glass

The glass composition with specific oxide ranges addresses the challenge of manufacturing glass with low thermal expansion and high Young's modulus, enabling easier production and improved transparency for semiconductor device support.

WO2024219377A1PCT designated stage expired Publication Date: 2024-10-24AGC INC
View PDF 4 Cites 0 Cited by

Patent Information

Application Number
PCT/JP2024/015074
Authority / Receiving Office
WO · WO
Patent Type
Applications
Current Assignee / Owner
Priority Date
2023-04-17
Filing Date
2024-04-16
Publication Date
2024-10-24

AI Technical Summary

Technical Problem

Manufacturing glass with a low coefficient of thermal expansion and high Young's modulus to suppress deflection is challenging, as it complicates the manufacturing process and may result in reduced transparency.

Method used

A glass composition with specific ranges of SiO2, B2O3, Al2O3, and rare earth oxides, optimized to balance thermal expansion, Young's modulus, and melting temperature, facilitating easier manufacturing while maintaining excellent transparency.

Benefits of technology

The optimized glass composition allows for facilitated manufacturing, suppressed deflection, and enhanced transparency, making it suitable for supporting semiconductor devices during manufacturing processes.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure JP2024015074_24102024_PF_FP_ABST
    Figure JP2024015074_24102024_PF_FP_ABST
Patent Text Reader

Abstract

The present invention suppresses curvature, facilitates manufacturing, and improves transmissivity. A glass (10) contains, in oxide-based mol%, SiO2 at 40%-60%, B2O3 at 0.01%-15%, and Al2O3 + rare earth oxides at 0%-20%. The ratio of the total content of Al2O3 and ΣRO with respect to the total content of SiO2 and Al2O3 and ΣRO ((Al2O3 + ΣRO) / (SiO2 + Al2O3 + ΣRO)) is 0.38 or more.
Need to check novelty before this filing date? Find Prior Art

Description

Glass

[0001] The present invention relates to glass.

[0002] Glass is sometimes used as a member for supporting semiconductor devices during the manufacturing process of the semiconductor devices. For example, Patent Document 1 describes a supporting glass substrate with a high Young's modulus to suppress deflection. In addition, the coefficient of thermal expansion may be reduced to suppress deflection due to temperature changes.

[0003] Japanese Patent Application Laid-Open No. 2021-20840

[0004] However, glass with a low thermal expansion coefficient and a high Young's modulus to suppress deflection can be difficult to manufacture and can also result in poor transmittance. Therefore, there is a demand for glass that is easy to manufacture and has excellent transmittance while suppressing deflection.

[0005] An object of the present invention is to provide a glass that is easy to manufacture and has excellent transparency while suppressing deflection.

[0006] The glass according to the present disclosure contains, in mole percent on an oxide basis, SiO 2 :40%~60%, B 2 O 3 :0.01%~15%, Al 2 O 3 + Rare earth oxide: 0% to 20%, SiO 2 and Al 2 O 3 and the total content of divalent oxides, ΣRO, 2 O 3 The ratio of the total content of ΣRO and ΣRO ((Al 2 O 3 +ΣRO) / (SiO 2 +Al 2 O 3 +ΣRO)) is 0.38 or more.

[0007] According to the present invention, it is possible to easily manufacture the membrane while suppressing bending, and to increase the transparency.

[0008] Fig. 1 is a schematic diagram of a glass according to this embodiment, and Fig. 2 is a schematic diagram for explaining deflection evaluation.

[0009] Preferred embodiments of the present invention will be described in detail below with reference to the accompanying drawings. The present invention is not limited to these embodiments, and when there are multiple embodiments, the present invention also includes combinations of the embodiments. Numerical values ​​include rounded ranges. Numerical ranges expressed as "to" refer to a range that includes the numbers before and after "to" as the lower and upper limits, and the same meaning will be used hereinafter.

[0010] (Glass) FIG. 1 is a schematic diagram of glass according to this embodiment. As shown in FIG. 1, glass 10 according to this embodiment is used as a glass substrate for manufacturing semiconductor packages, and more specifically, is a supporting glass substrate for manufacturing FOWLPs and the like. However, the use of glass 10 is not limited to the manufacture of FOWLPs and the like and is arbitrary. It may be a glass substrate used to support components, or may be used for purposes other than supporting components. Note that FOWLPs and the like include fan-out wafer level packages (FOWLPs) and fan-out panel level packages (FOPLPs).

[0011] (Glass Composition) Next, a preferred composition of the glass 10 will be described.

[0012] (SiO 2 ) The glass 10 is SiO 2 Contains (SiO 2 It is preferable that the content of SiO is higher than 0 mol %. 2 is a component that reduces the linear thermal expansion coefficient and controls the Young's modulus. In addition, in order to appropriately suppress the rise in the melting temperature and liquidus temperature, SiO 2 The content of SiO is preferably 60% or less. 2 has the effect of improving the acid resistance and sulfuric acid resistance of the glass. Glass 10 contains, in mole percent on an oxide basis, SiO 2The content of SiO is preferably 40% or more and 60% or less, preferably 41% or more and 59% or less, preferably 42% or more and 58% or less, preferably 43% or more and 57% or less, preferably 43.5% or more and 56% or less, preferably 44% or more and 55% or less, preferably 44.5% or more and 54% or less, preferably 45% or more and 53% or less, preferably 45.5% or more and 52% or less, preferably 46% or more and 51.5% or less, preferably 46.5% or more and 51% or less, preferably 47% or more and 50.5% or less, preferably 47.5% or more and 50% or less, and more preferably 48% or more and 49.5% or less. 2 By setting the content within this range, it is possible to easily manufacture the glass while suppressing warping. The content here refers to the ratio of the content to the entire glass 10 in mole percent based on oxides. That is, for example, SiO 2 The content of 40% or more and 60% or less means that the SiO content is 40% or more and 60% or less of the total amount of the glass 10 in mole percent based on oxides. 2 This means that the content ratio of is 40% or more and 60% or less.

[0013] (B 2 O 3 ) B 2 O 3 has the effect of suppressing devitrification due to crystallization of the glass, facilitating manufacturing, and controlling the Young's modulus. 2 O 3 Does not contain (B 2 O 3 The content of B may be 0 mol %, 2 O 3 The glass 10 may contain, in mole percent on an oxide basis, B 2 O 3 The content of is preferably 0.01% or more and 15% or less, preferably 1% or more and 12% or less, preferably 2% or more and 10% or less, preferably 3% or more and 9% or less, preferably 4% or more and 8% or less, preferably 5% or more and 7% or less, and more preferably 5.5% or more and 6.5% or less.2 O 3 When the content falls within this range, warping can be suppressed and manufacturing can be facilitated.

[0014] (Al 2 O 3 + rare earth oxide) Glass 10 is Al 2 O 3 and rare earth oxides. Here, the rare earth oxide may be a single type of rare earth oxide or a plurality of types of rare earth oxides. 2 O 3 The Young's modulus increases by containing rare earth oxides. 2 O 3 By not making the total content of Al and rare earth oxides too small, it is possible to appropriately suppress the decrease in Young's modulus. 2 O 3 and rare earth oxide total content (Al 2 O 3 + rare earth oxides) is preferably 0% or more and 20% or less, preferably 1% or more and 17% or less, preferably 3% or more and 16% or less, preferably 6% or more and 15% or less, preferably 7% or more and 14% or less, preferably 8% or more and 13% or less, preferably 9% or more and 12.5% ​​or less, and more preferably 10% or more and 12% or less. 2 O 3 By making the total content of Al and rare earth oxide fall within this range, the liquidus temperature can be lowered, making it easier to manufacture. 2 O 3 The total content of Al and rare earth oxides is the ratio of Al to the total content of the glass 10. 2 O 3 The glass 10 is a glass having a content of Al and a content of rare earth oxides. 2 O 3 The present invention is not limited to containing both Al and rare earth oxides. 2 O 3 The total content of Al and rare earth oxides is, for example, when no rare earth oxides are contained, 2 O 3refers to the content of Al 2 O 3 When no rare earth oxide is contained, the content of rare earth oxide refers to the content of the rare earth oxide. When multiple rare earth oxides are contained, the content of rare earth oxide refers to the total content of those rare earth oxides.

