Sealing material and sealing structure

The sealing material with specific viscosity and foamability addresses adhesion issues in high-temperature devices by suppressing the Leidenfrost phenomenon and reducing drying shrinkage, ensuring effective sealing and durability.

WO2024219196A1PCT designated stage expired Publication Date: 2024-10-24AGC INC
View PDF 2 Cites 0 Cited by

Patent Information

Application Number
PCT/JP2024/013289
Authority / Receiving Office
WO · WO
Patent Type
Applications
Current Assignee / Owner
Priority Date
2023-04-17
Filing Date
2024-03-29
Publication Date
2024-10-24

AI Technical Summary

Technical Problem

Conventional sealing materials fail to achieve sufficient adhesion to high-temperature surfaces, leading to poor sealing performance in high-temperature devices, particularly due to the Leidenfrost phenomenon and drying shrinkage issues.

Method used

A sealing material containing an inorganic component and moisture, with a viscosity of 10,000 mPa·s to 350,000 mPa·s at 25°C and high-temperature foamability, which suppresses the Leidenfrost phenomenon and enhances adhesion by forming a gel structure that traps water, reducing foam formation and drying shrinkage.

Benefits of technology

The sealing material achieves improved adhesion and reduced crack formation on high-temperature surfaces, maintaining sealing effectiveness and preventing deterioration in high-temperature environments.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure JPOXMLDOC01-APPB-T000001
    Figure JPOXMLDOC01-APPB-T000001
  • Figure JPOXMLDOC01-APPB-T000002
    Figure JPOXMLDOC01-APPB-T000002
  • Figure JPOXMLDOC01-APPB-T000003
    Figure JPOXMLDOC01-APPB-T000003
Patent Text Reader

Abstract

Provided is a sealing material containing an inorganic component and moisture, the sealing material having a viscosity of 10,000 mPa·s to 350,000 mPa·s at 25°C, the sealing material being configured to foam at 120°C.
Need to check novelty before this filing date? Find Prior Art

Description

Seal material and seal structure

[0001] The present disclosure relates to a seal material and a seal structure.

[0002] 2. Description of the Related Art High-temperature apparatuses having an internal space in which the atmosphere can be controlled, such as high-temperature atmospheric furnaces, are widely used in various fields.

[0003] In such high-temperature equipment, the sealing performance of the seal portion that seals the internal space from the outside may deteriorate during use of the high-temperature equipment, and in such cases, it may often become necessary to repair the seal portion while the high-temperature equipment is maintained at a high temperature.

[0004] Various sealing materials and sealing methods have been proposed for the so-called in-situ repair of such high-temperature equipment (for example, Patent Document 1).

[0005] Japanese Patent Application Laid-Open No. 2016-3313

[0006] In-situ repair of high-temperature equipment requires the installation of a sealant in the sealed portion at high temperatures to properly seal the internal space from the outside. However, conventional sealants do not always provide sufficient sealing. For example, even if a sealant exhibits good sealing properties at room temperature (25°C), it may become difficult to obtain sufficient adhesion of the sealant to the wall surface of the sealed portion at high temperatures, such as 300°C or higher.

[0007] An object of the present disclosure is to provide a sealing material that has good adhesion to the wall surface of a sealing portion in a high temperature range, and a sealing structure that uses the sealing material.

[0008] The present disclosure includes the following aspects. <1> A sealing material comprising an inorganic component and moisture, wherein the sealing material has a viscosity of 10,000 mPa·s to 350,000 mPa·s at 25°C, and wherein the sealing material foams at 120°C. <2> The sealing material according to <1>, wherein the inorganic component comprises at least one selected from the group consisting of aluminosilicates and silicates. <3> The sealing material according to <2>, wherein the inorganic component comprises the aluminosilicate, and wherein a ratio of the number of Si atoms to the number of Al atoms contained in the sealing material is 3.0 to 10.0. <4> The sealing material according to <3>, wherein the aluminosilicate comprises sodium aluminosilicate. <5> The sealing material according to <2>, wherein the inorganic component comprises the aluminosilicate, and wherein the amount of moisture contained in the sealing material is 40% by mass to 70% by mass of the entire sealing material. <6> The sealing material according to <2>, wherein the silicate comprises sodium silicate. <7> The sealing material according to any one of <1> to <6>, wherein, when the sealing material is placed in a sealing section at 300°C to form a foamed and cured product of the sealing material, the porosity of the foamed and cured product is 50% by volume or more. <8> The sealing material according to any one of <1> to <7>, wherein, when the sealing material is placed in contact with the surface of a plate at 300°C to form a foamed and cured product of the sealing material, the arithmetic mean roughness Ra of the surface of the foamed and cured product in contact with the surface is 1 mm or less. <9> The sealing material according to any one of <1> to <8>, used in a sealing section that isolates the internal space of a high-temperature device from the outside. <10> A sealing structure that is a foamed and cured product of the sealing material according to any one of <1> to <9>. <11> The sealing structure according to <10>, wherein the porosity is 50% by volume or more. <12> The sealing structure according to <10> or <11>, which is placed in a sealing section that isolates the internal space of a high-temperature device from the outside.

[0009] According to the present disclosure, it is possible to provide a sealing material that has good adhesion to the wall surface of a sealing portion in a high temperature range, and a sealing structure using the sealing material.

