Methods and systems for processing lithium compounds
The method optimizes lithium extraction from liquid resources by using lithium selective sorbents and controlled pH adjustments, effectively addressing inefficiencies in current extraction techniques by enhancing recovery efficiency and purity through the use of lithium selective sorbents and phosphate/metathesis salt treatments.
Patent Information
- Application Number
- PCT/US2024/025420
- Authority / Receiving Office
- WO · WO
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2023-04-21
- Filing Date
- 2024-04-19
- Publication Date
- 2024-10-24
AI Technical Summary
Current methods for extracting lithium from liquid resources, such as natural and synthetic brines, face inefficiencies in concentrating lithium to high purity levels, particularly in maintaining optimal ion exchange material performance and pH control during the extraction process.
A method involving the use of lithium selective sorbents, ion exchange materials, and controlled pH adjustments, where a liquid resource is contacted with a lithium selective sorbent to generate an enriched lithium eluate, followed by the addition of phosphate salts to precipitate lithium phosphate, and subsequent treatment with metathesis salts to produce soluble lithium salts, optimizing lithium recovery and purity.
This method enhances lithium recovery efficiency by maintaining optimal ion exchange material performance, improving lithium purity, and extending the material's useful lifetime, while reducing the need for excessive acid usage during elution.
Smart Images

Figure US2024025420_24102024_PF_FP_ABST
Abstract
Description
METHODS AND SYSTEMS FOR PROCESSING LITHIUM COMPOUNDSCROSS-REFERENCE
[0001] This application claims the benefit of U.S. Provisional Application Serial No. 63 / 461,168 filed April 21, 2023, which is hereby incorporated by reference in its entirety.BACKGROUND OF THE INVENTION
[0002] Lithium is an essential element for high-energy rechargeable batteries and other technologies. Lithium can be found in a variety of liquid solutions, including natural and synthetic brines and leachate solutions from minerals and recycled products.SUMMARY OF THE INVENTION
[0003] In an aspect, provided herein is a method of extracting lithium from a liquid resource, the method comprising: a) contacting a liquid resource to a lithium selective sorbent to yield an enriched lithium selective sorbent; b) contacting an eluent to the enriched lithium selective sorbent to generate a lithium eluate, wherein the pH of the eluent prior to contact with the enriched lithium selective sorbent is less than about 1; c) adding a phosphate salt to the lithium eluate to precipitate a lithium phosphate salt and generate a depleted lithium eluate; d) separating the lithium phosphate salt and the depleted lithium eluate; and e) contacting a metathesis salt, acid, or any combination thereof, to the lithium phosphate salt to generate a soluble lithium salt.
[0004] In an aspect, provided herein is a method of extracting lithium from a liquid resource, the method comprising: a) contacting a liquid resource to a lithium selective sorbent to yield an enriched lithium selective sorbent; b) contacting an eluent to the enriched lithium selective sorbent to generate a lithium eluate, wherein the concentration of lithium in the lithium eluate is less than about 1,500 mg / L; c) adding a phosphate salt to the lithium eluate to precipitate a lithium phosphate salt and generate a depleted lithium eluate; d) separating the lithium phosphate salt and the depleted lithium eluate; and e) contacting a metathesis salt, acid, or any combination thereof, to the lithium phosphate salt to generate a soluble lithium salt.
[0005] In an aspect, provided herein is a method of extracting lithium from a liquid resource, the method comprising: a) contacting a liquid resource to a lithium selective sorbent to yield an enriched lithium selective sorbent; b) contacting an eluent to the enriched lithium selective sorbent to generate a lithium eluate; c) adding a phosphate salt to the lithium eluate to precipitate a lithium phosphate salt and generate a depleted lithium eluate; d) separating the lithium phosphate salt and the depleted lithium eluate; and e) contacting a metathesis salt, an acid, or any combination thereof, to the lithium phosphate salt to generate a soluble lithium salt; wherein c) comprises: i. adding a first quantity of the phosphate salt to the lithium eluate to yield one or more metal phosphate precipitates comprising the one or more metals, ii. removing the one or more metal phosphate precipitates by filtration to yield a purified lithium solution, and iii. adding a second quantity of the phosphate salt to the purified lithium solution to yield the lithium phosphate salt.
[0006] In an aspect, provided herein is a method of extracting lithium from a liquid resource, the method comprising: a) contacting a liquid resource to a lithium selective sorbent to yield an enriched lithium selective sorbent; b) contacting an eluent to the enriched lithium selective sorbent to generate a lithium eluate; c) adding a phosphate salt to the lithium eluate to precipitate a lithium phosphate salt and generate a depleted lithium eluate; d) separating the lithium phosphate salt and the depleted lithium eluate; and e) contacting a metathesis salt to the lithium phosphate salt; f) heating the metathesis salt and the lithium phosphate salt to generate an insoluble phosphate salt and a soluble lithium salt; wherein the insoluble phosphate salt comprises phosphate and has a solubility in water of at most 0.29 g / L, and wherein the soluble lithium salt comprises lithium and has a solubility in water of at least 0.41 g / L;g) adding water to the insoluble phosphate salt and the soluble lithium salt to dissolve the soluble lithium salt; and h) separating the insoluble phosphate salt and dissolved soluble lithium salt by filtration.
[0007] In an aspect, provided herein is a method of extracting lithium from a liquid resource, the method comprising: a) contacting a liquid resource to a lithium selective sorbent to yield an enriched lithium selective sorbent; b) contacting an eluent to the enriched lithium selective sorbent to generate a lithium eluate; c) adding a phosphate salt to the lithium eluate to precipitate a lithium phosphate salt and generate a depleted lithium eluate; d) separating the lithium phosphate salt and the depleted lithium eluate; e) generating a lithium phosphate slurry comprising the lithium phosphate salt and adding an acid to generate an acidified lithium phosphate slurry or solution; f) adding a metathesis salt to acidified lithium phosphate slurry or solution to generate a water-insoluble phosphate salt and a water-soluble lithium salt; and g) separating the water-insoluble phosphate salt and the water-soluble lithium salt.
[0008] In an aspect, provided herein is a method of extracting lithium from a liquid resource, the method comprising: a) contacting a liquid resource to an ion exchange material to yield a lithiated ion exchange material, wherein the ion exchange material selectively exchanges lithium and hydrogen ions; b) contacting an eluent to the lithiated ion exchange material to generate a lithium eluate, wherein the eluent comprises phosphoric acid, and wherein the lithium eluate comprises dissolved lithium phosphate, c) adding a metathesis salt, a base, or any combination thereof, to the lithium eluate to precipitate a solid phosphate salt, and d) separating the solid phosphate salt.
[0009] In an aspect, provided herein is a method of preparing a non-aqueous lithium solution, the method comprising: a) generating a lithium phosphate salt; b) generating a lithium phosphate slurry comprising the lithium phosphate salt and a nonaqueous solvent;c) adding a metathesis salt to the lithium phosphate slurry to yield a solid precipitate and the non-aqueous lithium solution, wherein the solid precipitate is a phosphate salt resulting from the reaction of the metathesis salt and the lithium phosphate, and wherein the non-aqueous lithium solution comprises a dissolved lithium salt resulting from the reaction of the metathesis salt and the lithium phosphate.
[0010] In an aspect, provided herein is a method of preparing a lithium iron phosphate, the method comprising: a) generating a lithium phosphate salt; b) dissolving the lithium phosphate salt in ammonia to yield a lithium phosphate ammonia solution; c) contacting an iron source and a phosphate salt with the lithium phosphate ammonia solution to yield lithium iron phosphate; and d) crystallizing and isolating the lithium iron phosphate.
[0011] In an aspect, provided herein is a method of preparing a water soluble lithium salt, the method comprising: a) generating a lithium phosphate salt; b) contacting a metathesis salt to the lithium phosphate to yield a salt mixture; c) heating the salt mixture to generate a water-insoluble phosphate salt and the water- soluble lithium salt; wherein the water-insoluble phosphate salt comprises phosphate and has a solubility in water of at most 0.29 g / L, and wherein the water-soluble lithium salt comprises lithium and has a solubility in water of at least 0.41 g / L; d) adding water to the water-insoluble phosphate salt and the water-soluble lithium salt to dissolve the water-soluble lithium salt; and e) separating the water insoluble phosphate salt and dissolved water-soluble lithium salt by filtration.
[0012] In an aspect, provided herein is a method of preparing a water soluble lithium salt, the method comprising: a) generating an impure lithium solution, wherein the impure lithium solution comprises lithium and one or more metals, wherein the one or more metals join with phosphate to form one or more metal precipitates, and wherein one or more metal precipitates each have a solubility of at most 0.29 g / L;b) adding a phosphate salt to the impure lithium solution to yield one or more metal precipitates and a purified lithium solution; c) adding additional phosphate salt to the purified lithium solution to yield a lithium phosphate salt; d) contacting a metathesis salt to generate a water-insoluble phosphate salt and the water- soluble lithium salt; wherein the water-insoluble phosphate salt comprises phosphate and has a solubility in water of at most 0.29 g / L, and wherein the water-soluble lithium salt comprises lithium and has a solubility in water of at least 0.41 g / L.
[0013] In an aspect, provided herein is a method of preparing a lithium phosphate salt, the method comprising: a) generating an impure lithium solution, wherein the impure lithium solution comprises lithium and one or more metals, wherein the one or more metals join with carbonate or hydroxide to form one or more metal precipitates, and wherein one or more metal precipitates each have a solubility of at most 0.29 g / L; b) adding a hydroxide or carbonate salt to the impure lithium solution to yield one or more metal precipitates and a purified lithium solution; c) adding a phosphate salt to the purified lithium solution to yield a lithium phosphate salt.
[0014] In an aspect, provided herein is a method of isolating a solid lithium carbonate salt, the method comprising: a) generating a lithium phosphate salt; b) generating a lithium phosphate slurry comprising the lithium phosphate salt and water; c) adding a metathesis salt to the lithium phosphate slurry to generate a water-insoluble phosphate salt and a water-soluble lithium salt; wherein the water-insoluble phosphate salt comprises phosphate and has a solubility in water of at most 0.29 g / L, and wherein the water-soluble lithium salt comprises lithium and has a solubility in water of at least 0.41 g / L. d) separating the water-insoluble phosphate salt and the water-soluble lithium salt; e) adding a carbonate salt to the water soluble lithium salt in water to afford a lithium carbonate solution; f) precipitating solid lithium carbonate by heating the lithium carbonate solution; andg) isolating the solid lithium carbonate.
[0015] In an aspect, provided herein is a method of isolating a solid lithium phosphate salt, the method comprising: a) extracting lithium from a liquid resource to generate a lithium eluate, wherein the lithium eluate comprises water and lithium; b) adding a phosphate salt to the lithium eluate to generate the solid lithium phosphate salt; and c) isolating the lithium phosphate salt with a filter press.
[0016] In an aspect, provided herein is a method of extracting lithium from a liquid resource, the method comprising: a) generating a lithium eluate from the liquid resource, wherein the lithium eluate comprises lithium and one or more impurities; b) contacting the lithium eluate with a phosphate salt to generate a solid lithium phosphate salt and a depleted lithium eluate, wherein the solid lithium phosphate salt comprises lithium phosphate; c) separating the solid lithium phosphate salt and the depleted lithium eluate with one or more particle traps; d) immobilizing the solid lithium phosphate salt within the one or more particle traps; e) contacting the solid lithium phosphate salt with a liquid stream running through the one or more particle traps to yield a solution of lithium phosphate salt; and f) contacting a metathesis salt to the solid lithium phosphate salt generate a solid phosphate salt and a water-soluble lithium salt.
[0017] In an aspect, provided herein is a method of extracting lithium from a liquid resource, the method comprising: a) generating an impure lithium solution, wherein the impure lithium solution comprises lithium and one or more impurities; b) contacting the impure lithium solution with a fluoride salt to generate a solid lithium fluoride salt and a depleted lithium solution, wherein the solid lithium fluoride salt comprises lithium fluoride; c) separating the solid lithium fluoride salt and the depleted lithium solution with one or more particle traps; d) generating a slurry or dissolved solution comprising the solid lithium fluoride salt; and e) contacting a metathesis salt to a slurry or dissolved solution comprising the solid lithium fluoride salt to generate a second solid fluoride salt and a water-soluble lithium salt.INCORPORATION BY REFERENCE
[0018] All publications, patents, and patent applications mentioned in this specification are herein incorporated by reference to the same extent as if each individual publication, patent, or patent application was specifically and individually indicated to be incorporated by reference.BRIEF DESCRIPTION OF THE DRAWINGS
[0019] The novel features of the invention are set forth with particularity in the appended claims. A better understanding of the features and advantages of the present invention will be obtained by reference to the following detailed description that sets forth illustrative embodiments, in which the principles of the invention are utilized, and the accompanying drawings of which:
[0020] FIG. 1 provides a diagram of one or more systems configured for the practice of methods and processes for: 1) obtaining lithium phosphate from a synthetic lithium solution and 2) subsequently converting lithium phosphate into lithium hydroxide in a non-aqueous medium comprising methanol with an anion source (e.g., a metathesis salt) comprising calcium hydroxide.
[0021] FIG. 2 provides a diagram of one or more systems configured for the practice of methods and processes for: 1) obtaining lithium phosphate from a synthetic lithium solution and 2) subsequently converting lithium phosphate into lithium hydroxide in a non-aqueous medium comprising ammonia.
[0022] FIG. 3 provides a diagram of one or more systems configured for the practice of methods and processes for converting lithium phosphate into lithium hydroxide via a reaction with a solid anion source (e.g., a solid metathesis salt) comprising calcium oxide followed by hydrolysis.
[0023] FIG. 4 provides a diagram of one or more systems configured for the practice of methods and processes for: 1) solubilizing lithium phosphate in an aqueous medium comprising HC1 (e.g., an anion source) to generate an aqueous medium comprising dissolved lithium, chloride, and phosphate, and 2) subsequently separating lithium chloride from an aqueous medium comprising dissolved lithium, chloride, and phosphate using nanofiltration.
[0024] FIG. 5 provides a diagram of one or more systems configured for the practice of methods and processes for: 1) separating solid lithium phosphate from a synthetic lithium solution from which the lithium phosphate was formed by precipitation using a solid-liquid separation method comprising use of a filter press, and 2) subsequently solubilizing solid lithium phosphate contained within the filter press with a sulfuric acid solution to provide an aqueousmedium comprising lithium, sulfate, and phosphate that is free of solid lithium phosphate and can subsequently be contacted with an anion source (e.g., a metathesis salt) to generate lithium hydroxide.
[0025] FIG. 6 provides a diagram of one or more systems configured for the practice of methods and processes for converting lithium phosphate into lithium hydroxide via a reaction with a solid anion source (e.g., a metathesis salt) comprising calcium sulfate followed by hydrolysis.
[0026] FIG. 7 provides a diagram of one or more systems configured for the practice of methods and processes for: 1) converting lithium phosphate into lithium chloride in an aqueous medium with an anion source (e.g., a metathesis salt) comprising magnesium chloride, and 2) subsequently processing the aqueous medium comprising lithium chloride to provide solid lithium carbonate.
[0027] FIG. 8 provides a diagram of one or more systems configured for the practice of methods and processes for: 1) obtaining lithium phosphate from a synthetic lithium solution and2) subsequently converting lithium phosphate into lithium hydroxide in an aqueous medium with an anion source (e.g., a metathesis salt) comprising calcium hydroxide.
[0028] FIG. 9 provides a diagram of one or more systems configured for the practice of methods and processes for: 1) precipitating impurities from a synthetic lithium solution; 2) obtaining lithium phosphate from the synthetic lithium solution; and 3) subsequently converting lithium phosphate into lithium carbonate in an aqueous medium with an anion source (e.g., a metathesis salt) comprising calcium carbonate in the presence of a solubilizing agent comprising carbon dioxide.
[0029] FIG. 10 provides a diagram of one or more systems configured for the practice of methods and processes for: 1) precipitating impurities from a synthetic lithium solution; 2) obtaining lithium carbonate from the synthetic lithium solution to generate a mother liquor; and3) subsequently precipitating lithium phosphate from the mother liquor.
[0030] FIG. 11 provides a diagram of one or more systems configured for the practice of methods and processes for: 1) generating a synthetic lithium solution from hard rock comprising spodumene; 2) precipitating impurities from the synthetic lithium solution; 3) obtaining lithium phosphate from the synthetic lithium solution; and 4) subsequently converting lithium phosphate into lithium hydroxide in an aqueous medium with an anion source (e.g., a metathesis salt) comprising calcium hydroxide.
[0031] FIG. 12 provides a diagram of one or more systems configured for the practice of methods and processes for: 1) generating a synthetic lithium solution from hard rock comprising spodumene; 2) precipitating impurities from the synthetic lithium solution; 3) obtaining lithiumphosphate from the synthetic lithium solution; and 4) subsequently converting lithium phosphate into lithium hydroxide via a reaction with a solid anion source (e.g., a metathesis salt) comprising magnesium hydroxide followed by hydrolysis.
[0032] FIG. 13 provides a diagram of one or more systems configured for the practice of methods and processes for: 1) converting lithium phosphate into lithium sulfate in an aqueous medium with an anion source (e.g., a metathesis salt) comprising calcium sulfate, and 2) subsequently converting the lithium sulfate dissolved in the aqueous medium to lithium hydroxide using NaOH.
[0033] FIG. 14 provides a diagram of one or more systems configured for the practice of methods and processes for converting lithium phosphate into lithium chloride in an aqueous medium with an anion source (e.g., a metathesis salt) comprising magnesium chloride.
[0034] FIG. 15 provides a diagram of one or more systems configured for the practice of methods and processes for converting lithium phosphate into lithium hydroxide in a nonaqueous medium with an anion source (e.g., a metathesis salt) comprising calcium hydroxide.
[0035] FIG. 16 provides a diagram of one or more systems configured for the practice of methods and processes for converting lithium phosphate into lithium chloride in a non-aqueous medium with an anion source (e.g., a metathesis salt) comprising magnesium chloride.
[0036] FIG. 17 provides a diagram of one or more systems configured for the practice of methods and processes for: 1) converting lithium phosphate into lithium sulfate in a nonaqueous medium with an anion source comprising sulfuric acid, and 2) subsequently removing phosphate from the non-aqueous medium before solid lithium sulfate is obtained therefrom.
[0037] FIG. 18 provides a diagram of one or more systems configured for the practice of methods and processes for: 1) converting lithium phosphate into lithium sulfate in an aqueous medium with an anion source comprising sulfuric acid, and 2) subsequently removing phosphate from the aqueous medium before solid lithium sulfate is obtained therefrom.
[0038] FIG. 19 provides a diagram of one or more systems configured for the practice of methods and processes for the conversion of solid lithium phosphate into a homogenous solution comprising an aqueous medium and soluble lithium species enabled by the complete solubilization of lithium phosphate by sulfuric acid.
[0039] FIG. 20 provides a diagram of one or more systems configured for the practice of methods and processes for: 1) the production of lithium hydroxide from synthetic lithium solutions comprising phosphate, and 2) the production of phosphoric acid from precipitates comprising phosphate.
[0040] FIG. 21 provides a diagram of one or more systems configured for the practice of methods and processes for: 1) the production of lithium hydroxide from synthetic lithiumsolutions comprising phosphate; 2) subsequent conversion of said lithium hydroxide into lithium carbonate; and 3) the production of phosphoric acid from precipitates comprising phosphate.
[0041] FIG. 22 provides a diagram of one or more systems configured for the practice of methods and processes for the precipitation of lithium phosphate from synthetic lithium solutions comprising phosphate.
[0042] FIG. 23 provides a diagram of one or more systems configured for the practice of methods and processes for the production of LiFePC from lithium phosphate in a non-aqueous medium comprising ammonia.
[0043] FIG. 24 provides a diagram of one or more systems configured for the practice of methods and processes for: 1) precipitating impurities from a synthetic lithium solution comprising phosphate, and 2) subsequently producing lithium hydroxide and phosphoric acid from said synthetic lithium solution comprising phosphate using electrolysis.
[0044] FIG. 25 provides a diagram of one or more systems configured for the practice of methods and processes for: 1) obtaining solids comprising lithium fluoride from a synthetic lithium solution and 2) subsequently converting solids comprising lithium fluoride into lithium hydroxide in an aqueous medium using an anion source (e.g., a metathesis salt) comprising calcium hydroxide.
[0045] FIG. 26 provides a diagram of one or more systems configured for the practice of methods and processes for solubilizing lithium phosphate in phosphoric acid solutions.
[0046] FIG. 27 provides a diagram of one or more systems configured for the practice of methods and processes for: 1) obtaining lithium phosphate from a synthetic lithium solution; 2) solubilizing lithium phosphate with sulfuric acid to provide a solution comprising lithium sulfate and phosphoric acid; 3) precipitating phosphate from the solution comprising lithium sulfate and phosphoric acid by adding calcium hydroxide thereto; and 4) subsequently obtaining solid lithium carbonate from the resulting solution comprising lithium sulfate.
[0047] FIG. 28 provides a diagram of one embodiment of a system configured for carrying out a method comprising: 1) contacting a lithium phosphate salt to a metathesis salt, and 2) heating the lithium phosphate salt and the metathesis salt to provide a soluble lithium salt.
[0048] FIG. 29 provides a diagram of one embodiment of a system configured for carrying out a method comprising: 1) contacting a lithium phosphate salt to a metathesis salt, and 2) heating the lithium phosphate salt and the metathesis salt to provide a soluble lithium salt.
[0049] FIG. 30 provides a diagram of one embodiment of a system configured for carrying out a method comprising: 1) adding a first quantity of a phosphate salt to a lithium eluate to precipitate solids comprising impurities and phosphate, 2) separating the solids comprising impurities and phosphate from the lithium eluate, 3) adding a second quantity of a phosphate saltto a lithium eluate to precipitate a lithium phosphate salt, 4) contacting the lithium phosphate salt to a metathesis salt to provide a soluble (e.g., water-soluble) lithium salt and a waterinsoluble phosphate salt, and 5) separating a solution of the soluble lithium salt from the insoluble (e.g., water-insoluble) phosphate salt.DETAILED DESCRIPTION OF THE INVENTION
[0050] Lithium is an essential element for batteries and other technologies. Lithium is found in a variety of liquid resources, including natural and synthetic brines and leachate solutions from minerals, clays, and recycled products. Lithium is optionally extracted from such liquid resources using an ion exchange process based on inorganic ion exchange materials. These inorganic ion exchange materials absorb lithium from a liquid resource while releasing hydrogen, and then elute lithium in acid while absorbing hydrogen. This ion exchange process is optionally repeated to extract lithium from a liquid resource and yield a synthetic lithium solution. The synthetic lithium solution is optionally further processed into chemicals for the battery industry or other industries.
[0051] The present disclosure provided methods and systems for the processing of lithium compounds. Said processing can comprise one or more chemical reactions intended to convert one lithium compound into another lithium compound. Said processing can utilize a first solid, liquid, suspension, colloid, slurry, or solution comprising lithium as an input to provide a second solid, liquid, suspension, colloid, slurry, or solution comprising lithium as an output.Key Terms and Definitions
[0052] As used herein and in the appended claims, the singular forms “a,” “an,” and “the” include plural referents unless the context clearly dictates otherwise. Thus, for example, reference to “an agent” includes a plurality of such agents, and reference to “the cell” includes reference to one or more cells (or to a plurality of cells) and equivalents thereof known to those skilled in the art, and so forth. When ranges are used herein for physical properties, such as molecular weight, or chemical properties, such as chemical formulae, all combinations and subcombinations of ranges and specific embodiments therein are intended to be included. The term “about” when referring to a number or a numerical range means that the number or numerical range referred to is an approximation within experimental variability (or within statistical experimental error), and thus the number or numerical range, in some instances, will vary between 1% and 15% of the stated number or numerical range. The term “comprising” (and related terms such as “comprise” or “comprises” or “having” or “including”) is not intended toexclude that in other certain embodiments, for example, an embodiment of any composition of matter, composition, method, or process, or the like, described herein, “consist of’ or “consist essentially of’ the described features.
[0053] The terms “lithium”, “lithium ion”, and “Li+” are used interchangeably in the present specification and these terms are synonymous unless specifically noted to the contrary. The terms “hydrogen”, “hydrogen ion”, “proton”, and “H+” are used interchangeably in the present specification and these terms are synonymous unless specifically noted to the contrary.
[0054] As used herein, the words “column” and “vessel” are used interchangeably. In some embodiments described herein referring to a “vessel”, the vessel is a column. In some embodiments described herein referring to a “column”, the column is a vessel.
[0055] The term “the pH of the system” or “the pH of’ a component of a system, for example one or more tanks, vessels, columns, pH modulating units, or pipes used to establish fluid communication between one or more tanks, vessels, columns, or pH modulating units, refers to the pH of the liquid medium contained or present in the system, or contained or present in one or more components thereof. In some embodiments, the liquid medium contained in the system, or one or more components thereof, is a liquid resource. In some embodiments, the liquid medium contained in the system, or one or more components thereof, is a brine. In some embodiments, the liquid medium contained in the system, or one or more components thereof, is an acid solution, an aqueous solution, a wash solution, a salt solution, a salt solution comprising lithium ions, or a lithium-enriched solution. As used herein, pH is equal to the negative logarithmic value of the concentration of protons in the aqueous solution. The pH of the solutions described herein are preferably determined with a pH probe. However, many of the solutions described herein comprise high concentrations of ions (e.g., sodium) that are known to interfere with pH probe sensors. Therefore, solutions with high ion concentrations can lead to shifted readings. In such cases, pH probe values are confirmed by diluting the test solution, for example by 10X or 100X, and remeasuring via pH probe to ensure that the change in pH is consistent with the change in concentration of protons. Alternative methods of pH determination include chemical tests such as titration with colored indicators or litmus tests.
[0056] The term “concentration”, as used herein, refers to the amount of a chemical species within a given amount of liquid. In some embodiments, said concentration can be specified as the mass of a species dissolved in an amount of liquid (e.g. mg / L), or the number of moles of a species dissolved in an amount of liquid (e.g. mol / L). In some embodiments, concentration can be specified by the ratio of moles or mass of the species of interest to one or more other species dissolved in the same liquid. In some embodiments, only the mass concentration of an ionic species is stated; for example, a concentration of sodium (Na) is statedto be 100 milligrams per liter (mg / L). In such cases, the stated concentration refers to the mass concentration of the ion in solution, and does not include the mass of the anion; in the example stated above, such an ion may comprise chloride (C1-), nitrate (NO3 ), or sulfate (SO42').\
[0057] As used herein, the term “synthetic lithium solution” describes a solution comprising lithium that is not present in nature and obtained by a process for processing, refining, recovering or purifying lithium. In some embodiments, a synthetic lithium solution can be yielded by placing an acid into contact with a lithium-selective sorbent. In some embodiments, a synthetic lithium solution is a lithium eluate. In some embodiments, a synthetic lithium solution is used in place of a liquid resource. In some embodiments, a synthetic lithium solution is combined with a liquid resource. In some embodiments, a synthetic lithium solution is a leachate solution (e.g., a leachate of one or more ores, a leachate of one or more minerals, a leachate of one or more clays, a leachate of waste or recycled materials comprising lithium). In some embodiments, a synthetic lithium solution is a brine concentrated by solar evaporation.
[0058] The term “direct lithium extraction,” as used herein, refers to a process involving the sorption or adsorption of lithium from solution. Direct lithium extraction can be carried out with a lithium-selective sorbent. A lithium-selective sorbent can comprise an ion exchange material.
[0059] The term “eluate,” as used herein, refers to a liquid input to employed for the removal of lithium from a lithium-selective sorbent. An eluate can be acidic. An eluate that has been placed in contact with a lithium-selective sorbent that releases lithium into the eluate is a lithium eluate. A lithium eluate is a synthetic lithium solution. A synthetic lithium solution is a lithium eluate. In some embodiments, wherein the lithium-selective sorbent is an ion exchange material than has been exposed to a liquid resource comprising lithium, the eluate is an acidic solution. In such cases, the protons of the acidic eluate displace the lithium on the ion exchange material to yield a synthetic lithium eluate.