[0015] (Parameter A) SiO in glass 10, expressed in mole percent on an oxide basis 2 and Al 2 O 3 and ΣRO in Glass 10 2 O 3 The ratio of the total content of ΣRO and ΣRO ((Al 2 O 3 +ΣRO) / (SiO 2 +Al 2 O 3 +ΣRO)) is defined as parameter A. Here, ΣRO is the total content of divalent oxides. When multiple types of divalent oxides are contained, the total content of divalent oxides refers to the total content of those divalent oxides, and when only one type of divalent oxide is contained, it refers to the content of that divalent oxide. The parameter A of the glass 10 is preferably 0.38 or more, more preferably 0.39 or more and 0.5 or less, more preferably 0.395 or more and 0.495 or less, more preferably 0.4 or more and 0.49 or less, more preferably 0.405 or more and 0.485 or less, more preferably 0.41 or more and 0.48 or less, more preferably 0.415 or more and 0.475 or less, more preferably 0.42 or more and 0.47 or less, more preferably 0.425 or more and 0.465 or less, more preferably 0.43 or more and 0.46 or less, more preferably 0.435 or more and 0.455 or less, and more preferably 0.44 or more and 0.45 or less. When the parameter A is within this range, the melting temperature of the glass 10 can be lowered, making it easier to manufacture. Note that the glass 10 contains SiO 2 and Al 2 O 3 The present invention is not limited to including all of the divalent oxides, such as SiO 2 When it does not contain (SiO 2 +Al 2O 3 +ΣRO) 2 is treated as zero. Similarly, Al 2 O 3 If it does not contain (Al 2 O 3 +ΣRO) and (SiO 2 +Al 2 O 3 +ΣRO) 2 O 3 Similarly, if no divalent oxides are included, (Al 2 O 3 +ΣRO) and (SiO 2 +Al 2 O 3 +ΣRO) is treated as zero.

[0016] (Al 2 O 3 ) Al 2 O 3 has the effect of increasing the Young's modulus, suppressing deflection, and suppressing phase separation of the glass. 2 O 3 Does not contain (Al 2 O 3 The content of Al may be 0 mol %, 2 O 3 It may also contain Al 2 O 3 By making the content of Al 20% or less, it is possible to prevent the liquidus temperature from becoming high. 2 O 3 The content of Al is preferably 5% or more and 20% or less, preferably 6% or more and 18% or less, preferably 7% or more and 17% or less, preferably 8% or more and 16% or less, preferably 8.5% or more and 15% or less, preferably 9% or more and 14% or less, preferably 9.5% or more and 13% or less, preferably 10% or more and 12% or less, and more preferably 10.5% or more and 11% or less. 2 O 3 When the content falls within this range, warping can be suppressed and manufacturing can be facilitated.

[0017] (MgO) MgO increases Young's modulus without increasing density, and thus, by increasing the specific elastic modulus, deflection can be suppressed. It also has the effect of reducing the linear thermal expansion coefficient. On the other hand, by setting the MgO content to 30% or less, the liquidus temperature can be controlled low. Therefore, the glass 10 may not contain MgO (the MgO content is 0 mol%), but may also contain MgO. The MgO content of glass 10, expressed in mole percent on an oxide basis, is preferably 1% to 30%, more preferably 5% to 29.5%, more preferably 9% to 29%, more preferably 10% to 28.5%, more preferably 11% to 28%, more preferably 12% to 27.5%, more preferably 13% to 27%, more preferably 14% to 26.5%, more preferably 15% to 26%, more preferably 16% to 25.5%, more preferably 17% to 25%, more preferably 18% to 24.5%, more preferably 19% to 24%, more preferably 19.5% to 23.5%, and more preferably 20% to 23%. Having the MgO content within this range facilitates manufacturing while suppressing warping.

[0018] (CaO) CaO has the characteristic of increasing the specific elastic modulus second only to MgO among oxides of Group 2 elements, while not excessively reducing the linear thermal expansion coefficient. Furthermore, compared to MgO, it also has the characteristic of being less likely to increase the liquidus temperature. Therefore, glass 10 may be CaO-free (CaO content is 0 mol%), but it may also contain CaO. By reducing the CaO content to 10% or less, an increase in the linear thermal expansion coefficient can be suppressed and the liquidus temperature can be controlled low. The CaO content of glass 10, expressed in mol% based on oxide, is preferably 0.01% to 10% or less, more preferably 0.5% to 9%, more preferably 1% to 8%, more preferably 1.5% to 7%, more preferably 1.65% to 6%, more preferably 1.8% to 5%, and even more preferably 2% to 4%. The CaO content may be 0.5% or more and 2% or less, or 1% or more and 1.5% or less. When the CaO content is in this range, warping can be suppressed and manufacturing can be facilitated.

[0019] (SrO) SrO has the effect of improving the meltability of glass and lowering the liquidus temperature. Therefore, glass 10 may be free of SrO (SrO content is 0 mol%), but may also contain SrO. By controlling the SrO content to 10% or less, an increase in the linear thermal expansion coefficient can be suppressed and the liquidus temperature can be controlled low. In glass 10, the SrO content, expressed in mol% on an oxide basis, is preferably 0.01% to 10% or less, more preferably 0.5% to 9% or less, more preferably 1% to 8% or less, more preferably 1.5% to 7% or less, more preferably 1.65% to 6% or less, more preferably 1.8% to 5% or less, and more preferably 2% to 4% or less. Furthermore, the SrO content may be 0.5% to 2% or less, or may be 1% to 1.5% or less. By controlling the SrO content within this range, manufacturing can be facilitated while suppressing distortion.

[0020] (BaO) BaO has the effect of improving the meltability of glass and lowering the liquidus temperature. Therefore, glass 10 may be BaO-free (BaO content is 0 mol%), or may contain BaO. By keeping the BaO content at 10% or less, an increase in the linear thermal expansion coefficient can be suppressed and the liquidus temperature can be controlled low. The BaO content of glass 10, expressed in mol% on an oxide basis, is preferably 0.01% to 10% or less, more preferably 0.5% to 9% or less, more preferably 1% to 8% or less, more preferably 1.5% to 7% or less, more preferably 1.65% to 6% or less, more preferably 1.8% to 5% or less, and more preferably 2% to 4% or less. Furthermore, the BaO content may be 0.5% to 2% or less, or may be 1% to 1.5% or less. By keeping the BaO content within this range, manufacturing can be facilitated while suppressing distortion. Furthermore, by reducing the BaO content, it is possible to suppress the occurrence of cloudy defects on the surface when the glass is immersed in acid. Therefore, glass 10 may contain BaO, but it may not contain BaO. In glass 10, the BaO content, expressed in mole percent on an oxide basis, is preferably 10% or less, preferably 5% or less, preferably 3% or less, preferably 1% or less, preferably 0.8% or less, preferably 0.5% or less, more preferably 0.3% or less, and even more preferably 0.1% or less. By having the BaO content within this range, it is possible to suppress cloudy defects and improve the sulfuric acid resistance of the glass.

[0021] (Li 2 O) Li 2 Among alkali metal oxides, O has the effect of improving the solubility without decreasing the linear thermal expansion coefficient. 2 O-free (Li 2 The content of O may be 0 mol%, but 2 It may contain O. 2By setting the O content to 5% or less, the Young's modulus can be increased and the linear thermal expansion coefficient can be prevented from increasing. 2 The O content is preferably 0.01% or more and 5% or less, more preferably 0.1% or more and 4% or less, more preferably 0.15% or more and 3% or less, more preferably 0.2% or more and 2% or less, more preferably 0.25% or more and 1.5% or less, and more preferably 0.3% or more and 1% or less. 2 When the O content falls within this range, warping can be suppressed and manufacturing can be facilitated.

[0022] (Na 2 O) Na 2 Among alkali metal oxides, O has the effect of improving the solubility of glass and lowering the liquidus temperature. 2 No O content (Na 2 The content of O may be 0 mol%, but Na 2 It may contain O. 2 By keeping the O content at 5% or less, the Young's modulus can be increased and the linear thermal expansion coefficient can be prevented from increasing. 2 The O content is preferably 0.01% or more and 5% or less, more preferably 0.1% or more and 4% or less, more preferably 0.15% or more and 3% or less, more preferably 0.2% or more and 2% or less, more preferably 0.25% or more and 1.5% or less, and more preferably 0.3% or more and 1% or less. 2 When the O content falls within this range, warping can be suppressed and manufacturing can be facilitated.

[0023] (K 2 O) K 2 O has the effect of improving the melting property of the glass and lowering the liquidus temperature. 2 No O content (K 2 The content of O may be 0 mol%, but 2 It may contain O. 2By keeping the O content at 5% or less, the Young's modulus can be increased and the linear thermal expansion coefficient can be prevented from increasing. 2 The O content is preferably 0.01% or more and 5% or less, more preferably 0.1% or more and 4% or less, more preferably 0.15% or more and 3% or less, more preferably 0.2% or more and 2% or less, more preferably 0.25% or more and 1.5% or less, and more preferably 0.3% or more and 1% or less. 2 When the O content falls within this range, warping can be suppressed and manufacturing can be facilitated.