[0010] 1 is a cross-sectional view schematically illustrating an example of a seal structure according to the present disclosure, which is formed by installing an example of a seal material according to the present disclosure in a seal portion of a high-temperature device;

[0011] Hereinafter, embodiments of the present disclosure will be described in detail. However, the present disclosure is not limited to the following embodiments. In the following embodiments, components (including element steps, etc.) are not essential unless otherwise specified. The same applies to numerical values ​​and their ranges, and do not limit the present disclosure.

[0012] In the present disclosure, numerical ranges indicated using "to" include the numerical values ​​before and after "to" as the minimum and maximum values, respectively. In the present disclosure, each component may contain multiple corresponding substances. When multiple substances corresponding to each component are present in a composition, the proportion of each component means the total proportion of the multiple substances present in the composition, unless otherwise specified. In numerical ranges described in stages in the present disclosure, the upper or lower limit value described in one numerical range may be replaced with the upper or lower limit value of another numerical range described in stages. Furthermore, in numerical ranges described in the present disclosure, the upper or lower limit value of that numerical range may be replaced with a value shown in the examples. When embodiments in the present disclosure are described with reference to drawings, the configuration of the embodiment is not limited to the configuration shown in the drawings. Furthermore, the sizes of the components in each drawing are conceptual, and the relative size relationships between the components are not limited thereto. In the present disclosure, a combination of two or more preferred aspects is a more preferred aspect.

[0013] In this disclosure, the term "sealing material" refers to a material applied to a sealing portion of a high-temperature device or the like to seal the internal space of the device or the like from the outside. The term "sealing portion" refers to the area where the sealing material is installed. In addition, in this disclosure, the term "sealing structure" refers to a component formed in a sealing portion of a high-temperature device as a result of installing the "sealing material" in the high-temperature sealing portion of the high-temperature device. Therefore, when the "sealing material" is installed in the high-temperature sealing portion of the high-temperature device, a "sealing structure" is formed from the "sealing material."

[0014] [Sealing Material] A sealing material according to an embodiment of the present disclosure includes an inorganic component and moisture, has a viscosity of 10,000 mPa·s to 350,000 mPa·s at 25° C., and foams at 120° C. Hereinafter, the viscosity of the sealing material at 25° C. is also referred to as the "25° C. viscosity," and the property of foaming at 120° C. is also referred to as the "high-temperature foamability."

[0015] As mentioned above, even if a sealing material exhibits good sealing properties at a sealing portion at room temperature (25°C), it may be difficult to achieve adhesion to the wall surface of the sealing portion at high temperatures. Hereinafter, adhesion of a sealing portion to a wall surface at high temperatures will also be referred to as "high-temperature adhesion." One of the reasons why high-temperature adhesion is difficult to achieve is, for example, the Leidenfrost phenomenon. The Leidenfrost phenomenon is a phenomenon in which, when a liquid comes into contact with a solid whose temperature is higher than its boiling point, a layer of vapor generated from the liquid intervenes between the solid and the liquid. When the sealing material comes into contact with the wall surface of the sealing portion, if water vapor generated from the sealing material due to the Leidenfrost phenomenon intervenes between the sealing material and the wall surface of the sealing portion, it is thought that the adhesion of the sealing material to the wall surface of the sealing portion will be reduced.

[0016] In contrast, the sealing material of this embodiment contains an inorganic component and water, has a viscosity at 25°C within the above range, and has high-temperature foaming properties, thereby suppressing the Leidenfrost phenomenon. The reason for this is unclear, but it is presumed as follows: In a sealing material containing an inorganic component and water, having a viscosity at 25°C within the above range, and having high-temperature foaming properties, the inorganic component and water are mixed together to form a gel, which is thought to trap the water inside the sealing material and make it difficult for it to escape to the outside. Even if the temperature of the sealing material rises and the water turns into a gas, it is unlikely that the water will foam inside the sealing material and be released to the outside as water vapor. Therefore, it is presumed that the Leidenfrost phenomenon is suppressed, particularly compared to when the viscosity at 25°C is lower than the above range. Furthermore, the suppression of the Leidenfrost phenomenon improves the high-temperature adhesion of the sealing material.

[0017] In addition to suppressing the Leidenfrost phenomenon, the sealing material of this embodiment has a 25°C viscosity within the above range, which provides high conformability to the wall surface of the sealing portion. This high conformability to the wall surface of the sealing portion is believed to improve high-temperature adhesion compared to when the 25°C viscosity is higher than the above range. Furthermore, because the sealing material of this embodiment has high-temperature foaming properties, drying shrinkage of the sealing material due to a decrease in moisture content is suppressed even when it comes into contact with the wall surface of a sealing portion in a high-temperature range. Therefore, cracks due to drying shrinkage are less likely to occur. The method for obtaining a sealing material having a 25°C viscosity within the above range and high-temperature foaming properties is not particularly limited and is selected depending on the type of inorganic component contained in the sealing material. Examples of methods for obtaining a sealing material having a 25°C viscosity within the above range and high-temperature foaming properties include adjusting the stirring conditions during sealing material preparation and adjusting the moisture content of the sealing material.

[0018] <25°C Viscosity> The 25°C viscosity of the sealing material is 10,000 mPa·s or more, and from the viewpoint of improving high-temperature adhesion, it is preferably 30,000 mPa·s or more, and more preferably 50,000 mPa·s or more. The 25°C viscosity of the sealing material is 350,000 mPa·s or less, and from the viewpoint of improving high-temperature adhesion, it is preferably 300,000 mPa·s or less, and more preferably 200,000 mPa·s or less. The 25°C viscosity of the sealing material is 10,000 mPa·s to 3,500,000 mPa·s, preferably 30,000 mPa·s to 300,000 mPa·s, and more preferably 50,000 mPa·s to 200,000 mPa·s.