[0060] As used herein, the term “lithium purity” refers to the chemical purity of a lithium chemical, lithium compound, or a solution that comprises lithium or a lithium compound. In some embodiments, lithium purity can be expressed as the percentage of lithium in a solution as on the basis of the total metal ion content of the solution. In some embodiments, lithium purity is expressed in terms of the quantities or percentages of specific impurities that may be present in a lithium compound or a solution that comprises lithium.
[0061] As used herein, the term “process fluid” refers to any liquid or solution that used in any step or process according to the methods and systems for lithium recovery from a liquid resource as described herein. In some embodiments, the process fluid is the liquid resource. In some embodiments, the process fluid is the adjusting fluid. In some embodiments, the process fluid is the raffinate. In some embodiments, the process fluid is water. In some embodiments, theprocess fluid is acid (e.g., an acidic solution, a solution comprising acid). In some embodiments, the process fluid is base (e.g., a basic solution, a solution comprising base).
[0062] As used herein, the term “buffer” refers to a solution that can resist pH change upon the addition of an acidic or basic components. A buffer can neutralize small amounts of added acid or base, thus maintaining the pH of a solution comprising the buffer. In some embodiments, a buffer is a solution comprising a weak acid and a salt of the corresponding conjugate base. In some embodiments, a buffer is a solution comprising a weak base and a salt of the corresponding conjugate acid. A non-limiting example of a buffer is a solution of boric acid and sodium hydroxide.
[0063] The term “mother liquor,” as used herein, is a liquid byproduct of a process for the generation of solid lithium carbonate from a lithium-containing solution. Mother liquor as described herein is an aqueous solution that comprises lithium and additional salts.
[0064] In some embodiments of the systems and methods and processes disclosed herein, an ion exchange material is contacted with a liquid resource comprising lithium. The lithium in the liquid resource is absorbed by the ion exchange material to yield an enriched ion exchange material. In some embodiments, the enriched ion exchange material contains a higher lithium content then the ion exchange material. In some embodiments, the ion exchange material is a protonated ion exchange material. In some embodiments, the protonated ion exchange material is contacted with a liquid resource comprising lithium. The lithium in the liquid resource is absorbed via an ion exchange process to yield a lithiated ion exchange material. In some cases, the terms "enriched ion exchange material" and "lithiated ion exchange material" are used interchangeably.
[0065] In some embodiments, the chemical formula of the ion exchange material may vary throughout the ion exchange systems and processes described herein in terms of hydrogen and lithium stoichiometries, as the ion exchange materials readily exchange lithium and hydrogen depending on the aqueous solutions and gases that the ion exchange material is exposed to. In addition, fully lithiated or fully protonated ion exchange materials may not be the most stable form of the material, and is therefore commercially sold as another form. For example, many commercially available ion exchange materials benefit from an activation step or an initial treatment in which the material is wetted and activated with an acid wash to produce an ion exchange material that is in an ideal state for lithium absorption (termed pre-activated ion exchange materials herein). In some embodiments, the term “protonated ion exchange material” refers to material that has been activated and is capable of absorbing lithium. In some embodiments, the protonated ion exchange material is at least partially protonated. In some embodiments, the protonated ion exchange material is fully protonated. Following exposure to aliquid resource comprising lithium, the protonated ion exchange material absorbs lithium and releases hydrogen to form the lithiated ion exchange material. The stoichiometries of the ion exchange material and the lithiated ion exchange material may vary with both the lithium concentration of the liquid resource and the pH of the acidic solution. Therefore, in some embodiments, the material is in part best described by the solution or alternate phase the material has been exposed to most recently. As such, the term “ion exchange material” is meant to include the various states that the material may exist as throughout the ion exchange and preparatory process. In some embodiments, an ion exchange material comprises a protonated ion exchange material, a lithiated ion exchange material, and a pre-activated ion exchange material.
[0066] In some embodiments, the ion exchange material may benefit from an activation process. An ion exchange material that benefits from an activation process is termed “pre-activated ion exchange material.” In some embodiments, the pre-activated ion exchange material is selected from an oxide, a phosphate, an oxyfluoride, a fluorophosphate, and combinations thereof. In some embodiments, the pre-activated ion exchange material is selected Li4MnsOi2, L TisOn, Li2MO3(M = Ti, Mn, Sn), LiMn2O4, Lii.6Mm.6O4, LiM02(M = Al, Cu, Ti), Li4TiO4, Li7TinO24, Li3VO4, Li2Si3O7, LiFePO4, LiMnPO4, Li2CuP2O7, A1(OH)3, LiCl.xAl(OH)3.yH2O, SnO2.xSb2Os.yH2O, TiO2.xSb2Os.yH2O, solid solutions thereof, and combinations thereof. In some embodiments, the pre-activated ion exchange material is selected from the following list: LUMnsOn, Li4TisOi2, Lii.eMm.eC , Li2MO3(M = Ti, Mn, Sn), LiFePO4, solid solutions thereof, or combinations thereof.
[0067] In some embodiments, the processes described herein utilize lithium-selective sorbents that are exposed to a liquid resource and an acidic solution over the course of two or more cycles. The lithium-selective sorbent can be a protonated ion exchange material following exposure to an acidic solution that subsequently yields a lithiated ion exchange material following exposure to a liquid resource. Although the lithium-selective sorbents described herein are expressed as compounds with discrete stoichiometries, it should be understood that variable amounts of lithium ions and / or hydrogen ions are envisioned in each ion exchange material during the cyclic ion exchange processes described herein. For example, the lithiumselective sorbent that is the ion exchange material Li4TisOi2may be Li4TisOi2, Li3HTisOi2, Li2H2TisOi2, LiH3TisOi2, orH4TisOi2. Combinations of such states are also envisioned, and may be expressed as averages, for example LkiHi.MisOn, Li2 2Hi.8Ti50i2, Li2 3Hi.7Ti50i2, Li2 4Hi.6Ti50i2, etc. Applicant envisions that the lithium-selective sorbents that are the ion exchange materials listed below comprise the chemical entity listed, each compound that replaces one lithium ion for one hydrogen ion, and any combination of such states: Li4MnsOi2,Li4TisOi2, Li2MC>3 (M = Ti, Mn, Sn), LiMr^C , Li1.6Mn1.eO4, LiM02 (M = Al, Cu, Ti), Li4TiO4, Li7TinO24, LisVCU, Li2SisO7, LiFeP04, LiMnP04, and Li2CuP2O?.
[0068] In some embodiments, lithium-selective sorbent comprises an ion exchange material. In some embodiments, an ion exchange material comprises a chemical compound capable of exchanging lithium and hydrogen ions. In some embodiments, ion exchange material comprises a chemical compound capable of ion exchange of lithium and hydrogen, wherein the ion exchange material will uptake lithium selectively as opposed to uptaking other metals or metal ions (e.g., sodium, potassium, magnesium, other metal ions present in liquid resources). In some embodiments, ion exchange material is in the form of ion exchange particles. In some embodiments, ion exchange material or ion exchange beads comprise a coating material. In some embodiments, ion exchange material or ion exchange beads do not comprise a coating material. In some embodiments, ion exchange material is in the form of ion exchange beads. In some embodiments, ion exchange beads are porous.
[0069] The section headings used herein are for organizational purposes only and are not to be construed as limiting the subject matter described or preclude the combination of the subject matter of the disclosure under any one section heading with any other subject matter of the disclosure under any other section heading or any other subject matter of the disclosure. Embodiments described herein with any one or more features can be readily combined with the features of any embodiments described further herein. Embodiments described herein are not limiting so as to wholly describe all embodiments of the disclosure.Ion Exchange Materials, Particles, and Beads
[0070] In an aspect, disclosed herein are methods and systems for lithium recovery from a liquid resource. In some embodiments, the methods and systems disclosed herein utilize ion exchange materials. In some embodiments, an ion exchange material is utilized in a variety of forms or as a constituent of a construct that comprises one or more ion exchange materials. In some embodiments, an ion exchange material is utilized in a form that specifically enables or optimizes the performance of the method or system in which the ion exchange material is utilized. In some embodiments, an ion exchange material is utilized as a constituent of a construct that specifically enables or optimizes the performance of the method or system in which the ion exchange material is utilized. In some embodiments, ion exchange materials are coated. In some embodiments, ion exchange materials comprise a lithium-selective sorbent.
[0071] In some embodiments, ion exchange material is in the form of ion exchange particles. In some embodiments, ion exchange material is in the form of uncoated ion exchange particles. In some embodiments, ion exchange material is in the form of coated ion exchangeparticles. In some embodiments, ion exchange particles are coated or uncoated. In some embodiments, ion exchange particles are utilized as a mixture that comprises coated ion exchange particles and uncoated ion exchange particles. In some embodiments, ion exchange particles comprise one or more ion exchange materials. In some embodiments, ion exchange particles comprise a lithium-selective sorbent.
[0072] In some embodiments, ion exchange beads are a construct that comprises ion exchange material that can be used according to the methods and systems described herein. In some embodiments, ion exchange beads comprise ion exchange material. In some embodiments, the ion exchange material is coated or uncoated. In some embodiments, the ion exchange beads are porous.. In some embodiments, ion exchange beads comprise one or more ion exchange materials. In some embodiments, ion exchange beads comprise a lithium-selective sorbent.
[0073] Ion exchange beads can have diameters less than about one millimeter, contributing to a high pressure difference across a packed bed of ion exchange beads as a liquid resource and other fluids are pumped through the packed bed by application of an appropriate force. To minimize pressure across the packed bed of ion exchange beads and to minimize the associated appropriate force and amount of energy associated with applying said appropriate force, vessels with optimized geometries can be used to reduce the flow distance through the packed bed of ion exchange beads. These vessels can be networked with pH modulation units to achieve adequate control of the pH of the liquid resource.
[0074] In some embodiments, a network of vessels loaded with ion exchange beads comprises two vessels, three vessels, four vessels, five vessels, six vessels, seven vessels, eight vessels, nine vessels, 10 vessels, 11 vessels, 12 vessels, 13-14 vessels, 15-20 vessels, 20-30 vessels, 30-50 vessels, 50-70 vessels, 70-100 vessels, or more than 100 vessels.
[0075] In some embodiments, ion exchange material, or a form thereof, or a construct comprised thereof, is loaded into an ion exchange device described herein. In some embodiments, an ion exchange device comprises a column, tank, or vessel. In some embodiments, an ion exchange device is a component of a system for lithium recovery from a liquid resource. Alternating flows of liquid resource, eluent, and other process fluids are optionally flowed through an ion exchange device to extract lithium from the liquid resource and produce a synthetic lithium solution, which is eluted from the ion exchange device using an eluent. As liquid resource flows through the ion exchange device, the ion exchange material absorb lithium while releasing hydrogen, where both the lithium and hydrogen are cations. After the ion exchange material have absorbed lithium, an eluent is used to elute the lithium from the ion exchange material to produce a lithium eluate. A lithium eluate can be a synthetic lithiumsolution according to some embodiments. In some embodiments, an eluent comprises acid or an acid eluent.
[0076] Lithium is an essential element for batteries and other technologies. Lithium is found in a variety of liquid resources, including natural and synthetic brines and leachate solutions from minerals, clays, and recycled products. Lithium can be extracted from such liquid resources using an ion exchange process that utilizes ion exchange materials. In some embodiments, ion exchange beads comprise ion exchange materials in addition to other components. In some embodiments, ion exchange beads are utilized in methods for lithium recovery and systems for lithium recovery. Ion exchange materials can absorb lithium from a liquid resource while releasing hydrogen, and then elute lithium in acid while absorbing hydrogen. In methods for lithium recovery from a liquid resource, the ion exchange process can be repeated to extract lithium from a liquid resource and yield a synthetic lithium solution. The synthetic lithium solution can be further processed into chemicals for the battery industry or other industries.
[0077] In some embodiments, ion exchange particles comprise ion exchange materials. Ion exchange particles can be in the form of small particles, which together constitute a fine powder. Small sizes of ion exchange particles may be required to minimize the diffusion distance that lithium must travel to reach the core of the ion exchange particles and ensure the entirety of the ion exchange material within the ion exchange particle is utilized in the course of an ion exchange process or method for lithium recovery. In some cases, ion exchange particles are coated with coating materials that can minimize dissolution of the ion exchange particles while allowing efficient transfer of lithium and hydrogen to and from the ion exchange particles.
[0078] One major challenge for methods of lithium recovery from a liquid resource that comprise use of ion exchange particles is the loading of the ion exchange particles into an ion exchange device in such a way that liquid resource and acid flow through the ion exchange device with minimal clogging. Thus, ion exchange material and / or ion exchange particles can be formed into ion exchange beads that can be loaded into an ion exchange device. In some embodiments, ion exchange beads comprise ion exchange materials in addition to other components and can be utilized in methods for lithium recovery and systems for lithium recovery. The ion exchange beads, as loaded into an ion exchange device, can be loaded such that void spaces are present between the ion exchange beads, and these void spaces can facilitate flow of liquids through the column. In some embodiments, a flow is initiated, modulated, or terminated by pumping. In some embodiments, the ion exchange beads hold their constituent ion exchange particles in place and prevent free movement of ion exchange particles throughout the ion exchange device.
[0079] When ion exchange material is formed into ion exchange beads, the penetration of liquid resource and acid into the ion exchange beads by convention and diffusion can become unacceptably slow. A slow rate of convection and diffusion of the acid and liquid resource into the ion exchange beads can slow the kinetics of lithium absorption and release thereby. Slow kinetics of lithium absorption and release can create problems for the operation of an ion exchange device. Slow kinetics of lithium absorption and release can consequently require correspondingly slow flow rates through an ion exchange device. Slow kinetics of lithium absorption and release can also lead to low lithium recovery from the liquid resource and inefficient use of acid to elute the lithium according to the methods and systems described herein.
[0080] In some embodiments, the ion exchange beads comprise networks of pores that facilitate the transport of liquids flowed through an ion exchange device into the ion exchange beads. The geometry and physical dimensions of pore networks in ion exchange beads can be strategically controlled to allow for faster and more complete access of liquid resource, washing water, acid, and other process fluids into the interior of the ion exchange bead. Faster and more complete access of liquid resource, washing water, acid, and other process fluids into the interior of the ion exchange bead leads to a more effective delivery lithium and hydrogen to the ion exchange material therein. More effective delivery of lithium and hydrogen to the ion exchange material within an ion exchange bead can lead to greater lithium recovery according to the methods and systems described herein.
[0081] In some embodiments, the ion exchange beads are formed by mixing of ion exchange material, a structural matrix material, and a filler material. In some embodiments, the ion exchange beads are formed by mixing of ion exchange material and a structural matrix material. In some embodiments, the ion exchange beads are formed by mixing of ion exchange material and a structural matrix material. In some embodiments, the components of an ion exchange bead combined to form a physical mixture or a composite. In some embodiments wherein an ion exchange bead comprises a filler material, the filler material can be removed therefrom to form network of pores therein and yield a porous ion exchange bead. The filler material is dispersed in the bead in such a way to leave behind a pore structure that enables transport of lithium and hydrogen with fast kinetics. In some embodiments, an ion exchange bead comprises one or more ion exchange materials, one or more structural matrix materials, and one or more filler materials.
[0082] Ion exchange beads according to embodiments as described herein can be porous ion exchange beads.
[0083] Another challenge to consider and overcome in a method or system for lithium recovery from a liquid resource using ion exchange materials is the undesired dissolution and degradation of the ion exchange materials. Undesired dissolution and degradation of the ion exchange materials can occur during a step comprising lithium elution from the ion exchange material in acid. Undesired dissolution and degradation of the ion exchange materials can occur during a step comprising lithium extraction from a liquid resource by the ion exchange material. In some embodiments, to yield a synthetic lithium solution from the ion exchange process it is desirable to use a concentrated acid solution as an acid eluent in a step comprising lithium elution from the ion exchange material. However, concentrated acid solutions dissolve and degrade ion exchange materials, which can decrease the performance and useful lifetime of the materials. Therefore, in some embodiments the ion exchange beads contain coated ion exchange particles that are comprised of an ion exchange material and a coating material. The coating material can protect the ion exchange material from undesired dissolution and degradation during lithium elution from the ion exchange material into acid, during lithium uptake from a liquid resource into the ion exchange material, and during other steps of an ion exchange process according to the methods and systems described herein. In some embodiments, use of ion exchange beads that comprise coated ion exchange particles allows for the use of a concentrated acid as an acid eluent to yield a synthetic lithium solution.
[0084] In one aspect described herein, an ion exchange material is selected for use in ion exchange beads based on one or more properties of the ion exchange material. In some embodiments, desirable properties of the ion exchange material comprise high lithium absorption capacity, high selectivity for lithium extraction from a liquid resource relative to extraction of other ions such as sodium and magnesium, strong lithium uptake in liquid resources including those with low concentrations of lithium, facile elution of lithium with a small excess of acid, fast ionic diffusion throughout the ion exchange material, combinations thereof, and sub-combinations thereof. In one aspect described herein, a coating material is selected for use as a coating for ion exchange particles based on its ability to prevent undesirable dissolution and chemical degradation of the ion exchange particles during lithium elution from the ion exchange particles in acid and also during lithium uptake by the ion exchange particles from liquid resources. In some embodiments, the coating material is selected to facilitate one or more of the following objectives: using a coating material that has minimal negative impacts on the diffusion of lithium and hydrogen between the ion exchange material within the ion exchange particles and the liquid resource, enabling adherence of the ion exchange particles to a structural support or structural matrix material, and suppressing structural and mechanical degradation of the ion exchange particles.
[0085] In some embodiments, wherein ion exchange beads are used in an ion exchange device, the liquid resource containing lithium is flowed through the ion exchange device so that the ion exchange beads absorb lithium from the liquid resource while releasing hydrogen. After the ion exchange beads have absorbed lithium, an acid is pumped through the ion exchange device so that the ion exchange beads release lithium into the acid while absorbing hydrogen. In some embodiments, the ion exchange device is operated in a co-flow mode wherein the liquid resource and acid are alternately flowed through the ion exchange device in the same direction. In some embodiments, the ion exchange device is operated in counter-flow mode wherein the liquid resource and acid are alternately flowed through the ion exchange device in opposite directions. In some embodiments, in between flows of the liquid resource and flows of acid, water or other solutions is flowed through the ion exchange device for purposes such as adjusting pH in the ion exchange device or removing potential contaminants. In some embodiments, ion exchange beads form a fixed bed or a moving bed, wherein the moving bed can move in a direction opposed to the flows of liquid resource and acid. In some embodiments, ion exchange beads are moved between multiple ion exchange devices, wherein the ion exchange beads form a moving bed that can be transferred from one ion exchange device to another. In some embodiments, ion exchange beads are moved between multiple ion exchange devices, wherein different ion exchange devices are independently configured to accommodate a flow of liquid resource, a flow of acid, a flow of water, or a flow of another process fluid. In some embodiments, before or after the liquid resource is flowed through an ion exchange device, the liquid resource is subjected to other processes including other ion exchange processes, solvent extraction, evaporation, chemical treatment, precipitation to remove lithium, precipitation to remove other chemical species, or to otherwise treat the liquid resource.
[0086] In some embodiments, wherein ion exchange particles are used in an ion exchange device, the liquid resource containing lithium is flowed through the ion exchange device so that the ion exchange particles absorb lithium from the liquid resource while releasing hydrogen. After the ion exchange particles have absorbed lithium, an acid is pumped through the ion exchange device so that the ion exchange particles release lithium into the acid while absorbing hydrogen. In some embodiments, the ion exchange device is operated in a co-flow mode wherein the liquid resource and acid are alternately flowed through the ion exchange device in the same direction. In some embodiments, the ion exchange device is operated in counter-flow mode wherein the liquid resource and acid are alternately flowed through the ion exchange device in opposite directions. In some embodiments, in between flows of the liquid resource and flows of acid, water or other solutions are flowed through the ion exchange device for purposes such as adjusting pH in the ion exchange device or removing potentialcontaminants. In some embodiments, ion exchange particles form a fixed bed or a moving bed, wherein the moving bed can move in a direction opposed to the flows of liquid resource and acid. In some embodiments, ion exchange particles are moved between multiple ion exchange devices, wherein the ion exchange particles form a moving bed that can be transferred from one ion exchange device to another. In some embodiments, ion exchange particles are moved between multiple ion exchange devices, wherein different ion exchange devices are independently configured to accommodate a flow of liquid resource, a flow of acid, a flow of water, or a flow of another process fluid. In some embodiments, before or after the liquid resource is flowed through an ion exchange device, the liquid resource is subjected to other processes including other ion exchange processes, solvent extraction, evaporation, chemical treatment, precipitation to remove lithium, precipitation to remove other chemical species, or to otherwise treat the liquid resource.
[0087] In some embodiments, when ion exchange material is treated with acid a synthetic lithium solution is produced. In some embodiments, the synthetic lithium solution is further processed to produce lithium chemicals. In some embodiments, lithium chemicals produced from synthetic lithium solutions are provided for an industrial application. In some embodiments, lithium chemicals produced from synthetic lithium solutions are further processed to produce one or more alternative lithium chemicals that are contemplated for use in an application for which the one or more alternative lithium chemicals is better suited as compared to the lithium chemicals.
[0088] In some embodiments, an ion exchange material is selected from the following list: an oxide, a phosphate, an oxyfluoride, a fluorophosphate, or combinations thereof. In some embodiments, an ion exchange material is selected from the following list: I^MnsOn, Li4TisOi2, Li2MC>3 (M = Ti, Mn, Sn), LiMn2O4, Li1.6Mn1.eO4, LiM02 (M = Al, Cu, Ti), Li4TiO4, Li7TiiiO24, Li3VO4, Li2Si3O7, LiFePO4, LiMnPO4, Li2CuP2O7, A1(OH)3, LiCl.xAl(OH)3.yH2O, SnO2.xSb2O5.yH2O, TiO2.xSb2O5.yH2O, solid solutions thereof, or combinations thereof. In some embodiments, an ion exchange material is selected from the following list: Li4MnsOi2, Li4TisOi2, Li1.6Mn1.eO4, Li2MO3(M = Ti, Mn, Sn), LiFePO4, solid solutions thereof, or combinations thereof.
[0089] In some embodiments, a coating material used to form a coating on an ion exchange material or on ion exchange particles that comprise an ion exchange material is selected from the following list: a carbide, a nitride, an oxide, a phosphate, a fluoride, a polymer, carbon, a carbonaceous material, or combinations thereof. In some embodiments, a coating material is selected from the following list: TiCh, ZrCh, MoO2, SnCh, bfeOs, Ta20s, SiCh, Li2TiO3, Li2ZrO3, Li2SiO3, Li2MnO3, Li2MoO3, LiNbO3, LiTaO3, AIPO4, LaPCL, ZrP2O7,MOP2O7, MO2P3O12, BaS04, AIF3, SiC, TiC, ZrC, SisN4, ZrN, BN, carbon, graphitic carbon, amorphous carbon, hard carbon, diamond-like carbon, solid solutions thereof, or combinations thereof. In some embodiments, a coating material is selected from the following list: TiCh, ZrCh, MoO2, SiCh, Li2TiC>3, Li2ZrO3, Li2SiO3, Li2MnO3, LiNbCh, AIF3, SiC, SisN4, graphitic carbon, amorphous carbon, diamond-like carbon, or combinations thereof.
[0090] In some embodiments, the ion exchange particles have an average diameter that is selected from the following list: less than 10 nm, less than 100 nm, less than 1,000 nm, less than 10,000 nm, or less than 100,000 nm. In some embodiments, the ion exchange particles have an average size that is selected from the following list: less than 200 nm, less than 2,000 nm, or less than 20,000 nm.
[0091] It is recognized that measurements of average particle diameter can vary according to the method of determination utilized. Determination of said average particle diameter according to one method to obtain one or more values shall be understood to inherently encompass all other values that may be obtained using other methods. The average particle diameter can be determined using sieve analysis. The average particle diameter can be determined using optical microscopy. The average particle diameter can be determined using electron microscopy. The average particle diameter can be determined using laser diffraction. In some embodiments, the average particle diameter is determined using laser diffraction, wherein a Bettersizer ST instrument is used. In some embodiments, the average particle diameter is determined using a Bettersizer ST instrument. In some embodiments, the average particle diameter is determined using laser diffraction, wherein an Anton-Parr particle size analyzer (PSA) instrument is used. In some embodiments, the average particle diameter is determined using an Anton-Parr PSA instrument. The average particle diameter can be determined using dynamic light scattering. The average particle diameter can be determined using static image analysis. The average particle diameter can be determined using dynamic image analysis.
[0092] In some embodiments, the ion exchange particles are secondary particles comprised of smaller primary particles that have an average diameter selected from the following list: less than 10 nm, less than 100 nm, less than 1,000 nm, or less than 10,000 nm. In some embodiments, smaller primary particles comprise an ion exchange material.
[0093] In some embodiments, the ion exchange material or the ion exchange particles comprising an ion exchange material have a coating comprising a coating material with a thickness selected from the following list: less than 1 nm, less than 10 nm, less than 100 nm, or less than 1,000 nm. In some embodiments, the coating material has a thickness selected from the following list: less than 1 nm, less than 10 nm, or less than 100 nm.
[0094] In some embodiments, the ion exchange material and the coating material form one or more concentration gradients such that the chemical composition of coated ion exchange particles comprising the ion exchange material and the coating material ranges between two or more compositions. In some embodiments, the ion exchange material and the coating material form a concentration gradient within the coated ion exchange particles comprising the ion exchange material and the coating material that extends over a thickness selected from the following list: less than 1 nm, less than 10 nm, less than 100 nm, less than 1,000 nm, less than 10,000 nm, or less than 100,000 nm.
[0095] In some embodiments, coating thickness may be measured by any one or more of electron microscopy, optical microscopy, couloscopy, nanoindentation, atomic force microscopy, and X-ray fluorescence. In some embodiments, coating thickness may be inferred or extrapolated from data obtained according to an analytical method that indicates the bulk composition of the coated ion exchange particle, or the ion exchange material that further comprises the coating material. In some embodiments, coating thickness may be inferred by differential analysis of data obtained by analysis of ion exchange material that further comprises a coating material and data obtained by analysis ion exchange material that does not further comprise a coating material. In some embodiments, coating thickness may be inferred by differential analysis of data obtained by analysis of one or more coated ion exchange particles and data obtained by analysis of one or more uncoated ion exchange particles.
[0096] In some embodiments, the ion exchange material is synthesized by a method selected from the following list: hydrothermal, solvothermal, sol-gel, solid state, molten salt flux, ion exchange, microwave, ball milling, precipitation, or vapor deposition. In some embodiments, the ion exchange material is synthesized by a method selected from the following list: hydrothermal, solid state, or microwave.
[0097] In some embodiments, a coating material is deposited to form a coating by a method selected from the following list: chemical vapor deposition, atomic layer deposition, physical vapor deposition, hydrothermal, solvothermal, sol-gel, solid state, molten salt flux, ion exchange, microwave, wet impregnation, precipitation, titration, aging, ball milling, or combinations thereof. In some embodiments, the coating material is deposited to form a coating by a method selected from the following list: chemical vapor deposition, hydrothermal, titration, solvothermal, wet impregnation, sol-gel, precipitation, microwave, or combinations thereof.
[0098] In some embodiments, a coating material is deposited to form a coating with physical characteristics selected from the following list: crystalline, amorphous, full coverage, partial coverage, uniform, non-uniform, or combinations thereof.
[0099] In some embodiments, multiple coating materials are deposited to form multiple coatings on the ion exchange material in an arrangement selected from the following list: concentric, patchwork, or combinations thereof.
[0100] In some embodiments, the structural matrix material is selected from the following list: a polymer, an oxide, a phosphate, or combinations thereof. In some embodiments, a structural matrix material is selected from the following list: polyvinyl fluoride, polyvinylidene difluoride, polyvinyl chloride, poly vinylidene dichloride, polyethylene, polypropylene, polyphenylene sulfide, polytetrafluoroethylene, polytetrafluoroethylene, sulfonated polytetrafluoroethylene, polystyrene, polydivinylbenzene, polybutadiene, sulfonated polymer, carboxylated polymer, Nafion, copolymers thereof, and combinations thereof. In some embodiments, a structural matrix material is selected from the following list: polyvinylidene difluoride, polyvinyl chloride, sulfonated polytetrafluoroethylene, polystyrene, polydivinylbenzene, copolymers thereof, or combinations thereof. In some embodiments, a structural matrix material is selected from the following list: titanium dioxide, zirconium dioxide, silicon dioxide, solid solutions thereof, or combinations thereof. In some embodiments, the structural matrix material is selected for its thermal durability, acid resistance, and / or other chemical resistance.
