the matrix material nanosheets to the reduced graphene oxide nanosheets is 2 to 6:1; in some optional embodiments, the mass ratio of the matrix material nanosheets to the reduced graphene oxide nanosheets is 3 to 4:1. If the reduced graphene oxide nanosheet content is too high, the proportion of the matrix material nanosheets will be reduced, thereby reducing the adsorption capacity of lithium ions. If the reduced graphene oxide nanosheet content is too low, the improvement effect on the lithium ion capacity will be weak, resulting in an insignificant effect on the improvement of the lithium ion capacity. Therefore, the mass of the reduced graphene oxide nanosheets needs to be appropriately set.

[0058] In some optional embodiments, the gap between adjacent MnO2 nanosheets and reduced graphene oxide nanosheets is 2 to 6 nm, specifically, it can be 2 nm, 3 nm, 4 nm, 5 nm, 6 nm or any value between 2 and 6 nm. If the gap is too small, the space for accommodating lithium is reduced, which will reduce the lithium ion capacity; if the gap is too large, it is easy to cause the stability of the structure to decrease, thereby causing the collapse of the structure.

[0059] In some optional embodiments, the specific surface area of ​​the modified lithium ion sieve is greater than 119m 2 / g.

[0060] Another embodiment of the present disclosure provides a method for preparing the modified lithium ion sieve described in any of the aforementioned embodiments, comprising mixing the matrix material nanosheets and the reduced graphene oxide nanosheets in a solution system to obtain a lower layer of flocculent material, which is the modified lithium ion sieve.

[0061] In some optional embodiments, the preparation of the reduced graphene oxide nanosheets comprises mixing graphene oxide, a cationic modifier and a reducing agent and performing a hydrothermal reaction to obtain the reduced graphene oxide nanosheets.

[0062] It is difficult to stack reduced graphene oxide nanosheets directly with MnO2 nanosheets. The applicant has found that the three-dimensional layered skeleton structure of MnO2 nanosheets disclosed in patent CN115594223A carries a negative charge. Therefore, this embodiment uses a cationic modifier to modify the surface of graphene oxide so that the surface of graphene oxide carries a positive charge, thereby allowing the positive and negative charges between the graphene nanosheets and the MnO2 nanosheets to interact, thereby improving the conductivity and stability of the structure. Preferably, the positive charge is provided by ammonium ions and / or ammonium derivatives, and the positive charge density thereof is relatively high.

[0063] In addition, the surface of graphene oxide has more oxygen-containing functional groups, which makes its properties more active. Using a reducing agent to reduce graphene oxide is also beneficial to improving the stability of the modified lithium ion sieve structure.

[0064] In some embodiments, the cationic modifier is at least one of polydiallyl dimethyl ammonium chloride (PDDA), polydivinyl propyl dimethyl ammonium chloride (PDADMAC), polydimethyl diallyl ammonium chloride (PDM), and polyacrylamide (PAM); preferably, the cationic modifier is polydiallyl dimethyl ammonium chloride.

[0065] In some embodiments, the reducing agent is at least one of hydrazine hydrate and sodium borohydride, which have relatively strong reducing properties; preferably, the reducing agent is hydrazine hydrate.

[0066] In some embodiments, in the hydrothermal reaction step, the initial concentration of graphene oxide is 0.01 to 10 g / L; in some optional embodiments, the initial concentration of graphene oxide is 1 to 2.8 g / L; since the generated reduced graphene oxide has a positive charge on its surface, a too high concentration is not conducive to the uniform distribution of the positively charged modified reduced graphene oxide nanosheets in the solution, and a too low concentration is not conducive to improving production efficiency. Therefore, it is necessary to reasonably set the initial concentration of graphene oxide.

[0067] In some embodiments, in the hydrothermal reaction step, the mass ratio of graphene oxide and the cationic modifier is 1:(0.01~100), specifically, it can be 1:0.01, 1:0.1, 1:1, 1:10 or 1:100; preferably, the mass ratio of graphene oxide and the cationic modifier is 1:0.5-5, for example, it can be 1:0.5, 1:1, 1:1.5, 1:2, 1:2.5, 1:3, 1:3.5, 1:4, 1:4.5 or 1:5, so that the number of positive charges on the graphene oxide and the negative charges on the MnO2 nanosheets matches.