[0019] The 25°C viscosity of the sealing material is the viscosity measured at 25°C using an E-type viscometer. Specifically, the viscosity at 25°C is measured using an E-type viscometer (for example, TV-100E manufactured by Toki Sangyo Co., Ltd.) at a rotation speed of 10 rpm. The sample used for measuring the 25°C viscosity is a sealing material that has been left to stand at 25°C for 24 hours or more after preparation, and then stirred with a spoon 10 times or more, and then used within 5 minutes.

[0020] The reason for using a sealant that has been left at 25°C for 24 hours or more after preparation is that the viscosity of the sealant may change over time. For example, even if a sealant has a viscosity of 10,000 mPa·s to 350,000 mPa·s at 25°C within 10 minutes of preparation, the viscosity at 25°C after being left at 25°C for 24 hours or more (i.e., the above-mentioned 25°C viscosity) may be less than 10,000 mPa·s. An example of such a sealant is one that is gel-like immediately after preparation, but over time, the inorganic components microcrystallize to form fine particles, and the fine inorganic component particles disperse in the liquid to form micelles, resulting in a 25°C viscosity of less than 10,000 mPa·s. In contrast, the 25°C viscosity of the sealant of this embodiment, i.e., the viscosity at 25°C of the sealant after being left at 25°C for 24 hours or more after preparation, is measured, and since the value is within the above range, it is presumed that the gel-like state is maintained even after being left at 25°C for 24 hours or more. The reason for stirring with a spoon before measuring the viscosity is to measure the viscosity of the sealant in a stable gel state and the viscosity of the sealant in which inorganic component particles have formed and settled under the same conditions.

[0021] In this embodiment, the viscosity at 25°C is defined as η, and the viscosity of the sealing material at 25°C within 10 minutes after preparation is defined as η. 0 When this is the case, the viscosity change rate (%) of the sealing material at 25 ° C. |η 0 −η|×100 / η 0 From the viewpoint of storage stability of the sealing material, the viscosity change rate (%)|η of the sealing material at 25° C. is preferably 40% or less, more preferably 30% or less, even more preferably 20% or less, and particularly preferably 10% or less. 0 −η|×100 / η 0 is also referred to as the "viscosity change rate." The viscosity η of the sealing material at 25°C within 10 minutes after preparation 0 The measurement of viscosity at 25°C is carried out in the same manner as in the measurement of viscosity at 25°C, except that a sealing material used as a sample within 10 minutes after preparation is used.

[0022] <High-Temperature Foamability and Porosity at 300°C> The sealing material of this embodiment has high-temperature foamability. Having high-temperature foamability means that the sealing material has the property of foaming, i.e., generating bubbles, when heated to 120°C. Whether or not a sealing material has high-temperature foamability is confirmed as follows. Specifically, a state in which the sealing material expands in volume and bubbles are present in its cross section when held at 120°C for 10 minutes is considered to have "high-temperature foamability."

[0023] In the sealing material of this embodiment, from the viewpoint of suppressing the occurrence of cracks due to drying shrinkage, the porosity of the foamed and cured product when placed in a sealing section at 300°C to form a foamed and cured product is preferably 50% by volume or more, more preferably 60% by volume or more, and even more preferably 70% by volume or more. Hereinafter, the porosity of the foamed and cured product when placed in a sealing section at 300°C to form a foamed and cured product is also referred to as the "300°C porosity." From the viewpoint of obtaining a high-strength seal structure, the 300°C porosity of the sealing material is preferably 95% by volume or less, more preferably 90% by volume or less, and even more preferably 80% by volume or less. The 300°C porosity of the sealing material is preferably 50% by volume to 95% by volume, more preferably 60% by volume to 90% by volume, and even more preferably 70% by volume to 80% by volume.

[0024] The 300°C porosity of the sealing material is measured as follows. Specifically, first, a 500 cm3 volume of the sealing material is heated to 300°C. 3 The sealing material to be measured is poured into the container. The amount of sealing material to be poured is an amount that does not overflow the container with the foamed and cured product of the sealing material, that is, an amount that the volume of the foamed and cured product of the sealing material fits within the container. The volume of the poured sealing material is V 0 The volume of the obtained foamed and cured product is V 1 When the temperature is 300°C, the expansion coefficient A (%) of the sealing material and the porosity P (%) of the sealing material are expressed by the following formulas (1) and (2). Formula (1): Expansion coefficient A (%) = (V 1 / V 0) × 100 Formula (2): Porosity P (%) = [(expansion coefficient A (%) / specific gravity of sealing material) - (mass ratio of solid content (%) / true specific gravity of solid content of sealing material)] × 100 / (expansion coefficient A (%) / specific gravity of sealing material) Note that in the above formulas (1) and (2), the "specific gravity of sealing material" is a value calculated from the mass and volume of the sealing material, the "mass ratio of solid content (%)" is a value expressed as "100 - water content of sealing material (%)", and the "true specific gravity of solid content of sealing material" is a value measured by Archimedes' method using a pulverized product obtained by pulverizing a foamed and cured sealing material.