[0101] In some embodiments, the porous ion exchange bead is formed by a process comprising mixing ion exchange particles, structural matrix material, and filler material together at once. In some embodiments, the porous ion exchange bead is formed by a process comprising mixing the ion exchange particles and the structural matrix material, and then mixing the resulting mixture with the filler material. In some embodiments, the porous ion exchange bead is formed by a process comprising mixing the ion exchange particles and the filler material, and then mixing the resulting mixture with the structural matrix material. In some embodiments, the porous ion exchange bead is formed by a process comprising mixing the structural matrix material and the filler material, and then mixing the resulting mixture with the ion exchange particles.
[0102] In some embodiments, the porous ion exchange bead is formed by a process comprising mixing the ion exchange particles, the structural matrix material, and / or the filler material with a solvent that dissolves one or more of the components of the mixture. In some embodiments, the porous ion exchange bead is formed by a process comprising mixing the ion exchange particles, the structural matrix material, and / or the filler material as dry powders in a mixer or ball mill. In some embodiments, the porous ion exchange bead is formed by a process comprising mixing the ion exchange particles, the structural matrix material, and / or the filler material in a spray drier.
[0103] In some embodiments, the structural matrix material is a polymer that is dissolved in a solvent and subsequently mixed with the ion exchange particles and / or filler material using a solvent from the following list: N-methyl-2-pyrrolidone, dimethyl sulfoxide, tetrahydrofuran, dimethylformamide, dimethylacetamide, methyl ethyl ketone, or combinations thereof. In some embodiments, the filler material is a salt that is dissolved in a solvent and subsequently mixed with the ion exchange particles and / or structural matrix material using a solvent from the following list: water, ethanol, isopropyl alcohol, acetone, or combinations thereof.
[0104] In some embodiments, the ion exchange beads comprise a filler material that is a salt that can be dissolved out of the ion exchange bead to form a network of pores within the ion exchange bead. In some embodiments, the ion exchange beads comprise a filler material that is a salt that can be dissolved out of the ion exchange bead using a solution selected from the following list: water, ethanol, isopropyl alcohol, a surfactant mixture, an acid, a base, or combinations thereof. In some embodiments, the ion exchange beads comprise a filler material that is a material that thermally decomposes to form a gas at high temperature such that the thermal decomposition of the filler material forms a network of pores within the ion exchange bead. In some embodiments, the ion exchange beads comprise a filler material that is a material that thermally decomposes to form a gas at high temperature wherein the gas is selected from the following list: water vapor, oxygen, nitrogen, chlorine, carbon dioxide, nitrogen oxides, organic vapors, or combinations thereof.
[0105] In some embodiments, the ion exchange beads are formed from dry powder. In some embodiments, the ion exchange beads are formed using a mechanical press, a pellet press, a tablet press, a pill press, a rotary press, or combinations thereof. In some embodiments, the ion exchange beads are formed from a solvent slurry by dripping the solvent slurry into a solution comprising a different solvent. In some embodiments, the solvent slurry comprises N-methyl-2- pyrrolidone, dimethyl sulfoxide, tetrahydrofuran, dimethylformamide, dimethylacetamide, methyl ethyl ketone, or combinations thereof. In some embodiments, the solution comprising a different solvent comprises water, ethanol, iso-propyl alcohol, acetone, or combinations thereof.
[0106] In some embodiments, the ion exchange beads are approximately spherical with an average diameter selected from the following list: less than 10 pm, less than 100 pm, less than 1 mm, less than 1 cm, or less than 10 cm. In some embodiments, the porous ion exchange bead are approximately spherical with an average diameter selected from the following list: less than 200 pm, less than 2 mm, or less than 20 mm.
[0107] In some embodiments, the ion exchange beads are tablet-shaped with a diameter of less than 1 mm, less than 2 mm, less than 4 mm, less than 8 mm, or less than 20 mm and with a height of less than 1 mm, less than 2 mm, less than 4 mm, less than 8 mm, or less than 20 mm.
[0108] In some embodiments, the ion exchange beads are embedded in a support structure, which can be a membrane, a spiral-wound membrane, a hollow fiber membrane, or a mesh. In some embodiments, the ion exchange beads are embedded on a support structure comprised of a polymer, a ceramic, or combinations thereof. In some embodiments, the ion exchange beads are loaded directly into an ion exchange column with no additional support structure.
[0109] In some embodiments, the liquid resource has a lithium concentration selected from the following list: less than 100,000 mg / L, less than 10,000 mg / L, less than 1,000 mg / L, less than 100 mg / L, less than 10 mg / L, or combinations thereof. In some embodiments, the liquid resource has a lithium concentration selected from the following list: less than 5,000 mg / L, less than 500 mg / L, less than 50 mg / L, or combinations thereof.
[0110] In some embodiments, the acid used for eluting lithium from the ion exchange material is selected from the following list: hydrochloric acid, sulfuric acid, phosphoric acid, hydrobromic acid, chloric acid, perchloric acid, nitric acid, formic acid, acetic acid, or combinations thereof. In some embodiments, the acid used for eluting lithium from the ion exchange material is selected from the following list: hydrochloric acid, sulfuric acid, nitric acid, or combinations thereof.[OHl] In some embodiments, the acid used for recovering lithium from the ion exchange material has an acid concentration selected from the following list: less than 0.1 M, less than 1.0 M, less than 5 M, less than 10 M, or combinations thereof.
[0112] In some embodiments, the ion exchange material is utilized in an ion exchange process repeatedly over a number of cycles selected from the following list: greater than 10 cycles, greater than 30 cycles, greater than 100 cycles, greater than 300 cycles, or greater than 1,000 cycles. In some embodiments, the ion exchange material is utilized in an ion exchange process repeatedly over a number of cycles selected from the following list: greater than 50 cycles, greater than 100 cycles, or greater than 200 cycles.
[0113] In some embodiments, a cycle comprises contacting a lithium-selective sorbent with a liquid resource to provide a lithiated lithium-selective sorbent and contacting the lithiated lithium-selective sorbent with an acidic solution (e.g., acid) to provide a synthetic lithium solution (e.g., lithium eluate). In some embodiments, the lithium-selective sorbent is used (e.g., a process for generating a synthetic lithium solution is conducted) for at least 10 cycles, at least 50 cycles, at least 100 cycles, at least 250 cycles, at least 500 cycles, at least 1000 cycles, at least2000 cycles, at least 3000 cycles, at least 4000 cycles, at least 5000 cycles, at least 6000 cycles, at least 7000 cycles, at least 8000 cycles, at least 9000 cycles, or at least 10000 cycles.
[0114] In some embodiments, the synthetic lithium solution that is yielded from the ion exchange material is further processed into lithium chemicals, lithium compounds, or lithium raw materials using methods selected from the following list: solvent extraction, ion exchange, chemical precipitation, electrodialysis, electrowinning, evaporation with direct solar energy, evaporation with concentrated solar energy, evaporation with a heat transfer medium heated by concentrated solar energy, evaporation with heat from a geothermal brine, evaporation with heat from combustion, or combinations thereof.
[0115] In some embodiments, the synthetic lithium solution that is yielded from the ion exchange material is further processed into lithium chemicals selected from the following list: lithium chloride, lithium carbonate, lithium hydroxide, lithium metal, lithium metal oxide, lithium metal phosphate, lithium sulfide, or combinations thereof. In some embodiments, the synthetic lithium solution that is yielded from the ion exchange material is further processed into lithium chemicals that are solid, liquid, hydrated, or anhydrous.
[0116] In some embodiments, the lithium chemicals produced using the synthetic lithium solution are used in an industrial application selected from the following list: lithium batteries, metal alloys, glass, grease, or combinations thereof. In some embodiments, the lithium chemicals produced using the synthetic lithium solution derived from the ion exchange material are used in an industrial application selected from the following list: lithium batteries, metal alloys, glass, grease, or combinations thereof. In some embodiments, the lithium chemicals produced using the synthetic lithium solution derived from the coated ion exchange particles are used in an application selected from the following list: lithium batteries, lithium-ion batteries, lithium sulfur batteries, lithium solid-state batteries, and combinations thereof.
[0117] In some embodiments, the ion exchange materials are synthesized in a lithiated state, wherein a sublattice of the ion exchange material is fully or partially occupied by lithium. In some embodiments, the ion exchange materials are synthesized in a hydrogenated state, wherein a sublattice of the ion exchange material is fully or partially occupied by hydrogen.The Lithium Selective Sorbent
[0118] For the purposes of this disclosure, the term lithium-selective sorbent comprises all lithium-selective ion exchange materials. Ion exchange materials that selectively absorb and release lithium ions are lithium-selective ion exchange materials. In some embodiments, ion exchange beads comprise a lithium-selective sorbent. In some embodiments, ion exchange particles comprise a lithium-selective sorbent. In some embodiments, lithium-selective sorbentscomprise an inorganic material that selectively absorbs lithium over other ions. In some embodiments, a lithium selective sorbent is a crystalline lithium salt aluminate, a lithium aluminum intercalate, LiCl 2A1(OH)3, crystalline aluminum trihydroxide (Al(0H)3), gibbsite, beyerite, nordstrandite, alumina hydrate, bauxite, amorphous aluminum trihydroxide, activated alumina layered lithium-aluminum double hydroxides, Li Ah OHjeCl, combinations thereof, compounds thereof, or solid solutions thereof.
[0119] Lithium-selective ion exchange materials can be used in a method for lithium recovery from a liquid resource. Lithium-selective ion exchange materials can be used in a system for lithium recovery from a liquid resource. Lithium-selective ion exchange materials can be used in an ion exchange device. Lithium-selective ion exchange materials absorb lithium from a liquid resource while releasing hydrogen, and then elute lithium in an eluent while absorbing hydrogen from the eluent. This ion exchange process is optionally repeated to extract lithium from a liquid resource and yield a synthetic lithium solution. The synthetic lithium solution is optionally further processed into chemicals for the battery industry or other industries.
[0120] The performance parameters of lithium recovery by an ion exchange material are reflected in the ability of the ion exchange material to absorb lithium from a liquid resource in high quantity and in high purity over long periods time. When a given amount of an ion exchange material contacts a given amount of liquid resource, wash solution, eluent solution, or other process fluids, the effectiveness of selective lithium absorption, washing, lithium release / elution, or other treatment depends on effective contact of process fluids with the ion exchange material. In some embodiments, effective contact implies that a given amount of ion exchange material is contacted with the same amount of process fluid, and that the composition of said fluid is the same as that contacting the entirety of the ion exchange material . As such, in some embodiments, it is essential that devices for lithium recovery be configured in a manner such that the ion exchange material can make uniform contact with process fluids. In some embodiments, uniform contact implies that a liquid resource from which lithium is extracted uniformly contacts an ion exchange material which absorbs lithium while releasing protons.
[0121] Optimizing the performance parameters of lithium recovery is advantageous for lithium production from liquid resources using ion exchange processes that utilize one or more ion exchange materials. Disclosed herein are methods and systems for optimizing the performance parameters of lithium recovery using ion exchange materials that comprise lithiumselective sorbents by adjusting the concentration of lithium and pH of a liquid resource to be placed in contact with the ion exchange material. Adjusting the concentration of lithium in aliquid resource can yield a concentration-adjusted liquid resource according to some embodiments.
[0122] Adjusting the concentration of lithium in a liquid resource can result in the most optimal utilization of an ion exchange material utilized for lithium recovery, and helps ensure a prolonged lifetime of the ion exchange material. In some embodiments, the concentration of lithium in a liquid resource is increased to result in the most optimal utilization of an ion exchange material. In some embodiments, the concentration of lithium in a liquid resource is decreased to result in the most optimal utilization of an ion exchange material. In some embodiments, the pH of the liquid resource is adjusted in addition to the concentration of lithium in a liquid resource to result in the most optimal utilization of an ion exchange material.
[0123] In some embodiments, the most optimal utilization of an ion exchange material results in improved or optimized performance parameters for lithium recovery. In some embodiments, improved or optimized performance parameters comprise a longer useful lifetime of the ion exchange material used in the methods and systems described herein. In some embodiments, improved or optimized performance parameters comprise a higher lithium production rate for flow of the same amount of liquid resource across the ion exchange material used in the methods and systems described herein. In some embodiments, improved or optimized performance parameters comprise a higher lithium purity of the lithium provided by the ion exchange material used in the methods and systems described herein. In some embodiments, improved or optimized performance parameters comprise a greater quantity of lithium provided by a given quantity of ion exchange material over its useful lifetime when the ion exchange material is used according to the methods and systems described herein. In some embodiments, improved or optimized performance parameters comprise an increase in overall lithium recovery.Embodiments Comprising Other Lithium-Selective Sorbents
[0124] According to some embodiments of methods and systems for lithium recovery from a liquid resource, lithium is extracted from the liquid resources using inorganic lithiumselective sorbents that absorb lithium ions preferentially over other ions. In some embodiments, lithium-selective sorbents comprise lithium-selective ion exchange materials. As used herein, the term “lithium-selective ion-exchange material” refers to embodiments of “lithium-selective sorbent”. In some embodiments, the lithium-selective sorbent is a lithium-selective ionexchange material. In some embodiments, the lithium-selective sorbent comprises lithiumselective ion-exchange beads. In some embodiments, the lithium selective sorbent comprises ion exchange beads. In some embodiments, the lithium-selective sorbent comprises lithium-selective -3 Ilion-exchange particles. In some embodiments, the lithium selective sorbent comprises ion exchange particles. In some embodiments, the lithium-selective sorbent is an ion exchange material.
[0125] In some embodiments, lithium-selective sorbents include other inorganic materials that selectively absorb lithium over other ions. In some embodiments, lithium-selective sorbents selectively absorb lithium over other ions by processes that do not comprise ion exchange. In some embodiments, the lithium-selective sorbent is a crystalline lithium salt aluminate, a lithium aluminum intercalate, LiCl*2Al(OH)3, crystalline aluminum trihydroxide (Al(0H)3), gibbsite, beyerite, nordstrandite, alumina hydrate, bauxite, amorphous aluminum trihydroxide, activated alumina layered lithium-aluminum double hydroxides, Li A12(OH)eCl, combinations thereof, compounds thereof, or solid solutions thereof.
[0126] An aspect of the invention described herein is a device wherein the lithiumselective sorbent comprises an ion exchange material. An aspect of the invention described herein is a process wherein the lithium-selective sorbent comprises an ion-exchange material. An aspect of the invention described herein is a system wherein the lithium-selective sorbent comprises an ion-exchange material. An aspect of the invention described herein is a lithiumselective sorbent which extracts lithium from a liquid resource.
[0127] An aspect of the disclosure is a device, system, and associated process wherein the lithium-selective sorbent comprises a lithium aluminate intercalate. In some embodiments, the lithium aluminate intercalate mixed with a polymer material. In some embodiments, the polymer material comprises a chloro-polymer, a fluoro-polymer, a chloro-fluoro-polymer, a hydrophilic polymer, a hydrophobic polymer, co-polymers thereof, mixtures thereof, or combinations thereof. In some embodiments, the polymer material comprises a co-polymer, a block co-polymer, a linear polymer, a branched polymer, a cross-linked polymer, a heat-treated polymer, a solution processed polymer, co-polymers thereof, mixtures thereof, or combinations thereof. In some embodiments, the polymer material comprises low density polyethylene, high density polyethylene, polypropylene, polyester, polytetrafluoroethylene (PTFE), types of polyamide, polyether ether ketone (PEEK), polysulfone, polyvinylidene fluoride (PVDF), poly (4-vinyl pyridine-co-styrene) (PVPCS), polystyrene (PS), polybutadiene, acrylonitrile butadiene styrene (ABS), polyvinyl chloride (PVC), ethylene tetrafluoroethylene polymer (ETFE), poly (chlorotrifluoroethylene) (PCTFE), ethylene chlorotrifluoro ethylene (Halar), polyvinylfluoride (PVF), fluorinated ethylene-propylene (FEP), perfluorinated elastomer, chlorotrifluoroethylenevinylidene fluoride (FKM), perfluoropoly ether (PFPE), perfluoro-3,6- dioxa-4-methyl-7-octene-sulfonic acid (NAFION® (copolymer of perfluoro-3,6-dioxa-4- methyl-7-octene-sulfonic acid and tetrafluoroethylene)), polyethylene oxide, polyethyleneglycol, sodium polyacrylate, polyethylene-block-poly(ethylene glycol), polyacrylonitrile (PAN), polychloroprene (neoprene), polyvinyl butyral (PVB), expanded polystyrene (EPS), polydivinylbenzene, co-polymers thereof, mixtures thereof, or combinations thereof. In some embodiments, the polymer material comprises polyvinylidene fluoride (PVDF), polyvinyl chloride (PVC), ethylene chlorotrifluoro ethylene (Halar), poly (4-vinyl pyridine-co-styrene) (PVPCS), polystyrene (PS), acrylonitrile butadiene styrene (ABS), expanded polystyrene (EPS), polyphenylene sulfide, sulfonated polymer, carboxylated polymer, other polymers, co-polymers thereof, mixtures thereof, or combinations thereof. In some embodiments, the polymer material is combined with the lithium aluminate intercalate particles by dry mixing, mixing in solvent, emulsion, extrusion, bubbling one solvent into another, casting, heating, evaporating, vacuum evaporation, spray drying, vapor deposition, chemical vapor deposition, microwaving, hydrothermal synthesis, polymerization, co-polymerization, cross-linking, irradiation, catalysis, foaming, other deposition methods, or combinations thereof. In some embodiments, the polymer material is combined with the lithium aluminate intercalate particles using a solvent comprising N-methyl-2-pyrrolidone, dimethyl sulfoxide, tetrahydrofuran, dimethylformamide, dimethylacetamide, methyl ethyl ketone, ethanol, acetone, other solvents, or combinations thereof. In a further aspect, a coating can be deposited onto the lithium aluminate intercalate particles using a solvent comprising N-methyl-2-pyrrolidone, dimethyl sulfoxide, tetrahydrofuran, dimethylformamide, dimethylacetamide, methyl ethyl ketone, ethanol, acetone, or combinations thereof.
[0128] In some embodiments, the lithium aluminate intercalate comprises particles that have an average diameter less than about 10 nm, less than about 100 nm, less than about 1,000 nm, less than about 10,000 nm, or less than about 100,000 nm. In some embodiments, the lithium aluminate intercalate comprises particles that have an average size less than about 100 nm, less than about 1,000 nm, or less than about 10,000 nm. In some embodiments, the lithium aluminate intercalate particles comprise secondary particles comprised of smaller primary particles wherein the smaller primary particles have an average diameter less than about 10 nm, less than about 100 nm, less than about 1,000 nm, less than about 10,000 nm, or less than about 100,000 nm.
[0129] In a further aspect described herein, the lithium aluminate intercalate particles have an average diameter less than about 10 nm, less than about 100 nm, less than about 1,000 nm, less than about 10,000 nm, or less than about 100,000 nm. In a further aspect, the lithium aluminate intercalate particles have an average size less than about 100 nm, less than about 1,000 nm, or less than about 10,000 nm. In a further aspect, the lithium aluminate intercalate particles are optionally secondary particles comprised of smaller primary particles that have anaverage diameter less than about 10 nm, less than about 100 nm, less than about 1,000 nm, less than about 10,000 nm, or less than about 100,000 nm.Embodiments Comprising One or More Filler Materials Mixed within a Bed of Lithium- Selective Sorbent
[0130] In some embodiments, the ion exchange material is loaded into an ion exchange device as described herein, wherein the ion exchange material absorbs lithium from a liquid resource placed into contact therewith. In some embodiments, the ion exchange material is loaded into an ion exchange device as described herein, and a non-sorbent material is co-loaded into the same ion exchange device. In some embodiments, the non-sorbent material is inert to all process fluids used in a method or system for lithium recovery from a liquid resource. In some embodiments, the non-sorbent material is inert to liquid resource. In some embodiments, the non-sorbent material is inert to acid. In some embodiments, the non-sorbent material is inert to washing water. In some embodiments, the non-sorbent material is inert to base.
[0131] In some embodiments, the lithium-selective sorbent is loaded into an ion exchange device as described herein, wherein the lithium-selective sorbent absorbs lithium from a liquid resource placed into contact therewith. In some embodiments, the lithium-selective sorbent comprises an ion exchange material. In some embodiments, the lithium-selective sorbent is loaded into an ion exchange device as described herein, and a non-sorbent material is coloaded into the same ion exchange device. In some embodiments, the non-sorbent material is inert to all process fluids used in a method or system for lithium recovery from a liquid resource. In some embodiments, the non-sorbent material is inert to liquid resource. In some embodiments, the non-sorbent material is inert to acid. In some embodiments, the non-sorbent material is inert to washing water. In some embodiments, the non-sorbent material is inert to base.
[0132] In some embodiments, the non-sorbent material is termed a “filler material”, “inert material”, “packing material”, or “packing” such that these terms can be used interchangeably in the present disclosure. In some embodiments, the non-sorbent material is coloaded into an ion exchange device with a lithium-selective sorbent. In some embodiments, the lithium-selective sorbent is loaded into the ion exchange device first, and the non-sorbent material is subsequently loaded into the ion exchange device. In some embodiments, the non- sorbent material is loaded into the ion exchange device first, and the lithium-selective sorbent is subsequently loaded into the ion exchange device. In some embodiments, loading of the ion exchange device is alternated between non-sorbent material, lithium-selective sorbent, or a mixture thereof, until the ion exchange device is loaded to the intended loading -level. In someembodiments, the non-sorbent material is removed from the ion exchange device after the ion exchange device is loaded with the lithium-selective sorbent.
[0133] In some embodiments, the filler material comprises glass, silica, gravel, activated carbon, ceramic, alumina, zeolite, calcite, diatomaceous earth, cellulose, polymers, copolymers, titanium foam, titanium sponge, mixtures thereof or combinations thereof. In some embodiments, the filler material comprises a porous material. In some embodiments, the filler material is diatomaceous earth. For the purposes of this disclosure, the term “diatomaceous earth” also refers to “diatomite” or “kieselgur / kieselguhr”, or “celite”. In some embodiments, the filler material comprises polycarbonate, polyvinyl chloride, high density polyethylene, low density polyethylene, polylactic acid, polyimide, poly(methyl methacrylate), polypropylene, polyvinylidene difluoride, polytetrafluoroethylene, polystyrene, acrylonitrile butadiene styrene, poly ether ether ketone, copolymers thereof, mixtures thereof, or combinations thereof. In some embodiments, the filler material is placed on top of the vessel, on the bottom of the vessel, or both. In some embodiments, the filler material is mixed with the ion exchange material, a form thereof, or a construct comprised thereof. Another aspect described herein are ion exchange devices for use according to the methods and systems for lithium recovery from a liquid resource as described herein, wherein the ion exchange device comprises a vessel loaded with one or more beds comprising ion exchange material and a filler material, wherein the filler material is mixed with the one or more beds of ion exchange material, thereby providing support for the one or more beds and / or enabling for better flow distribution of the liquid resource or process fluid entering, passing through, or exiting the vessel. In some embodiments, better flow distribution ensures that each quantity or incremental sub-quantity of the ion exchange material within the ion exchange bed contacts the same amount of liquid resource or process fluid and that the hydrostatic pressure required to achieve the desired rate of flow across the bed is about uniform across the surface and within cross sections of the ion exchange bed. In some embodiments, better flow distribution is efficient flow distribution.
[0134] In some embodiments, efficient flow distribution within the ion exchange device occurs via one or more shaped objects or particles that are packed within one or more of the compartments that comprise the ion exchange device. In some embodiments, the filler material comprises one or more shaped objects or particles. In some embodiments, the filler material is comprised of objects or particles shaped as a sphere, spheroid, ovaloid, cross, tube, torus, ring, saddle ring, tubes, triangles, other complex geometric shape, or combinations thereof. In some embodiments, the filler material is distributed in an ion exchange device with a random particle density. In some embodiments, the filler material is distributed in an ion exchange device with a uniform particle density. In some embodiments, the filler material comprises one of more typesof filler material, randomly added and distributed within the ion exchange device. In some embodiments, the filler material consists of one of more types of filler material, added and distributed within the ion exchange device within well-defined regions. In some embodiments, parts, chambers, compartments, or vessels of the of the ion exchange device are empty while other parts, chambers, compartments, or vessels of the same ion exchange device contain filler material.
[0135] In some embodiments, the non-sorbent material increases the flow uniformity of the liquid resource through the bed of lithium-selective sorbent mixed with the non-sorbent material, as compared to the flow uniformity when the liquid resource flows through a bed of lithium-selective sorbent that is not mixed with a non-sorbent material. In some embodiments, the fluid pressure required to flow a liquid resource through a bed of lithium-selective sorbent mixed with the non-sorbent material is lower than the fluid pressure required to flow a liquid resource through a bed of lithium-selective sorbent with similar length and at a similar flow rate.
[0136] In some embodiments, the filler material is shaped as a sphere, spheroid, ovaloid, cross, tube, torus, ring, saddle ring, tubes, triangles, other complex geometric shape, or a combination thereof. In some embodiments, the filler material is distributed with a random particle density. In some embodiments, the filler material is distributed with uniform particle density. In some embodiments, the filler material comprises one of more types of filler material, randomly added and distributed within the ion exchange device. In some embodiments, the non- sorbent material comprises one of more types of non-sorbent material, randomly added and distributed within the ion exchange device. In some embodiments, the filler material comprises one of more types of filler material, added and distributed within the ion exchange device within well-defined regions. In some embodiments, parts, chambers, compartments, or vessels of the of the ion exchange device are empty, and parts, chambers, compartments, or vessels of the same ion exchange device contain filler material. In some embodiments, one end of the ion exchange device containing the lithium-selective sorbent comprises a packed bed of non-sorbent material, such that the liquid resource comprising lithium enters the ion exchange device and first contacts the lithium-selective sorbent, followed by the non-sorbent material. In some embodiments, one end of the ion exchange device containing the lithium-selective sorbent comprises a packed bed of non-sorbent material, such that the liquid resource comprising lithium enters the ion exchange device and first contacts the non-sorbent material, followed by the lithium-selective sorbent. In some embodiments, both ends of the ion exchange device containing the lithium-selective sorbent comprise a packed bed of non-sorbent material, such that the liquid resource comprising lithium enters the ion exchange device and first contacts the non-sorbent material, followed by the lithium-selective sorbent, followed by the same or a different non-sorbent material. In someembodiments, one or more parts, chambers, compartments, or vessels of the ion exchange device containing the lithium-selective sorbent comprise a packed bed of non-sorbent material, such that the liquid resource comprising lithium enters the parts, chambers, compartments, or vessels of the ion exchange device and alternates between contacting the non-sorbent material, followed by the lithium-selective sorbent.
[0137] In some embodiments, the non-sorbent material comprises particles with an average diameter of less than about 10 pm, less than about 20 pm, less than about 30 pm, less than about 40 pm, less than about 50 pm, less than about 60 pm, less than about 70 pm, less than about 80 pm, less than about 90 pm, less than about 100 pm, less than about 200 pm, less than about 300 pm, less than about 400 pm, less than about 500 pm, less than about 600 pm, less than about 700 pm, less than about 800 pm, less than about 900 pm, less than about 1000 pm, less than about 2000 pm; more than about 10 pm, more than about 20 pm, more than about 30 pm, more than about 40 pm, more than about 50 pm, more than about 60 pm, more than about 70 pm, more than about 80 pm, more than about 90 pm, more than about 100 pm, more than about 200 pm, more than about 300 pm, more than about 400 pm, more than about 500 pm, more than about 600 pm, more than about 700 pm, more than about 800 pm, more than about 900 pm, more than about 1000 pm, more than about 2000 pm. In some embodiments, the non-sorbent material comprises particles with an average diameter of from about 1 pm to about 5 pm, from about 5 pm to about 10 pm, from about 10 pm to about 20 pm, from about 20 pm to about 40 pm, from about 40 pm to about 80 pm, from about 80 pm to about 200 pm, from about 100 pm to about 400 pm, from about 200 pm to about 800 pm, from about 400 pm to about 1000 pm, from about 600 pm to about 2000 pm, from about 1000 pm to about 2000 pm. In some embodiments, the non-sorbent material comprises particles with an average diameter from about 10 pm to about 200 pm.