[0068] In some embodiments, in the hydrothermal reaction step, the mass ratio of graphene oxide to the reducing agent is 1: (0.01-100), specifically, it can be 1:0.01, 1:0.1, 1:1, 1:10 or 1:100; preferably, the mass ratio of graphene oxide to the reducing agent is 1: (0.1-1), for example, it can be 1:0.1, 1:0.2, 1:0.3, 1:0.4, 1:0.5, 1:0.6, 1:0.7, 1:0.8, 1:0.9 or 1:1, so that the amount of reducing agent is sufficient to react with the oxygen-containing functional groups on the graphene oxide.

[0069] In some embodiments, the temperature of the hydrothermal reaction step is 30-100°C, and the time is 0.1-10 h; in some optional embodiments, the temperature of the hydrothermal reaction step is 70-90°C, for example, 70°C, 75°C, 80°C, 85°C and 90°C, and the time is 3-8 h, for example, 3 h, 4 h, 5 h, 6 h, 7 h and 8 h.

[0070] In some optional embodiments, the mixing step is ultrasonic mixing or mechanical stirring, preferably ultrasonic mixing;

[0071] In some optional embodiments, the mixing step lasts for 1 to 60 minutes, preferably, the reagent mixing time is 6 to 20 minutes;

[0072] In some optional embodiments, the lower flocculent layer is separated by centrifugation, and the speed of the centrifugation step is 6000-30000 rpm, and the time is 1-60 minutes; in some optional embodiments, the speed is 10000-20000 rpm, and the time is 8-20 minutes, until the mass of the solid phase no longer increases or almost no longer increases;

[0073] In some optional embodiments, after the mixing step, the separated lower layer flocculants are dried to obtain a dried modified lithium ion sieve. The drying temperature is 65 to 85° C. Too high a temperature may damage the product structure, and too low a temperature may result in too slow drying efficiency. The drying time is 1 to 18 hours, and the drying is stopped when the weight hardly changes.

[0074] Another embodiment of the present disclosure provides a modified lithium ion sieve electrode, which is obtained by coating a mixture of the modified lithium ion sieve, a conductive agent, and a binder on a current collector and drying the mixture.

[0075] In some optional embodiments, the conductive agent is at least one of acetylene black, conductive carbon black, graphene and carbon nanotubes; preferably, the conductive agent is conductive carbon black or carbon nanotubes.

[0076] In some optional embodiments, the binder is at least one of polyvinylidene fluoride (PVDF), carboxymethyl cellulose (CMC) and polytetrafluoroethylene (PTFE); preferably, the binder is polyvinylidene fluoride.

[0077] In some optional embodiments, the mass ratio of the modified lithium ion sieve, conductive agent, and binder is 8: (0.5-1.5): (0.8-9); preferably, the ratio of the modified lithium ion sieve, conductive agent, and binder is 8:1:1. The conductive agent can improve the conductivity of the electrode, but too much conductive agent will reduce the proportion of the modified lithium ion sieve, thereby reducing the lithium extraction effect; too little binder will reduce the bonding effect and prevent the modified lithium ion sieve from effectively agglomerating. Similarly, too much binder will also reduce the proportion of the modified lithium ion sieve, thereby reducing the lithium extraction effect.

[0078] In some optional embodiments, the modified lithium ion sieve is dried at a temperature of 50 to 100° C. for 1 to 12 hours. Too high a temperature may damage the product structure, and too low a temperature may result in too slow drying efficiency.

[0079] In some optional embodiments, when the device is operated for the first time, a modified lithium ion sieve electrode can be placed in the brine chamber, and an inert electrode can be placed in the lithium salt chamber as a counter electrode. Then, an external potential is used to drive the lithium ions in the brine chamber to embed into the ion sieve to obtain a modified lithium ion sieve electrode in a lithium-intercalated state, wherein the external potential can be between 0.1 and 1.5 V. Preferably, the external potential should be between 0.6 and 1 V. The external potential is kept constant until the current is lower than 0.1 mA and the reaction is stopped.