[0024] Glass 10 may contain alkali metal components, but preferably does not. The total content of alkali metal components in glass 10, expressed in mole percent on an oxide basis, is preferably 1% or less, more preferably 0.001% to 0.1%, even more preferably 0.003% to 0.05%, and even more preferably 0.005% to 0.01%. Such a low total content of alkali metal components can suppress deterioration of the properties of metal or oxide coatings applied to the glass surface during manufacturing processes such as FOWLP. Here, alkali metal components refer to Group 1 metals, such as Li, Na, K, and Rb, or their oxides contained in glass 10.

[0025] (ZnO) ZnO has the effect of improving the meltability of glass and increasing the Young's modulus. Therefore, glass 10 may be ZnO-free (ZnO content is 0 mol%), but it may also contain ZnO. By keeping the ZnO content at 10% or less, an increase in the linear thermal expansion coefficient can be suppressed and the liquidus temperature can be controlled. The ZnO content of glass 10, expressed in mole percent on an oxide basis, is preferably 0.01% to 10% or less, more preferably 0.1% to 9% or less, more preferably 0.2% to 8% or less, more preferably 0.4% to 7% or less, more preferably 0.6% to 6% or less, more preferably 0.8% to 5% or less, and more preferably 1% to 4% or less. By keeping the ZnO content within this range, manufacturing can be facilitated while suppressing deflection.

[0026] (P 2 O 5 ) P 2 O 5 has the effect of improving the melting property of the glass and lowering the linear thermal expansion coefficient. 2 O 5 Does not contain (P 2 O 5 The content of P may be 0 mol %, 2 O 5 It may contain P 2 O 5 By making the content of P 5% or less, it is possible to increase the Young's modulus without deteriorating the chemical resistance and to suppress an increase in the linear thermal expansion coefficient. 2 O 5 The content of is preferably 0.01% or more and 5% or less, more preferably 0.1% or more and 4% or less, more preferably 0.15% or more and 3% or less, more preferably 0.2% or more and 2% or less, more preferably 0.25% or more and 1.5% or less, and more preferably 0.3% or more and 1% or less. 2 O 5 When the content falls within this range, warping can be suppressed and manufacturing can be facilitated.

[0027] (ZrO2 ) ZrO 2 can increase the Young's modulus without reducing the linear thermal expansion coefficient. 2 has the effect of improving the acid resistance and sulfuric acid resistance of the glass. 2 Does not contain (ZrO 2 The content of ZrO may be 0 mol %, 2 It may contain ZrO 2 The liquidus temperature can be controlled by making the content of 10% or less. 2 The content of ZrO is preferably 0.01% or more and 10% or less, more preferably 0.2% or more and 7% or less, more preferably 0.5% or more and 4% or less, more preferably 0.7% or more and 4% or less, and even more preferably 1% or more and 2% or less. 2 When the content falls within this range, warping can be suppressed and manufacturing can be facilitated.

[0028] (TiO 2 ) TiO 2 can increase the Young's modulus without relatively decreasing the linear thermal expansion coefficient. 2 has the effect of improving the acid resistance and sulfuric acid resistance of the glass. 2 Does not contain (TiO 2 The content of TiO may be 0 mol %, 2 It may contain TiO 2 The liquidus temperature can be controlled by making the content of 10% or less. 2 The content of TiO is preferably 0.01% or more and 10% or less, more preferably 0.2% or more and 7% or less, more preferably 0.5% or more and 4% or less, more preferably 0.7% or more and 4% or less, and even more preferably 1% or more and 2% or less. 2 When the content falls within this range, warping can be suppressed and manufacturing can be facilitated.

[0029] (Y 2 O3 ) Y 2 O 3 has the effect of improving the melting property of the glass and increasing the Young's modulus. 2 O 3 Does not contain (Y 2 O 3 The content of Y may be 0 mol %, 2 O 3 Y 2 O 3 The linear thermal expansion coefficient can be controlled by making the content of Y 7% or less. 2 O 3 The content of Y is preferably 0.1% or more and 7% or less, more preferably 0.7% or more and 6% or less, more preferably 1% or more and 5% or less, more preferably 1.5% or more and 4% or less, and more preferably 2% or more and 3% or less. 2 O 3 When the content falls within this range, warping can be suppressed and manufacturing can be facilitated.

[0030] (Gd 2 O 3 ) Gd 2 O 3 has the effect of improving the melting property of the glass and increasing the Young's modulus. 2 O 3 Non-containing (Gd 2 O 3 The content of Gd may be 0 mol %, 2 O 3 It may contain Gd 2 O 3 The coefficient of linear thermal expansion can be controlled by making the content of Gd 7% or less. 2 O 3 The content of Gd is preferably 0.1% or more and 7% or less, more preferably 0.7% or more and 6% or less, more preferably 1% or more and 5% or less, more preferably 1.5% or more and 4% or less, and more preferably 2% or more and 3% or less. 2 O 3When the content falls within this range, warping can be suppressed and manufacturing can be facilitated.

[0031] (La 2 O 3 ) La 2 O 3 has the effect of improving the melting property of the glass and increasing the Young's modulus. 2 O 3 Does not contain (La 2 O 3 The content of La may be 0 mol%, 2 O 3 It may contain La 2 O 3 The linear thermal expansion coefficient can be controlled by making the content of La 7% or less. 2 O 3 The content of La is preferably 0.1% or more and 7% or less, more preferably 0.7% or more and 6% or less, more preferably 1% or more and 5% or less, more preferably 1.5% or more and 4% or less, and more preferably 2% or more and 3% or less. 2 O 3 When the content falls within this range, warping can be suppressed and manufacturing can be facilitated.

[0032] (W.O. 3 ) WO 3 has the effect of improving the melting property of the glass and increasing the Young's modulus. 3 Does not contain (WO 3 The content of WO may be 0 mol %. 3 It may contain WO 3 By making the content of WO 7% or less, it is possible to suppress an increase in the linear thermal expansion coefficient and control the liquidus temperature. 3 The content of WO is preferably 0.1% or more and 7% or less, more preferably 0.3% or more and 5% or less, more preferably 0.5% or more and 3% or less, more preferably 0.8% or more and 2.5% or less, and more preferably 1% or more and 2% or less. 3When the content falls within this range, warping can be suppressed and manufacturing can be facilitated.

[0033] (Ta 2 O 5 ) Ta 2 O 5 has the effect of lowering the linear thermal expansion coefficient and increasing the Young's modulus. 2 O 5 has the effect of improving the acid resistance and sulfuric acid resistance of the glass. 2 O 5 Does not contain (Ta 2 O 5 The content of Ta may be 0 mol %, 2 O 5 It may contain Ta 2 O 5 The liquidus temperature can be controlled by making the content of Ta 10% or less. 2 O 5 The content of Ta is preferably 0.1% or more and 10% or less, more preferably 0.5% or more and 5% or less, more preferably 1% or more and 4% or less, more preferably 1.5% or more and 3.5% or less, and more preferably 2% or more and 3% or less. 2 O 5 When the content falls within this range, warping can be suppressed and manufacturing can be facilitated.

[0034] (MnO) MnO has the effect of increasing the Young's modulus. However, MnO may increase the liquidus temperature, and even a small amount of MnO can cause the glass to be colored dark brown to black. Therefore, it is preferable that glass 10 does not contain MnO. The MnO content of glass 10, expressed in mole percent on an oxide basis, is preferably 5% or less, preferably 3% or less, preferably 0.1% or less, more preferably 0.001% or more and 0.05% or less, and even more preferably 0.005% or more and 0.01% or less. By keeping the MnO content within this range, a decrease in light transmittance can be suppressed.

[0035] (PbO) PbO has the effect of increasing Young's modulus, but is an oxide that places a heavy burden on the environment. Therefore, it is preferable that glass 10 does not contain PbO. In glass 10, the PbO content, expressed in mole percent based on oxide, is preferably 0.1% or less, more preferably 0.05% or less, and even more preferably 0.01% or less. By keeping the PbO content within this range, the environmental burden can be reduced.