[0138] In some embodiments, the non-sorbent material is porous. In some embodiments, the non-sorbent material has an average pore opening size of less than about 0.1 nm, less than about 1 nm, less than about 10 nm, less than about 100 nm, less than about 1 pm, less than about 10 pm, less than about 20 pm, less than about 30 pm, less than about 40 pm, less than about 50 pm, less than about 60 pm, less than about 70 pm, less than about 80 pm, less than about 90 pm, less than about 100 pm, less than about 200 pm, less than about 300 pm, less than about 400 pm, less than about 500 pm, less than about 600 pm, less than about 700 pm, less than about 800 pm, less than about 900 pm, less than about 1000 pm, less than about 2000 pm. In some embodiments, the non-sorbent material has an average pore opening size of more than about 0.1 nm, more than about 1 nm, more than about 10 nm, more than about 100 nm, more than about 1 pm, more than about 10 pm, more than about 20 pm, more than about 30 pm, more than about40 pm, more than about 50 pm, more than about 60 pm, more than about 70 pm, more than about 80 pm, more than about 90 pm, more than about 100 pm, more than about 200 pm, more than about 300 pm, more than about 400 pm, more than about 500 pm, more than about 600 pm, more than about 700 pm, more than about 800 pm, more than about 900 pm, more than about 1000 pm, more than about 2000 pm. In some embodiments, the non-sorbent material has an average pore opening size of rom about 0.1 nm to about 1 nm, from about 1 nm to about 10 nm, from about 10 nm to about 100 nm, from about 100 nm to about 1 pm, from 1 pm to about 10 pm, from about 1 pm to about 5 pm, from about 5 pm to about 10 pm, from about 10 pm to about 20 pm, from about 20 pm to about 40 pm, from about 40 pm to about 80 pm, from about 80 pm to about 200 pm, from about 100 pm to about 400 pm, from about 200 pm to about 800 pm, from about 400 pm to about 1000 pm, from about 600 pm to about 2000 pm, from about 1000 pm to about 2000 pm. In some embodiments, the non-sorbent material comprises particles with an average diameter from about 10 pm to about 200 pm.
[0139] In some embodiments, the packed density of the non-sorbent material is less than about 0.1 g / mL, less than about 0.5 g / mL, less than about 1 g / mL, less than about 3 g / mL nm, less than about 5 g / mL, less than about 10 g / mL. In some embodiments, the packed density of the non-sorbent material is more than about 0.1 g / mL, more than about 0.5 g / mL, more than about 1 g / mL, more than about 3 g / mL nm, more than about 5 g / mL, more than about 10 g / mL. In some embodiments, the packed density of the non-sorbent material is from about 0.1 g / mL to about 0.5 g / mL, from about 0.5 g / mL to about 1 g / mL, from about 0.5 g / mL to about 3 g / mL nm, from about 3 g / mL to about 5 g / mL, from about 5 g / mL to about 10 g / mL.
[0140] In some embodiments, the lithium-selective sorbent is loaded into the ion exchange device as a slurry or suspension. In some embodiments, the liquid component of the slurry is water, acid, base, or a solvent. In some embodiments, the percentage of liquid in the slurry is less than about 1 %, less than about, 2%, less than about 5 %, less than about 10 %, less than about 20%, less than about 50 %, less than about 75 %, less than about 90 %, more than about 1 %, more than about, 2%, more than about 5 %, more than about 10 %, more than about 20%, more than about 50 %, more than about 75 %, more than about 90 %, between about 0 % and 5%, between about 5 % and 10 %, between about 10% and 20 %, between about 20 % and 50 %, between about 50 % and 75 %, between about 75 % and 90 %, between about 90 % and 100 %. In some embodiments, the percentage of solids in the slurry is less than about 1 %, less than about, 2%, less than about 5 %, less than about 10 %, less than about 20%, less than about 50 %, less than about 75 %, less than about 90 %, more than about 1 %, more than about, 2%, more than about 5 %, more than about 10 %, more than about 20%, more than about 50 %, more than about 75 %, more than about 90 %, between about 0 % and 5%, between about 5 % and 10%, between about 10% and 20 %, between about 20 % and 50 %, between about 50 % and 75 %, between about 75 % and 90 %, between about 90 % and 100 %. In some embodiments, the ion exchange beads are loaded into the ion exchange device as a dry powder. In some embodiments, the ion exchange particles are loaded into the ion exchange device as a dry powder. In some embodiments, the lithium-selective sorbent is loaded into the ion exchange device as a dry powder.
[0141] In some embodiments, the non-sorbent material is loaded into the ion-exchange vessel as a slurry or suspension. In some embodiments, the liquid component of such slurry is water, acid, base, or a solvent. In some embodiments, the percentage of liquid in the slurry is less than about 1 %, less than about, 2%, less than about 5 %, less than about 10 %, less than about 20%, less than about 50 %, less than about 75 %, less than about 90 %, more than about 1 %, more than about, 2%, more than about 5 %, more than about 10 %, more than about 20%, more than about 50 %, more than about 75 %, more than about 90 %, between about 0 % and 5%, between about 5 % and 10 %, between about 10% and 20 %, between about 20 % and 50 %, between about 50 % and 75 %, between about 75 % and 90 %, between about 90 % and 100 %. In some embodiments, the percentage of solids in the slurry is less than about 1 %, less than about, 2%, less than about 5 %, less than about 10 %, less than about 20%, less than about 50 %, less than about 75 %, less than about 90 %, more than about 1 %, more than about, 2%, more than about 5 %, more than about 10 %, more than about 20%, more than about 50 %, more than about 75 %, more than about 90 %, between about 0 % and 5%, between about 5 % and 10 %, between about 10% and 20 %, between about 20 % and 50 %, between about 50 % and 75 %, between about 75 % and 90 %, between about 90 % and 100 %. In some embodiments, the non- sorbent material is loaded into the ion-exchange vessel as a dry powder.
[0142] In some embodiments, the non-sorbent material is mixed with the lithiumselective sorbent in a tank, then liquid is added and the contents are agitated to make a suspension, and the resulting suspension is loaded into the ion exchange device. In some embodiments, the liquid added to make the suspension is water, acid, base, or a solvent. In some embodiments, the percentage of liquid in the suspension is less than about 1 %, less than about, 2%, less than about 5 %, less than about 10 %, less than about 20%, less than about 50 %, less than about 75 %, less than about 90 %, more than about 1 %, more than about, 2%, more than about 5 %, more than about 10 %, more than about 20%, more than about 50 %, more than about 75 %, more than about 90 %, between about 0 % and 5%, between about 5 % and 10 %, between about 10% and 20 %, between about 20 % and 50 %, between about 50 % and 75 %, between about 75 % and 90 %, between about 90 % and 100 %. In some embodiments, the ion exchange beads are loaded into the ion-exchange vessel as a dry mixture. In some embodiments,the percentage of solids in the suspension is less than about 1 %, less than about, 2%, less than about 5 %, less than about 10 %, less than about 20%, less than about 50 %, less than about 75 %, less than about 90 %, more than about 1 %, more than about, 2%, more than about 5 %, more than about 10 %, more than about 20%, more than about 50 %, more than about 75 %, more than about 90 %, between about 0 % and 5%, between about 5 % and 10 %, between about 10% and 20 %, between about 20 % and 50 %, between about 50 % and 75 %, between about 75 % and 90 %, between about 90 % and 100 %. In some embodiments, the non-sorbent material and the lithium-selective sorbent are loaded into the ion exchange device as a dry mixture.The Liquid Resource
[0143] As a liquid resource flows through an ion exchange device, the ion exchange material absorbs lithium while releasing hydrogen, causing a decrease in the pH of the liquid resource from which lithium is being extracted. pH values of less than about 6 in said liquid resource result in sub-optimal performance of the ion-exchange process because the higher hydrogen concentrations found at low pH result in the reversal of ion-exchange, wherein hydrogen is absorbed while lithium is released. Said sub-optimal process performance is manifested as, but is not limited to, a slower uptake of lithium by the ion exchange material, lower purity of the lithium eluted from the ion exchange material, lower lithium uptake capacity of the ion exchange material, degradation of the ion exchange material, decreased lifetime of the ion exchange material which necessitates more frequent replacement thereof, slower elution of lithium from the ion exchange material in the presence of acid, and higher amounts of acid being required for the elution of lithium from the ion exchange material.
[0144] In some embodiments, the pH value of the liquid resource can be maintained above a value of 6 by addition of an alkali. In some embodiments, said alkali is added before flow of the liquid resource through a bed or ion exchange material, or after flow of said liquid resource through a bed of ion exchange material, but not within the bed of ion exchange material where the lithium extraction process occurs. In some embodiments, the pH of the liquid resource decreases to a suboptimal value of less than about 6 during the time it takes for the liquid resource to flow through a bed of ion exchange material. Thus, in some embodiments systems and methods described herein are used to moderate the decrease in pH of the liquid resource during contact of the liquid resource with ion exchange material.
[0145] In some embodiments, a system is used to adjust the concentration of lithium in the liquid resource before it contacts an ion exchange material that extracts lithium from the liquid resource while releasing protons into the liquid resource. In some embodiments, said system decreases the lithium concentration of the liquid resource, such that less lithium isabsorbed by the ion exchange material over the same amount of contact time, and therefore fewer protons are released into the liquid resource by the ion exchange material during this absorption process, leading to a higher pH of the liquid resource as it contacts the ion exchange material. In some embodiments, adjustment of the lithium concentration in the liquid resource is achieved by mixing the liquid resource with a raffinate stream, said raffinate stream comprising the liquid resource which has contacted ion exchange material to absorb a portion of the lithium. Raffinate or a raffinate stream can comprise a lithium-depleted liquid resource. A solution comprising a liquid resource and a raffinate can comprise a concentration-adjusted liquid resource according to some embodiments. As a result of combining a raffinate stream with a liquid resource, the lithium remaining in the raffinate stream will be put into contact with the ion exchange material more than once, leading to multiple contacts of said lithium with the ion exchange material and multiple opportunities for uptake of said lithium by the ion exchange material. The result is an increase in the overall recovery of lithium by the methods and systems described herein as compared to methods and systems that do not comprise combining a raffinate with a liquid resource prior to placing the resulting mixture in contact with an ion exchange material.
[0146] The production of lithium chemicals and lithium feedstocks suitable for industrial applications can involve the recovery of lithium from resources that contain lithium in addition to other components. Resources containing lithium in addition to other components can be a liquid resource. In some embodiments, the liquid resource is selected from the following list: a natural brine, a dissolved salt flat, a geothermal brine, seawater, concentrated seawater, desalination effluent, a concentrated brine, a processed brine, liquid from an ion exchange process, liquid from a solvent extraction process, a synthetic brine, leachate from ores, leachate from minerals, leachate from clays, leachate from sediments, leachate from recycled products, leachate from recycled materials, or combinations thereof. In some embodiments, a liquid resource is selected from the following list: a natural brine, a dissolved salt flat, a concentrated brine, a processed brine, a synthetic brine, a geothermal brine, liquid from an ion exchange process, liquid from a solvent extraction process, leachate from minerals, leachate from clays, leachate from recycled products, leachate from recycled materials, or combinations thereof. In some embodiments, the liquid resource is optionally pre-treated prior to entering the ion exchange reactor to remove suspended solids, hydrocarbons, organic molecules, iron, certain metals, or other chemical or ionic species. In some embodiments, the liquid resource is optionally fed into the ion exchange reactor without any pre-treatment. In some embodiments, the liquid resource is injected into a reservoir, salt lake, salt flat, basin, or other geologic deposit after lithium has been removed from the liquid resource. In some embodiments, other speciesare recovered from the liquid resource before or after lithium recovery. In some embodiments, the pH of the liquid resource is adjusted before, during, or after lithium recovery. In some embodiments, a method for lithium recovery comprises placing a liquid resource or a solution comprising a liquid resource into contact with ion exchange material. In some embodiments, the lithium concentration of the liquid resource is adjusted before, during, or after lithium recovery. In some embodiments, a liquid resource is an aqueous solution comprising lithium suitable for use according to the methods and systems for lithium recovery disclosed herein.
[0147] In one embodiment, the liquid resource is a natural brine, a dissolved salt flat, seawater, concentrated seawater, a geothermal brine, a desalination effluent, a concentrated brine, a processed brine, an oilfield brine, a liquid from an ion exchange process, a liquid from a solvent extraction process, a synthetic brine, a leachate from an ore or combination of ores, a leachate from a mineral or combination of minerals, a leachate from a clay or combination of clays, a leachate from recycled products, a leachate from recycled materials, or combinations thereof. In some embodiments, the liquid resource is a brine.
[0148] In one embodiment, the liquid resource is at a temperature of -20 to 20 °C, 20 to 50 °C, 50 to 100 °C, 100 to 200 °C, or 200 to 400 °C. In one embodiment, the liquid resource is heated or cooled to precipitate or dissolve species in the brine, or to facilitate removal of metals from the liquid resource.
[0149] In one embodiment, the liquid resource contains lithium at a concentration of less than 1 mg / L, 1 to 50 mg / L, 50 to 200 mg / L, 200 to 500 mg / L, 500 to 2,000 mg / L, 2,000 to 5,000 mg / L, 5,000 to 10,000 mg / L, 10,000 to 20,000 mg / L, 20,000 to 80,000 mg / L, or greater than 80,000 mg / L.
[0150] In one embodiment, the liquid resource contains magnesium at a concentration of 0.01 to 0.1 mg / L, 0.1 to 1 mg / L, 1 to 10 mg / L, 10 to 100 mg / L, 100 to 1,000 mg / L, 1,000 to 10,000 mg / L, 10,000 to 50,000 mg / L, 50,000 to 100,000 mg / L, 100,000 to 150,000 mg / L, or greater than 150,000 mg / L. In one embodiment, the liquid resource contains calcium at a concentration of 0.01 to 0.1 mg / L, 0.1 to 1 mg / L, 1 to 10 mg / L, 10 to 100 mg / L, 100 to 1,000 mg / L, 1,000 to 10,000 mg / L, 10,000 to 50,000 mg / L, 50,000 to 100,000 mg / L, 100,000 to 150,000 mg / L, or greater than 150,000 mg / L. In one embodiment, the liquid resource contains strontium at a concentration of 0.01 to 0.1 mg / L, 0.1 to 1 mg / L, 1 to 10 mg / L, 10 to 100 mg / L, 100 to 1,000 mg / L, 1,000 to 10,000 mg / L, 10,000 to 50,000 mg / L, 50,000 to 100,000 mg / L, 100,000 to 150,000 mg / L, or greater than 150,000 mg / L. In one embodiment, the liquid resource contains barium at a concentration of 0.01 to 0.1 mg / L, 0.1 to 1 mg / L, 1 to 10 mg / L, 10 to 100 mg / L, 100 to 1,000 mg / L, 1,000 to 10,000 mg / L, 10,000 to 50,000 mg / L, 50,000 to 100,000 mg / L, 100,000 to 150,000 mg / L, or greater than 150,000 mg / L.
[0151] In one embodiment, the liquid resource contains multivalent cations at a concentration of 0.01 to 0.1 mg / L, 0.1 to 1 mg / L, 1 to 10 mg / L, 10 to 100 mg / L, 100 to 1,000 mg / L, 1,000 to 10,000 mg / L, 10,000 to 50,000 mg / L, 50,000 to 100,000 mg / L, 100,000 to 150,000 mg / L, or greater than 150,000 mg / L. In one embodiment, the liquid resource contains multivalent ions at a concentration of 0.01 to 0.1 mg / L, 0.1 to 1 mg / L, 1 to 10 mg / L, 10 to 100 mg / L, 100 to 1,000 mg / L, 1,000 to 10,000 mg / L, 10,000 to 50,000 mg / L, 50,000 to 100,000 mg / L, 100,000 to 150,000 mg / L, or greater than 150,000 mg / L. In one embodiment, the liquid resource contains non-lithium impurities at a concentration of 0.01 to 0.1 mg / L, 0.1 to 1 mg / L, 1 to 10 mg / L, 10 to 100 mg / L, 100 to 1,000 mg / L, 1,000 to 10,000 mg / L, 10,000 to 50,000 mg / L, 50,000 to 100,000 mg / L, 100,000 to 150,000 mg / L, or greater than 150,000 mg / L. In one embodiment, the liquid resource contains transition metals at a concentration of 0.01 to 0.1 mg / L, 0.1 to 1 mg / L, 1 to 10 mg / L, 10 to 100 mg / L, 100 to 1,000 mg / L, 1,000 to 10,000 mg / L, 10,000 to 50,000 mg / L, 50,000 to 100,000 mg / L, 100,000 to 150,000 mg / L, or greater than 150,000 mg / L. In one embodiment, the liquid resource contains iron at a concentration of 0.01 to 0.1 mg / L, 0.1 to 1 mg / L, 1 to 10 mg / L, 10 to 100 mg / L, 100 to 1,000 mg / L, 1,000 to 10,000 mg / L, 10,000 to 50,000 mg / L, 50,000 to 100,000 mg / L, 100,000 to 150,000 mg / L, or greater than 150,000 mg / L. In one embodiment, the liquid resource contains manganese at a concentration of 0.01 to 0.1 mg / L, 0.1 to 1 mg / L, 1 to 10 mg / L, 10 to 100 mg / L, 100 to 1,000 mg / L, 1,000 to 10,000 mg / L, 10,000 to 50,000 mg / L, 50,000 to 100,000 mg / L, 100,000 to 150,000 mg / L, or greater than 150,000 mg / L.
[0152] In one embodiment, the liquid resource is treated to produce a pre-treated liquid resource which has certain metals removed. The term liquid resource as used in this disclosure shall be understood to also encompass a pre-treated liquid resource as described herein. In one embodiment, the pre-treated liquid resource contains iron at a concentration of less than 0.01, 0.01 to 0.1 mg / L, mg / L, 0.1 to 1.0 mg / L, 1.0 to 10 mg / L, 10 to 100 mg / L, or 100 to 1,000 mg / L. In one embodiment, the pre-treated liquid resource contains manganese at a concentration of less than 0.01, 0.01 to 0.1 mg / L, mg / L, 0.1 to 1.0 mg / L, 1.0 to 10 mg / L, 10 to 100 mg / L, or 100 to 1,000 mg / L. In one embodiment, the pre-treated liquid resource contains lead at a concentration of less than 0.01, 0.01 to 0.1 mg / L, mg / L, 0.1 to 1.0 mg / L, 1.0 to 10 mg / L, 10 to 100 mg / L, or 100 to 1,000 mg / L. In one embodiment, the pre-treated liquid resource contains zinc at a concentration of less than 0.01, 0.01 to 0.1 mg / L, mg / L, 0.1 to 1.0 mg / L, 1.0 to 10 mg / L, 10 to 100 mg / L, or 100 to 1,000 mg / L. In one embodiment, the pre-treated liquid resource contains lithium at a concentration of 1 to 50 mg / L, 50 to 200 mg / L, 200 to 500 mg / L, 500 to 2,000 mg / L, or greater than 2,000 mg / L.
[0153] In one embodiment, the pre-treated liquid resource is processed to recover metals such as lithium and yield a lithium-depleted liquid resource. In some embodiments, a lithium- depleted liquid resource is a raffinate. In one embodiment, the lithium-depleted liquid resource contains residual quantities of the recovered metals at a concentration of less than 0.01, 0.01 to 0.1 mg / L, mg / L, 0.1 to 1.0 mg / L, 1.0 to 10 mg / L, 10 to 100 mg / L, 100 to 1,000 mg / L, or 1,000 to 10,000 mg / L.
[0154] In one embodiment, the pH of the liquid resource is corrected to less than 0, 0 to 1, 1 to 2, 2 to 4, 4 to 6, 6 to 8, 4 to 8, 8 to 9, 9 to 10, 9 to 11, or 10 to 12. In one embodiment, the pH of the liquid resource is corrected to 2 to 4, 4 to 6, 6 to 8, 4 to 8, 8 to 9, 9 to 10, 9 to 11, or 10 to 12. In one embodiment, the pH of the liquid resource is corrected to precipitate or dissolve metals.
[0155] In one embodiment, metals are precipitated from the liquid resource to form precipitates. In one embodiment, precipitates include transition metal hydroxides, oxyhydroxides, sulfide, flocculants, aggregate, agglomerates, or combinations thereof. In one embodiment, the precipitates comprise Li, Na, K, Rb, Cs, Fr, Be, Mg, Ca, Sr, Ba, Ra, Sc, Y, Ti, ,Zr, Hf, V, Nb, Ta, Cr, Mo, W ,Mn, Tc, Fe, Fe, Ru, Os, Co, Rh, Ir, Ni, Pd Pt, Cu, Ag, Au, Zn, Cd, Hg, B, Al, Ga, In, Si, Ge, Sn, Pb, As, Sb, Bi, Se, Te, Po, Br, I, At, other metals, or combinations thereof. In one embodiment, the precipitates are concentrated into a slurry, a filter cake, a wet filter cake, a dry filter cake, a dense slurry, or a dilute slurry.
[0156] In one embodiment, the precipitates contain iron at a concentration of less than 0.01 mg / kg, 0.01 to 1 mg / kg, 1 to 100 mg / kg, 100 to 10,000 mg / kg, or 10,000 to 800,000 mg / kg. In one embodiment, the precipitates contain manganese at a concentration of less than 0.01 mg / kg, 0.01 to 1 mg / kg, 1 to 100 mg / kg, 100 to 10,000 mg / kg, or 10,000 to 800,000 mg / kg. In one embodiment, the precipitates contain lead at a concentration of less than 0.01 mg / kg, 0.01 to 1 mg / kg, 1 to 100 mg / kg, 100 to 10,000 mg / kg, or 10,000 to 800,000 mg / kg. In one embodiment, the precipitates contain arsenic at a concentration of less than 0.01 mg / kg, 0.01 to 1 mg / kg, 1 to 100 mg / kg, 100 to 10,000 mg / kg, or 10,000 to 800,000 mg / kg. In one embodiment, the precipitates contain magnesium at a concentration of less than 0.01 mg / kg, 0.01 to 1 mg / kg, 1 to 100 mg / kg, 100 to 10,000 mg / kg, or 10,000 to 800,000 mg / kg. In one embodiment, the precipitates contain Li, Na, K, Rb, Cs, Fr, Be, Mg, Ca, Sr, Ba, Ra, Sc, Y, Ti, ,Zr, Hf, V, Nb, Ta, Cr, Mo, W ,Mn, Tc, Fe, Fe, Ru, Os, Co, Rh, Ir, Ni, Pd Pt, Cu, Ag, Au, Zn, Cd, Hg, B, Al, Ga, In, Si, Ge, Sn, Pb, As, Sb, Bi, Se, Te, Po, Br, I, At, or other metals at a concentration of less than 0.01 mg / kg, 0.01 to 1 mg / kg, 1 to 100 mg / kg, 100 to 10,000 mg / kg, or 10,000 to 800,000 mg / kg. In some embodiments, the precipitates are toxic and / or radioactive. In some embodiments, precipitates are redissolved by combining the precipitates with an acidicsolution. In one embodiment, precipitates are redissolved by combining the precipitates with an acidic solution in a mixing apparatus. In one embodiment, precipitates are redissolved by combining the precipitates with an acidic solution using a high-shear mixer.Treatment of the Liquid Resource
[0157] In some embodiments, the pH of the liquid resource is adjusted before, during and / or after contact with ion exchange material to maintain the pH within a range that is suitable, preferred, or ideal for lithium recovery.
[0158] To adjust the pH of a liquid resource to be within a range that is suitable, preferred, or ideal for lithium recovery, bases such as NaOH, LiOH, KOH, Mg(OH)2, Ca(OH)2, CaO, NH3, Na2SO4, K2SO4, NaHSO4, KHSO4, NaOCl, KOC1, NaC104, KC1O4, NaH2BO3, Na2HBO3, Na3BO3, KH2BO3, K2HBO3, K3BO3, MgHBO3, CaHBO3, NaHCO3, KHCO3, NaCO3, KCO3, MgCO3, CaCO3, Na2O, K2O, Na2CO3, K2CO3, Na3PO4, Na2HPO4, NaH2PO4, K3PO4, K2HPO4, KH2PO4, CaHPO4, MgHPO4, sodium acetate, potassium acetate, magnesium acetate, poly(vinylpyridine), poly(vinylamine), polyacrylonitrile are optionally added to the liquid resource as solids, aqueous solutions, or other forms. For liquid resources that contain divalent ions such as Mg, Ca, Sr, or Ba, addition of base to the liquid resource can cause the formation of precipitates, such as Mg(OH)2 or Ca(OH)2, which can hinder lithium recovery. These precipitates hinder lithium recovery in at least three ways. First, formation of precipitates can remove base from solution, leaving less base available in solution to neutralize protons and maintain pH within a range that is suitable, preferred, or ideal for lithium recovery. Second, precipitates that form due to base addition can hinder flow through an ion exchange device, including hindering flow over the surfaces of ion exchange material, through the pores of porous ion exchange beads, and through the voids between ion exchange material. This hindering of flow can prevent lithium from being absorbed by the ion exchange material utilized in lithium recovery. The hindering of flow can also cause large pressure differences between the inlet and outlet of an ion exchange device utilized for lithium recovery. Third, precipitates in an ion exchange device utilized for lithium recovery can dissolve when placed in contact with an acid eluent, and thereby contaminate the synthetic lithium solution produced by the ion exchange device utilized for lithium recovery.
[0159] For ion exchange material to absorb lithium from a liquid resource for the purpose of lithium recovery, an ideal pH range for the liquid resource is optionally 5 to 7, a preferred pH range is optionally 4 to 8, and a suitable pH range is optionally 1 to 9. In one embodiment, an pH range for the liquid resource is optionally about 1 to about 14, about 2 to about 13, about 3 to about 12, about 4 to about 12, about 4.5 to about 11, about 5 to about 10,about 5 to about 9, about 2 to about 5, about 2 to about 4, about 2 to about 3, about 3 to about 8, about 3 to about 7, about 3 to about 6, about 3 to about 5, about 3 to about 4, about 4 to about 10, about 4 to about 9, about 4 to about 8, about 4 to about 7, about 4 to about 6, about 4 to about 5, about 5 to about 6, about 5 to about 7, about 5 to about 8, about 6 to about 7, about 6 to about 8, or about 7 to about 8.
[0160] In one embodiment, the liquid resource is subjected to treatment prior to ion exchange. In some embodiments, said treatment comprises filtration, gravity sedimentation, centrifugal sedimentation, magnetic fields, other methods of solid-liquid separation, or combinations thereof. In some embodiments, precipitated metals are removed from the liquid resource using a filter. In some embodiments, the filter is a belt filter, plate-and-frame filter press, pressure vessel containing filter elements, rotary drum filter, rotary disc filter, cartridge filter, a centrifugal filter with a fixed or moving bed, a metal screen, a perforate basket centrifuge, a three-point centrifuge, a peeler type centrifuge, or a pusher centrifuge. In some embodiments, the filter uses a scroll or a vibrating device. In some embodiments, the filter is horizontal, vertical, or uses a siphon.
[0161] In some embodiments, a filter cake is prevented, limited, or removed by using gravity, centrifugal force, an electric field, vibration, brushes, liquid jets, scrapers, intermittent reverse flow, vibration, crow-flow filtration, or pumping suspensions across the surface of the filter. In some embodiments, the precipitated metals and a liquid is moved tangentially to the filter to limit filter cake growth. In some embodiments, gravitational, magnetic, centrifugal sedimentation, or other means of solid-liquid separation are used before, during, or after filtering to prevent filter cake formation.
[0162] In some embodiments, a filter comprises a screen, a metal screen, a sieve, a sieve bend, a bent sieve, a high frequency electromagnetic screen, a resonance screen, or combinations thereof. In some embodiments, one or more particle traps are a solid-liquid separation apparatus.
[0163] In some embodiments, one or more solid-liquid separation apparatuses are used in series or in parallel. In some embodiments, a dilute slurry is removed from the tank, transferred to an external solid-liquid separation apparatus, and separated into a concentrated slurry and a solution with low or no suspended solids. In some embodiments, the concentrated slurry is returned to the tank or transferred to a different tank. In some embodiments, precipitate metals are transferred from a liquid resource tank to another liquid resource tank, from an acid tank to another acid tank, from a washing tank to another washing tank, from a liquid resource tank to a washing tank, from a washing tank to an acid tank, from an acid tank to a washing tank, or from an acid tank to a liquid resource tank.