[0025] <300°C Ra> In the sealing material of this embodiment, from the viewpoint of improving high-temperature adhesion, when the foamed and cured product is placed in contact with the surface of a plate at 300°C, the arithmetic mean roughness Ra of the surface in contact with the surface of the plate is preferably 1 mm or less, more preferably 0.5 mm or less, even more preferably 0.2 mm or less, and particularly preferably 0.1 mm or less. Hereinafter, the arithmetic mean roughness Ra of the surface in contact with the surface of the plate when the foamed and cured product is placed in contact with the surface of a plate at 300°C is also referred to as "300°C Ra." A sealing material that suppresses the Leidenfrost phenomenon, has good conformability to the plate surface, and suppresses the occurrence of cracks due to drying shrinkage is thought to have a small 300°C Ra value. The lower limit of 300°C Ra is not particularly limited, and may be, for example, 0.01 mm. The 300° C. Ra is preferably 0.01 mm to 1 mm, more preferably 0.01 mm to 0.5 mm, even more preferably 0.01 mm to 0.2 mm, and particularly preferably 0.01 mm to 0.1 mm.

[0026] The 300°C Ra is measured as follows: A plate having a surface arithmetic mean roughness Ra of 10 μm or less is heated to 300°C, a sealant is applied directly to the surface, and the sealant is maintained for 10 minutes to obtain a foamed and cured product. The temperature of the plate is then lowered to 25°C, the foamed and cured product is peeled off the surface of the plate, and the arithmetic mean roughness Ra of the surface that was in contact with the plate surface is measured by the following method. The plate used for measuring the 300°C Ra is not particularly limited as long as the surface arithmetic mean roughness Ra is 10 μm or less, and examples thereof include a metal plate and a ceramic plate.

[0027] The arithmetic mean roughness Ra is measured in accordance with JIS B0601 (1994) as follows: A laser microscope (for example, VK-X3000 manufactured by Keyence) is used as the measuring device, and the three-dimensional shape of the surface is observed at a magnification of 100. From the roughness curve obtained from the obtained three-dimensional shape, the arithmetic mean roughness Ra is determined under the conditions of a reference length of 8 mm and a cutoff value of 8 mm.

[0028] <Composition> The sealing material of this embodiment contains at least an inorganic component and water. The inorganic component contained in the sealing material is not particularly limited as long as it can maintain the viscosity of the entire sealing material at 25°C within the above range. The sealing material may contain only one inorganic component or two or more inorganic components. Examples of inorganic components include inorganic oxides. Specific examples of inorganic components include inorganic acid metal salts such as aluminosilicates, silicates, and polyborates. Among these, aluminosilicates and silicates are preferred from the standpoints of safety, heat resistance, and cost, and aluminosilicates are more preferred. Here, "silicate" refers to a silicate that does not contain aluminum atoms, i.e., a silicate other than aluminosilicates. Examples of metal salts include alkali metal salts. Specific examples of alkali metal salts include sodium salts, potassium salts, and lithium salts. Among these, sodium salts are preferred from the standpoint of availability. The sealing material preferably contains alkali metal atoms, and more preferably sodium atoms. The sealing material may contain only one alkali metal atom or two or more alkali metal atoms.

[0029] The amount of water contained in the sealing material is not particularly limited, as long as the viscosity of the entire sealing material at 25°C falls within the above range and the sealing material has high-temperature foaming properties. Hereinafter, the amount of water relative to the entire sealing material is also referred to as the "water content." The preferred water content of the sealing material varies depending on the type of inorganic component contained in the sealing material. Examples of the water content of the sealing material include 30% to 70% by mass. From the viewpoint of improving high-temperature adhesion, the water content of the sealing material is preferably 70% by mass or less, and more preferably 60% by mass or less. Furthermore, from the viewpoint of improving high-temperature adhesion, the water content of the sealing material is preferably 30% by mass or more, and more preferably 35% by mass or more. The water content of the sealing material is preferably 30% by mass to 70% by mass, and more preferably 35% by mass to 60% by mass. When the water content of the sealing material is equal to or less than the upper limit, the Leidenfrost phenomenon is easily suppressed, and when the water content is equal to or greater than the lower limit, the seal portion exhibits good conformability to the wall surface.

[0030] The moisture content of the sealing material is measured as follows: Using a differential thermobalance (TG-8120 Thermo Plus EVO2 manufactured by Rigaku Corporation), the moisture content is determined by the attenuation of weight when the material is held at 150° C. for 1 hour.

[0031] The sealing material of the present embodiment may contain components other than the inorganic component and water as necessary. The total content of the inorganic component and water in the entire sealing material is preferably 80% by mass or more, more preferably 90% by mass or more, and even more preferably 95% by mass or more, and may be 100% by mass.

[0032] Furthermore, as described above, the inorganic component contained in the sealing material preferably contains an inorganic acid metal salt, more preferably contains at least one selected from the group consisting of aluminosilicates, silicates, and polyborates, further preferably contains at least one selected from the group consisting of aluminosilicates and silicates, particularly preferably contains an aluminosilicate, and extremely preferably contains sodium aluminosilicate.

[0033] The inorganic components contained in the sealant may include inorganic acid metal salts and other inorganic components other than inorganic acid metal salts. Examples of other inorganic components include inorganic oxide particles used for purposes such as adjusting the viscosity of the sealant, improving application properties in high-temperature areas, and improving the mechanical strength of the foamed, cured product. Examples of inorganic oxide particles include silica, alumina, alumina hydrate, titania, zirconia, zeolite, and clay compounds. When the inorganic components contained in the sealant include inorganic oxide particles, the content of the inorganic oxide particles relative to the total inorganic components is, for example, 20 to 70% by mass. The content of the inorganic acid metal salt relative to the total inorganic components contained in the sealant is preferably 30% by mass or more, more preferably 50% by mass or more, even more preferably 70% by mass or more, even more preferably 80% by mass or more, particularly preferably 90% by mass or more, extremely preferably 95% by mass or more, and may even be 100% by mass.