[0036] (Fe 2 O 3 ) Glass 10 is Fe 2 O 3 It is preferable that the glass 10 does not contain Fe as an external percentage, expressed as mass % on an oxide basis. 2 O 3 The content of Fe is preferably 0.1% or less, more preferably 0.001% or more and 0.05% or less, and even more preferably 0.005% or more and 0.01% or less. 2 O 3 Such a low content of Fe can suppress the decrease in light transmittance. 2 O 3 The content of Fe is based on the oxide. 2 O 3 Fe contained in glass 10 relative to the total mass of all components of glass 10 excluding 2 O 3 It refers to the mass ratio of

[0037] (Y 2 O 3 +Gd 2 O 3 +La 2 O 3 +Nd 2 O 3 +Ta 2 O 5 +Nb 2 O 5 Glass 10 contains, in mole percent on an oxide basis, Y 2 O 3 and G-d 2 O 3 and La 2 O 3 and Nd 2 O 3 and Ta2 O 5 and Nb 2 O 5 The total content of (Y 2 O 3 +Gd 2 O 3 +Ta 2 O 5 +La 2 O 3 +Nd 2 O 3 +Nb 2 O 5 ) is preferably 0.5% or more, more preferably 1% to 10%, more preferably 2% to 8%, more preferably 3% to 7%, and even more preferably 4% to 6%. The total content of these components may be 1% to 4%, or 1.5% to 2%. When the total content of these components is within this range, manufacturing can be facilitated while suppressing deflection. Note that glass 10 does not need to contain all of the above components, and may contain only some of the components. Also, glass 10 may not contain any of the above components. That is, for example, Y 2 O 3 If Y is not included, 2 O 3 +Gd 2 O 3 +Ta 2 O 5 +La 2 O 3 +Nd 2 O 3 +Nb 2 O 5 ) in (Y 2 O 3 ) is treated as zero, and the same applies if no other components are included.

[0038] ((Al 2 O 3 +MgO) / (SiO 2 +Al 2 O 3 +B 2 O 3 + MgO)) Glass 10 contains, in mole percent on an oxide basis, SiO 2 and Al2 O 3 and B 2 O 3 and MgO and the total content of Al 2 O 3 The ratio of the total content of Al and MgO ((Al 2 O 3 +MgO) / (SiO 2 +Al 2 O 3 +B 2 O 3 The total content of these components in this range can increase Young's modulus and suppress deflection. Note that glass 10 contains SiO 2 and Al 2 O 3 and B 2 O 3 and MgO. 2 O 3 If it does not contain (Al 2 O 3 +MgO) and (SiO 2 +Al 2 O 3 +B 2 O 3 +MgO) 2 O 3 ) is treated as zero, and the same applies if no other components are included.

[0039] (MgO / ΣRO) In glass 10, the ratio of the MgO content (MgO / ΣRO) to the total content of divalent oxides (ΣRO), expressed in mole percent on an oxide basis, is preferably 0.3 to 1, more preferably 0.4 to 0.9, more preferably 0.45 to 0.875, more preferably 0.5 to 0.85, more preferably 0.55 to 0.825, and even more preferably 0.6 to 0.8. It may also be 0.75% to 0.95%, or 0.8% to 0.9%. By having the total content of these components fall within this range, the linear thermal expansion coefficient can be reduced, thereby suppressing deflection. Note that glass 10 is not limited to containing divalent oxides such as MgO. For example, if MgO is not contained, the MgO in (MgO / ΣRO) is treated as zero, and if divalent oxides other than MgO are not contained, the content of divalent oxides other than MgO in (MgO / ΣRO) is treated as zero.

[0040] (Value of N) In glass 10, the number N of oxides contained in glass 10 that has a content of 0.5% or more is preferably 5 or more, more preferably 7 or more, more preferably 8 or more, more preferably 9 or more, and even more preferably 10 or more. Such a high value of N allows the liquidus temperature to be lowered, making production easier.

[0041] It is preferable that the glass 10 does not contain a sintered body. In other words, the glass 10 is preferably a glass that is not a sintered body. The term "sintered body" as used herein refers to a component in which a plurality of particles are heated at a temperature lower than the melting point to bond the particles together. Sintered bodies have a relatively high porosity due to the inclusion of pores, but the glass 10 is not a sintered body and therefore has a low porosity, typically 0%. However, the inclusion of unavoidable traces of pores is permitted. The porosity here refers to the so-called true porosity, which is the sum of the volumes of pores (voids) that are open to the outside and pores (voids) that are not open to the outside, divided by the total volume (apparent volume). The porosity can be measured, for example, according to JIS R 1634:1998, "Method for measuring the density and open porosity of sintered fine ceramics."

[0042] The glass used for the glass 10 is preferably amorphous glass, i.e., an amorphous solid. This glass may be crystallized glass containing crystals on the surface or inside, but amorphous glass is preferred from the viewpoint of density. Among ceramics, those produced by sintering methods are preferably not used because they have low transmittance and high density.

[0043] (Shape of Glass) Next, the shape of the glass 10 will be described. As shown in FIG. 1 , the glass 10 is a plate-shaped glass substrate including a surface 12, which is one main surface, and a surface 14, which is the main surface opposite to the surface 12. The surface 14 may be parallel to the surface 12, for example. The glass 10 may have a circular disk shape when viewed in a plan view, i.e., from a direction perpendicular to the surface 12. However, the shape is not limited to a disk and may be any shape, such as a polygonal plate such as a rectangle. Note that the above shapes also include those having a notch or orientation flat provided on the outer periphery.

[0044] Furthermore, the thickness D of the glass 10, i.e., the length between the surface 12 and the surface 14, is preferably 0.1 mm or more and 5.0 mm or less, more preferably 0.1 mm or more and 2.0 mm or less, and even more preferably 0.1 mm or more and 0.5 mm or more. By setting the thickness D to 0.1 mm or more, the glass 10 can be prevented from becoming too thin, thereby suppressing breakage due to bending or impact. By setting the thickness D to 2.0 mm or less, the glass can be prevented from becoming too heavy, and by setting the thickness D to 0.5 mm or less, the glass can be further prevented from becoming too heavy.

[0045] (Glass Characteristics) Next, the characteristics of the glass 10 will be described.

[0046] (Young's modulus) The Young's modulus E of the glass 10 is preferably 80 GPa or more, more preferably 85 GPa to 180 GPa, more preferably 88 GPa to 170 GPa, more preferably 90 GPa to 160 GPa, more preferably 93 GPa to 150 GPa, more preferably 95 GPa to 145 GPa, more preferably 97 GPa to 140 GPa, more preferably 98 GPa to 135 GPa, and even more preferably 99 GPa to 130 GPa. By setting the Young's modulus E within this range, deflection can be appropriately suppressed. If the Young's modulus is too high, cutting, grinding, and polishing become difficult.

[0047] (Young's Modulus Parameter) The Young's modulus parameter Y of the glass 10 calculated from the composition is preferably 0.8 or more, more preferably 0.85 to 1.8, more preferably 0.88 to 1.7, more preferably 0.9 to 1.6, more preferably 0.93 to 1.5, more preferably 0.95 to 1.45, more preferably 0.97 to 1.4, more preferably 0.98 to 1.35, and even more preferably 0.99 to 1.3. By setting the Young's modulus parameter within this range, deflection can be appropriately suppressed. The Young's modulus parameter Y is calculated from the following formula (1):

[0048] Y=(123-0.54[SiO 2 ]+0.3[Al 2 O 3 ]−1.15[B 2 O 3 ]+0.21[MgO]-0.2[CaO]-0.1[SrO]-1.2[BaO]+[Li 2 O]-2.8[K 2 O]+0.05[ZnO]+1.46[ZrO 2 ]-0.05[TiO 2 ]+1.6[Y 2 O 3 " + 1.35 [Gd 2 O 3 ]+1.37[La 2 O 3 ]+[Ta 2 O 5 ]) / 100 ... (1)

[0049] The oxide R contained in the glass 10 in terms of mole percent based on oxides is x O y (R is an element constituting the oxide, and x and y are any integers) content is [R x O y The content here is expressed as the percentage of oxide R relative to the entire glass 10 in mole percent based on oxide. x O y That is, for example, in formula (1), [SiO 2 ] is the SiO 2 content relative to the entire glass 10 in mole percent on an oxide basis. 2 The ratio of the content of the oxides represented by formula (1) is inclusive. Furthermore, glass 10 does not necessarily contain all of the oxides represented by formula (1). In formula (1), the content of oxides not contained in glass 10 is treated as 0. Furthermore, glass 10 may contain components other than the oxides represented by formula (1).