[0164] In some embodiments, solid-liquid separation apparatuses use gravitational sedimentation. In some embodiments, solid-liquid separation apparatuses include a settling tank, a thickener, a clarifier, a gravity thickener. In some embodiments, solid-liquid separation apparatuses are operated in batch mode, semi -batch mode, semi-continuous mode, or continuous mode. In some embodiments, solid-liquid separation apparatuses include a circular basin thickener with slurry entering through a central inlet such that the slurry is dispersed into the thickener with one or more raking components that rotate and concentrate the ion exchange particles into a zone where the particles can leave through the bottom of the thickener.
[0165] In some embodiments, solid-liquid separation apparatuses comprise a deep cone, a deep cone tank, a deep cone compression tank, or a tank wherein the slurry is compacted by weight. In some embodiments, solid-liquid separation apparatuses comprise a tray thickener with a series of thickeners oriented vertically with a center axle and raking components. In some embodiments, solid-liquid separation apparatuses comprise a lamella type thickener with inclined plates or tubes that are smooth, flat, rough, or corrugated. In some embodiments, solidliquid separation apparatuses comprise a gravity clarifier that comprises a rectangular basin with feed at one end and overflow at the opposite end optionally with paddles and / or a chain mechanism to move particles. In some embodiments, the solid-liquid separation apparatuses comprise a particle trap.
[0166] In some embodiments, the solid-liquid separation apparatuses use centrifugal sedimentation. In some embodiments, solid-liquid separation apparatuses comprise a tubular centrifuge, a multi-chamber centrifuge, a conical basket centrifuge, a scroll-type centrifuge, a sedimenting centrifuge, or a disc centrifuge. In some embodiments, precipitated metals are discharged continuously or intermittently from the centrifuge. In some embodiments, the solidliquid separation apparatus is a hydrocyclone. In some embodiments, solid-liquid separation apparatus is an array of hydrocyclones or centrifuges in series and / or in parallel. In some embodiments, sumps are used to reslurry the precipitated metals. In some embodiments, the hydrocyclones comprise multiple feed points. In some embodiments, a hydrocyclone is used upside down. In some embodiments, liquid is injected near the apex of the cone of a hydrocyclone to improve sharpness of cut. In some embodiments, a weir rotates in the center of the particle trap with a feed of slurried precipitated metals entering near the middle of the apparatus such that precipitated metals get trapped at the bottom and center of the apparatus due to a “teacup effect”.System for Extracting Lithium from a Liquid Resource
[0167] In one aspect described herein, is a system for lithium recovery from a liquid resource comprising an ion exchange device wherein one or more vessels are independently configured to simultaneously accommodate porous ion exchange beads moving in one direction and alternately acid, liquid resource, and optionally other process fluids moving in the net opposite direction. This lithium recovery system produces an eluate that comprises lithium and optionally contains other ions.
[0168] In one aspect described herein, is an ion exchange device for lithium recovery from a liquid resource comprising a stirred tank reactor, an ion exchange material, and a pH modulating unit for increasing the pH of the liquid resource in the stirred tank reactor.
[0169] In one aspect described herein, is an ion exchange device for lithium recovery from a liquid resource comprising a stirred rank reactor, an ion exchange material, a pH modulating unit for increasing the pH of the liquid resource in the stirred tank reactor, and a compartment for containing the ion exchange material in the stirred tank reactor while allowing for removal of liquid resource, washing fluid, acid, and other process fluids from the stirred tank reactor.
[0170] In one embodiment, at least one of the one or more vessels are fitted with a conveyer system suitably outfitted to move porous ion exchange beads upward and simultaneously allow a net flow of acid, liquid resource, and optionally other process fluids, downward. In one embodiment, the conveyor system comprises fins with holes. In one embodiment, the fins slide upward over a sliding surface that is fixed in place In one embodiment, all of the one or more vessels are fitted with a conveyor system suitably outfitted to move porous ion exchange beads upward and simultaneously allow a net flow of acid, liquid resource, and optionally other process solutions, downward. In one embodiment, there are an even number of vessels. In one embodiment, there are an odd number of vessels. In one embodiment, the vessels are columns.
[0171] In some embodiments, structures with holes are used to move the ion exchange material through one or more vessels. In some embodiments, the holes in the structures with holes are less than 10 microns, less than 100 microns, less than 1,000 microns, or less than 10,000 microns in diameter. In some embodiments, the structures with holes are attached to a conveyer system. In some embodiments, the structures with holes comprise a porous compartment, porous partition, or another porous structure. In some embodiments, the structures with holes contain a bed of fixed or fluidized ion exchange material. In some embodiments, the structures with holes contain ion exchange material while allowing liquid resource, aqueous solution, acid solution, or other process fluids to pass through the structures with holes.
[0172] In some embodiments, the porous ion exchange beads comprise one or more ion exchange materials that reversibly exchange lithium and hydrogen and a structural matrix material sufficient to form and support a pore network. In some embodiments, the liquid resource comprises a natural brine, a dissolve salt flat, a concentrated brine, a processed brine, a filtered brine, a liquid from an ion exchange process, a liquid from a solvent extraction process, a synthetic brine, leachate from ores, leachate from minerals, leachate from clays, leachate from recycled products, leachate from recycled materials, or combinations thereof.Ion Exchange Devices
[0173] In some embodiments, an ion exchange device comprises a column loaded with ion exchange material, or a form thereof, or a construct comprised thereof. In some embodiments, a pH modulating unit is connected to an ion exchange device loaded with ion exchange material. In some embodiments, the pH modulating unit comprises one or more tanks.
[0174] In some embodiments, an ion exchange device comprises a vessel loaded with ion exchange material, or a form thereof, or a construct comprised thereof . In some embodiments, the pH modulating unit is in fluid communication with the vessel loaded with ion exchange material.
[0175] In some embodiments, an ion exchange device comprises one or more columns loaded with a fixed or fluidized bed of ion exchange beads. In some embodiments, a column comprises a cylindrical construct with an inlet and an outlet. In some embodiments, a column comprises a non-cylindrical construct with an inlet and an outlet. In some embodiments, a column comprises inlets and outlets for pumping of the liquid resource and other process fluids, and additional doors or hatches for loading and unloading ion exchange beads to and from the column. In some embodiments, the column comprises one or more security devices to decrease the risk of theft of the ion exchange beads the column may contain. In some embodiments, ion exchange beads comprise one or more ion exchange materials that can reversibly absorb lithium from a liquid resource and release lithium in an eluent. In some embodiments, the ion exchange material is comprised of ion exchange particles that are optionally protected with coating material such as SiCh, ZrCh, TiCh, polyvinyl chloride, or polyvinyl fluoride to limit dissolution or degradation of the ion exchange material. In some embodiments, the ion exchange beads comprise a structural matrix material such as an acid-resistant polymer that binds the ion exchange material. In some embodiments, the ion exchange beads contain pores that facilitate penetration of liquid resource, acid, aqueous solutions, and other process fluids into the ion exchange beads to, for example, deliver lithium and hydrogen to and from the bead or to wash the bead. In one embodiment, the pores of the ion exchange beads are structured to form aconnected network of pores with a distribution of pore sizes. In one embodiment, the pores of the ion exchange beads are structured by incorporating filler materials into the ion exchange beads during production and later removing the filler material using a liquid or gas.Recirculating Batch System
[0176] In one embodiment of a system for lithium recovery from a liquid resource comprises a recirculating batch system comprising a column containing ion exchange material that is connected to one or more tanks for mixing base into the liquid resource, settling out any precipitates that may form following base addition to the liquid resource, and storing the liquid resource prior to reinjection of the liquid resource into the column or the one or more tanks. In one embodiment of the recirculating batch system, the liquid resource is loaded into the one or more tanks, pumped through the column, pumped through the one or more tanks, and then returned to the column in a loop. In one embodiment, the liquid resource optionally traverses this loop repeatedly. In one embodiment, the liquid resource is configured to recirulate through the column to enable lithium uptake by the ion exchange material. In one embodiment, base is added to the liquid resource such that the pH of the liquid resource adjusted to be within a range that is ideal, preferred, or suitable for lithium uptake by ion exchange material. In one embodiment, base is added to the liquid resource such that the pH of the liquid resource is adjusted to be within a range that minimizes the amount of precipitates in the column.
[0177] In one embodiment, as the liquid resource is pumped through the recirculating batch system, the pH of the liquid resource drops in the column due to hydrogen release from the ion exchange material during lithium uptake, and the pH of the liquid resource is adjusted upward by the addition of base as a solid, aqueous solution, or another form. In one embodiment, the column drives the ion exchange reaction to near completion, and the pH of the liquid resource leaving the column approaches the pH of the liquid resource entering the column. In one embodiment, the amount of base added to the liquid resource in the column is modulated to neutralize the hydrogen released by the ion exchange material while preventing the formation of precipitates. In one embodiment, an excess of base or a transient excess of base is added to the liquid resource in the column in such a way that precipitates form. In one embodiment, precipitates form transiently in the column and then are redissolved partially or fully by the hydrogen that is released from the ion exchange material within the column. In some embodiments of a system for lithium recovery from a liquid resource, base is added to the liquid resource prior to the liquid resource entering the column, after the liquid resource has exited the column, prior to the liquid resource entering one or more tanks, or after the liquid resource has exited one or more tanks.
[0178] In one embodiment of the recirculating batch system, the one or more tanks comprise a mixing tank where base is mixed with the liquid resource. In one embodiment, the one or more tanks comprise a settling tank, wherein precipitates such as Mg(OH)2 optionally settle to the bottom of the settling tank to avoid injection of the precipitates into the column. In one embodiment, the one or more tanks comprise a storage tank wherein the liquid resource is stored prior to reinjection into the ion exchange column, mixing tank, settling tank, or other one or more tanks. In one embodiment, the one or more tanks comprise an acid recirculation tank. In one embodiment, one or more tanks in the recirculating batch system can serve a combination of purposes including as a base mixing tank, a settling tank, a acid recirculation tank, or a storage tank. In some embodiments, any one or more tanks cannot fulfill two functions at the same time. As one non-limiting example, a tank cannot simultaneously fulfill the functions of a mixing tank and a settling tank.
[0179] In some embodiments, the recirculating batch system comprises a mixing tank that comprises a continuous stirrer. In some embodiments, the recirculating batch system is configured such that liquid resource and base or a combination thereof is added to the mixing tank. In some embodiments, the continuous stirrer comprises a static mixer, a paddle mixer, or a turbine impeller mixer. In some embodiments, the continuous stirrer comprises the mixing tank being configured such that liquid resource and base input at the top of the tank become mixed prior to reaching the bottom of the mixing tank. In some embodiments, the base is added to the mixing tank as a solid or as an aqueous solution. In some embodiments, the base is added to the mixing tank continuously at a constant rate or at a variable rate. In one embodiment, the base is added to the mixing tank discretely in constant or variable aliquots or batches. In one embodiment, the quantity of base added to the mixing tank corresponds to the measurement of one or more pH meters, which optionally sample liquid resource downstream of the ion exchange device or elsewhere in the recirculating batch system. In one embodiment, filters are optionally used to prevent precipitates from leaving the mixing tank. In one embodiment, the filters are optionally plastic mesh screens, packed columns containing granular media such as sand, silica, or alumina, packed columns containing porous filter media, or a membrane.
[0180] In one embodiment of the recirculating batch system, the settling tank is optionally a settling tank with influent at bottom and effluent at top or a settling tank with influent on one end and effluent on another end. In one embodiment, chambered weirs are used to fully settle precipitates before liquid resource is recirculated into a reactor. In one embodiment, solid precipitates are collected at the bottom of the settling tank and recirculated into the mixing tank. In one embodiment, precipitates such as Mg(OH)2 settle near the bottom of the settling tank. In one embodiment, liquid resource is removed from the top of the settlingtank, preferably wherein the amount of suspended precipitates is minimal. In one embodiment, the precipitates settle under forces such as gravity, centrifugal action, or other forces. In one embodiment, filters are used to prevent precipitates from leaving the settling tank. In one embodiment, the filters are plastic mesh screens, small packed columns containing granular media such as sand, silica, or alumina, small packed columns containing porous media filter, or a membrane. In one embodiment, baffles are optionally used to ensure settling of the precipitate and to prevent the precipitate from exiting the settling tank and entering the column.
[0181] In one embodiment of the recirculating batch system, precipitates are collected from the settling tank and combined with the liquid resource in a mixing tank or elsewhere to adjust the pH of the liquid resource.
[0182] In one embodiment of the recirculating batch system, one or more ion exchange columns are optionally connected to one or more tanks or set of tanks. In one embodiment of the recirculating batch system, there are multiple ion exchange columns recirculating liquid resource through a shared set of mixing, settling, and storage tanks. In one embodiment of the recirculating batch system, there is optionally one ion exchange column recirculating liquid resource through multiple sets of mixing, settling, and storage tanks.Column Interchange System
[0183] An aspect of the invention described herein is a system wherein ion exchange material is loaded into a plurality of columns. In some embodiments, the pH modulating unit comprises a plurality of tanks connected to the plurality of columns, wherein each of the plurality of tanks is immediately connected to one of the plurality of columns. In some embodiments, two or more of the plurality of tanks connected to the plurality of columns forms at least one circuit. In some embodiments, three or more of the plurality of tanks connected to the plurality of columns forms at least two circuits. In some embodiments, three or more of the plurality of tanks connected to the plurality of columns forms at least three circuits. In some embodiments, at least one circuit is a liquid resource circuit. In some embodiments, at least one circuit is a water washing circuit. In some embodiments, at least one circuit is an acid circuit, wherein the acid is an acid eluent. In some embodiments, at least two circuits are water washing circuits.
[0184] In one embodiment of a system for lithium recovery, the system comprises a column interchange system wherein a series of columns are connected to form a liquid resource circuit, an acid circuit, a water washing circuit, and optionally other circuits containing process fluids. In one embodiment of the liquid resource circuit, liquid resource flows through a first column in the liquid resource circuit, then into a next column in the liquid resource circuit, andso on, such that lithium is removed from the liquid resource by ion exchange as the liquid resource flows through one or more columns that contain ion exchange material. In one embodiment of the liquid resource circuit, base is added to the liquid resource before or after each column or selected columns in the liquid resource circuit to maintain the pH of the liquid resource in an ideal, preferred, or suitable range for lithium uptake by ion exchange material. In one embodiment of the acid circuit, acid flows through a first column in the acid circuit, then into a next column in the acid circuit, and so on, such that lithium is eluted from the columns with acid eluent to produce a synthetic lithium solution. In one embodiment of the acid circuit, acid flows through a first column in the acid circuit, then optionally into a next column in the acid circuit, and so on, such that lithium is eluted from the columns with acid eluent to produce a synthetic lithium solution. In one embodiment of the water washing circuit, water flows through a first column in the water washing circuit, then optionally into a next column in the water washing circuit, and so on, such that liquid resource or raffinate in the void space, pore space, or head space of the columns and the ion exchange material therein is washed out.
[0185] In one embodiment of the column interchange system, columns are interchanged such that each column is a fluid component of the liquid resource circuit, the water washing circuit, and the acid circuit at selected stages or points in time. In one embodiment, the ion exchange material within the first column of the liquid resource circuit are loaded with lithium by passing a sufficient quantity of liquid resource through the first column, and then the first column is interchanged be a fluid component of the water washing circuit to remove liquid resource and / or raffinate from the void space, pore space, or head space of the first column and the ion exchange material therein. In one embodiment, the first column in the water washing circuit is washed to remove liquid resource and / or raffinate therein, and then the first column is interchanged to be a fluid component of the acid circuit, wherein lithium is eluted from the ion exchange material in the column with acid to yield a synthetic lithium solution. In one embodiment, acid or acid eluent is passed through the first column in the acid circuit and then then interchanged to be a fluid component of the liquid resource circuit, wherein the ion exchange material inside the column absorbs lithium from the liquid resource. In one embodiment of the column interchange system, two water washing circuits are used to wash the columns after both the liquid resource circuit and the acid circuit. In one embodiment of the column interchange system, the columns are interchanged to be a fluid component of the water washing circuit only after the columns have been a fluid component of the liquid resource circuit, such that a column that is a fluid component of the acid circuit is not typically interchanged to be a fluid component of the water washing circuit. In some embodiments of the column interchange system, excess acid in the column after a column has been a fluidcomponent of the acid circuit is typically neutralized once the column is interchanged to be a fluid component of the liquid resource circuit and liquid resource is flowed through the column.
[0186] In one embodiment of the column interchange system, the first column in the liquid resource circuit is interchanged to become the last column in the water washing circuit. In one embodiment of the column interchange system, the first column in the water washing circuit is interchanged to become the last column in the acid circuit. In one embodiment of the column interchange system, the first column in the acid circuit is interchanged to become the last column in the liquid resource circuit.
[0187] In one embodiment of the column interchange system, each column in the liquid resource circuit contains one or more tanks or junctions that allow for adding base into the liquid resource and optionally settling any precipitates that may form following base addition to the liquid resource. In one embodiment of the column interchange system, each column in the liquid resource circuit has an associated one or more tanks or junctions for removing precipitates or other particles via settling or filtration. In one embodiment of the column interchange system, each column or plurality of columns has an associated one or more settling tanks or filters that remove particulates including particulates that detach from ion exchange material, forms thereof, or constructs comprised thereof.
[0188] In one embodiment of the column interchange system, the liquid resource circuit comprises a number of the columns that is optionally less than about 3, less than about 10, less than about 30, or less than about 100. In one embodiment of the column interchange system, the acid circuit comprises a number of the columns that is optionally less than about 3, less than about 10, less than about 30, or less than about 100. In one embodiment of the column interchange system, the water washing circuit comprises a number of the columns that is optionally less than about 3, less than about 10, less than about 30, or less than about 100. In certain embodiments, the liquid resource circuit comprises a number of columns in the inclusive range of 1 to 10. In certain embodiments, the acid circuit comprises a number of columns in the inclusive range of 1 to 10. In certain embodiments, the water washing circuit comprises a number of columns in the inclusive range of 1 to 10.
[0189] In one embodiment of the column interchange system, the column interchange system comprises one or more liquid resource circuits, one or more acid circuits, and one or more water washing circuits. In one embodiment of the column interchange system, the ion exchange material within the columns is removed and replaced with a separate portion of ion exchange material without interruption to operation of the circuits within the column interchange system. In one embodiment of the column interchange system, the ion exchange material within the columns is removed following its useful lifetime and replaced with aseparate portion of ion exchange material that is within its useful lifetime without interruption to operation of the circuits within the column interchange system.
[0190] In one embodiment of the column interchange system, the columns contain fluidized beds of ion exchange material. In one embodiment of the column interchange system, the columns comprise means of fluidizing or maintaining the fluidity of a bed of ion exchange material. In some embodiments, means of fluidizing or maintaining the fluidity of a bed of ion exchange material comprise one or more overhead stirrers and / or one or more pumps. In one embodiment of the column interchange system, the columns contain fluidized beds of ion exchange material.
[0191] In one embodiment of a system for lithium recovery, ion exchange material is loaded into columns and following the uptake of lithium from a liquid resource by the ion exchange material, lithium is eluted from the column using an acid recirculation loop. In one embodiment of the acid recirculation loop, acid is flowed through an ion exchange column, into a tank, and then recirculated through the ion exchange column to optimize lithium elution. In some embodiments of the ion exchange system, ion exchange material is loaded into ion exchange columns and following lithium uptake from liquid resource, lithium is eluted from each ion exchange column using a once-through flow of acid. In some embodiments of the ion exchange system, ion exchange material is loaded into an ion exchange column and following lithium uptake from liquid resource, lithium is eluted from the ion exchange column using a column interchange circuit.
[0192] In some embodiments of the ion exchange system, ion exchange columns are loaded with lithium by flowing liquid resource through the columns using a recirculating batch system and then lithium is eluted from the columns using a column interchange system. In some embodiments of the ion exchange system, ion exchange columns are loaded with lithium by flowing liquid resource through the columns using a column interchange system and then lithium is eluted from the columns using a recirculating batch system. In some embodiments of the ion exchange system, ion exchange columns are loaded with lithium by flowing liquid resource through the columns using a recirculating batch system and then lithium is eluted from the columns using a recirculating batch system. In some embodiments of the ion exchange system, ion exchange columns are loaded with lithium by flowing liquid resource through the columns using a column interchange system and then lithium is eluted from the columns using a column interchange system.Stirred Tank system
[0193] An aspect of the invention described herein is a system for lithium recovery wherein the pH modulating unit is a tank comprising: a) one or more compartments; and b) means for moving the liquid resource through the one or more compartments. In an embodiment, ion exchange material is loaded in at least one compartment of the pH modulating unit. In an embodiment, the means for moving the liquid resource through the one or more compartments is a pipe. In a further embodiment, the means for moving the liquid resource through the one or more compartments is a pipe and suitably a configured pump. In an embodiment, the tank further comprises a means for circulating the liquid resource throughout the tank. In an embodiment, the means for circulating the liquid resource throughout the tank is a mixing device. In an embodiment, the tank further comprises an injection port. In some embodiments, the tank further comprises one or more injection ports. In some embodiments, the tank further comprises a plurality of injection ports.
[0194] An aspect described herein is a system for lithium recovery from a liquid resource comprising a tank, wherein the tank further comprises: a) one or more compartments; b) ion exchange material; c) a mixing device; and d) a pH modulating unit for adjusting the pH of the liquid within the system, wherein the ion exchange material is used to extract lithium ions from the liquid resource in an ion exchange process. In one embodiment, the pH modulating unit adjusts the pH of the liquid resource in the system. In some embodiments, ion exchange material is loaded into at least one of the one or more compartments of the tank. In some embodiments, the ion exchange material is fluidized in at least one of the one or more compartments of the tank. In some embodiments, the ion exchange material is non-fluidized in at least one of the one or more compartments of the tank. In some embodiments, the ion exchange material occupies a fixed position in at least one of the one or more compartments of the tank.
[0195] In some embodiments, the pH modulating unit comprises a pH measuring device and an inlet for adding base to a liquid inside the pH modulating unit. In some embodiments, the pH measuring device is a pH probe. In some embodiments, the inlet is a pipe. In some embodiments, the inlet is an injection port.
[0196] In some embodiments, the tank further comprises a porous partition. In some embodiments, the porous partition is a porous polymer partition. In some embodiments, the porous partition is a mesh or membrane. In some embodiments, the porous partition is a polymer mesh or polymer membrane. In some embodiments, the porous partition comprises one or more layers of mesh, membrane, or other porous structure. In some embodiments, the porous partition comprises one or more coarse meshes that provide structural support and one or more finemeshes and / or membranes selected to enable filtration or a filtering action. In some embodiments, the porous partition comprises a polyether ether ketone mesh, a polypropylene mesh, a polyethylene mesh, a polysulfone mesh, a polyester mesh, a polyamide mesh, a polytetrafluoroethylene mesh, an ethylene tetrafluoroethylene polymer mesh, a stainless steel mesh, a stainless steel mesh coated in polymer, a stainless steel mesh coated in ceramic, or a combination thereof, wherein the mesh is a course mesh, a fine mesh, or a combination thereof. In some embodiments, the porous polymer partition comprises a mesh comprising one or more blends of two or more of a polyether ether ketone, a polypropylene, a polyethylene, a polysulfone, a polyester, a polyamide, a polytetrafluoroethylene, or an ethylene tetrafluoroethylene polymer. In some embodiments, the porous partition comprises a polyether ether ketone membrane, a polypropylene membrane, a polyethylene membrane, a polysulfone membrane, a polyester membrane, a polyamide membrane, a polytetrafluoroethylene membrane, an ethylene tetrafluoroethylene polymer membrane, or combinations thereof.
[0197] In some embodiments of a system for lithium recovery from a liquid resource, the system comprises a stirred tank system comprised of a tank containing liquid resource and permeable bead compartments such as permeable pallets, cases, boxes, or other containers, wherein the bead permeable compartments are loaded with ion exchange beads and the liquid resource is added to, stirred throughout, and removed from the tank in a batch process. In one embodiment of the stirred tank system, base is added directly to the tank gradually, in separate aliquots, at a constant rate or a variable rate, or in a single aliquot as a solid or in an aqueous solution. In some embodiments, the stirred tank system is configured to operate in a batch process, wherein the batch process comprises an extraction stage and an elution stage. In some embodiments, the extraction stage comprises the uptake of lithium from the liquid resource by the ion exchange beads within the permeable bead compartments, such that the liquid resource becomes depleted in lithium and the ion exchange beads become enriched in lithium. In some embodiments, the elution stage comprises the release of lithium from the ion exchange beads within the permeable bead compartments into an eluent. In some embodiments an eluent is an acid or an acid eluent. In one embodiment, the stirred tank system comprises one or more additional tanks and the permeable bead containers are placed into the one or more additional tanks for the elution stage. In one embodiment of the stirred tank system, the permeable bead compartments are located at the bottom of the tank during the extraction stage, and after the extraction stage is completed, the liquid resource is removed, and the tank is filled eluent in such a way that the permeable bead compartments are in contact with a volume of eluent that is sufficient to carry out the elution stage.
[0198] In some embodiments of a system for lithium recovery from a liquid resource, the system comprises a stirred tank system wherein ion exchange beads are suspended using plastic structural supports in a tank with an internal mixing device. In some embodiments, the stirred tank system is configured to operate in a batch process, wherein the batch process comprises an extraction stage and an elution stage. In some embodiments, the extraction stage comprises the uptake of lithium from the liquid resource by the ion exchange beads, such that the liquid resource becomes depleted in lithium and the ion exchange beads become enriched in lithium. In some embodiments, the elution stage comprises the release of lithium from the ion exchange beads into an eluent. In some embodiments an eluent is an acid or an acid eluent. In one embodiment of the stirred tank system, liquid resource is removed from the tank and passed through a column wherein hydrogen ions in the liquid resource are neutralized using base provided as a solution, as a solid, or as an ion exchange resin to yield a pH-corrected stream. In some embodiment, the pH-corrected stream is input back into the stirred tank system. In one embodiment of the stirred tank system, liquid resource that has passed through the tank containing ion exchange beads is returned to the opposite end of the tank through a pipe that is optionally internal or external to the tank. In one embodiment of the stirred tank system, base is optionally added to the liquid resource inside the tank or added to a separate base addition tank that is outside the tank.
[0199] In some embodiments of the stirred tank system, the stirred tank system is configured to operate in a continuous process instead of a batch process. In some embodiments, the continuous process comprises continuous addition and removal of liquid resource from the stirred tank system. In one embodiment of the recirculating batch system, the recirculating batch system is configured to operate in a continuous process instead of a batch process.
[0200] In one embodiment of the ion exchange device, liquid resource is combined with ion exchange beads in a stirred tank reactor. In one embodiment, the ion exchange beads are comprised of coated particles, uncoated particles, porous beads, or combinations thereof.
[0201] In one embodiment of the ion exchange device, a stirred tank reactor is used to fluidize the ion exchange material in a liquid resource to enable absorption of lithium from the liquid resource into the ion exchange material. In one embodiment, a stirred tank reactor is used to fluidize the ion exchange material in a washing fluid to remove residual liquid resource, acid, process fluids, contaminants, or combinations thereof from the ion exchange materials. In one embodiment, a stirred tank reactor is used to fluidize the ion exchange material in an acid eluent to elute lithium from the ion exchange beads while replacing the lithium in the ion exchange material with protons. In one embodiment, a single stirred tank reactor is used to mix ion exchange material sequentially and repetitively with a liquid resource, washing fluid, and acid.
[0202] In some embodiments, the system for lithium recovery from a liquid resource comprises a tank, wherein the tank further comprises: a) one or more compartments; b) ion exchange material; c) a mixing device; and d) a pH modulating unit for changing the pH of the liquid resource in the system, wherein the ion exchange material is used to extract lithium ions from the liquid resource, further comprises another tank, wherein the other tank further comprises: a) one or more compartments; b) ion exchange beads; c) a mixing device; and d) a pH modulating unit for changing the pH of the liquid resource in the system. In some embodiments, the tank is in fluid communication with the other tank.