[0034] Below, as examples of the sealing material of this embodiment, a sealing material containing an aluminosilicate as an inorganic component, a sealing material containing a silicate as an inorganic component, and a sealing material containing a polyborate as an inorganic component will be described.

[0035] <Sealing material containing aluminosilicate> Examples of aluminosilicate include sodium aluminosilicate, potassium aluminosilicate, and lithium aluminosilicate, and among these, sodium aluminosilicate is preferred. In the sealing material containing aluminosilicate, the number of Si atoms N Si Number of Al atoms N Al Ratio to N Si / N Al In terms of improving high-temperature adhesion, the ratio N is preferably 3.0 to 10.0. Si / N Al When the value of the ratio N is in the above range, the viscosity at 25°C is in the above range and the sealing material tends to have high-temperature foaming properties. Si / N Al It is presumed that this is because the network structure of the inorganic component is easily formed when the value of ratio N is within the above range. Si / N AlThe value of N is preferably 3.0 or more. Si / N Al The value of the ratio N is preferably 10.0 or less, more preferably 8.0 or less, even more preferably 7.0 or less, even more preferably 5.0 or less, particularly preferably 4.5 or less, and extremely preferably 3.5 or less. Si / N Al The value is more preferably 3.0 to 7.0, even more preferably 3.0 to 5.0, particularly preferably 3.0 to 4.5, and most preferably 3.0 to 3.5.

[0036] In a sealing material containing an aluminosilicate, the number of Si atoms N contained in the sealing material Si The number of alkali metal atoms in M Ratio to N Si / N M From the viewpoint of improving high-temperature adhesion, is preferably 0.5 to 2.5, more preferably 1.5 to 2.2, and even more preferably 1.6 to 1.8.

[0037] The above ratio N Si / N Al and ratio N Si / N M The value of the ratio N is measured as follows. Specifically, a measurement sample of the sealing material is crushed in a mortar, and then measured using a fluorescent X-ray analyzer: ZSX Primus IV manufactured by Rigaku Corporation. Si / N Al and ratio N Si / N M There is no particular limitation on the method for controlling the value of the ratio N. For example, in a sealing material containing an aluminosilicate obtained by mixing silicate, aluminate, and water as described below, the mixing ratio of silicate and aluminate can be adjusted to control the value of the ratio N. Si / N Al and ratio N Si / N M The value of may be controlled.

[0038] From the viewpoint of improving high-temperature adhesion, the moisture content of the sealing material containing aluminosilicate is preferably 70% by mass or less, more preferably 65% ​​by mass or less, and even more preferably 60% by mass or less. Furthermore, from the viewpoint of improving high-temperature adhesion, the moisture content of the sealing material containing aluminosilicate is preferably 40% by mass or more, more preferably 45% by mass or more, and even more preferably 50% by mass or more. The moisture content of the sealing material containing aluminosilicate is preferably 40% by mass to 70% by mass, more preferably 45% by mass to 65% by mass, and even more preferably 50% by mass to 60% by mass. For example, in the case of a sealing material containing aluminosilicate obtained by mixing silicate, aluminate, and water as described below, the moisture content of the sealing material containing aluminosilicate may be controlled by adjusting the amount of water added.

[0039] A sealing material containing aluminosilicate can be obtained, for example, by mixing silicate, aluminate, and water. The silicate and aluminate may contain the same or different alkali metal atoms, preferably the same. The sealing material containing aluminosilicate is preferably a sealing material obtained by mixing sodium silicate, sodium aluminate, and water. A method for controlling the 25°C viscosity and high-temperature foamability of a sealing material containing aluminosilicate includes, for example, using a stirrer to adjust the stirring speed, stirring time, and mixing ratio of silicate, aluminate, and water. The stirring speed may be, for example, 500 rpm or more, preferably 3000 rpm or more. The upper limit of the stirring speed is not particularly limited, and may be, for example, 50,000 rpm. The stirring time may be, for example, 1 minute or more, and preferably 3 minutes or more. The upper limit of the stirring time is not particularly limited, and may be, for example, 10 minutes.

[0040] <Sealing material containing silicate> Examples of silicate include sodium silicate, potassium silicate, and lithium silicate, with sodium silicate being preferred. Hereinafter, the term "sealing material containing silicate" refers to a sealing material containing silicate but not containing aluminum atoms, i.e., a sealing material containing silicate but not containing aluminosilicate. The moisture content of the silicate-containing sealing material is preferably 30% to 50% by mass from the viewpoint of improving high-temperature adhesion. A moisture content within the above range for a silicate-containing sealing material facilitates the formation of a sealing material with a 25°C viscosity within the above range and high-temperature foamability. While the reason for this is unclear, it is presumed that a moisture content within the above range facilitates the formation of a network structure of inorganic components. The moisture content of the silicate-containing sealing material is preferably 50% by mass or less, more preferably 45% by mass or less. Furthermore, the moisture content of the silicate-containing sealing material is preferably 30% by mass or more, more preferably 35% by mass or more. The moisture content of the silicate-containing sealing material is more preferably 35% by mass to 40% by mass. In a sealing material containing silicate, methods for controlling the moisture content include, for example, mixing powdered silicate with a predetermined amount of moisture, or using microwave heating to remove moisture evenly from the entire commercially available silicate (liquid) to achieve a target composition.