[0050] (Linear Thermal Expansion Coefficient) The linear thermal expansion coefficient α of the glass 10 is preferably 6 ppm / ° C. or less, more preferably 3 ppm / ° C. or more and 5.9 ppm / ° C. or less, more preferably 3.5 ppm / ° C. or more and 5.8 ppm / ° C. or less, more preferably 4 ppm / ° C. or more and 5.7 ppm / ° C. or less, more preferably 4.2 ppm / ° C. or more and 5.6 ppm / ° C. or less, more preferably 4.4 ppm / ° C. or more and 5.5 ppm / ° C. or less, more preferably 4.6 ppm / ° C. or more and 5.4 ppm / ° C. or less, and even more preferably 4.8 ppm / ° C. or more and 5.3 ppm / ° C. or less. The linear thermal expansion coefficient α of the glass 10 may be in the following range. The linear thermal expansion coefficient α of glass 10 is preferably 6.5 ppm / ° C. or less, more preferably 3 ppm / ° C. to 6.4 ppm / ° C., more preferably 3.5 ppm / ° C. to 6.3 ppm / ° C., more preferably 4 ppm / ° C. to 6.2 ppm / ° C., more preferably 4.5 ppm / ° C. to 6.1 ppm / ° C., more preferably 5 ppm / ° C. to 6 ppm / ° C., more preferably 5.5 ppm / ° C. to 5.9 ppm / ° C., more preferably 5.6 ppm / ° C. to 5.85 ppm / ° C., and even more preferably 5.7 ppm / ° C. to 5.8 ppm / ° C. In addition, the linear thermal expansion coefficient α of glass 10 may be in the following range. The linear thermal expansion coefficient α of the glass 10 is preferably 5.0 ppm / °C or less, more preferably 3.6 ppm / °C to 4.9 ppm / °C, more preferably 3.7 ppm / °C to 4.8 ppm / °C, more preferably 3.8 ppm / °C to 4.7 ppm / °C, more preferably 3.85 ppm / °C to 4.65 ppm / °C, more preferably 3.9 ppm / °C to 4.6 ppm / °C, more preferably 3.95 ppm / °C to 4.55 ppm / °C, more preferably 4 ppm / °C to 4.5 ppm / °C, more preferably 4.1 ppm / °C to 4.45 ppm / °C, and even more preferably 4.2 ppm / °C to 4.4 ppm / °C. By setting the linear thermal expansion coefficient within this range, deflection can be appropriately suppressed. The linear thermal expansion coefficient α is the average thermal expansion coefficient in the range of 50° C. to 200° C., and is a value measured in accordance with DIN-51045-1 as a standard for thermal expansion measurement.For example, a thermal expansion meter DIL 402 Expedis Supreme manufactured by NETZSCH is used as the measuring device to measure in the range of 30°C to 300°C, and the average thermal expansion coefficient in the range of 50°C to 200°C may be taken as the linear thermal expansion coefficient.

[0051] (Thermal Expansion Parameter) The thermal expansion parameter C of glass 10 calculated from the composition is preferably 1.2 or less, more preferably 0.6 to 1.18, more preferably 0.7 to 1.16, more preferably 0.8 to 1.14, more preferably 0.84 to 1.12, more preferably 0.88 to 1.1, more preferably 0.92 to 1.08, and even more preferably 0.96 to 1.06. The thermal expansion parameter C of glass 10 may also be in the following ranges. The thermal expansion parameter C is preferably 1.3 or less, more preferably 0.6 to 1.28, more preferably 0.7 to 1.26, more preferably 0.8 to 1.24, more preferably 0.9 to 1.22, more preferably 1 to 1.2, more preferably 1.1 to 1.18, more preferably 1.12 to 1.17, and even more preferably 1.14 to 1.16. In addition, the thermal expansion parameter C of the glass 10 may be in the following range. The thermal expansion parameter C is preferably 1.0 or less, more preferably 0.72 to 0.98, more preferably 0.74 to 0.96, more preferably 0.76 to 0.94, more preferably 0.77 to 0.93, more preferably 0.78 to 0.92, more preferably 0.79 to 0.91, more preferably 0.8 to 0.9, more preferably 0.82 to 0.89, and even more preferably 0.84 to 0.88. By setting the thermal expansion parameter C in this range, the linear thermal expansion coefficient can be kept low and deflection can be appropriately suppressed. The thermal expansion parameter C is calculated from the following formula (2):

[0052] C=(14.098-0.1245[SiO 2 ]-0.131[Al 2 O 3 ]−0.101[B 2 O 3]-0.051[MgO]+0.013[CaO]+0.053[SrO]+0.018[BaO]+0.041[Li 2 O]+0.395[Na 2 O]-0.066[ZnO]-0.033[ZrO 2 ]-0.072[TiO 2 ]+0.035[Y 2 O 3 ]+0.074[Gd 2 O 3 ]+0.074[La 2 O 3 ]-0.091[Ta 2 O 5 ]) / 5 ... (2)

[0053] Glass 10 does not need to contain all of the oxides represented by formula (2). In formula (2), the content of oxides not contained in glass 10 is treated as 0. Furthermore, glass 10 may contain components other than the oxides represented by formula (2).

[0054] (Liquidus temperature) Liquidus temperature T of glass 10 L is preferably 1,300°C or lower, more preferably 800°C or higher and 1,290°C or lower, more preferably 825°C or higher and 1,280°C or lower, more preferably 850°C or higher and 1,270°C or lower, more preferably 875°C or higher and 1,260°C or lower, more preferably 900°C or higher and 1,250°C or lower, more preferably 925°C or higher and 1,240°C or lower, more preferably 950°C or higher and 1,230°C or lower, more preferably 975°C or higher and 1,220°C or lower, more preferably 1,000°C or higher and 1,210°C or lower, and even more preferably 1,200°C or lower. By setting the liquidus temperature within this range, production can be facilitated. The liquidus temperature can be evaluated by placing glass particles that pass through a sieve with a mesh width of 4.0 mm but do not pass through a sieve with a mesh width of 2.3 mm on a platinum dish, holding the sieve for 1 hour in an electric furnace set at a predetermined temperature, and measuring the temperature at which crystals precipitate.

[0055] (Liquidus Parameter) The liquidus parameter L of glass 10 calculated from the composition is preferably 10.5 or less, more preferably 6.4 or more and 10.4 or less, more preferably 7.2 or more and 10.3 or less, more preferably 7.6 or more and 10.2 or less, more preferably 7.7 or more and 10.1 or less, more preferably 7.8 or more and 10 or less, more preferably 7.9 or more and 9.9 or less, and even more preferably 8 or more and 9.8 or less. Setting the liquidus parameter L within this range makes it possible to maintain a low liquidus temperature and facilitate production. The liquidus parameter L is calculated from the following formula (3):

[0056] L=(-642.5+20.6[SiO 2 ]+31.9[Al 2 O 3 ]+2.85[B 2 O 3 ]+11.24[MgO]+17.3[CaO]+1.75[SrO]+31.41[BaO]-6.86[Li 2 O]+37.96[K 2 O]+11.47[ZnO]+25.83[ZrO 2 ]+41.0[TiO 2 ]+12.32[Y 2 O 3 ]−1.18[Gd 2 O 3 ]−1.18[La 2 O 3 ]+24.46[Ta 2 O 5 ]) / 125 ... (3)

[0057] Glass 10 does not necessarily contain all of the oxides represented by formula (3). In formula (3), the content of oxides not contained in glass 10 is treated as 0. Furthermore, glass 10 may contain components other than the oxides represented by formula (3).

[0058] (melting temperature T 2 , working temperature T 3 , molding temperature T 4 ) Melting temperature T of glass 10 2is preferably 1000°C or higher and 1550°C or lower, more preferably 1100°C or higher and 1500°C or lower, more preferably 1150°C or higher and 1450°C or lower, more preferably 1200°C or higher and 1400°C or lower, and even more preferably 1250°C or higher and 1350°C or lower. 2 The viscosity η is 10 2 The melting temperature T 2 This relatively low temperature makes it easier to melt. 3 is preferably 1000°C or higher and 1400°C or lower, more preferably 1050°C or higher and 1350°C or lower, more preferably 1080°C or higher and 1300°C or lower, more preferably 1100°C or higher and 1250°C or lower, and more preferably 1130°C or higher and 1200°C or lower. 3 The viscosity η is 10 3 The temperature at which the viscosity becomes dPa·s. 3 Such a relatively low temperature makes it easy to form the glass 10. 4 The molding temperature T is preferably 900°C or higher and 1250°C or lower, more preferably 950°C or higher and 1200°C or lower, more preferably 1000°C or higher and 1150°C or lower, and even more preferably 1030°C or higher and 1100°C or lower. 4 The viscosity η is 10 4 The temperature at which the viscosity becomes dPa·s. Molding temperature T 4 Such a relatively low melting temperature T 2 , working temperature T 3 , molding temperature T 4 can be measured by the inner cylinder rotation method or the like.

[0059] (Glass Transition Temperature) The glass transition temperature of the glass 10 is preferably 600° C. or higher and 850° C. or lower, more preferably 620° C. or higher and 800° C. or lower, more preferably 640° C. or higher and 780° C. or lower, more preferably 660° C. or higher and 760° C. or lower, more preferably 680° C. or higher and 740° C. or lower, more preferably 690° C. or higher and 730° C. or lower, and even more preferably 695° C. or higher and 720° C. The glass transition temperature can be measured according to the method specified in JIS R3103-3:2001 "Viscosity and viscosity fixed points of glass - Part 3: Method for measuring transition temperature by thermal expansion method."