[0203] In some embodiments, the system for lithium recovery from a liquid resource comprises a tank, wherein the system further comprises another tank, wherein the other tank further comprises: a) one or more compartments; b) ion exchange material; c) a mixing device; and d) an acid inlet for adding acid to the system. In a further embodiment, the ion exchange material is moved between the tank and the other tank.
[0204] In some embodiments, the system for lithium recovery from a liquid resource comprises a tank, wherein the tank further comprises: a) one or more compartments; b) ion exchange material; c) a mixing device; and d) a pH modulating unit for changing the pH of the liquid resource in the system, wherein the ion exchange material is used to extract lithium ions from the liquid resource, further comprises a plurality of tanks, each tank further comprising: a) one or more compartments; b) ion exchange material; c) a mixing device; and d) a pH modulating unit for changing the pH of the liquid resource in the system. In some embodiments, each tank of the system is in fluid communication with each other tank of the system.
[0205] In some embodiments, the system further comprises another plurality of tanks, wherein each tank further comprises: a) one or more compartments; b) ion exchange material; and c) a mixing device.
[0206] In some embodiments, the system for lithium recovery from a liquid resource is configured to operate in a batch mode. In some embodiments, the system for lithium recovery from a liquid resource is configured to operate in a continuous mode. In some embodiments, the system for lithium recovery from a liquid resource is configured to operate in a batch mode and a continuous mode. In some embodiments, one or more tanks in the system for lithium recovery from a liquid resource are configured to operate in a batch mode and one or more tanks in the system are configured to operate in a continuous mode. In some embodiments, one or more tanks in the system for lithium recovery from a liquid resource are configured to operate in a batch mode and one or more tanks in the system are configured to operate in a semi -continuous mode. In some embodiments, one or more tanks in the system for lithium recovery from a liquid resource are configured to operate in a semi-continuous mode and one or more tanks in thesystem are configured to operate in a continuous mode. In some embodiments, one or more tanks in the system for lithium recovery from a liquid resource are configured to operate in a batch mode, one or more tanks in the system for lithium recovery from a liquid resource are configured to operate in a semi -continuous mode, and one or more tanks in the system are configured to operate in a continuous mode. In some embodiments, the system for lithium recovery from a liquid resource is configured to operate in a semi-continuous mode, a batch mode, a continuous mode, or combinations thereof.
[0207] In one embodiment of the system for lithium recovery from a liquid resource, a plurality of stirred tank reactors are used to mix ion exchange material with a liquid resource, washing fluid, and acid eluent. In one embodiment, the stirred tank reactors are different sizes and can contain different volumes of a liquid resource, washing fluid, and acid eluent. In one embodiment, the stirred tanks are cylindrical, conical, rectangular, pyramidal, or a combination thereof. In one embodiment of the system for lithium recovery from a liquid resource, the ion exchange material moves through the plurality of stirred tank reactors in the opposite direction of the liquid resource, the washing fluid, or the acid eluent.
[0208] In one embodiment of the system for lithium recovery from a liquid resource, a plurality of stirred tank reactors is used where one or more stirred tank reactors mix the ion exchange material with a liquid resource, one or more stirred tank reactors mix the ion exchange material with a washing fluid, and one or more stirred tank reactors mix the ion exchange material with an acid eluent.
[0209] In one embodiment of the system for lithium recovery from a liquid resource, stirred tank reactors are operated in a continuous, semi -continuous, or batch mode where a liquid resource flows continuously, semi -continuously, or batch-wise through the stirred tank reactor. In one embodiment of the system for lithium recovery from a liquid resource, stirred tank reactors are operated in a continuous, semi-continuous, or batch mode where the ion exchange material flows continuously, semi-continuously, or batch-wise through the stirred tank reactor. In one embodiment of the system for lithium recovery from a liquid resource, stirred tank reactors are operated in a mode where the ion exchange material remain in the tank while flows of liquid resource, washing fluid, or acid eluent are flowed through the tank in continuous, semi- continuous, or batch flows.
[0210] In one embodiment, ion exchange material is loaded into or removed from the stirred tank reactors through the top, the bottom, or the side of the tank.
[0211] In one embodiment of the system for lithium recovery from a liquid resource, stirred tank reactors comprise one or more compartments. In one embodiment, the compartments contain ion exchange material in a bed that is fluidized, fixed, partially fluidized, partially fixed,alternatively fluidized, alternatively fixed, or combinations thereof. In one embodiment, the compartments are comprised of a porous support at the bottom of the compartment, the sizes of the compartment, the top of the compartment, or combinations thereof. In one embodiment, the compartments are conical, cylindrical, rectangular, pyramidal, other shapes, or combinations thereof. In one embodiment, the compartment is located at the bottom of the tank. In one embodiment, the shape of the compartment conforms to the shape of the stirred tank reactor. In one embodiment, the compartment is partially or fully comprised of the tank of the stirred tank reactor.
[0212] In one embodiment, the compartment is comprised of a porous structure. In one embodiment, the compartment is comprised of a polymer, a ceramic, a metal, or combinations thereof. In one embodiment, the compartment is comprised be comprised partially or fully of a porous material or a mesh. In one embodiment, the compartment is at the top of the tank. In one embodiment, the compartment is separated from the rest of the tank with one or more porous materials. In one embodiment, the compartment is at the top of the tank. In one embodiment, the compartment is separated from the rest of the tank with a bilayer mesh comprising one layer of coarse mesh for strength and one layer of fine mesh to contain smaller particles in the compartment. In one embodiment, the compartment allows liquid or process fluid to flow freely through the stirred tank reactor and through the compartment. In one embodiment, the compartment is open on the top. In one embodiment, the compartment contains the ion exchange material in the tank but allow the ion exchange material to move throughout the tank. In one embodiment, the compartment comprises a majority or minority of the tank volume. In one embodiment, the compartment represents a fraction of the volume of the tank that is greater than 1 percent, greater than 10 percent, greater than 50 percent, greater than 90 percent, greater than 99 percent, or greater than 99.9 percent. In one embodiment, one or more devices for stirring, mixing, or pumping is used to move liquid or process fluid through the compartment, the stirred tank reactor, or combinations thereof.
[0213] In one embodiment of the system for lithium recovery from a liquid resource, stirred tank reactors are arranged into a network where flows of liquid resource, washing fluid, and acid are directed through different columns. In one embodiment, a network of stirred tank reactors involves physical movement of the ion exchange material through the various stirred tank reactors. In one embodiment, a network of stirred tank reactors involves no physical movement of the ion exchange material through the various stirred tank reactors. In one embodiment, a network of stirred tank reactors involves switching of flows of liquid resource, washing fluid, and acid through the various stirred tank reactors. In one embodiment, liquid resource is entered into the stirred tank reactors in a continuous or batch mode. In oneembodiment, liquid resource is mixed with ion exchange material in one or more reactors before exiting the system. In one embodiment, a network of stirred tank reactors involves a liquid resource circuit with counter-current exposure of ion exchange material to flows of liquid resource. In one embodiment, a network of stirred tank reactors involves a washing circuit with counter-current exposure of ion exchange material to flows of washing fluid. In one embodiment, a network of stirred tank reactors involves an acid circuit with counter-current exposure of ion exchange material to flows of acid. In one embodiment, the washing fluid is water, an aqueous solution, or a solution containing an anti-scalant.
[0214] In one embodiment of the stirred tank reactor, acid is added at the beginning of elution of lithium from the ion exchange material. In one embodiment of the stirred tank reactor, acid is added at the beginning of elution of lithium from the ion exchange material and again during elution of lithium from the ion exchange material. In one embodiment of the stirred tank reactor, an acid of lower concentration is added at the start of elution of lithium from the ion exchange material and additional acid of higher concentration is added to continue elution of lithium from the ion exchange material.
[0215] An aspect described herein is a system for lithium recovery from a liquid resource, comprising: a) ion exchange material; b) a tank comprising one or more compartments; and c) a mixing device, wherein the ion exchange material is used to extract lithium ions from the liquid resource.
[0216] In some embodiments, the ion exchange material is loaded in at least one of the one or more compartments. In some embodiments, the ion exchange material is fluidized or partially fluidized in at least one of the one or more compartments. In some embodiments, the ion exchange material occupies a fixed position in at least one of the one or more compartments. In some embodiments, the ion exchange material is mounted in at least one of the one or more compartments.
[0217] An aspect described herein is a system for lithium recovery from a liquid resource, comprising: a) a column comprising ion exchange material; and b) a pH modulating unit for changing the pH of the liquid resource in the system for lithium recovery from a liquid resource, wherein the pH modulating unit is in fluid communication with the column, wherein the ion exchange material is used to extract lithium ions from the liquid resource.Other Types of Systems
[0218] An aspect described herein is a system for lithium recovery from a liquid resource, comprising: a) a plurality of columns, wherein each of the plurality of columns comprises ion exchange material; and b) a pH modulating unit for changing the pH of the liquidresource in the system, wherein the pH modulating unit is in fluid communication with each of the plurality of columns, wherein the ion exchange material is used to extract lithium ions from the liquid resource.
[0219] In some embodiments, the pH modulating unit comprises a plurality of tanks, wherein each of the plurality of tanks is immediately connected to one of the plurality of columns. In one embodiment, the pH modulating unit comprises a plurality of tanks, wherein each of the plurality of tanks is in immediate liquid communication with one of the plurality of columns. In some embodiments, two or more of the plurality of tanks connected to two or more of the plurality of columns forms at least one circuit. In some embodiments, two or more of the plurality of tanks connected to two or more of the plurality of columns forms at least two circuits. In some embodiments, three or more of the plurality of tanks connected to three or more of the plurality of columns forms at least two circuits. In some embodiments, three or more of the plurality of tanks connected to three or more of the plurality of columns forms at least three circuits.
[0220] In some embodiments, the pH modulating unit comprises a plurality of tanks, wherein each of the plurality of tanks is connected to the of the plurality of columns through a filtration system. In some embodiments, two or more of the plurality of tanks are connected to two or more of the plurality of columns through a filtration system to form at least one circuit. In some embodiments, two or more of the plurality of tanks are connected to two or more of the plurality of columns through a filtration system to form at least two circuits. In some embodiments, three or more of the plurality of tanks are connected to two or more of the plurality of columns through a filtration system to form at least two circuits. In some embodiments, three or more of the plurality of tanks are connected to two or more of the plurality of columns through a filtration system to form at least three circuits.
[0221] In some embodiments, the filtration system comprises a bag filter, a candle filter, a cartridge filter, a media filter, a depth filter, a sand filter, a membrane filter, an ultrafiltration system, a microfiltration filter, a nanofiltration filter, a cross-flow filter, a dead-end filter, a drum filter, a filter press, or a combination thereof. In some embodiments, the filtration system comprises one or more perforated outer walls that are an optional component of any one or more tanks, such that a liquid resource or process fluid on one side of the perforated outer wall is filtered when passed through the perforated outer wall. In some embodiments, the perforated outer wall comprises an insert that is placed into a tank, wherein liquid resource provided to the tank through an inlet is filtered by the perforated outer wall prior to the liquid resource leaving the tank through an outlet. In some embodiments, the filter system comprises one or more filters that independently have openings of an average size less than about 0.02 pm, less than about 0.1pm, less than about 0.2 pm, less than about 1 pm, less than about 2 pm, less than about 5 pm, less than about 10 pm, less than about 25 pm, less than about 100 pm, less than about 1000 pm. In some embodiments, the openings in perforated outer walls are more than about 0.02 pm, more than about 0.1 pm, more than about 0.2 pm, more than about 1 pm, more than about 2 pm, more than about 5 pm, more than about 10 pm, more than about 25 pm, more than about 100 pm. In some embodiments, the openings in perforated outer walls are about 0.02 pm to about 0.1 pm, from about 0.1 pm to about 0.2 pm, from about 0.2 pm to about 0.5 pm, from about 0.5 pm to about 1 pm, from about 1 pm to about 5 pm, from about 5 pm to about 10 pm, from about 10 pm to about 25 pm, from about 25 pm to about 100 pm. In some embodiments, a filter, a perforated outer wall, or a means for filtering comprises low density polyethylene, high density polyethylene, polypropylene, polyester, polytetrafluoroethylene (PTFE), types of polyamide, polyether ether ketone (PEEK), polysulfone, polyvinylidene fluoride (PVDF), poly (4-vinyl pyridine-co-styrene) (PVPCS), polystyrene (PS), polybutadiene, acrylonitrile butadiene styrene (ABS), polyvinyl chloride (PVC), ethylene tetrafluoroethylene polymer (ETFE), poly (chlorotrifluoroethylene) (PCTFE), ethylene chlorotrifluoro ethylene (Halar), polyvinylfluoride (PVF), fluorinated ethylene-propylene (FEP), perfluorinated elastomer, chlorotrifluoroethylenevinylidene fluoride (FKM), perfluoropoly ether (PFPE), perfluoro-3,6- dioxa-4-methyl-7-octene-sulfonic acid (NAFION® (copolymer of perfluoro-3,6-dioxa-4- methyl-7-octene-sulfonic acid and tetrafluoroethylene)), polyethylene oxide, polyethylene glycol, sodium polyacrylate, polyethylene-block-poly(ethylene glycol), polyacrylonitrile (PAN), polychloroprene (neoprene), polyvinyl butyral (PVB), expanded polystyrene (EPS), polydivinylbenzene, co-polymers thereof, mixtures thereof, or combinations thereof. In some embodiments, a filter, a perforated outer wall, or a means for filtering comprises a coating material comprising polyvinylidene fluoride (PVDF), polyvinyl chloride (PVC), ethylene chlorotrifluoro ethylene (Halar), poly (4-vinyl pyridine-co-styrene) (PVPCS), polystyrene (PS), acrylonitrile butadiene styrene (ABS), expanded polystyrene (EPS), polyphenylene sulfide, sulfonated polymer, carboxylated polymer, other polymers, co-polymers thereof, mixtures thereof, or combinations thereof. In some embodiments, a filter, a perforated outer wall, or a means for filtering comprises iron, stainless steel, nickel, carbon steel, titanium, Hastelloy, Inconel, zirconium, tantalum, alloys thereof, mixtures thereof, or combinations thereof.
[0222] In some embodiments, at least one circuit is a liquid resource circuit. In some embodiments, at least one circuit is a water washing circuit. In some embodiments, at least two circuits are water washing circuits. In some embodiments, at least one circuit is an acid circuit.
[0223] An aspect described herein is a system for lithium recovery from a liquid resource comprising ion exchange material and a plurality of vessels, wherein each of theplurality of vessels is configured to transport the ion exchange material along the length of the vessel and the ion exchange material is used to extract lithium ions from the liquid resource. In some embodiments, at least one of the plurality of vessels comprises an acidic solution. In some embodiments, at least one of the plurality of vessels comprises the liquid resource. In some embodiments, each of the plurality of vessels is configured to transport the ion exchange beads by means of a pipe system or an internal conveyer system.
[0224] An aspect described herein is a system for lithium recovery from a liquid resource comprising ion exchange material and a plurality of columns, wherein each of the plurality of columns is configured to transport the ion exchange material along the length of the column and the ion exchange material is used to extract lithium ions from the liquid resource.
[0225] In some embodiments, at least one of the plurality of columns comprises an acidic solution. In some embodiments, at least one of the plurality of columns comprises the liquid resource. In some embodiments, each of the plurality of columns is configured to transport the ion exchange material by means of a pipe system or an internal conveyer system.
[0226] In some embodiments, the ion exchange beads comprise an ion exchange material in the form of ion exchange particles. In some embodiments, at least a portion of the ion exchange material is in the form of ion exchange particles. In some embodiments, the ion exchange particles are selected from uncoated ion exchange particles, coated ion exchange particles, and combinations thereof. In some embodiments, the ion exchange particles are uncoated ion exchange particles. In some embodiments, the ion exchange particles are coated ion exchange particles. In some embodiments, the ion exchange particles comprise a mixture of uncoated ion exchange particles and coated ion exchange particles.
[0227] In some embodiments, the coated ion exchange particles comprise an ion exchange material and a coating material. In some embodiments, coated ion exchange particles comprise a coating material. In some embodiments, the coating material of the coated ion exchange particles comprises a carbide, a nitride, an oxide, a phosphate, a fluoride, a polymer, carbon, a carbonaceous material, or combinations thereof. In some embodiments, the coating material of the coated ion exchange particles is selected from the group consisting of TiCh, ZrCh, MoO?, SnC>2, Nb20s, Ta20s, SiCh, Li2TiO3, Li2ZrOs, Li2SiO3, Li2MnO3, Li2MoO3, LiNbCh, LiTaCh, A1PO4, LaPO4, ZrP2O7, MOP2O7, MO2P3O12, BaSO4, A1F3, SiC, TiC, ZrC, Si3N4, ZrN, BN, carbon, graphitic carbon, amorphous carbon, hard carbon, diamond-like carbon, solid solutions thereof, and combinations thereof.
[0228] In some embodiments, the ion exchange material of the coated ion exchange particles comprises an oxide, a phosphate, an oxyfluoride, a fluorophosphate, or combinations thereof. In some embodiments, the ion exchange material of the coated ion exchange particles isselected from the group consisting of I^MnsOn, Li^isOn, Li2TiO3, Li2MnO3, Li2SnO3, LiMn2O4, Li1.6Mn1.eO4, LiAlCh, LiCuO2, LiTiO2, Li4TiO4, Li7TinO24, Li3VO4, Li2Si3O?, LiFePO4, LiMnPO4, Li2CuP2O7, A1(OH)3, LiCl.xAl(OH)3.yH2O, SnO2.xSb2O5.yH2O, TiO2.xSb2O5.yH2O, solid solutions thereof, and combinations thereof; wherein x is from 0.1-10; and y is from 0.1-10.
[0229] In some embodiments, the uncoated ion exchange particles comprise an ion exchange material. In some embodiments, the ion exchange material of the uncoated ion exchange particles comprises an oxide, a phosphate, an oxyfluoride, a fluorophosphate, or combinations thereof. In some embodiments, the ion exchange material of the uncoated ion exchange particles is selected from the group consisting of Li4MnsOi2, Li4TisOi2, Li2TiO3, Li2MnO3, Li2SnO3, LiMn2O4, Li1.6Mn1.eO4, LiA102, LiCuO2, LiTiO2, Li4TiO4, Li7TinO24, Li3VO4, Li2Si3O7, LiFePO4, LiMnPO4, Li2CuP2O7, A1(OH)3, LiCl.xAl(OH)3.yH2O, SnO2.xSb2O5.yH2O, TiO2.xSb2O5.yH2O, solid solutions thereof, and combinations thereof; wherein x is from 0.1-10; and y is from 0.1-10.
[0230] In some embodiments, the ion exchange beads are porous. In some embodiments, the porous ion exchange beads comprise a network of pores that allows liquids, such as process fluids, to move quickly from the surface of the porous ion exchange beads to a plurality of ion exchange particles comprised therein. In some embodiments, a porous ion exchange beads comprise a network of pores that allows a liquid, such as a process fluid, to move from the surface of the porous ion exchange beads to a plurality of ion exchange particles comprised therein. In some embodiments, the porous ion exchange beads comprise a network of pores that allows a liquid to move quickly from the surface of the porous ion exchange bead to a plurality of ion exchange particles comprised therein. In some embodiments, a single ion exchange bead comprises a network of pores and an ion exchange material in the form of a plurality of ion exchange particles, wherein the ion exchange particles are individually coated or uncoated. In some embodiments, ion exchange beads comprise a structural matrix material. In some embodiments, a network of pores comprises a structural matrix material. In some embodiments, a structural matrix material is a material that allows for a network of pores to be formed and maintained. In some embodiments, a structural matrix material is a polymer or mixture of polymers.
[0231] An aspect of the disclosure described herein is a system for lithium recovery from a liquid resource that comprises a column, wherein the column further comprises a plurality of injection ports, wherein the plurality of injection ports are used to increase the pH of the liquid resource in the system.
[0232] In one embodiment of the system for lithium recovery from a liquid resource, the system is a mixed base system comprising a column and a mixing chamber where base is mixed into the liquid resource immediately prior to injection of the liquid resource into the column.
[0233] In one embodiment of the system for lithium recovery from a liquid resource, the system is a ported column system with multiple ports for injection of aqueous solutions of base, wherein the ports are spaced at intervals along the direction of flow of liquid resource through the column. As liquid resource flows through the column, there is a region of the column where the ion exchange material experiences the greatest rate of lithium absorption, and this region moves through the column over time in the direction of liquid resource flow. In some embodiments of the ported column system, base is injected near the region of the column where the ion exchange material experiences the greatest rate of lithium absorption to neutralize protons released by the ion exchange material. In some embodiments, in regions of the columns where the ion exchange material is enriched in lithium and the rate of release of protons therefrom has slowed, the quantity of base injected into the column is decreased or terminated to avoid formation of precipitates. pH Modulation
[0234] In one embodiment of the system for lithium recovery from a liquid resource, the system has a moving bed of ion exchange material that moves in a direction opposite to the direction of flow of liquid resource, wherein base is injected at one or more fixed points near the region of the column where the ion exchange reaction is proceeding at a maximum rate to neutralize the protons released from the ion exchange material. In one embodiment of the system for lithium recovery from a liquid resource, the base added to the liquid resource comprises NaOH, LiOH, KOH, Mg(OH)2, Ca(OH)2, CaO, NH3, Na2SO4, K2SO4, NaHSO4, KHSO4, NaOCl, KOC1, NaC104, KC1O4, NaH2BO3, Na2HBO3, Na3BO3, KH2BO3, K2HBO3, K3BO3, MgHBO3, CaHBO3, NaHCO3, KHCO3, NaCO3, KCO3, MgCO3, CaCO3, Na2O, K2O, Na2CO3, K2CO3, Na3PO4, Na2HPO4, NaH2PO4, K3PO4, K2HPO4, KH2PO4, CaHPO4, MgHPO4, sodium acetate, potassium acetate, magnesium acetate, poly(vinylpyridine), poly(vinylamine), polyacrylonitrile, other bases, or combinations thereof. In one embodiment, the base is added to the liquid resource in its pure form or as an aqueous solution. In one embodiment, the base is added to the liquid resource in a gaseous state such as, in a non-limiting example, gaseous NH3. In one embodiment, the base is added to the liquid resource in a steady stream, a variable stream, in steady aliquots, or in variable aliquots. In some embodiments, the base is generated in the liquid resource in situ by using an electrochemical cell to remove H2and Cl2gases from the liquid resource. In some embodiments, H2and Cl2gases generated from a liquid resource usingan electrochemical cell is combined to create HC1 acid for subsequent use in acid, acid eluent, or other process fluids.
[0235] In some embodiments, a solid base is mixed with a liquid resource to create a basic solution. In some embodiments, a solid base is mixed with a liquid resource to create a basic solution, and the resulting basic solution is added to a second volume of a liquid resource to increase the pH of the second volume of a liquid resource. In some embodiments, solid base is mixed with a liquid resource to create a basic solution, wherein the resulting basic solution is used to adjust or control the pH of a second solution. In some embodiments, a solid base is mixed with a liquid resource to create a basic slurry. In some embodiments, a solid base is mixed with a liquid resource to create a basic slurry, and the resulting basic slurry is added to a second volume of a liquid resource to increase the pH of the second volume of a liquid resource. In some embodiments, solid base is mixed with a liquid resource to create a basic slurry, wherein the resulting basic slurry is used to adjust or control the pH of a second solution. In some embodiments, base is added to a liquid resource as a mixture or slurry of base and liquid resource.
[0236] In one embodiment of the system for lithium recovery from a liquid resource, the liquid resource flows through a pH control column containing solid base particles that comprise NaOH, CaO, or Ca(OH)2, which dissolve into the liquid resource and raise the pH of the liquid resource. In some embodiments of the system for lithium recovery from a liquid resource, the liquid resource flows through a pH control column containing immobilized regeneratable hydroxyl-containing ion exchange resins which react with hydrogen ions, or regeneratable base species such as immobilized polypyridine that conjugates acid, thereby neutralizing acid in the liquid resource. When the ion exchange resin has been depleted of its hydroxyl groups or is fully conjugated with acid, it can be regenerated with a base such as NaOH.
[0237] In some embodiments of the system for lithium recovery from a liquid resource, pH meters are installed in tanks, pipes, columns, and other components of the system to monitor pH and control the rates and amounts of base addition at various locations throughout the system.
[0238] In some embodiments of the system for lithium recovery from a liquid resource, the columns, tanks, pipes, and other components of the system are optionally constructed using plastic, metal with a plastic lining, or other materials that are resistant to corrosion by liquid resource, base, or acid.
[0239] In some embodiments of the system for lithium recovery from a liquid resource, the columns are optionally washed with water that is mildly acidic, optionally including a buffer, to remove any basic precipitates from the column prior to acid elution.
[0240] In some embodiments, after the ion exchange material within an ion exchange device becomes saturated or nearly saturated with lithium, the lithium is flushed out of the ion exchange device using acid. In some embodiments, the acid is flowed through the ion exchange device one or more times to elute the lithium. In some embodiments, the acid is flowed through the ion exchange device using a recirculating batch system that comprises the ion exchange device in fluid connection to a tank. In some embodiments, a recirculating batch system comprises one or more tanks. In some embodiments, a tank within a recirculating batch system comprises an ion exchange device. In some embodiments, the tank is configured to accommodate a flow of liquid resource or acid. In some embodiments, a plurality of tanks is configured to accommodate a flow of acid flows in one or more tanks and a separate flow of liquid resource in a separate one or more tanks. In some embodiments, acid is input into the top of an ion exchange device, be allowed to percolate through the ion exchange device by means of a natural or applied force, and be immediately recirculated into the ion exchange device. In some embodiments, acid is added to an ion exchange device without utilizing a tank configured to accommodate acid or a flow of acid.
[0241] In one embodiment of the system for lithium recovery from a liquid resource, the ion exchange device is washed with water after liquid resource and acid have been passed through the ion exchange device, wherein the effluent water produced by washing the ion exchange device with water is treated using pH neutralization and reverse osmosis to yield water suitable for use as a process fluid.
[0242] In some embodiments of the system for lithium recovery from a liquid resource, the ion exchange device is optionally shaped like a cylinder, a rectangle, or another shape. In some embodiments, the ion exchange device optionally has a cylinder shape with a height that is greater or less than its diameter. In some embodiments, the ion exchange device has a cylinder shape with a height that is less than 10 cm, less than 1 meter, or less than 10 meters. In some embodiments, the ion exchange device has a cylinder shape with a diameter that is less than 10 cm, less than 1 meter, or less than 10 meters.
[0243] In some embodiments of the system for lithium recovery from a liquid resource, the system is optionally resupplied with ion exchange material by swapping out an ion exchange device with a new ion exchange device loaded with ion exchange material. In some embodiments of the system for lithium recovery from a liquid resource, the system is optionally resupplied with ion exchange material by removing ion exchange material from the ion exchange device and loading ion exchange material into the ion exchange device that does not comprise the removed ion exchange material. In some embodiments of the system for lithium recovery from a liquid resource, ion exchange material is resupplied to all ion exchange devicesin the system simultaneously. In some embodiments of the system for lithium recovery from a liquid resource, ion exchange material is resupplied to one or more ion exchange devices at a time. In one embodiment of the system for lithium recovery from a liquid resource, ion exchange material is resupplied to one or more ion exchange devices without interrupting the operation of other ion exchange devices within the system.