[0041] In a sealing material containing silicate, the number of Si atoms N contained in the sealing material Si The number of alkali metal atoms in M Ratio to N Si / N M From the viewpoint of foaming property and cell breaking property, the ratio N is preferably 1.5 to 2.0. Si / N M The value of N is measured by the above-mentioned method. Si / N M The method for controlling the value of is not particularly limited, and examples thereof include a method of selecting the type of silicate to be used. A sealing material containing silicate can be obtained, for example, by mixing silicate and water and controlling the water content by the above-mentioned method or the like.

[0042] <Sealing material containing polyborate> Examples of polyborate include sodium polyborate, potassium polyborate, lithium polyborate, etc., and among these, sodium polyborate is preferred. In a sealing material containing polyborate, a method for controlling the water content may include, for example, mixing boric acid and sodium borate and dissolving the mixture in water, thereby increasing the solubility in water, and utilizing this to control the water concentration.

[0043] In a sealing material containing polyborate, the number of B atoms contained in the sealing material, N B The number of alkali metal atoms in M Ratio to N B / N M The value of the ratio N Si / N M The ratio N in the sealing material containing polyborate is measured by the same method as the value of B / N M The method for controlling the value of is not particularly limited, and examples thereof include a method of selecting the type of polyborate to be used. A sealing material containing a polyborate can be obtained, for example, by mixing a polyborate with water and controlling the water content by the above-mentioned method or the like.

[0044] <Applications> The sealing material of this embodiment is used, for example, in a sealing portion that isolates the internal space of a high-temperature device from the outside. The sealing material of this embodiment has good adhesion to the sealing portion even in a high-temperature range. The temperature of the sealing portion is, for example, 150°C to 600°C, but may also be 200°C to 600°C, 300°C to 600°C, or 400°C to 600°C. The temperature of the sealing portion refers to the temperature measured on the wall surface of the sealing portion using a thermometer.

[0045] [Sealing structure] A sealing structure according to an embodiment of the present disclosure is a foamed and cured product of the sealing material according to the above-described embodiment. The sealing structure according to this embodiment is installed in a sealing section that isolates the internal space of a high-temperature device from the outside, for example, and is obtained by installing the above-described sealing material in the sealing section in a high-temperature range to form a foamed and cured product.

[0046] The porosity of the seal structure is preferably 50% by volume or more, more preferably 60% by volume or more, and even more preferably 70% by volume or more, from the viewpoint of preventing cracks from occurring due to drying shrinkage during the manufacturing process. The porosity of the seal structure is preferably 95% by volume or less, more preferably 90% by volume or less, and even more preferably 85% by volume or less, from the viewpoint of strength. When the volume of the sealing material before obtaining the seal structure is known, the porosity of the seal structure can be calculated by multiplying the volume of the sealing material by V 0 and the volume of the seal structure is V 1 On the other hand, when the volume of the sealing material before obtaining the seal structure is unknown, the porosity Ps (%) of the seal structure can be calculated by using the true specific gravity of the solid content of the seal structure, the mass of the seal structure, M (g), and the apparent volume of the seal structure, V (cm 3 ), porosity Ps (%) is expressed by the following formula (3): Formula (3): Porosity Ps (%) = (M / (ρ × V)) × 100 In the above formula (3), ρ is a value calculated from the volume and weight determined by Archimedes' method using a pulverized product of the seal structure, and V is a value measured by Archimedes' method.

[0047] The apparent density of the seal structure is, for example, 0.8 g / cm 3 The following are listed, and from the viewpoint of crack suppression during the manufacturing process, 0.7 g / cm 3 Preferably, 0.5 g / cm or less 3 The apparent density of the seal structure is more preferably 0.1 g / cm from the viewpoint of strength. 3 More than 0.2 g / cm 3 More preferably, 0.3 g / cm 3 The above is more preferable. The apparent density of the seal structure can be determined by dividing the mass of the seal structure by the apparent volume of the seal structure.

[0048] An example of a seal structure of this embodiment installed in a seal section that isolates the internal space of a high-temperature device from the outside world, and an example of the high-temperature device will be described below. Fig. 1 is a cross-sectional view that schematically shows an example of a seal structure of this embodiment formed in a seal section of the high-temperature device. As shown in Fig. 1, the seal structure 100 is installed in a seal section 20 that closes a gap 15 of a high-temperature device 10.

[0049] More specifically, the high-temperature device 10 has a first wall member 30 and a second wall member 31, and the first and second wall members 30, 31 form an internal space 40 within the high-temperature device 10. However, a gap 15 exists between the first wall member 30 and the second wall member 31, and a seal member 42 is filled into the gap 15 to seal the gap 15. This forms a seal portion 20, and the internal space 40 is isolated from the outside world. However, if the high-temperature device 10 is used for a long period of time, for example, the seal member 42 may deteriorate, and its sealing performance may decrease. In such a case, it may become necessary to repair the seal member 42 while the high-temperature device 10 is in use, i.e., while the seal portion 20 is at a high temperature.

[0050] The seal structure 100 is provided for such in-situ repair. That is, by configuring the seal portion 20 with the seal structure 100, the sealing performance of the high-temperature device 10 can be maintained.