[0060] (Density) The density of the glass 10 is 2.6 g / cm 3 3.6g / cm or more 3 Preferably, 2.7 g / cm or less 3 3.4g / cm or more 3 More preferably, 2.75 g / cm 3 3.35g / cm or more 3 More preferably, 2.8 g / cm or less 3 3.3g / cm or more 3 More preferably, 2.85 g / cm 3 3.25g / cm or more 3 More preferably, 2.9 g / cm 3 3.2g / cm or more 3 The following is even more preferred:

[0061] (Liquidus Viscosity) Liquidus viscosity log η of Glass 10 L The viscosity (dPa s) is preferably 2 or more and 7 or less, more preferably 2.2 or more and 6.5 or less, more preferably 2.4 or more and 6 or less, more preferably 2.6 or more and 5.5 or less, more preferably 2.8 or more and 5 or less, more preferably 2.9 or more and 4.5 or less, and more preferably 3 or more and 4.2 or less. The liquidus viscosity refers to the viscosity of glass 10 at the liquidus temperature. Such a relatively high liquidus temperature makes production easier. The liquidus viscosity can be determined by measuring a temperature-viscosity curve using an inner cylinder rotation method or the like and calculating the viscosity at the liquidus temperature.

[0062] (Fracture toughness value) Fracture toughness value K of glass 10 ICis 0.5 MPa m 0.5 2MPa・m or more 0.5 Preferably, 0.7 MPa m or less 0.5 1.5MPa・m or more 0.5 More preferably, 0.8 MPa m 0.5 1.4MPa・m or more 0.5 More preferably, 0.9 MPa m 0.5 1.3MPa・m or more 0.5 The following is more preferable: Fracture toughness value K IC When the fracture toughness value K is within this range, breakage of the glass 10 can be suppressed. IC It can be measured using a pre-crack introduction fracture test method (SEPB method: Single-Edge-Precracked-Beam method) as defined in, for example, JIS R1607:2015 “Room temperature fracture toughness test method for fine ceramics”.

[0063] (Light Transmittance) The internal transmittance of glass 10 having a thickness D of 0.7 mm for light (ultraviolet rays) with a wavelength of 308 nm is preferably 30% or more, more preferably 35% or more, even more preferably 40% or more, even more preferably 45% or more, even more preferably 50% or more, even more preferably 55% or more, and even more preferably 60% or more. Having a transmittance for light with a wavelength of 308 nm within this range allows for appropriate transmission of ultraviolet rays. Furthermore, the internal transmittance of glass 10 having a thickness D of 0.7 mm for light with a wavelength of 350 nm (ultraviolet rays) is preferably 30% or more, more preferably 40% or more, even more preferably 50% or more, even more preferably 60% or more, even more preferably 70% or more, even more preferably 75% or more, and even more preferably 77% or more. Having a transmittance for light with a wavelength of 350 nm within this range allows for appropriate transmission of ultraviolet rays. Furthermore, the internal transmittance of glass 10 having a thickness D of 0.7 mm for light with a wavelength of 550 nm (visible light) is preferably 70% or more, more preferably 75% or more, even more preferably 80% or more, even more preferably 85% or more, even more preferably 86% or more, even more preferably 87% or more, and even more preferably 88% or more. Having a transmittance for light with a wavelength of 550 nm within this range allows for appropriate transmission of visible light. Furthermore, the internal transmittance of glass 10 having a thickness D of 0.7 mm for light with a wavelength of 1064 nm (infrared light) is preferably 80% or more, more preferably 85% or more, and even more preferably 90% or more. Having a transmittance for light with a wavelength of 1064 nm within this range allows for appropriate transmission of infrared light. The transmittance can be measured by measuring a spectral transmittance curve using a spectrophotometer or the like.

[0064] (Sulfuric acid resistance) When the glass 10 was exposed to acid (sulfuric acid), the weight change (weight loss) was 0.20 mg / cm 2 Preferably, it is 0.10 mg / cm or less. 2 Preferably, it is 0.050 mg / cm or less. 2 Preferably, it is 0.030 mg / cm or less. 2Preferably, it is 0.020 mg / cm or less. 2 Preferably, it is 0.015 mg / cm or less. 2 Preferably, it is 0.010 mg / cm or less. 2 Preferably, it is 0.008 mg / cm or less. 2 Preferably, it is 0.005 mg / cm or less. 2 It is preferable that the concentration is 0.003 mg / cm or less. 2 It is even more preferable that the weight change amount of the glass 10 when exposed to acid is so small that the glass 10 can be used in an acid environment. Furthermore, the glass 10 can be used repeatedly in the acid treatment process. The weight change amount when exposed to acid refers to the absolute value of the difference between the weight of the glass 10 after exposure to acid and the weight of the glass 10 before exposure to acid, divided by the surface area of ​​the glass 10 before exposure to acid. The conditions for exposure to acid may be arbitrary, but here, the conditions are as follows: sulfuric acid (H ) at a pH of 2 and a temperature of 40°C. 2 SO 4 ) for 2 hours.

[0065] Furthermore, it is preferable that the light transmittance of the glass 10 does not change before and after exposure to acid. In determining the change in transmittance after exposure to acid, a case where no opacity was observed on the surface when visually observed was rated as ○ (no change in transmittance), and a case where an opacity was observed was rated × (change in transmittance). Such a small change in transmittance when the glass 10 was exposed to acid means that the glass 10 can be used in an acid environment. Furthermore, it can be used repeatedly in the acid treatment process. The state before exposure to acid refers to the state after the weight of the glass 10 has been measured and before exposure to acid. The state after exposure to acid refers to the state after the weight of the glass 10 has been measured and the glass has been exposed to acid. The conditions for exposure to acid may be arbitrary, but here, the glass 10 was exposed to sulfuric acid (H ) at a pH of 2 and a temperature of 40°C. 2 SO 4 ) for 2 hours.

[0066] As described above, it is preferable that the glass 10 of the present embodiment has high sulfuric acid resistance. The high sulfuric acid resistance of the glass 10 has the effect of making it difficult for the light transmittance of the glass 10 to be impaired even after exposure to sulfuric acid. Furthermore, the high sulfuric acid resistance of the glass can suppress the formation of surface precipitates when exposed to sulfuric acid. Surface precipitates may contaminate processes when glass that has undergone a process including sulfuric acid immersion is introduced into a subsequent process. By suppressing surface precipitates, process contamination can be suppressed.

[0067] (Sulfuric Acid Resistance Parameter) The sulfuric acid resistance parameter S of glass 10, calculated from the BaO content and the weight change upon exposure to acid, is preferably −3 or less, more preferably −3.5 or less, more preferably −4.0 or less, more preferably −4.5 or less, more preferably −4.7 or less, more preferably −5.0 or less, more preferably −5.3 or less, and even more preferably −5.5 or less. By setting the sulfuric acid resistance parameter S within this range, the occurrence of cloudy defects (cloudy portions) upon exposure to acid can be suppressed. The sulfuric acid resistance parameter S is calculated from the following equation (4):

[0068] S=[BaO]+3.75×log 10 (Weight change upon exposure to acid) (4)

[0069] The BaO content and the weight change upon exposure to acid shown in formula (4) may be zero.

[0070] (Acid Resistance Parameter) The acid resistance parameter T of glass 10 calculated from the composition is preferably −1.0 or greater, more preferably −0.5 or greater, more preferably 0.0 or greater, more preferably 0.15 or greater, more preferably 0.3 or greater, more preferably 0.5 or greater, more preferably 0.65 or greater, more preferably 0.8 or greater, more preferably 0.9 or greater, more preferably 1.0 or greater, and even more preferably 1.05 or greater. By setting the acid resistance parameter T within this range, weight change upon exposure to acid (e.g., sulfuric acid) can be suppressed. The acid resistance parameter T is calculated from the following equation (5):

[0071] A=0.100[SiO 2 ]+0.017[Al2 O 3 ]+0.025[B 2 O 3 ]+0.044[MgO]+0.003[CaO]-0.001[SrO]-0.001[BaO]+0.036[Li 2 O]+0.002[ZnO]+0.183[ZrO 2 ]+0.114[TiO 2 ]+0.012[Y 2 O 3 ]-0.060[Gd 2 O 3 ]-0.001[La 2 O 3 ]+0.329[Ta 2 O 5 ]−5.947 ... (5)

[0072] The content of oxide RxOy (R is an element constituting the oxide, and x and y are arbitrary integers) contained in glass 10 in mol% notation based on oxides is expressed as [RxOy]. The content here refers to the ratio of the content of oxide RxOy to the total content of glass 10 in mol% notation based on oxides. That is, for example, [SiO 2 ] is the SiO 2 content relative to the entire glass 10 in mole percent on an oxide basis. 2 The formula (5) indicates the ratio of the content of the oxides. Furthermore, glass 10 does not have to contain all of the oxides shown in formula (5). In formula (5), the content of oxides not contained in glass 10 is treated as 0. Furthermore, glass 10 may contain components other than the oxides shown in formula (5).