[0080] The inert electrode is one of a graphite electrode, a platinum metal sheet, a carbon fiber, etc. Preferably, the inert electrode is a graphite electrode; the inert electrode and the working electrode should have approximately the same area, maintain the same position, and face each other.

[0081] Another embodiment of the present disclosure provides a use of the modified lithium ion sieve described in any one of the aforementioned embodiments in extracting lithium elements.

[0082] Another embodiment of the present disclosure provides a device for electrochemically extracting lithium from a salt lake, as shown in FIG1 , comprising:

[0083] Electrodes, including a modified lithium ion sieve electrode as a cathode electrode and a modified lithium ion sieve electrode in a lithium-intercalated state as an anode electrode;

[0084] A lithium salt chamber, wherein the anode electrode is disposed in the lithium salt chamber;

[0085] A brine chamber, wherein the cathode electrode is disposed in the brine chamber;

[0086] Anion membrane: used to separate the lithium salt chamber and the brine chamber.

[0087] Electrochemical lithium extraction uses an external electric field to achieve the embedding and extraction of lithium ions in brine into the ion sieve, without involving acid dissolution and lithium removal, so the ion sieve has a long life. Combining the electrochemical device in this embodiment for lithium extraction can increase the lithium extraction rate by more than 80%, greatly improving the use value of the MnO2-based lithium ion sieve and fully reducing the cost of use, thereby improving production efficiency.

[0088] Another embodiment of the present disclosure provides a method for electrochemically extracting lithium from a salt lake using the device described in any one of the aforementioned embodiments, wherein an external potential is applied between the cathode electrode and the anode electrode to drive the Li + The lithium-ion sieve is embedded in the ion sieve to form a lithium-ion sieve, and the lithium-ion sieve embedded in the lithium salt chamber is formed. + The reaction is then carried out to the lithium salt chamber to obtain lithium salt. The external potential can be between 0.1 and 1.5 V, preferably between 0.6 and 1 V, and the external potential is kept constant until the current is less than 0.1 mA, which stops the reaction.

[0089] The features and performance of the present disclosure are further described in detail below with reference to the embodiments.

[0090] Example 1:

[0091] This embodiment provides a method for electrochemically extracting lithium from a salt lake, comprising the following steps:

[0092] S1. Take 5 g of graphene oxide (GO) material and dissolve it in 2 L of deionized water. Then add 2.5 g of PDDA modifier and 0.5 g of hydrazine hydrate and mix them at 80 °C for 6 h to obtain a positively charged modified rGO nanosheet solution.

[0093] S2, taking 15 g of MnO2 nanosheet material and mixing it with the positively charged rGO solution in step S2, and then mechanically stirring it at 1000 r / min for 20 min;

[0094] S3, centrifuging the product obtained in step 2 at 10000 r / min for 8 min, collecting the solid product at the bottom, and drying it at 65 ° C for 8 h to obtain a positively charged rGO-MnO2 modified lithium ion sieve;

[0095] S4, 16g of modified lithium ion sieve in step S3, 2g of conductive carbon black and 2g of PVDF were dissolved in 10ml of NMP solvent and mixed evenly to form a slurry, and then applied to 100cm 2 Electrode 1 was prepared on the current collector and dried at 70°C for 6 h.

[0096] S5, place the prepared electrode 1 as the cathode in the brine chamber, 100cm 2 The inert electrode is placed in the lithium salt chamber as a counter electrode, and an external potential of 0.6 V is driven to cause lithium ions in the brine chamber to be embedded in the ion sieve to obtain a lithium-intercalated electrode 2;

[0097] S6, the electrode 1 obtained in step S4 is placed in the brine chamber as a cathode, the electrode 2 obtained in step S5 is placed in the lithium salt chamber as an anode, and the Li in the brine chamber is driven by a potential of 0.6 V. + The lithium salt chamber is embedded in the ion sieve to form a lithium-ion sieve. + Take it out to the lithium salt chamber to obtain lithium salt.