[0051] The temperature of the seal portion 20 to which the seal structure 100 is applied varies depending on the high-temperature device 10. The temperature of the seal portion 20 to which the seal structure 100 is applied can be, for example, in the range of 150°C to 600°C. The first wall member 30 and the second wall member 31 that form the seal portion 20 to which the seal structure 100 is installed may be made of any heat-resistant material, such as metal (e.g., heat-resistant metal) and ceramics (e.g., firebrick).

[0052] The seal structure 100 is formed by applying the seal material in the above-described embodiment to the seal portion 20 of the high-temperature equipment 10, causing the seal material to foam and harden. The method for applying the seal material to the seal portion 20 of the high-temperature equipment 10 is not particularly limited. For example, a method of filling the seal material into the seal portion 20 of the high-temperature equipment 10 using a trowel or spatula may be used. Note that, for safety reasons, when the seal portion 20 is at a high temperature, a method that allows the seal material to be applied from a relatively remote position, such as a mortar injector or a spray application method, may be used.

[0053] The high-temperature equipment 10 includes, but is not limited to, various types of furnaces such as a coal coke oven, an iron ore blast furnace, a glass melting furnace, and a glass forming furnace. Fig. 2 shows a schematic configuration of a high-temperature equipment 210, which is an example of the high-temperature equipment 10. The high-temperature equipment 210 shown in Fig. 2 includes a metal container 220 and an electric furnace 230 that houses the metal container 220.

[0054] The metal container 220 is made of stainless steel and has a roughly rectangular parallelepiped shape. One side of the metal container 220 is open, and this opening is rectangular, measuring 150 mm x 20 mm. The internal volume of the metal container 220 is approximately 10 L. The metal container 220 is placed inside the electric furnace 230 with the open portion protruding outward from the electric furnace 230. The length of the protruding portion 226 protruding from the electric furnace 230 is approximately 10 mm. Another opening is provided in a portion of the metal container 220, and this opening is connected to the air gas buffer tank 240. When installing the sealing material, the electric furnace is heated to approximately 550°C. As a result, the protruding portion 226 of the metal container 220 is heated to approximately 350°C.

[0055] The sealing material is installed, for example, as follows: The sealing material is filled from the vicinity of the protruding portion 226 of the metal container 220 toward the inside of the metal container 220. As a result, the sealing material 250 is installed on the protruding portion 226 to form a seal structure, sealing the opening. The installation depth of the sealing material 250 is 20 mm from the tip of the protruding portion 226. Ten minutes after the sealing material 250 is filled, the buffer tank 240 is opened and air gas is supplied into the metal container 220. With the opening sealed by the seal structure, the pressure inside the metal container 220 can be set to, for example, 10,000 Pa.

[0056] Hereinafter, embodiments of the present disclosure will be described in detail using examples, but the embodiments of the present disclosure are not limited to these. In the following description, Examples A3 to A8, A13 to A17, and B5 to B8 are Examples, and Examples A1 to A2, A9 to A12, A18 to A20, B1 to B4, and B9 are Comparative Examples.

[0057] [Example A] <Preparation of sealing material> (Examples A1 to A19) Sodium silicate (water glass No. 1 and No. 3, manufactured by Nippon Chemical Industry Co., Ltd.), sodium aluminate (sodium aluminate powder, manufactured by Hokuriku Chemical Industry Co., Ltd.), and water were mixed and stirred at a stirring speed of 3000 rpm for 3 minutes using a mixer (manufactured by Yamato Scientific, product name: Cutter Mixer R-15E), to obtain sealing materials of Examples A1 to A19, respectively. The amounts of sodium silicate, sodium aluminate, and water added were determined based on the SiO 2 , Al 2 O 3 , Na 2 O and H 2 The composition ratio (mass %) of O was set to the values ​​shown in Tables 1 and 2. 2 The composition ratio (mass %) of O corresponds to the amount of moisture in the sealing material. Si Number of Al atoms N Al Ratio to N Si / N Al These are also shown in Tables 1 and 2.

[0058] (Example A20) A sealing material of Example A20 was obtained in the same manner as in Example A7, except that the stirring speed was changed to 1500 rpm and the stirring time was changed from 3 minutes to 1 minute. 2 , Al 2 O 3 , Na 2 O and H 2 The composition ratio (mass%) of O and the ratio of N Si / N Al are also shown in Table 2.

[0059] <Measurement of sealing material> The viscosity η of the sealing material at 25°C and the viscosity η of the sealing material at 25°C within 10 minutes after preparation were measured by the above-mentioned method. 0 Measure the viscosity change rate (%): |η 0 −η|×100 / η 0 was determined. The results are shown in Tables 1 and 2. Using the method described above, it was confirmed whether the sealing material had high-temperature foaming properties (i.e., whether it had high-temperature foaming properties or not). The results are shown in Tables 1 and 2. Using the method described above, the sealing material was placed in a sealed area at 300°C to form a foamed and cured product, and the expansion coefficient of the foamed and cured product (i.e., 300°C porosity) was measured. The 300°C porosity was calculated assuming a specific gravity of the sealing material of 1.5 and a true specific gravity of the solid content of the sealing material of 1.8. The results are shown in Tables 1 and 2.