[0244] In some embodiments of system for lithium recovery from a liquid resource, a point of lithium saturation comprises a set of conditions wherein ion exchange material is unable to extract lithium ions from liquid resource or extract lithium ions from liquid resource at an acceptable rate despite the liquid resource having a pH value and lithium concentration that are ideal, preferred, or suitable for the extraction of lithium therefrom by ion exchange material. In some embodiments of the system for lithium recovery from a liquid resource, pumping of the liquid resource continues until the ion exchange material approaches a point of lithium saturation over a period of time that is optionally less than about 1 hours, less than about 2 hours, less than about 4 hours, less than about 8 hours, less than about 24 hours, less than about 48 hours, or less than about one week. In some embodiments of system for lithium recovery from a liquid resource, pumping of the liquid resource continues until the ion exchange material approaches a point of lithium saturation over a period of time that is optionally greater than about one week. In some embodiments of system for lithium recovery from a liquid resource, pumping of the liquid resource continues until the ion exchange material approaches a point of lithium saturation over a period of time that is optionally between 30 minutes and 24 hours. In some embodiments of system for lithium recovery from a liquid resource, a point of hydrogen saturation comprises a set of conditions wherein ion exchange material is unable to extract hydrogen ions from acid at an acceptable rate despite the acid having a pH value that is ideal, preferred, or suitable for the extraction of hydrogen therefrom by ion exchange beads. In some embodiments of system for lithium recovery from a liquid resource, pumping of acid continues until the ion exchange material approaches a point of hydrogen saturation over a period of time that is optionally less than about 1 hours, less than about 2 hours, less than about 4 hours, less than about 8 hours, less than about 24 hours, or less than about 48 hours. In some embodiments of system for lithium recovery from a liquid resource, pumping of acid continues until the ion exchange material approaches a point of hydrogen saturation over a period of time that is optionally greater than about one 48 hours. In some embodiments of system for lithium recovery from a liquid resource, pumping of acid continues until the ion exchange material approaches a point of hydrogen saturation over a period of time that is optionally between 30 minutes and 24 hours.Base and Acid Generation
[0245] In some embodiments of the methods and systems described herein, acid and base are generated using an electrochemical cell. In some embodiments, acid and base are generated using an electrochemical cell that comprises electrodes. In some embodiments, acid and base are generated using an ion-conducting membrane. In some embodiments, the ionconducting membrane is a cation-conducting membrane, an anion-conducting membrane or combinations thereof. In some embodiments, the ion-conducting membrane comprises sulfonated tetrafluoroethylene-based fluoropolymer-copolymer, sulfonated polytetrafluoroethylene, sulfonated fluoropolymer, MK-40, co-polymers, or combinations thereof.
[0246] In some embodiments, the ion-conducting membrane comprises a functionalized polymer structure. In some embodiments, the functionalized polymer structure comprises polyarylene ethers, polysulfones, polyether ketones, polyphenylenes, perfluorinated polymers, polybenzimidazole, polyepichlorohydrins, unsaturated polypropylene, polyethylene, polystyrene, polyvinylbenzyl chlorides, polyphosphazenes, polyvinyl alcohol, polytetrafluoroethylene, polyvinyl chloride, polyvinylidene fluoride, alterations of these polymers or other kinds of polymers, or composites thereof. In some embodiments, the ionconducting membrane comprises a cation-conducting membrane that allows for transfer of lithium ions across the ion-conducting membrane but prevents transfer of anion groups across the ion-conducting membrane. In some embodiments, the ion-conducting membrane has a thickness from about 1 pm to about 1000 pm. In some embodiments, the ion-conducting membrane has a thickness from about 1 mm to about 10 mm.
[0247] In some embodiments, acid and base are generated using an electrochemical cell that comprises electrodes. In some embodiments, the electrodes are comprised of titanium, niobium, zirconium, tantalum, magnesium, titanium dioxide, oxides thereof, or combinations thereof. In some embodiments, the electrodes comprise a coating thereon of platinum, TiCh, ZrCh, Nb2Os, Ta20s, SnCh, IrCh, RuCh, mixed metal oxides, graphene, derivatives thereof, or combinations thereof.
[0248] In some embodiments of a system for lithium recovery from a liquid resource, a chlor-alkali plant is used to generate HC1 and NaOH from an aqueous NaCl solution. In some embodiments, the HC1 generated by the chlor-alkali plant is used as an acid or as an acid eluent. In some embodiments, the NaOH generated by the chlor-alkali plant is used to adjust the pH of the liquid resource. In some embodiments, the NaOH generated by the chlor-alkali plant is used to precipitate impurities from a synthetic lithium solution.
[0249] In some embodiments of a system for lithium recovery from a liquid resource, the system comprises one or more electrochemical or electrolysis systems. The terms “electrochemical” and “electrolysis” are used interchangeably in the present specification and these terms are synonymous unless specifically noted to the contrary. In some embodiments, an electrolysis system is comprised of one or more electrochemical cells. In some embodiments, an electrochemical system is used to produce HC1 and NaOH. In some embodiments, an electrochemical system converts a salt solution into acid and base. In some embodiments, an electrochemical system converts a salt solution containing NaCl, KC1, and / or other chlorides into base and acid. In some embodiments, a salt solution comprising precipitates recovered from the liquid resource is fed into an electrochemical system to produce acid and base. In some embodiments, an electrolysis system converts a lithium salt solution to form a lithium hydroxide solution, an acidified solution, and optionally a dilute lithium salt solution. In some embodiments, the lithium salt solution comprises a synthetic lithium solution provided according to the methods and systems described herein that has optionally been concentrated and / or purified. In some embodiments, the acidified solution generated from an electrolysis system is provided to an ion exchange device to elute lithium in the form of a synthetic lithium solution.
[0250] In some embodiments, a lithium salt solution comprises acid derived from an acid eluent or an ion exchange device. In some embodiments, acid in the lithium salt solution derived from an acid eluent or an ion exchange device passes through an electrolysis system wherein the acid is further acidified to form an acidified solution. In some embodiments, a lithium salt solution is purified to remove impurities without neutralizing the acid in the lithium salt solution prior to the lithium salt solution being fed into an electrolysis system.
[0251] In some embodiments, an acidified solution produced by an electrolysis system comprises lithium ions from the lithium salt solution fed into the electrolysis system. In some embodiments, an acidified solution comprising lithium ions leaves the electrolysis system and is provided to an ion exchange device to elute lithium in the form of a synthetic lithium solution.
[0252] In some embodiments of an electrolysis system, the electrolysis cells are electrochemical cells. In some embodiments of an electrochemical cell, the ion-conducting membranes are cation-conducting and / or anion-conducting membranes. In some embodiments, the electrochemical cell is a two-compartment cell with a cation-conducting membrane that allows for transfer of lithium ions between the compartments but prevents transfer of anion groups such as chloride, sulfate, and hydroxide groups between the compartments.
[0253] In some embodiments of an electrolysis system, the electrolysis cells are electrodialysis cells. In some embodiments of an electrodialysis cell, the ion-conductingmembranes are cation-conducting and / or anion-conducting membranes. In some embodiments, the electrodialysis cell is a two-compartment cell with a cation-conducting membrane that allows for transfer of lithium ions between the compartments but prevents transfer of anion groups such as chloride, sulfate, and hydroxide groups between the compartments.
[0254] In some embodiments of an electrolysis system, the electrolysis cells are membrane electrolysis cells. In some embodiments of a membrane electrolysis cell, the ionconducting membranes are cation-conducting and / or anion-conducting membranes. In some embodiments, the membrane electrolysis cell is a two-compartment cell with a cationconducting membrane that allows for transfer of lithium ions between the compartments but prevents transfer of anion groups such as chloride, sulfate, and hydroxide groups between the compartments.
[0255] In some embodiments, the membrane electrolysis cell is a three-compartment cell with a cation-conducting membrane that allows for transfer of lithium ions separating a compartment with an electrochemically reducing electrode from a central compartment and with an anion-conducting membrane that allows for transfer of anions separating a compartment with an electrochemically oxidizing electrode from the central compartment. In some embodiments, the cation-conducting membrane prevents transfer of anions such as chloride, sulfate, or hydroxide. In some embodiments, the anion-conducting membrane prevents transfer of cations such as lithium, sodium, or protons.
[0256] In some embodiments of the membrane electrolysis cell, the ion-conducting membranes are comprised of Nafion®, sulfonated tetrafluoroethylene, sulfonated fluoropolymer, MK-40, co-polymers, other membrane materials, composites, or combinations thereof. In some embodiments of the membrane electrolysis cell, the cation-conducting membranes are comprised of a functionalized polymer structure which comprises Nafion®, sulfonated tetrafluoroethylene, sulfonated fluoropolymer, co-polymers, different polymers, composites of polymers, or combinations thereof. In some embodiments of the membrane electrolysis cell, the ion-conducting membrane comprises polymer structures functionalized with sulfone groups, carboxylic acid groups, phosphate groups, other negatively charged functional groups, or combinations thereof.
[0257] In some embodiments of the electrochemical cell, the ion-conducting membranes are comprised of Nafion®, sulfonated tetrafluoroethylene, sulfonated fluoropolymer, MK-40, co-polymers, other membrane materials, composites, or combinations thereof. In some embodiments of the electrochemical cell, the cation-conducting membranes are comprised of a functionalized polymer structure that comprises Nafion®, sulfonated tetrafluoroethylene, sulfonated fluoropolymer, co-polymers, different polymers, composites of polymers, orcombinations thereof. In some embodiments of the electrochemical cell, the ion-conducting membranes comprise polymer structures functionalized with sulfone groups, carboxylic acid groups, phosphate groups, other negatively charged functional groups, or combinations thereof.
[0258] In some embodiments of the electrodialysis cell, the membranes are comprised of Nafion®, sulfonated tetrafluoroethylene, sulfonated fluoropolymer, MK-40, co-polymers, other membrane materials, composites, or combinations thereof. In some embodiments of the electrodialysis cell, the cation-conducting membranes are comprised of a functionalized polymer structure that comprises Nafion®, sulfonated tetrafluoroethylene, sulfonated fluoropolymer, copolymers, different polymers, composites of polymers, or combinations thereof. In some embodiments of the electrodialysis cell, the cation-conducting membranes comprise polymer structures functionalized with sulfone groups, carboxylic acid groups, phosphate groups, other negatively charged functional groups, or combinations thereof.
[0259] In some embodiments of the membrane electrolysis cell, an ani on-conducting membrane is comprised of a functionalized polymer structure. In some embodiments of the electrochemical cell, an anion-conducting membrane is comprised of a functionalized polymer structure. In some embodiments of the electrodialysis cell, an anion-conducting membrane is comprised of a functionalized polymer structure. In some embodiments, a functionalized polymer structure is comprised of polyarylene ethers, polysulfones, polyether ketones, polyphenylenes, perfluorinated polymers, polybenzimidazole, polyepichlorohydrins, unsaturated polypropylene, polyethylene, polystyrene, polyvinylbenzyl chlorides, polyphosphazenes, polyvinyl alcohol, polytetrafluoroethylene, polyvinyl chloride, polyvinylidene fluoride, alterations of these polymers or other kinds of polymers, or composites thereof. In some embodiments of the ion-conducting membrane, the functional groups are part of the polymer backbone. In some embodiments of the ion-conducting membrane, functional groups are added using plasma techniques, radiation-grafting, or by other functionalization reactions. In some embodiments of the ion-conducting membrane, the functional groups include benzyltrialkylammonium, alkyl-side-chain quaternary ammonium groups, crosslinking diammonium groups, quinuclidinium-based quaternary ammonium groups, imidazolium groups, pyridinium groups, pentamethylguanidinium groups, alkali stabilised quaternary phosphonium groups, metal containing cation groups, other cation containing groups, or combinations thereof.
[0260] In some embodiments of the membrane electrolysis cell, the ion-conducting membrane has a thickness of less than 10 pm, less than 50 pm, less than 200 pm, less than 400 pm, or less than 1,000 pm. In some embodiments of the membrane electrolysis cell, the ionconducting membranes has a thickness of greater than 1,000 pm. In some embodiments of the membrane electrolysis cell, the ion-conducting membrane has a thickness of about 1 pm toabout 1000 pm, about 1 gm to about 800 pm, about 1 gm to about 600 gm, about 1 gm to about 400 gm, about 1 gm to about 200 gm, about 1 gm to about 100 gm, about 1 gm to about 90 gm, about 1 gm to about 80 gm, about 1 gm to about 70 gm, about 1 gm to about 60 gm, about 1 gm to about 50 gm, about 1 gm to about 40 gm, about 1 gm to about 30 gm, about 1 gm to about 20 gm, about 1 gm to about 15 gm, or about 1 gm to about 10 gm.
[0261] In some embodiments of the electrochemical cell, the ion-conducting membrane has a thickness of less than 10 gm, less than 50 gm, less than 200 gm, less than 400 gm, or less than 1,000 gm. In some embodiments of the electrochemical cell, the ion-conducting membranes has a thickness of greater than 1,000 gm. In some embodiments of the electrochemical cell, the ion-conducting membrane has a thickness of about 1 gm to about 1000 gm, about 1 gm to about 800 gm, about 1 gm to about 600 gm, about 1 gm to about 400 gm, about 1 gm to about 200 gm, about 1 gm to about 100 gm, about 1 gm to about 90 gm, about 1 gm to about 80 gm, about 1 gm to about 70 gm, about 1 gm to about 60 gm, about 1 gm to about 50 gm, about 1 gm to about 40 gm, about 1 gm to about 30 gm, about 1 gm to about 20 gm, about 1 gm to about 15 gm, or about 1 gm to about 10 gm.
[0262] In some embodiments of the electrodialysis cell, the ion-conducting membrane has a thickness of less than 10 gm, less than 50 gm, less than 200 gm, less than 400 gm, or less than 1,000 gm. In some embodiments of the electrodialysis cell, the ion-conducting membranes have a thickness of greater than 1,000 gm. In some embodiments of the electrodialysis cell, the ion-conducting membrane has a thickness of about 1 gm to about 1000 gm, about 1 gm to about 800 gm, about 1 gm to about 600 gm, about 1 gm to about 400 gm, about 1 gm to about 200 gm, about 1 gm to about 100 gm, about 1 gm to about 90 gm, about 1 gm to about 80 gm, about 1 gm to about 70 gm, about 1 gm to about 60 gm, about 1 gm to about 50 gm, about 1 gm to about 40 gm, about 1 gm to about 30 gm, about 1 gm to about 20 gm, about 1 gm to about 15 gm, or about 1 gm to about 10 gm.
[0263] In some embodiments, an electrolysis system contains electrolysis cells that are two-compartment electrolysis cells or three-compartment electrolysis cells.
[0264] In some embodiments of a two-compartment electrolysis cell, the cell contains a first compartment that contains an electrochemically oxidizing electrode. A lithium salt solution enters the first compartment and is converted into an acidified solution. In some embodiments of a two-compartment electrolysis cell, the cell contains a second compartment containing an electrochemically reducing electrode. This second compartment takes as an input water or a dilute LiOH solution and produces as an output a more concentrated LiOH solution. In some embodiments, the compartments of an electrolysis cell are separated by a cation-conducting membrane that limits transport of anions between the compartments.
[0265] In some embodiments of a three-compartment electrolysis cell, the cell contains a first compartment containing an electrochemically oxidizing electrode. The first compartment takes as an input water or a dilute salt solution, and produces as an output an acidified solution. In some embodiments of a three-compartment electrolysis cell, the cell contains a second compartment containing an electrochemically reducing electrode. This second compartment takes as an input a water or dilute hydroxide solution, and produces as an output a more concentrated hydroxide solution. In some embodiments of a three-compartment electrolysis cell, the cell contains a third compartment containing no electrode, which is located between the first and second compartment, and takes as an input a concentrated lithium salt solution, and produces as an output a dilute lithium salt solution. In some embodiments, the first and the third compartments are separated by an anion-conducting membrane that limits transport of cations between the compartments. In one embodiment, the second and the third compartments are separated by a cation-conducting membrane that limits transport of anions between the compartments.
[0266] In some embodiments of the electrolysis cell, the electrodes are comprised of titanium, niobium, zirconium, tantalum, magnesium, titanium dioxide, oxides thereof, or combinations thereof. In one embodiment of the electrolysis cell, the electrodes are coated with platinum, TiCh, ZrCh, bfeOs, Ta20s, SnCh, IrCh, RuCh, PtOx, mixed metal oxides, graphene, derivatives thereof, or combinations thereof. In some embodiments of the electrolysis cell, the electrodes are comprised of steel, stainless steel, nickel, nickel alloys, steel alloys, or graphite.
[0267] In some embodiments of the electrolysis system, the lithium salt solution is a LiCl solution optionally containing HC1. In one embodiment of the electrolysis system, the electrochemically oxidizing electrode oxides chloride ions to produce chlorine gas.
[0268] In some embodiments of the electrolysis system, the lithium salt solution is a Li2SO4 solution optionally containing H2SO4. In some embodiments of the electrolysis system, the electrochemically oxidizing electrode oxidizes water, hydroxide, or other species to produce oxygen gas.
[0269] In some embodiments of the electrolysis system, the electrochemically reducing electrode reduces hydrogen ions to produce hydrogen gas. In some embodiments of the electrolysis system, the chamber containing the electrochemically reducing electrode produces a hydroxide solution or increases the hydroxide concentration of a solution.
[0270] In some embodiments, phosphoric acid is used to elute lithium from a lithiumselective sorbent to provide a synthetic lithium solution comprising phosphate. In some embodiments, sulfuric acid is used to elute lithium from a lithium-selective sorbent to provide a synthetic lithium solution comprising sulfate. In some embodiments, electrolysis of a syntheticlithium solution comprising phosphate is more efficient than electrolysis of a synthetic lithium solution comprising chloride. In some embodiments, electrolysis of a synthetic lithium solution comprising sulfate is more efficient than electrolysis of a synthetic lithium solution comprising chloride.
[0271] In some embodiments of the electrolysis system, chlorine and hydrogen gas are burned to produce HC1 in an HC1 burner. In some embodiments, the HC1 burner is a column maintained at approximately 100-300 or 300-2,000 degrees Celsius. In some embodiments, HC1 produced in the HC1 burner is cooled through a heat exchange process and subsequently dissolved into water in an absorption tower configured to produce aqueous HC1 solution. In some embodiments, the HC1 solution produced from the HC1 burner is used as an acid eluent to elute lithium from an ion exchange device to yield a synthetic lithium solution.
[0272] In some embodiments, the pH of the acidified solution leaving the electrolysis cell is 0 to 1, -2 to 0, 1 to 2, less than 2, less than 1, or less than 0. In some embodiments, the membrane electrolysis cell is an electrodialysis cell with multiple compartments. In some embodiments, the electrodialysis cell has more than about two, more than about five, more than about 10, or more than about twenty compartments.
[0273] In some embodiments, the base added to precipitate metals from the liquid resource comprises calcium hydroxide or sodium hydroxide. In some embodiments, the base is added to the liquid resource as an aqueous solution with a base concentration that is less than 1 N, 1-2 N, 2-4 N, 4-10 N, 10-20 N, or 20-40 N. In some embodiments, the base is added to the liquid resource as a solid.
[0274] In some embodiments, the acid is added to the precipitated metals to dissolve the precipitated metals before mixing the redissolved metals with the liquid resource. In some embodiments, the acid is added to the liquid resource to acidify the liquid resource, such that the precipitated metals are then combined with the liquid resource to redissolve the precipitated metals.
[0275] In some embodiments, acid from the electrochemical cell is used as an acid eluent to elute lithium from an ion exchange device to yield a synthetic lithium solution. In some embodiments, base from the electrochemical cell is used to neutralize protons released from the ion exchange material.Some Embodiments of Methods of Generating a Synthetic Lithium Solution
[0276] An aspect of the disclosure described herein are methods and systems for lithium recovery from a liquid resource. In some embodiments, lithium provided according to the methods and systems for lithium recovery from a liquid resource described herein is in the formof a synthetic lithium solution. In some embodiments, a synthetic lithium solution is an aqueous solution comprising lithium that is produced by a process contacting an acid or acid eluent with ion exchange material. In some embodiments, an aqueous solution comprising lithium that is produced by a process contacting an acid eluent with ion exchange material is referred to as a lithium eluate. In some embodiments, a synthetic lithium solution is a lithium eluate. For the purposes of this disclosure, a lithium eluate according to all embodiments described herein is a synthetic lithium solution.
[0277] In some embodiments, a method for generating a synthetic lithium solution from a liquid resource comprises: providing an ion exchange device comprising a tank, ion exchange particles that selectively absorbs lithium from a liquid resource and elute a synthetic lithium solution when treated with an acid after absorbing lithium ions from said liquid resource, one or more particle traps, and optionally a means of modulating the pH of the liquid resource; flowing a liquid resource into said ion exchange device thereby allowing the ion exchange particles to selectively absorb lithium from the liquid resource; treating the ion exchange particles with an acid to yield the synthetic lithium solution; and passing the synthetic lithium solution through the one or more particle traps prior to collecting the synthetic lithium solution. In some embodiments, the method for generating a synthetic lithium solution from a liquid resource further comprises one or more steps wherein the ion exchange material is washed with washing water.
[0278] In some embodiments, the system for lithium recovery from a liquid resource comprises a tank. In some embodiments, the tank has a spherical shape. In some embodiments, the tank has a cylindrical shape. In some embodiments, the tank has a rectangular shape. In some embodiments, the tank has a conical shape. In some embodiments, the tank has a partially conical shape. In some embodiments, the conical shape allows the ion exchange particles to settle into a settled bed so that liquid can be removed from above the settled bed. In some embodiments, the partial conical shape allows the ion exchange particles to settle into a settled bed so that liquid can be removed from above the settled bed.
[0279] In some embodiments, modulation of the pH of the liquid resource occurs in the tank. In some embodiments, modulation of the pH of the liquid resource occurs prior to injection into the tank. In some embodiments, one or more particle traps comprise one or more filters inside the tank. In some embodiments, one or more particle traps comprise one filter. In some embodiments, one or more particle traps comprise one filter. In some embodiments, one or more particle traps comprise two filters. In some embodiments, one or more particle traps comprise three filters. In some embodiments, one or more particle traps comprise four filters. In some embodiments, one or more particle traps comprise five filters.
[0280] In some embodiments, one or more particle traps are located at the bottom of the tank. In some embodiments, one or more particle traps are located close to the bottom of the tank. In some embodiments, one or more particle traps are located above the bottom of the tank. In some embodiments, one or more particle traps are located in the middle the bottom of the tank. In some embodiments, one or more particle traps are located at the top of the tank. In some embodiments, one or more particle traps are located at various locations of the tank.
[0281] In some embodiments, one or more particle traps comprise one or more meshes. In some embodiments, one or more particle traps comprises one mesh. In some embodiments, one or more particle traps comprises two meshes. In some embodiments, one or more particle traps comprises three meshes. In some embodiments, one or more particle traps comprises four meshes. In some embodiments, one or more particle traps comprises five meshes. In some embodiments, all the meshes of the one or more particle traps are identical. In some embodiments, at least one of the meshes of the one or more particle traps is not identical to the other the meshes of the one or more particle traps.
[0282] In some embodiments, one or more meshes comprise a pore size of less than about 200 microns, less than about 175 microns, less than about 150 microns, less than about 100 microns, less than about 75 microns, less than about 50 microns, less than about 25 microns, less than about 10 microns, more than about 1 micron, more than about 5 micron, more than about 10 microns, more than about 20 microns, more than about 30 microns, more than about 40 microns, more than about 50 microns, more than about 60 microns, more than about 70 microns, more than about 80 microns, more than about 90 microns, more than about 100 microns, more than about 125 microns, more than about 150 microns, more than about 175 microns from about 1 micron to about 200 microns, from about 5 microns to about 175 microns, from about 10 microns to about 150 microns, from about 10 microns to about 100 microns, from about 10 microns to about 90 microns, from about 10 microns to about 80 microns, from about 10 microns to about 70 microns, from about 10 microns to about 60 microns, or from about 10 microns to about 50 microns.
[0283] In some embodiments, one or more particle traps comprise multi-layered meshes. In some embodiments, the multi-layered meshes comprise at least one finer mesh for filtration and at least one coarser mesh for structural support. In some embodiments, one or more particle traps comprise one or more meshes supported by a structural support. In some embodiments, one or more particle traps comprise one or more polymer meshes. In some embodiments, the one or more polymer meshes are selected from the group consisting of poly etheretherketone, ethylene tetrafluorethylene, polyethylene terephthalate, polypropylene, and combinations thereof. In some embodiments, the one or more meshes comprise a monofilament mesh. In someembodiments, the one or more meshes comprise a multi-weave mesh. In some embodiments, the one or more meshes are constructed from one or more types of fibers. In some embodiments, said one or more fibers are weaved into one or more weave patterns. In some embodiments, said weave patterns comprise a plain weave, a twilled weave, a plain filter loth weave, a Dutch Weave, a twilled filter cloth weave, a twilled Dutch Weave, a micron weave, mixtures thereof, or combinations thereof.
[0284] In some embodiments, one or more particle traps comprise one or more meshes comprising a metal wire mesh. In some embodiments, the metal wire mesh is coated with a polymer. In some embodiments, the ion exchange device is configured to move ion exchange material into one or more columns for washing. In some embodiments, the ion exchange device is configured to allow the ion exchange material to settle into one or more columns for washing. In some embodiments, the columns are affixed to the bottom of the tank. In some embodiments, the one or more particle traps comprise one or more filters mounted in one or more ports through the wall of the tank.
[0285] In some embodiments, the one or more particle traps comprise one or more filters external to the tank, and with provision for fluid communication between said one or more filters and the tank. In some embodiments, the one or more particle traps comprise one or more gravity sedimentation devices external to the tank, and with provision for fluid communication between said one or more gravity sedimentation devices and the tank. In some embodiments, the one or more particle traps comprise one or more filter presses external to the tank. In some embodiments, the one or more particle traps comprise one or more vertical pressure filters external to the tank. In some embodiments, the one or more particle traps comprise one or more pressure leaf filters external to the tank. In some embodiments, the one or more particle traps comprise one or more belt filters external to the tank.
[0286] In some embodiments, one or more particle traps comprise one or more gravity sedimentation devices internal to the tank. In some embodiments, one or more particle traps comprise one or more centrifugal sedimentation devices external to the tank, and with provision for fluid communication between said one or more centrifugal sedimentation devices and the tank. In some embodiments, said sedimentations devices comprise a clarifier, a lamellar clarifier, a reflux clarifier, or any other device design to sediment the solids to the bottom while facilitating flow of a solid-lean liquid from the top. In some embodiments, one or more particle traps comprise one or more centrifugal sedimentation devices internal to the tank. In some embodiments, one or more particle traps comprise one or more settling tanks, one or more centrifugal devices, or combinations thereof external to the tank, and with provision for fluid communication between the one or more settling tanks, centrifugal devices, or combinationsthereof, and the tank. In some embodiments, one or more particle traps comprise one or more meshes, one or more centrifugal devices, or combinations thereof external to the tank, and with provision for fluid communication between said one or more meshes, centrifugal devices, or combinations thereof, and the tank. In some embodiments, one or more particle traps comprise one or more settling tanks, one or more meshes, or combinations thereof external to the tank, and with provision for fluid communication between said one or more settling tanks, meshes, or combinations thereof, and the tank. In some embodiments, one or more particle traps comprise one or more meshes, one or more settling tanks, one or more centrifugal devices, or combinations thereof external to the tank, and with provision for fluid communication between said one or more meshes, one or more settling tanks, centrifugal devices, or combinations thereof, and the tank.
[0287] In some embodiments, the ion exchange particles are stirred. In some embodiments, the ion exchange particles are stirred by a mixer. In some embodiments, the ion exchange particles are stirred by a propeller. In some embodiments, the ion exchange particles are stirred by a hydrofoil. In some embodiments, the stirring or agitation of the ion exchange particles is aided by the presence of one or more baffles in the tank. In some embodiments, said baffles are oriented perpendicular to the direction of rotation of the mixing device. In some embodiments, the ion exchange particles are fluidized by pumping solution into the tank near the bottom of the tank. In some embodiments, the ion exchange particles are fluidized by pumping solution from the tank back into the tank near the bottom of the tank. In some embodiments, the ion exchange particles are fluidized by pumping a slurry of the ion exchange particles from near the bottom of the tank to a higher level in the tank. In some embodiments, the ion exchange particles are fluidized by injecting a gas into a flow distributor at the bottom of said tank. In some embodiments, the gas comprises compressed air, air, nitrogen, argon, oxygen, or a combination thereof.
[0288] In some embodiments, the method for lithium recovery from a liquid resource further comprises one or more staged elution tanks, wherein intermediate eluate solutions comprising mixtures of protons and lithium ions are stored and used further to elute lithium from ion exchange particles . In some embodiments, the method for lithium recovery from a liquid resource further comprises one or more staged elution tanks, wherein intermediate eluate solutions comprising mixtures of protons and lithium ions are mixed with acid and used further to elute lithium from ion exchange particles.
[0289] In some embodiments, the ion exchange particles further comprise a coating material. In some embodiments, the coating material is a polymer. In some embodiments, the coating of the coating material comprises a chloro-polymer, a fluoro-polymer, a chloro-fluoro-polymer, a hydrophilic polymer, a hydrophobic polymer, co-polymers thereof, mixtures thereof, or combinations thereof.