[0073] (Glass Manufacturing Method) Glass 10 may be manufactured by any method, but is manufactured by the following method, for example. First, raw materials such as silica sand and soda ash, which are the raw materials for the compounds contained in glass 10, are heated to a predetermined temperature (e.g., 1500°C to 1600°C) and melted. Then, the molten raw materials (glass) are refined and then formed into a plate shape in a forming step. The formed glass has the composition range of glass 10 described above based on oxides. Then, glass 10 is manufactured by subjecting the glass formed in the forming step to an annealing step. Note that the method for manufacturing glass 10 is not limited to the above and may be any method. For example, the annealing step is not essential. Furthermore, various methods can be adopted for the forming step when manufacturing glass 10, and examples thereof include a melt casting method, a downdraw method (e.g., an overflow downdraw method, a slot-down method, and a redraw method), a float method, a roll-out method, and a press method.

[0074] Next, an example of a manufacturing process when the glass 10 is used in FOWLP manufacturing will be described. In FOWLP manufacturing, a plurality of semiconductor chips are bonded to the glass 10, and the semiconductor chips are covered with a sealing material to form an element substrate. Then, the glass 10 and the element substrate are separated, and the side of the element substrate opposite the semiconductor chips is bonded to, for example, another piece of glass 10. Then, wiring, solder bumps, etc. are formed on the semiconductor chips, and the element substrate and the glass 10 are separated again. Then, the element substrate is cut into individual semiconductor chips to obtain semiconductor devices.

[0075] (Effects) As described above, the glass 10 according to the first aspect of the present disclosure contains, in mole percent on an oxide basis, SiO 2 :40%~60%, B 2 O 3 :0.01%~15%, Al 2 O 3 + Rare earth oxide: 0% to 20%, SiO 2 and Al 2 O 3 Al relative to the total content of ΣRO 2 O 3Parameter A, which is the ratio of the total content of ΣRO and ΣRO, is 0.38 or more. According to the present disclosure, when parameter A is in the above range, the melting temperature of glass 10 can be lowered, facilitating production. Furthermore, when the contents of other components are in the above ranges, warping can be suppressed. Therefore, according to the present disclosure, production can be facilitated while suppressing warping. Furthermore, for example, glass with a high Young's modulus and a low thermal expansion coefficient to suppress warping may have a high melting temperature, making production difficult. In contrast, in the present disclosure, by using the above composition, the melting temperature can be suppressed from becoming high, facilitating production.

[0076] Glass 10 according to a second aspect of the present disclosure is glass 10 according to the first aspect, wherein the glass contains, in mole percent on an oxide basis, SiO 2 :41%~59%, B 2 O 3 :1%~12%, Al 2 O 3 :5%~20%, (Y 2 O 3 +Gd 2 O 3 +Ta 2 O 5 +La 2 O 3 +Nd 2 O 3 +Nb 2 O 5 By setting the content of each component within this range, warping can be suppressed while facilitating production.

[0077] Glass 10 according to a third aspect of the present disclosure is glass 10 according to the first or second aspect, and preferably has a transmittance of 30% or more at a thickness of 0.7 mm for light with a wavelength of 308 nm. A transmittance in this range allows for appropriate transmission of ultraviolet light.

[0078] Glass 10 according to a fourth aspect of the present disclosure is glass 10 according to any one of the first to third aspects, and is glass 10 in which, expressed in mol % on an oxide basis, 2 O 3 +MgO) / (SiO 2 +Al 2 O3 +B 2 O 3 +MgO)}≦1.0, 0.3≦(MgO) / ΣRO)≦1, 0%≦Al 2 O 3 + rare earth oxide≦20%. This makes it possible to increase the Young's modulus, decrease the coefficient of linear thermal expansion, and decrease the liquidus temperature, thereby making it possible to suppress deflection and facilitate manufacturing.

[0079] Glass 10 according to a fifth aspect of the present disclosure is glass 10 according to any one of the first to fourth aspects, and preferably has a Young's modulus parameter Y calculated by formula (1) of 0.8 or more, a thermal expansion parameter C calculated by formula (2) of 1.2 or less, and a liquidus parameter L calculated by formula (3) of 10.5 or less. This makes it possible to increase the Young's modulus, decrease the linear thermal expansion coefficient, and lower the liquidus temperature, thereby suppressing deflection and facilitating production.

[0080] The glass 10 according to a sixth aspect of the present disclosure is the glass 10 according to any one of the first to fifth aspects, and is preferably used as a substrate. The glass 10 according to the present disclosure is suitably used as a substrate.

[0081] The glass 10 according to a seventh aspect of the present disclosure is the glass 10 according to the sixth aspect, and is preferably used in the manufacture of at least one of a fan-out wafer-level package and a fan-out panel-level package. The glass 10 is suitable for these applications.

[0082] Examples Next, examples will be described. Tables 1 to 117 show the properties of the glass of each example. Note that the embodiment may be modified as long as the effects of the invention are achieved.

[0083]

[0084] Example 1 In Example 1, a glass having the composition shown in Table 1 was produced. In Example 1, a raw plate having a diameter of 320 mm and a thickness of 6 mm was produced using a melt-casting method. Next, multiple plates having a diameter of 300 mm and a thickness of 3 mm were cut out from the center of the raw plate. Both sides of these plates were polished using cerium oxide as an abrasive to obtain glass having a thickness of 0.7 mm.

[0085] For the glass of Example 1, Young's modulus E (GPa) was measured. Young's modulus was measured by the ultrasonic pulse method specified in JIS R 1602:1995 "Testing method for elastic modulus of fine ceramics." The bulk density of the sample was measured by the Archimedes method, and the longitudinal wave velocity and shear wave velocity were measured using an ultrasonic thickness gauge 38DL PLUS manufactured by Olympus Corporation to determine the Young's modulus value. For the glass of Example 1, linear thermal expansion coefficient α (ppm / °C) was measured. Measurement was performed using a thermal dilatometer (DIL 402 Expedis Supreme) manufactured by NETZSCH as the measuring device in the range of 30°C to 300°C, and the average thermal expansion coefficient in the range of 50°C to 200°C was taken as the linear thermal expansion coefficient α. For the glass of Example 1, the liquidus temperature T L The liquidus temperature T L The viscosity of the glass of Example 1 was measured by placing glass particles that passed through a sieve with a mesh width of 4.0 mm but did not pass through a sieve with a mesh width of 2.3 mm on a platinum dish, and then holding the dish in an electric furnace set at a predetermined temperature for 1 hour to measure the temperature at which crystals precipitated. 2 (℃), working temperature T 3 (℃), molding temperature T 4 The dissolution temperature T 2 , working temperature T 3 , molding temperature T 4 was measured by the inner cylinder rotation method. For the glass of Example 1, the Young's modulus parameter Y was calculated using the above formula (3). For the glass of Example 1, the thermal expansion parameter C was calculated using the above formula (2). For the glass of Example 1, the liquid phase parameter L was calculated using the above formula (3). For the glass of Example 1, the glass transition temperature (°C) was measured. The glass transition temperature was measured by obtaining an expansion curve until the glass softened using a thermal expansion measuring device. For the glass of Example 1, the density (g / cm 3 ) was measured. The density was measured by the Archimedes method. The liquidus viscosity of the glass of Example 1 was measured. The liquidus viscosity was measured by measuring the temperature-viscosity curve by the inner cylinder rotation method and calculating the viscosity at the liquidus temperature. The fracture toughness value K IC(MPa m 0.5 The fracture toughness value K IC was measured using the single-edge precracked beam (SEPB) method, as defined in JIS R1607:2015 "Room temperature fracture toughness test method for fine ceramics." For the glass of Example 1, the transmittance for light with a wavelength of 308 nm, the transmittance for light with a wavelength of 350 nm, the transmittance for light with a wavelength of 550 nm, and the transmittance for light with a wavelength of 1064 nm were measured. The transmittance measurements were performed by measuring a spectral transmittance curve using an ultraviolet-visible spectrophotometer (UH4150 model, manufactured by Hitachi High-Tech Corporation). For the glass of Example 1, the weight (mg) before and after the acid immersion test were measured, and the weight loss (weight change) was calculated using the method described in the above embodiment. In the acid immersion test, the specimen was immersed in sulfuric acid (H 2 SO 4 ) for 2 hours. The weights before and after the acid immersion test were measured with high precision using an electronic balance. For the glass of Example 1, the sulfuric acid resistance parameter S was calculated using the above-mentioned formula (4). For the glass of Example 1, the acid resistance parameter T was calculated using the above-mentioned formula (5). The measurement results and calculation results are shown in Table 1.