[0060] <Evaluation of sealing material and measurement of sealing structure> Using the method described above, a foamed and cured product was placed in contact with the surface of a plate at 300°C to form a foamed and cured product. The arithmetic mean roughness Ra (i.e., 300°C Ra) of the surface in contact with the plate surface was measured to evaluate high-temperature adhesion. A stainless steel plate with a surface arithmetic mean roughness Ra of 10 μm was used as the plate. The results are shown in Tables 1 and 2. A smaller 300°C Ra value indicates better high-temperature adhesion. The surface of the foamed and cured product obtained by measuring the 300°C Ra in contact with the plate surface was observed with a magnifying glass (magnification ×10) to check for the presence or absence of cracks. The results are shown in Tables 1 and 2. The sealing materials of Examples A3 to A8 and A13 to A17 had good workability, and among them, the workability of the sealing materials of Examples A7 and A15 was particularly good.

[0061]

[0062]

[0063] As can be seen from Tables 1 and 2, the sealing materials of Examples A3 to A8 and A13 to A17 had higher high-temperature adhesion than the sealing materials of Examples A1 to A2, A9 to A12, and A18 to A20.

[0064] [Example B] <Preparation of sealing material> (Examples B1 to B9) Sodium silicate (powdered sodium silicate, and sodium silicate No. 1 and No. 3, manufactured by Nippon Chemical Industry Co., Ltd.) and water were mixed, and the mixture was stirred at a stirring speed of 3000 rpm for 3 minutes using a mixer (manufactured by Yamato Scientific, product name: Cutter Mixer R-15E), and then dried (microwave heated) to obtain sealing materials of Examples B1 to B9. Note that the drying treatment was carried out so that the water content of the sealing material reached the H 2 The composition ratio of O (mass %) was adjusted to the value shown in the table. 2 , Na 2 O and H 2 The composition ratio of O (mass%) and the number of Si atoms, N Si The number of sodium atoms in Na Ratio to N Si / N Na are also shown in Table 3.

[0065] <Measurement of sealing material> In the same manner as in Example A1, the viscosity η at 25°C and the viscosity η at 25°C within 10 minutes after the preparation of the sealing material were measured. 0 The viscosity change rate (%), the presence or absence of high-temperature foamability, and the 300°C porosity were measured. The 300°C porosity was calculated using the measurement data of the weight and apparent volume of the seal structure and the true specific gravity of the solid content of the seal material, which was 1.5. The results are shown in Table 3. <Evaluation of seal material and measurement of seal structure> In the same manner as in Example A1, high-temperature adhesion was evaluated by measuring the 300°C Ra. Also, in the same manner as in Example A1, the presence or absence of cracking was confirmed. The results are shown in Table 3. In Example B7, the seal structure, which was the foamed and cured product obtained by measuring the 300°C Ra, was found to have an apparent density of 0.42 g / cm by the method described above. 3The sealing materials of Examples B5 to B8 had good workability, and among them, the sealing material of Example B7 had particularly good workability.

[0066]

[0067] As can be seen from Table 3, the sealing materials of Examples B5 to B8 had higher high-temperature adhesion than the sealing materials of Examples B1 to B4 and B9. Furthermore, the sealing materials of Examples B5 to B8 had good workability.

[0068] The disclosure of Japanese Patent Application No. 2023-067238, filed on April 17, 2023, is incorporated herein by reference in its entirety. In addition, all documents, patent applications, and technical standards described herein are incorporated herein by reference to the same extent as if each individual document, patent application, and technical standard was specifically and individually indicated to be incorporated by reference.

[0069] 10, 210 High-temperature device 15 Gap 20 Seal portion 30 First wall member 31 Second wall member 40 Internal space 42 Seal member 100 Seal structure 220 Metal container 226 Protrusion 230 Electric furnace 240 Buffer tank 250 Seal material (seal structure)

Claims

1. A sealing material comprising an inorganic component and moisture, the sealing material having a viscosity of 10,000 mPa·s to 350,000 mPa·s at 25°C, and foaming at 120°C.

2. The sealing material according to claim 1, wherein the inorganic component comprises at least one selected from the group consisting of aluminosilicates and silicates.

3. The sealing material according to claim 2, wherein the inorganic component includes the aluminosilicate, and the ratio of the number of Si atoms to the number of Al atoms contained in the sealing material is 3.0 to 10.

0.

4. The sealing material according to claim 3, wherein the aluminosilicate comprises sodium aluminosilicate.

5. The sealing material according to claim 2, wherein the inorganic component includes the aluminosilicate, and the amount of moisture contained in the sealing material is 40% by mass to 70% by mass with respect to the entire sealing material.

6. The sealant according to claim 2, wherein the silicate comprises sodium silicate.

7. The sealing material according to claim 1, wherein when the sealing material is placed in a sealing section at 300°C to form a foamed and cured product of the sealing material, the porosity of the foamed and cured product is 50 volume % or more.

8. The sealing material according to claim 1, wherein when the sealing material is placed in contact with the surface of a plate at 300°C to form a foamed and cured product of the sealing material, the arithmetic mean roughness Ra of the surface of the foamed and cured product in contact with the surface is 1 mm or less.

9. The sealing material according to claim 1, which is used in a sealing portion that isolates the internal space of a high-temperature device from the outside world.

10. A seal structure comprising a foamed and cured product of the seal material according to any one of claims 1 to 9.

11. The seal structure according to claim 10, wherein the porosity is 50 volume % or more.

12. The seal structure according to claim 10, which is installed in a seal section that isolates the internal space of a high-temperature device from the outside world.

Citation Information

Patent Citations

  • Seal material and seal structure

    JP2021038839A

  • Method of manufacturing seal structure, and seal structure

    JP2022028540A