[0098] Example 2:

[0099] This embodiment provides a method for electrochemically extracting lithium from a salt lake, comprising the following steps:

[0100] S1. Take 2.8g of graphene oxide (GO) material and dissolve it in 1L of deionized water. Then add 1.4g of PDM modifier and 0.56g of sodium borohydride and mix them at 70℃ for 3h to obtain a positively charged rGO nanosheet solution.

[0101] S2, taking 9 g of MnO2 nanosheet material and mixing it with the positively charged rGO solution in step S1, and then ultrasonically treating it for 12 min;

[0102] S3, centrifuging the product obtained in step S2 at 12000 r / min for 20 min, collecting the solid product at the bottom, and drying it at 80°C for 7 h to obtain a positively charged rGO-MnO2 modified lithium ion sieve;

[0103] S4, 8g of modified lithium ion sieve in step S3, 1g of carbon nanotubes and 1g of PVDF were dissolved in 5ml of NMP solvent and mixed evenly to form a slurry, and then applied to 100cm 2 Electrode 1 was prepared on a graphite plate and dried at 65°C for 9 h.

[0104] S5, place the prepared electrode 1 as the cathode in the brine chamber, 100cm 2 The graphite plate is placed in the lithium salt chamber as the counter electrode, and an external potential of 0.8 V is applied to drive the lithium ions in the brine chamber to embed into the ion sieve to obtain a lithium-intercalated electrode 2;

[0105] S6, the electrode 1 obtained in step S4 is placed in the brine chamber as a cathode, the electrode 2 obtained in step S5 is placed in the lithium salt chamber as an anode, and the Li in the brine chamber is driven by a potential of 0.8 V. + The lithium salt chamber is embedded in the ion sieve to form a lithium-ion sieve. + Take it out to the lithium salt chamber to obtain lithium salt.

[0106] Example 3:

[0107] This embodiment provides a method for electrochemically extracting lithium from a salt lake, comprising the following steps:

[0108] S1. Dissolve 2 g of graphene oxide (GO) material in 1 L of deionized water, add 2 g of PAM modifier and 2 g of hydrazine hydrate, mix and react at 90 °C for 8 h to obtain a positively charged modified rGO nanosheet solution.

[0109] S2, taking 7 g of MnO2 nanosheet material and mixing it with the positively charged rGO solution in step S1, and then mechanically stirring it at 1000 r / min for 16 min;

[0110] S3, centrifuging the product obtained in step S2 at 16000 r / min for 12 min, collecting the solid product at the bottom, and drying it at 70°C for 6 h to obtain a positively charged rGO-MnO2 modified lithium ion sieve;

[0111] S4, 6.4g of modified lithium ion sieve in step S3, 0.8g of conductive carbon black and 0.8g of PVDF were dissolved in 5ml of NMP solvent and mixed evenly to form a slurry, and then applied to 100cm 2 Electrode 1 was prepared on the current collector and dried at 70°C for 6 h.

[0112] S5, place the prepared electrode 1 as the cathode in the brine chamber, 100cm 2 The inert electrode is placed in the lithium salt chamber as a counter electrode, and an external potential of 0.7 V is driven to cause lithium ions in the brine chamber to be embedded in the ion sieve to obtain a lithium-intercalated electrode 2;

[0113] S6, the electrode 1 obtained in step S4 is placed in the brine chamber as a cathode, the electrode 2 obtained in step S5 is placed in the lithium salt chamber as an anode, and the Li in the brine chamber is driven by a potential of 0.7 V. + The lithium salt chamber is embedded in the ion sieve to form a lithium-ion sieve. + Take it out to the lithium salt chamber to obtain lithium salt.

[0114] Example 4:

[0115] This embodiment provides a method for electrochemically extracting lithium from a salt lake, comprising the following steps:

[0116] S1. Take 5 g of graphene oxide (GO) material and dissolve it in 5 L of deionized water. Then add 25 g of PDADMAC modifier and 2.5 g of sodium borohydride and mix them at 75 °C for 6 h to obtain a positively charged modified rGO nanosheet solution.