[0086] (Examples 2 to 821) In Examples 2 to 821, glasses were produced in the same manner as in Example 1, except that the glass compositions were as shown in Table 1. The measurement results and calculation results for each example are shown in Tables 1 to 117.

[0087] (Evaluation) The deflection and manufacturability of each glass example were evaluated. The deflection evaluation was performed based on the Bi-Metal warpage calculation defined in the literature by S. Timoshenko, "Analysis of Bi-Metal Thermostats," J. Opt. Soc. Am. 11 (1925) 233. FIG. 2 is a schematic diagram for explaining the deflection evaluation. Here, the amount of warpage δ is defined as the amount of vertical displacement of the edge of the glass 10, with the center of the second surface 14 used as the height reference, when the glass 10 is cooled from a high temperature of 200°C to a low temperature of 20°C during the process of molding and bonding a semiconductor substrate with resin to the first surface 12 side of the glass 10 processed into the shape of FIG. 1, as shown in FIG. 2. Specifically, the amount of warpage δ is calculated using the following equation (4):

[0088]

[0089] Here, as shown in FIG. 2, L is the length of the glass 10 in the warp direction (the horizontal direction in FIG. 2), and α 1 is the linear thermal expansion coefficient of the resin substrate 20, and α 2 is the linear thermal expansion coefficient of the glass 10, and T 2 is the temperature after cooling (here 20°C), and T 1 is the temperature before cooling (here, 200°C). 1 / a 2 and h is a 1 +a 2 and n is E 1 / E 2 Here, a 1 is the thickness of the resin substrate 20, and a 2 is the thickness of the glass 10, and E 1 is the Young's modulus of the resin substrate 20, and E 2is the Young's modulus of the glass 10. For the deflection evaluation, the resin substrate 20 to be bonded to the glass 10 was assumed to have a thickness of 0.3 mm and a Young's modulus of 31.5 GPa, taking into consideration the implementation of semiconductors. Assuming application to various manufacturing processes, two linear thermal expansion coefficients were assumed: {linear thermal expansion coefficient of glass (ppm / °C)} + 0.5 ppm / °C and {linear thermal expansion coefficient of glass (ppm / °C)} - 0.5 ppm / °C. The amount of warpage δ was calculated for each case when the thickness of the glass 10 was 0.7 mm and the length L = 300 mm. In judging the deflection, a sum of the absolute values ​​of the calculated δ values ​​of 1.732 mm or less was marked as ◯, and a sum greater than 1.732 mm was marked as ×. Manufacturability refers to ease of manufacture, and was evaluated as ◯ when the liquidus temperature was less than 1300° C. and the melting temperature was less than 1400° C., and x when at least one of the liquidus temperature of 1300° C. or higher and the melting temperature of 1400° C. or higher was satisfied. In the evaluation of transmittance, ◯ was evaluated when the glass 10 having a thickness D of 0.7 mm had an internal transmittance of 70% or higher for light with a wavelength of 350 nm, an internal transmittance of 85% or higher for light with a wavelength of 550 nm, and an internal transmittance of 80% or higher for light with a wavelength of 1064 nm, and x was evaluated when the internal transmittance of 350 nm light was less than 70%, or the internal transmittance of 550 nm light was less than 85%, or the internal transmittance of 1064 nm light was less than 80%.

[0090] As shown in Tables 1 to 117, SiO 2 The content of is 40% to 60%, B 2 O 3 The content of is 0.01% to 15%, Al 2 O 3 Examples 1 to 759 and 770 to 821, which are working examples in which the total content of rare earth oxides and rare earth oxides is 0% to 20% and the parameter A is 0.38 or more, were evaluated as ◯ in the deflection assessment, manufacturability assessment, and permeability assessment, indicating that they can be easily manufactured and have high permeability while suppressing deflection. On the other hand, Examples 760 to 769, which are comparative examples, were evaluated as × in at least one of the manufacturability assessment, deflection assessment, and permeability assessment, indicating that they cannot be easily manufactured or are not suitable as substrates.

[0091] Furthermore, sulfuric acid resistance (permeability) was checked for some examples as an optional evaluation. As an evaluation method, the method for determining the change in permeability after exposure to acid described in the above embodiment was used, and it is preferable that there is no change in permeability. In determining the change in permeability after exposure to acid, when no cloudy part was observed on the surface by visual observation, it was marked as ○, and when cloudy part was observed, it was marked as ×.

[0092] Although the embodiments of the present invention have been described above, the embodiments are not limited to the contents of these embodiments. Furthermore, the above-described components include those that can be easily imagined by a person skilled in the art, those that are substantially the same, and those that are within the scope of what is called equivalents. Furthermore, the above-described components can be combined as appropriate. Furthermore, various omissions, substitutions, or modifications of the components can be made without departing from the spirit of the above-described embodiments.

[0093] 10. Glass

Claims

1. In mole percent based on oxide, SiO 2 :40%~60%, B 2 O 3 :0.01%~15%, Al 2 O 3 + Rare earth oxide: 0% to 20%, containing SiO 2 and Al 2 O 3 and the total content of divalent oxides, ΣRO, 2 O 3 The ratio of the total content of Al and ΣRO 2 O 3 +ΣRO) / (SiO 2 +Al 2 O 3 +ΣRO)) is 0.38 or more.

2. In terms of oxide mole percent, SiO 2 :41%~59%, B 2 O 3 :1%~12%, Al 2 O 3 :5%~20%, (Y 2 O 3 +Gd 2 O 3 +Ta 2 O 5 +La 2 O 3 +Nd 2 O 3 +Nb 2 O 5 2. The glass of claim 1 , comprising:

3. The glass according to claim 1 or 2, which has a transmittance of 30% or more for light with a wavelength of 308 nm when the glass has a thickness of 0.7 mm.

4. In terms of oxide mol%, 0.1≦(Al 2 O 3 +MgO) / (SiO 2 +Al 2 O 3 +B 2 O 3 +MgO)}≦1, 0.3≦(MgO) / ΣRO)≦1, 0%≦Al 2 O 3 + rare earth oxides≦20%, where ΣRO refers to the total divalent oxide content in the glass.

5. The oxide R contained in the glass, expressed in mole percent based on oxides x O y The content of [R x O y ], the Young's modulus parameter Y calculated by the following formula (1) is 0.8 or more, the thermal expansion parameter C calculated by the following formula (2) is 1.2 or less, and the liquid phase parameter L calculated by the following formula (3) is 10.5 or less. 2 ]+0.3[Al 2 O 3 ]−1.15[B 2 O 3 ]+0.21[MgO]-0.2[CaO]-0.1[SrO]-1.2[BaO]+[Li 2 O]-2.8 [K 2 O]+0.05[ZnO]+1.46[ZrO 2 ]-0.05[TiO 2 ]+1.6[Y 2 O 3 " + 1.35 [Gd 2 O 3 ]+1.37[La 2 O 3 ]+[Ta 2 O 5 ]) / 100...(1) C=(14.098-0.1245[SiO 2 ]-0.131[Al 2 O 3 ]−0.101[B 2 O 3 ]-0.051[MgO]+0.013[CaO]+0.053[SrO]+0.018[BaO]+0.041[Li 2 O]+0.395[Na 2 O]-0.066[ZnO]-0.033[ZrO 2 ]-0.072[TiO 2 ]+0.035[Y 2 O 3 ]+0.074[Gd 2 O 3 ]+0.074[La 2 O 3 ]-0.091[Ta 2 O 5 ]) / 5 ・・・(2) L=(-642.5+20.6[[SiO 2 ]+31.9[Al] 2 Oh 3 ]+2.85[L 2 Oh 3 ]. 2 O]+37.96[K 2 O]+11.47[[OO]+25.83[[OO 2 ]+41.0[TiO 2 ]+12.32434 2 Oh 3 ]-1.18[G] 2 Oh 3 ]-1.18[] 2 Oh 3 ]+24.46[Ta 2 Oh 5 ]) / 125 ・・・(3) 6. The glass according to claim 1 or 2, which is used as a substrate.

7. The glass of claim 6 for use in the manufacture of at least one of a fan-out wafer level package and a fan-out panel level package.

Citation Information

Patent Citations

  • Glass for communication package window

    JP2004244226A

  • Glass substrate and laminated substrate

    WO2018051987A1

  • Support glass base plate

    WO2021019911A1

  • Support glass substrate, multi-layer body, method for producing multi-layer body, and method for producing semiconductor package

    WO2023026770A1