[0117] S2, taking 20 g of MnO2 nanosheet material and mixing it with the positively charged rGO solution in step S1, and then ultrasonically treating it for 20 min;

[0118] S3, centrifuging the product obtained in step S2 at 13000 r / min for 16 min, collecting the solid product at the bottom, and drying it at 85°C for 6 h to obtain a positively charged rGO-MnO2 modified lithium ion sieve;

[0119] S4, 20g of modified lithium ion sieve in step S3, 2.5g of carbon nanotubes and 2.5g of PVDF were dissolved in 12ml of NMP solvent and mixed evenly to form a slurry, and then applied to 100cm 2 Electrode 1 was prepared on the current collector and dried at 65°C for 8 h.

[0120] S5, place the prepared electrode 1 as the cathode in the brine chamber, 100cm 2 The inert electrode is placed in the lithium salt chamber as a counter electrode, and an external potential of 0.6 V is driven to cause lithium ions in the brine chamber to be embedded in the ion sieve to obtain a lithium-intercalated electrode 2;

[0121] S6, the electrode 1 obtained in step S4 is placed in the brine chamber as a cathode, the electrode 2 obtained in step S5 is placed in the lithium salt chamber as an anode, and the Li in the brine chamber is driven by a potential of 0.6 V. + The lithium salt chamber is embedded in the ion sieve to form a lithium-ion sieve. + Take it out to the lithium salt chamber to obtain lithium salt.

[0122] Example 5:

[0123] This embodiment provides a method for electrochemically extracting lithium from a salt lake, comprising the following steps:

[0124] S1. Take 3 g of graphene oxide (GO) material and dissolve it in 2 L of deionized water. Then add 9 g of PDDA modifier and 2.4 g of hydrazine hydrate and mix them at 85 °C for 5 h to obtain a positively charged modified rGO nanosheet solution.

[0125] S2, taking 10.8 g of MnO2 nanosheet material and mixing it with the positively charged rGO solution in step S1, and then mechanically stirring it at 800 rpm for 6 min;

[0126] S3, centrifuging the product obtained in step S2 at 20000 r / min for 10 min, collecting the solid product at the bottom, and drying it at 70°C for 9 h to obtain a positively charged rGO-MnO2 modified lithium ion sieve;

[0127] S4, 12g of modified lithium ion sieve in step S3, 1.5g of carbon nanotubes and 1.5g of PVDF were dissolved in 6ml of NMP solvent and mixed evenly to form a slurry, and then coated on a 100cm 2 Electrode 1 was prepared on the current collector and dried at 80°C for 7 h.

[0128] S5, place the prepared electrode 1 as the cathode in the brine chamber, 100cm 2 The inert electrode is placed in the lithium salt chamber as a counter electrode, and an external potential of 0.8 V is driven to cause lithium ions in the brine chamber to be embedded in the ion sieve to obtain a lithium-intercalated electrode 2;

[0129] S6, the electrode 1 obtained in step S4 is placed in the brine chamber as a cathode, the electrode obtained in step S5 is placed in the lithium salt chamber as an anode, and the Li in the brine chamber is driven by a potential of 0.8 V. + The lithium salt chamber is embedded in the ion sieve to form a lithium-ion sieve. + Take it out to the lithium salt chamber to obtain lithium salt.

[0130] Example 6

[0131] The difference from Example 1 is that in step S2, mechanical stirring is replaced by ultrasonic treatment.

[0132] Example 7:

[0133] The difference from Example 1 is that the amount of PDDA added in step S1 is 50 g.

[0134] Example 8:

[0135] The difference from Example 1 is that the amount of hydrazine hydrate added in step S1 is 10 g.

[0136] Comparative Example 1:

[0137] The difference from Example 1 is that S1-S3 are not performed, that is, the MnO2 nanosheets are directly prepared as lithium ion sieves and lithium is extracted from salt lake brine.

[0138] Comparative Example 2:

[0139] The difference from Example 1 is that in step S1, no positive charge modifier is added, that is, only GO and the reducing agent are mixed to obtain the rGO solution and prepare the lithium ion sieve.

[0140] Comparative Example 3:

[0141] The difference from Example 1 is that no reducing agent is added in step S1, that is, only GO and the positive charge modifier are mixed to obtain an rGO solution and prepare a lithium ion sieve.

[0142] Comparative Example 4:

[0143] The difference from Example 1 is that in step S1, 5 g of graphene oxide (GO) material is dissolved in 0.5 L of deionized water.

[0144] Comparative Example 5:

[0145] The difference from Example 1 is that the temperature of the hydrothermal reaction in step S1 is 120°C.

[0146] Comparative Example 6:

[0147] The difference from Example 1 is that the amount of MnO2 nanosheets added in step S2 is 5 g.

[0148] Comparative Example 7:

[0149] The difference from Example 1 is that the amount of MnO2 nanosheets added in step S2 is 40 g.

[0150] Comparative Example 8:

[0151] The difference from Example 1 is that the preparation method of MnO2 nanosheets in step S2 is referred to CN 111001404A, specifically comprising the following steps:

[0152] S1. Manganese sulfate monohydrate (MnSO4·H2O) was completely dissolved in a pure aqueous solution, followed by the addition of a 40 wt.% sodium permanganate (NaMnO4) solution at a molar ratio of 3:2. The mixture was ultrasonically shaken for 5 minutes, allowed to stand at 25°C for 24 hours, filtered, washed until the filtrate was transparent, and dried to obtain amorphous manganese oxide.

[0153] S2. The amorphous manganese oxide dried in step S1 was dispersed in a pure aqueous solution, and then reacted at 80 ° C for 24 h, filtered, washed, and dried to obtain γ-MnO2;

[0154] S3. The γ-MnO2 in step S2 was calcined at 350°C for 3h to obtain a β-MnO2 nanosheet catalyst.

[0155] The modified lithium ion sieves prepared in each embodiment and comparative example were characterized by SEM, wherein the SEM spectra of the modified lithium ion sieves obtained in embodiment 1 and comparative example 1 are shown in Figures 2 and 3, respectively. It can be seen from Figures 2 and 3 that without using positive charge and reducing agent to modify graphene oxide, the modified ion sieves obtained have more structural collapse and poor stability. The effects of the salt lake electrochemical lithium extraction method in the embodiments and comparative examples were evaluated, wherein the main elements and concentrations in the salt lake brine used are shown in Table 1, the measured specific surface area of ​​the modified lithium ion sieve material is shown in Table 2, and the Li + The extraction rate and lithium concentration in the remaining brine are shown in Table 3, and the types and contents of impurities in the lithium salt chamber are shown in Table 4.

[0156] Table 1 Concentrations of main elements in salt lake brine

[0157] Table 2 Specific surface area of ​​modified lithium ion sieve materials prepared in each embodiment

[0158] Table 3 Single lithium extraction rate and residual brine lithium concentration of each embodiment and comparative example

[0159] The foregoing description is merely a preferred embodiment of the present disclosure and is not intended to limit the present disclosure. Those skilled in the art will readily appreciate that various modifications and variations are possible. Any modifications, equivalent substitutions, or improvements made within the spirit and principles of the present disclosure shall be included within the scope of protection of the present disclosure. Industrial Applicability

[0160] The modified lithium ion sieve disclosed in the present invention is composed of alternating stacks of MnO2 nanosheets and graphene, and has an increased specific surface area, more lithium embedding sites, and a stable skeleton structure, which effectively improves the specific surface area of ​​the unmodified lithium ion sieve. This material is applied to an electrochemical lithium extraction device, and the lithium ions in the brine are embedded in and extracted from the ion sieve by utilizing an external electric field, without involving acid dissolution and lithium removal. The ion sieve has a long life and can effectively increase the lithium extraction rate, greatly improving the use value of the MnO2-based lithium ion sieve and fully reducing the cost of use, thereby improving production efficiency and having great application prospects.

Claims

1. A modified lithium ion sieve, It is characterized in that The invention comprises alternately stacked matrix material nanosheets and reduced graphene oxide nanosheets, wherein the matrix material nanosheets are MnO 2 Nanosheets.

2. The modified lithium ion sieve according to claim 1, It is characterized in that The matrix material nanosheet is a MnO nanosheet with a three-dimensional layered skeleton structure. 2 Nanosheets.

3. The modified lithium ion sieve according to claim 1 or 2, It is characterized in that The reduced graphene oxide nanosheets are reduced graphene oxide nanosheets modified with positive charges.

4. The modified lithium ion sieve according to claim 3, It is characterized in that The positive charge is provided by ammonium and / or ammonium derivatives.

5. The modified lithium ion sieve according to any one of claims 1 to 4, It is characterized in that The mass ratio of the matrix material nanosheets to the reduced graphene oxide nanosheets is (2-6):

1.

6. The modified lithium ion sieve according to any one of claims 1 to 5, It is characterized in that Adjacent to the MnO 2 The gap between the nanosheets and the reduced graphene oxide nanosheets is 2 to 6 nm.

7. The modified lithium ion sieve according to any one of claims 1 to 6, It is characterized in that The specific surface area of ​​the modified lithium ion sieve is greater than 119 m 2 / g.

8. A method for preparing the modified lithium ion sieve according to any one of claims 1 to 7, It is characterized in that The modified lithium ion sieve is obtained by mixing the matrix material nanosheets and the reduced graphene oxide nanosheets in a solution system to obtain a lower layer of flocculants.

9. The method for preparing the modified lithium ion sieve according to claim 8, It is characterized in that The preparation of the reduced graphene oxide nanosheets comprises mixing graphene oxide, a cationic modifier and a reducing agent and performing a hydrothermal reaction to obtain the reduced graphene oxide nanosheets.

10. The method for preparing the modified lithium ion sieve according to claim 9, It is characterized in that The cationic modifier is at least one of polydiallyl dimethyl ammonium chloride, polydiethylene propyl dimethyl ammonium chloride, polydimethyl diallyl ammonium chloride and polyacrylamide.

11. A method for preparing the modified lithium ion sieve according to claim 9 or 10, It is characterized in that The reducing agent is at least one of hydrazine hydrate and sodium borohydride.

12. A method for preparing a modified lithium ion sieve according to any one of claims 9 to 11, It is characterized in that In the hydrothermal reaction step, the initial concentration of graphene oxide is 0.01 to 10 g / L.

13. A method for preparing a modified lithium ion sieve according to any one of claims 9 to 12, It is characterized in that The initial concentration of graphene oxide is 1 to 2.8 g / L.

14. A method for preparing a modified lithium ion sieve according to any one of claims 9 to 13, It is characterized in that In the hydrothermal reaction step, the mass ratio of graphene oxide to the cationic modifier is 1:(0.01-100).

15. A method for preparing a modified lithium ion sieve according to any one of claims 9 to 14, It is characterized in that The mass ratio of graphene oxide to the cationic modifier is 1:(0.5-5).

16. A method for preparing a modified lithium ion sieve according to any one of claims 9 to 15, It is characterized in that In the hydrothermal reaction step, the mass ratio of graphene oxide to reducing agent is 1:(0.01-100).

17. A method for preparing a modified lithium ion sieve according to any one of claims 9 to 16, It is characterized in that The mass ratio of graphene oxide to the reducing agent is 1:(0.1~1).

18. A method for preparing a modified lithium ion sieve according to any one of claims 9 to 17, It is characterized in that The temperature of the hydrothermal reaction step is 30-100° C. and the time is 0.1-10 h.

19. A method for preparing a modified lithium ion sieve according to any one of claims 9 to 18, It is characterized in that The temperature of the hydrothermal reaction step is 70-90° C. and the time is 3-8 hours.

20. A method for preparing a modified lithium ion sieve according to any one of claims 9 to 19, It is characterized in that The mixing in the step of preparing reduced graphene oxide nanosheets is ultrasonic mixing or mechanical stirring.

21. A method for preparing a modified lithium ion sieve according to any one of claims 9 to 20, It is characterized in that The mixing time in the step of preparing reduced graphene oxide nanosheets is 1 to 60 minutes.

22. A method for preparing a modified lithium ion sieve according to any one of claims 9 to 21, It is characterized in that The mixing time in the step of preparing reduced graphene oxide nanosheets is 6 to 20 minutes.

23. A method for preparing a modified lithium ion sieve according to any one of claims 9 to 22, It is characterized in that In the step of preparing the reduced graphene oxide nanosheets, the lower layer of flocculants is separated by centrifugation after mixing, and the rotation speed of the centrifugation step is 6000 to 30000 rpm and the time is 1 to 60 minutes.

24. A method for preparing a modified lithium ion sieve according to any one of claims 9 to 23, It is characterized in that In the step of preparing the reduced graphene oxide nanosheets, the lower layer of flocculants is separated by centrifugation after mixing, and the rotation speed of the centrifugation step is 10,000 to 20,000 rpm and the time is 8 to 20 minutes.

25. A method for preparing a modified lithium ion sieve according to any one of claims 9 to 24, It is characterized in that In the step of preparing the reduced graphene oxide nanosheets, the separated lower layer flocculants are dried to obtain a dried modified lithium ion sieve, and the drying step temperature is 65 to 85° C. and the time is 1 to 18 hours.

26. A modified lithium ion sieve electrode, It is characterized in that The method is obtained by coating a mixture of the modified lithium ion sieve according to any one of claims 1 to 25, a conductive agent and a binder on a current collector and drying the mixture.

27. The modified lithium ion sieve electrode according to claim 26, It is characterized in that The conductive agent is at least one of acetylene black, conductive carbon black, graphene and carbon nanotubes.

28. The modified lithium ion sieve electrode according to claim 26 or 27, It is characterized in that The binder is at least one of polyvinylidene fluoride, carboxymethyl cellulose and polytetrafluoroethylene.

29. The modified lithium ion sieve electrode according to any one of claims 26 to 28, It is characterized in that The mass ratio of the modified lithium ion sieve, the conductive agent and the binder is 8: (0.5-1.5): (0.8-9).

30. The modified lithium ion sieve electrode according to any one of claims 26 to 29, It is characterized in that The modified lithium ion sieve is dried at a temperature of 50 to 100° C. for a time of 1 to 12 hours.

31. The modified lithium ion sieve electrode according to any one of claims 26 to 30, It is characterized in that The modified lithium ion sieve electrode is placed in a brine chamber, and an inert electrode is placed in a lithium salt chamber as a counter electrode. Then, the lithium ions in the brine chamber are driven to embed into the ion sieve by an external potential to obtain a modified lithium ion sieve electrode in a lithium-intercalated state.

32. Use of the modified lithium ion sieve according to any one of claims 1 to 25 or the modified lithium ion sieve electrode according to any one of claims 26 to 31 in extracting lithium.

33. A device for electrochemical lithium extraction from salt lakes with the modified lithium ion sieve electrode according to any one of claims 26 to 31, It is characterized in that include: Electrodes, including a modified lithium ion sieve electrode as a cathode electrode and a modified lithium ion sieve electrode in a lithium-intercalated state as an anode electrode; A lithium salt chamber, wherein the anode electrode is disposed in the lithium salt chamber; A brine chamber, wherein the cathode electrode is arranged in the brine chamber; Anion membrane: used to separate the lithium salt chamber and the brine chamber.

34. A method for electrochemically extracting lithium from salt lakes using the device of claim 33, It is characterized in that An external potential is applied between the cathode electrode and the anode electrode to drive the Li + The lithium-ion sieve is embedded in the ion sieve to form a lithium-ion sieve, and the Li-ion sieve of the lithium-ion sieve in the lithium salt chamber is embedded in the ion sieve. + Take it out to the lithium salt chamber to obtain lithium salt.

Citation Information

Patent Citations

  • Method and device for separating magnesium and lithium and enriching lithium from salt lake brine

    CN102382984A

  • Preparation method for modified graphene and application of modified graphene to positive materials for lithium batteries

    CN104716322A

  • Polyaniline nanotube modified ultrathin graphene membrane electrode and preparation method thereof

    CN106024427A

  • Preparation method of carbon / manganese dioxide composite material for lithium battery

    CN108199033A

  • Inorganic nano sheet-enabled lithium-exchanging surface-mediated cells

    US20130216894A1