[0290] In some embodiments of the methods and systems for lithium recovery from a liquid resource disclosed herein, the pH of the intermediate eluate solutions is modulated to control elution of lithium and / or non-lithium impurities from the ion exchange material. In some embodiments, pH of the intermediate eluate solutions is modulated by adding protons, such as in an acid and / or an acidic solution, to the intermediate eluate solutions. In some embodiments, pH of the intermediate eluate solutions is modulated by adding protons, such as in an acid and / or an acidic solution, to the intermediate eluate solutions prior to removing impurities therefrom.
[0291] In some embodiments, the acid added to the intermediate eluate solutions comprises sulfuric acid, phosphoric acid, hydrochloric acid, hydrobromic acid, carbonic acid, nitric acid, or combinations thereof. In some embodiments, the acid added to the intermediate eluate solutions comprises the same acid as does the acid eluent originally contacted with the ion exchange material. In some embodiments, the acid added to the intermediate eluate solutions comprises a different acid than does the acid eluent originally contacted with the ion exchange material.
[0292] In some embodiments, more protons are added to the intermediate eluate solutions, forming protonated intermediate eluate solutions that is again contacted with ion exchange material to elute more lithium into the protonated intermediate eluate solutions. In some embodiments, more protons are added to the intermediate eluate solutions by adding an acid or acidic solution thereto to form protonated intermediate eluate solutions. In some embodiments, protons are added to intermediate eluate solutions before passing the resulting protonated intermediate eluate solutions through one or more ion exchange devices as described herein.
[0293] In some embodiments of the methods and systems for lithium recovery from a liquid resource disclosed herein, an anti-scalant or chelating agent is added to the liquid resource to limit formation of precipitates. In some embodiments, ion exchange material is utilized in the form of packed beds wherein the packed beds are partially or temporarily fluidized. In some embodiments, ion exchange material is utilized in the form of fluidized beds wherein the fluidized beds are partially or temporarily packed. In some embodiments, ion exchange material is washed using water or an aqueous washing solution before and / or after contacting the ion exchange material with liquid resource and / or acid. In some embodiments, washing water comprises an aqueous washing solution. In some embodiments, an aqueous washing solution comprises water, salt, chelating compounds, ethylenediaminetetraacetic acid, salts of ethylenediaminetetraacetate, compounds of ethylenediaminetetraacetate, and / or anti -seal ants. Insome embodiments, the eluent used to elute lithium from the ion exchange material comprises water, salt, chelating compounds, ethylenediaminetetraacetic acid, salt of ethylenediaminetetraacetate, compounds of ethylenediaminetetraacetate, and / or anti -seal ants.
[0294] In some embodiments, a chelating agent or anti-scalant is used to form a soluble complex to avoid the formation of precipitates in a synthetic lithium solution. In some embodiments, a chelating agent or anti-scalant is used to form a soluble complex to avoid or redissolve precipitates. In some embodiments, a chelating agent or anti-scalants is used to limit or reduce precipitation of multivalent cations. In some embodiments, the chelating agent or anti- scalant is selected from ethylenediaminetetraacetic acid (EDTA), disodium EDTA, calcium disodium EDTA, tetrasodium EDTA, citric acid, maleic acid, silicate compounds, amorphous silicate compounds, crystalline layered silicate compounds, phosphonic acid compounds, egtazic acid (or salts thereof), aminotris(methylenephosphonic acid) (ATMP), nitrilotrimethylphosphonic acid (NTMP), ethylenediamine tetra(methylene phosphonic acid) (EDTMP), diethylenetriamine penta(methylene phosphonic acid) (DTPMP), polyphosphonate, polyacrylate, polyacrylic acid, nitrilotriacetic acid (NTA), sodium hexametaphosphate (SHMP), or combinations thereof. In some embodiments, a threshold inhibitor is used to block the formation of nuclei that initiate precipitate formation in a synthetic lithium solution. In some embodiments, a retardant is used to prevent the growth of precipitates in synthetic lithium solution. In some embodiments, a threshold inhibitor or retardant comprises one or more compounds that to limit, control, eliminate, or redissolve precipitates. In some embodiments, compounds that limit, control, eliminate, or redissolve precipitates include phosphinopolycarboxylic acid, sulfonated polymer, polyacrylic acid, p-tagged sulfonated polymer, diethylenetriamine penta, bis-hexamethylene triamine, compounds thereof, modifications thereof, or combinations thereof.
[0295] In some embodiments, anti-scalants, chelating agents, or other means of antiscaling are used to avoid scaling in the nanofiltration membrane units.
[0296] In some embodiments, lithium is eluted from an ion exchange material enriched in lithium by contacting an eluent with the ion exchange material to provide a synthetic lithium solution. In some embodiments, the lithium purity of the synthetic lithium solution changes in time as a portion of eluent is contacted with the ion exchange material. In some embodiments, the lithium purity of the synthetic lithium solution increases as additional eluent is contacted with the ion exchange material. In some embodiments, multiple aliquots of eluent are used to elute lithium from a given quantity of ion exchange material. In some embodiments, aliquots of eluent are of different volumes. In some embodiments, aliquots of eluent are of substantially the same volume. In some embodiments, the first aliquot of eluent is contacted with the ionexchange material to provide a first aliquot of synthetic lithium solution. In some embodiments, subsequent aliquots of eluent are then contacted with the ion exchange material to produce subsequent aliquots of synthetic lithium solution. In some embodiments, the first aliquot of synthetic lithium solution comprises lower lithium purity than subsequent aliquots of synthetic lithium solution. In some embodiments, the volume of the first aliquot of eluent is selected to provide a first aliquot of synthetic lithium solution that is enriched in impurities such that the subsequent aliquots of synthetic lithium solution comprise a higher lithium purity than does the first aliquot of synthetic lithium solution. In some embodiments, adjusting fluid comprises synthetic lithium solution that is enriched in impurities.
[0297] In some embodiments, a synthetic lithium solution is a leachate solution comprising lithium that is obtained by processing hard rock. In some embodiments, said hard rock comprises spodumene. In some embodiments, said hard rock comprises a lithium containing mineral. Hard rock can comprise one or more minerals. In some embodiments, to obtain the synthetic lithium solution from hard rock, the hard rock is ground, milled, crushed, or a combination thereof. In some embodiments, to obtain the synthetic lithium solution from hard rock, the hard rock is roasted at one or more temperatures between about 300 K to about 2000 K. In some embodiments, to obtain the liquid resource from hard rock, the hard rock is ground, milled, crushed, or a combination thereof after it has been roasted. In some embodiments, to obtain the liquid resource from hard rock, the hard rock is subjected to a leaching step, wherein the hard rock is contacted with an acid. In some embodiments, the hard rock is roasted prior to the leaching step. In some embodiments, the acid comprises sulfuric acid. In some embodiments, the acid is selected from the following list: hydrochloric acid, sulfuric acid, phosphoric acid, hydrobromic acid, chloric acid, perchloric acid, nitric acid, formic acid, acetic acid, or combinations thereof. In some embodiments, the acid is selected from the following list: hydrochloric acid, sulfuric acid, nitric acid, or combinations thereof. In some embodiments, the leaching step is conducted at a temperature that is about 250 degrees Celsius. In some embodiments, the leaching step is conducted at a temperature that is greater than about 250 degrees Celsius. In some embodiments, the leaching step is conducted at a temperature that is less than about 250 degrees Celsius. A synthetic lithium solution that is a leachate solution comprising lithium that is obtained by processing hard rock can be utilized in any embodiment of the present disclosure that utilizes a synthetic lithium solution obtained from a direct lithium extraction process that entails extracting lithium from a liquid resource with a lithium-selective sorbent. Non-limiting examples of the present disclosure that utilize synthetic lithium solutions obtained from hard rock are provided in Example 11 and Example 12.Methods of modulating pH for the extraction of lithium
[0298] An aspect of the invention described herein is a method of extracting lithium ions from a liquid resource, comprising: flowing the liquid resource through the column of the system described above to produce a lithiated ion exchange material; and treating the resulting lithiated ion exchange material with an acid solution to produce a salt solution comprising lithium ions.
[0299] An aspect of the invention described herein is a method of extracting lithium ions from a liquid resource, comprising: flowing the liquid resource through the plurality of columns of the system described above to produce a lithiated ion exchange material; and treating the resulting lithiated ion exchange material with an acid solution to produce a salt solution comprising lithium ions.
[0300] An aspect of the invention described herein is a method of extracting lithium ions from a liquid resource, comprising: flowing the liquid resource through the tank of the system described above to produce a lithiated ion exchange material; and treating the resulting lithiated ion exchange material with an acid solution to produce a salt solution comprising lithium ions.
[0301] An aspect of the invention described herein is a method of extracting lithium ions from a liquid resource, comprising: flowing the liquid resource through the column of the system described above to produce a lithiated ion exchange material; and treating the resulting lithiated ion exchange material with an acid solution to produce a salt solution comprising lithium ions.
[0302] In some embodiments, the liquid resource is selected from the following list: a natural brine, a dissolved salt flat, a geothermal brine, seawater, concentrated seawater, desalination effluent, a concentrated brine, a processed brine, liquid from an ion exchange process, liquid from a solvent extraction process, a synthetic brine, leachate from ores, leachate from minerals, leachate from clays, leachate from recycled products, leachate from recycled materials, or combinations thereof. In some embodiments, a liquid resource is selected from the following list: a natural brine, a dissolved salt flat, a concentrated brine, a processed brine, a synthetic brine, a geothermal brine, liquid from an ion exchange process, liquid from a solvent extraction process, leachate from minerals, leachate from clays, leachate from recycled products, leachate from recycled materials, or combinations thereof. In some embodiments, the liquid resource is optionally pre-treated prior to entering the ion exchange reactor to remove suspended solids, hydrocarbons, or organic molecules. In some embodiments, the liquid resource is optionally entered the ion exchange reactor without any pre-treatment following from its source.
[0303] In an embodiment, the liquid resource is a natural brine, a dissolved salt flat, seawater, concentrated seawater, a desalination effluent, a concentrated brine, a processed brine, an oilfield brine, a liquid from an ion exchange process, a liquid from a solvent extraction process, a synthetic brine, a leachate from an ore or combination of ores, a leachate from a mineral orcombination of minerals, a leachate from a clay or combination of clays, a leachate from recycled products, a leachate from recycled materials, or combinations thereof.
[0304] In some embodiments, the liquid resource is selected with a lithium concentration selected from the following list: less than 100,000 ppm, less than 10,000 ppm, less than 1,000 ppm, less than 100 ppm, less than 10 ppm, or combinations thereof. In some embodiments, a liquid resource is selected with a lithium concentration selected from the following list: less than 5,000 ppm, less than 500 ppm, less than 50 ppm, or combinations thereof.
[0305] In some embodiments, the acid used for recovering lithium from the ion exchange reactor is selected from the following list: hydrochloric acid, sulfuric acid, phosphoric acid, hydrobromic acid, chloric acid, perchloric acid, nitric acid, formic acid, acetic acid, or combinations thereof. In some embodiments, the acid used for recovering lithium from the porous ion exchange beads is selected from the following list: hydrochloric acid, sulfuric acid, nitric acid, or combinations thereof.
[0306] In an embodiment, the acid solution comprises hydrochloric acid, sulfuric acid, phosphoric acid, hydrobromic acid, chloric acid, perchloric acid, nitric acid, formic acid, acetic acid, or combinations thereof.
[0307] In some embodiments, the acid used for recovering lithium from the ion exchange system has a concentration selected from the following list: less than 0.1 M, less than 1.0 M, less than 5 M, less than 10 M, or combinations thereof. In some embodiments, the acid used for recovering lithium from the porous ion exchange beads has a concentration greater than 10 M.
[0308] In an embodiment, acids with distinct concentrations are used during the elution process. In an embodiment, acid with a lower concentration is first added to elute lithium from the ion exchange material and then additional acid of a greater concentration is added to elute more lithium into the solution and increase the concentration of lithium in the eluate.
[0309] In some embodiments, the ion exchange beads perform the ion exchange reaction repeatedly while maintaining adequate lithium uptake capacity over a number of cycles selected from the following list: greater than 10 cycles, greater than 30 cycles, greater than 100 cycles, greater than 300 cycles, or greater than 1,000 cycles. In some embodiments, the porous ion exchange beads perform the ion exchange reaction repeatedly over a number of cycles selected from the following list: greater than 50 cycles, greater than 100 cycles, or greater than 200 cycles. In some embodiments, adequate lithium uptake capacity is optionally defined as a percentage of initial uptake capacity selected from the following list: greater than 95%, greater than 90%, greater than 80%, greater than 60%, or greater than 20%. In some embodiments, adequate lithium uptake capacity is optionally defined as a percentage of initial uptake capacity such as less than 20%.
[0310] In some embodiments, the synthetic lithium solution that is yielded from the ion exchange reactor is further processed into lithium raw materials using methods selected from the following list: solvent extraction, ion exchange, chemical precipitation, electrodialysis, el ectrowinning, electrolysis, evaporation with direct solar energy, evaporation with concentrated solar energy, evaporation with a heat transfer medium heated by concentrated solar energy, evaporation with heat from a geothermal brine, evaporation with heat from combustion, pH neutralization, or combinations thereof. In some embodiments, the synthetic lithium solution that is yielded from the ion exchange reactor is concentrated using reverse osmosis or membrane technologies.
[0311] In some embodiments, the synthetic lithium solution that is yielded from the ion exchange reactor is further processed into lithium chemicals selected from the following list: lithium chloride, lithium carbonate, lithium hydroxide, lithium metal, lithium metal oxide, lithium metal phosphate, lithium sulfide, or combinations thereof. In some embodiments, the synthetic lithium solution that is yielded from the porous ion exchange beads is further processed into lithium chemicals that are solid, liquid, hydrated, or anhydrous.
[0312] In some embodiments, the lithium chemicals produced using the ion exchange reactor are used in an industrial application selected from the following list: lithium batteries, metal alloys, glass, grease, or combinations thereof. In some embodiments, the lithium chemicals produced using the coated ion exchange particles are used in an application selected from the following list: lithium batteries, lithium-ion batteries, lithium sulfur batteries, lithium solid-state batteries, and combinations thereof.
[0313] In some embodiments, the ion exchange materials are synthesized in a lithiated state with a sublattice fully or partly occupied by lithium. In some embodiments, the ion exchange materials are synthesized in a hydrated state with a sublattice fully or partly occupied by hydrogen.
[0314] In some embodiments, the ion exchange material extracts lithium ions from a liquid resource. During the extraction of lithium ions from a liquid resource by the ion exchange material, the pH of the liquid resource optionally decreases. Increasing the pH of the liquid resource in the system by using a pH modulating setup maintains the pH in a range that is suitable for lithium ion uptake by the ion exchange material. In an embodiment, the pH modulating setup comprises measuring the pH of the system and adjusting the pH of the system to an ideal pH range for lithium extraction. In an embodiment, for ion exchange material to absorb lithium from liquid resource, an ideal pH range for the liquid resource is optionally 6 to 9, a preferred pH range is optionally 4 to 9, and an acceptable pH range is optionally 2 to 9. In an embodiment, the pH modulating setup comprises measuring the pH of the system andwherein the pH of the system is less than 6, less than 4, or less than 2, the pH of the system is adjusted to a pH of 2 to 9, a pH of 4 to 9, or a pH of 6 to 9.
[0315] Another aspect described herein is a method of extracting lithium ions from a liquid resource, comprising: a) flowing the liquid resource into a system comprising a tank to produce a lithiated ion exchange mateiral, wherein the tank further comprises (i) one or more compartments, (ii) an ion exchange material, (iii) a mixing device, and (iv) a pH modulating setup for changing the pH of the liquid resource in the system; and b) treating the lithiated ion exchange material from a) with an acid solution to produce a hydrogen-rich ion exchange material and a salt solution comprising lithium ions.
[0316] In some embodiments, the method further comprises, prior to b), washing the lithiated ion exchange material with an aqueous solution. In some embodiments, the method further comprises, subsequent to b), washing the hydrogen-rich ion exchange material with an aqueous solution. In some embodiments, the aqueous solution is water.
[0317] In some embodiments, the method further comprises, prior to b), flowing the lithiated ion exchange material into a washing system. In some embodiments, the method further comprises, prior to b), transferring a suspension comprising the lithiated ion exchange material. In some embodiments, the method further comprises, prior to b), flowing the lithiated ion exchange material into a washing system and washing the lithiated ion exchange material with a solution. In some embodiments, the method further comprises, prior to b), flowing the lithiated ion exchange material into a washing system and washing the lithiated ion exchange material with a solution comprising water. In some embodiments, the method further comprises, prior to b), flowing the lithiated ion exchange material into a washing system and washing the lithiated ion exchange material with an aqueous solution. In some embodiments, the lithiated ion exchange material is washed with an aqueous solution.
[0318] In some embodiments, the method further comprises, prior to b), flowing the lithiated ion exchange material into a stripping system. In some embodiments, the method further comprises, prior to b), flowing the lithiated ion exchange material into a stripping system and stripping the lithiated ion exchange material. In some embodiments, the method further comprises, prior to b), flowing the lithiated ion exchange material into a stripping system and stripping volatile components from the lithiated ion exchange material. In some embodiments, the method further comprises, prior to b), flowing the lithiated ion exchange material into a stripping system and stripping volatile components comprising water from the lithiated ion exchange material.
[0319] In some embodiments, the pH modulating setup comprises a pH measuring device and an inlet for adding base to the tank. In some embodiments, the pH measuring device is a pHprobe. In some embodiments, the inlet is a pipe. In some embodiments, the inlet is an injection port.
[0320] In some embodiments, the method further comprises, during a), measuring a change in pH of the liquid resource using the pH modulating setup. In some embodiments, the measured change in pH triggers adding a base to maintain lithium uptake. In some embodiments, a change in pH to below a pH value of about 2 to about 9 triggers the addition of a base to maintain lithium uptake. In some embodiments, a change in pH to below a pH value of about 2, of about 3, of about 4, of about 5, of about 6, of about 7, of about 8, or of about 9 triggers the addition of a base to maintain lithium uptake. In some embodiments, a change in pH to below a pH of about 2 to about 4, of about 3 to about 5, of about 4 to about 6, of about 5 to about 7, of about 6 to about 8, or of about 7 to about 9 triggers the addition of a base to maintain lithium uptake. In some embodiments, base is added to the liquid resource to maintain the pH of the liquid resource in a range of about 2-3, 3-4, 4-5, 5-6, 6-7, 7-8, or 8-9. In some embodiments, base is added to the liquid resource to maintain the pH of the liquid resource in a range of about 4-5, 5-6, 6-7, or 7-8. In some embodiments, base is added to the liquid resource to maintain the pH of the liquid resource in a range of about 4.0-4.5, 4.5-5.0, 5.0-5.5, 5.5-6.0, 6.0-6.5, 6.5-7.0, 7.0-7.5, or 7.5- 8.0. In some embodiments, the pH of a liquid resource is maintained in a target range that is high enough to facilitate lithium uptake and low enough to avoid precipitation of metal salts from the liquid resource. In some embodiments, the pH of a liquid resource is maintained below a pH of about 8 to avoid precipitation of Mg salts. In some embodiments, the pH of a liquid resource is maintained below a pH of about 2, below a pH of about 3, below a pH of about 4, below a pH of about 5, below a pH of about 6, below a pH of about 7, below a pH of about 8, or below a pH of about 9 to avoid precipitation of metal salts. In some embodiments, the pH of the liquid resource drops out of a target pH range due to release of protons from an ion exchange material and a pH modulating setup adjusts the pH of the liquid resource back to within a target pH range. In some embodiments, the pH of the liquid resource is adjusted above a target pH range prior to the liquid resource entering the system and then protons released from the ion exchange material decrease the pH of the system into the target range. In some embodiments, the pH of the liquid resource is controlled in a certain range and the range is changed over time. In some embodiments, the pH of the liquid resource is controlled in a certain range and then the pH of the liquid resource is allowed to drop. In some embodiments, the pH of the liquid resource is controlled in a certain range and then the pH of the liquid resource is allowed to drop to solubilize colloids or solids. In some embodiments, base is added to a liquid resource to neutralize protons without measuring pH. In some embodiments, base is added to a liquid resource to neutralize protons with monitoring of volumes or quantities of the base. In someembodiments, the pH of the liquid resource is measured to monitor lithium uptake by an ion exchange material. In some embodiments, the pH of the liquid resource is monitored to determine when to separate a liquid resource from an ion exchange material. In some embodiments, the rate of change of the pH of the liquid resource is measured to monitor the rate of lithium uptake. In some embodiments, the rate of change of the pH of the liquid resource is measured to determine when to separate a liquid resource from an ion exchange material.
[0321] In some embodiments, the tank further comprises a porous partition. In some embodiments, the porous partition is a porous polymer partition. In some embodiments, the porous partition is a mesh or membrane. In some embodiments, the porous partition is a polymer mesh or polymer membrane. In some embodiments, the porous partition comprises one or more layers of mesh, membrane, or other porous structure. In some embodiments, the porous partition comprises one or more coarse meshes that provide structural support and one or more fine meshes and / or membranes that provide filtration. In some embodiments, the porous partition comprises a polyether ether ketone mesh, a polypropylene mesh, a polyethylene mesh, a polysulfone mesh, a polyester mesh, a polyamide mesh, a polytetrafluoroethylene mesh, an ethylene tetrafluoroethylene polymer mesh, a stainless steel mesh, a stainless steel mesh coated in polymer, a stainless steel mesh coated in ceramic, or a combination thereof, wherein the mesh is a course mesh, a fine mesh, or a combination thereof. In some embodiments, the porous polymer partition comprises a mesh comprising one or more blends of two or more of a polyether ether ketone, a polypropylene, a polyethylene, a polysulfone, a polyester, a polyamide, a polytetrafluoroethylene, or an ethylene tetrafluoroethylene polymer. In some embodiments, the porous partition comprises a polyether ether ketone membrane, a polypropylene membrane, a polyethylene membrane, a polysulfone membrane, a polyester membrane, a polyamide membrane, a polytetrafluoroethylene membrane, an ethylene tetrafluoroethylene polymer membrane, or combinations thereof.
[0322] In some embodiments, the method further comprises, after a), draining the liquid resource through the porous partition after the production of the lithiated ion exchange material.
[0323] In some embodiments, the method further comprises, after b), draining the salt solution comprising lithium ions through the porous partition after the production of the hydrogen-rich ion exchange material.
[0324] In some embodiments, the method further comprises, subsequent to a), flowing the lithiated ion exchange material into another system comprising a tank to produce the hydrogenrich ion exchange material and the salt solution comprising lithium ions, wherein the tank of the other system further comprises (i) one or more compartments, and (ii) a mixing device.
[0325] In some embodiments, the system comprises a plurality of tanks and each of the plurality of tanks further comprises (i) one or more compartments, (ii) an ion exchange material, (iii) a mixing device, and (iv) a pH modulating setup for changing the pH of the system.
[0326] An aspect described herein is a method of extracting lithium ions from a liquid resource, comprising: a) flowing the liquid resource into a first system comprising a tank, wherein the tank of the first system further comprises (i) one or more compartments, (ii) an ion exchange material, (iii) a mixing device, and (iv) a pH modulating setup for changing the pH of the liquid resource in the first system, to produce a lithiated ion exchange material; b) flowing the lithiated ion exchange material of a) into a second system comprising a tank, wherein the tank of the second system further comprises (i) one or more compartments, and (ii) a mixing device; and c) treating the lithiated ion exchange from b) with an acid solution to produce a hydrogen-rich ion exchange material and a salt solution comprising lithium ions.
[0327] In some embodiments, the method further comprises, subsequent to a), washing the lithiated ion exchange material with an aqueous solution.
[0328] In some embodiments, the method further comprises, prior to b), adding an aqueous solution to the lithiated ion exchange material to form a fluidized lithiated ion exchange material.
[0329] In some embodiments, the method further comprises, subsequent to c), washing the hydrogen-rich ion exchange material with an aqueous solution. In some embodiments, the aqueous solution is water.
[0330] In some embodiments, the pH modulating setup comprises a pH measuring device and an inlet for adding base. In some embodiments, the pH measuring device is a pH probe. In some embodiments, the inlet is a pipe. In some embodiments, the inlet is an injection port.
[0331] In some embodiments, the method further comprises, during a), measuring a change in pH of the liquid resource using the pH modulating setup. In some embodiments, the change in pH triggers adding a base to maintain lithium uptake.
[0332] An aspect described herein is a method of extracting lithium ions from a liquid resource, comprising: a) flowing the liquid resource into a first system comprising a plurality of tanks to produce a lithiated ion exchange material, wherein each of the plurality of tanks in the first system is in fluid communication with every other one of the plurality of tanks in the first system and, each of the plurality of tanks in the first system further comprises (i) one or more compartments, (ii) an ion exchange material, (iii) a mixing device, and (iv) a pH modulating setup for changing the pH of each of the plurality of tanks in the first system; b) flowing the lithiated ion exchange material into a second system comprising a plurality of tanks, wherein each of the plurality of tanks in the second system is in fluid communication with every otherone of the plurality of tanks in the second system and, each of the plurality of tanks in the second system further comprises (i) one or more compartments, and (ii) a mixing device; and c) treating the lithiated ion exchange material from b) with an acid solution in at least one of the plurality of tanks in the second system to produce a hydrogen-rich ion exchange material and a salt solution comprising lithium ions.
[0333] In some embodiments, the method further comprises, subsequent to c), washing the hydrogen-rich ion exchange material with an aqueous solution in at least one of the plurality of tanks in the second system.
[0334] In some embodiments, the method is operated in a batch mode. In some embodiments, the method is operated in a continuous mode. In some embodiments, the method is operated in continuous and batch mode. In some embodiments, the method is operated in continuous mode, a batch mode, a semi -continuous mode, or combinations thereof.
[0335] In some embodiments, the pH modulating setup comprises a pH measuring device and an inlet for adding base. In some embodiments, the pH measuring device is a pH probe. In some embodiments, the inlet is a pipe. In some embodiments, the inlet is an injection port.
[0336] In some embodiments, the method further comprises, during a), measuring a change in pH of the liquid resource using the pH modulating setup. In some embodiments, the change in pH triggers adding a base to maintain lithium uptake.
[0337] An aspect described herein is a method of extracting lithium ions from a liquid resource, comprising: a) flowing the liquid resource into a first system comprising a tank to produce a lithiated ion exchange material, wherein the tank further comprises (i) one or more compartments, (ii) ion exchange material, and (iii) a mixing device; b) flowing the lithiated ion exchange material from a) into a second system comprising a tank, wherein the tank further comprises (i) one or more compartments, (ii) an acid solution, and (iii) a mixing device; and c) stripping the lithiated ion exchange material to produce hydrogen-rich ion exchange material and a salt solution comprising lithium ions.
[0338] In some embodiments, prior to b), the lithiated ion exchange material is washed. In some embodiments, the lithiated ion exchange material is washed with an aqueous solution.
[0339] An aspect described herein is a method of extracting lithium ions from a liquid resource, comprising: a) providing a system comprising an ion exchange material, a tank comprising one or more compartments; and a mixing device, wherein (i) the ion exchange material is oxidebased and exchanges hydrogen ions with lithium ions, and (ii) the mixing device is capable of moving the liquid resource around the tank comprising one or more compartments; b) flowing the liquid resource into the system of a), thereby contacting the liquid resource with the ion exchange material, wherein the ion exchange material exchanges hydrogen ions with lithiumions in the liquid resource to produce lithiated ion exchange material; c) removing the liquid resource from the system of b); d) flowing an acid solution into the system of c) thereby contacting the acid solution with the lithiated ion exchange material, wherein the lithiated ion exchange material exchanges lithium ions with the hydrogen ions in the acid solution to produce the ion exchange material and a salt solution comprising lithium ions from the lithiated ion exchange material; and e) collecting the salt solution comprising the lithium ions for further processing.
[0340] In some embodiments, the salt solution comprising lithium ions undergoes crystallization.
[0341] A method of extracting lithium ions from a liquid resource, comprising: a) flowing the liquid resource through a system comprising an ion exchange material and a plurality of columns, wherein the plurality of columns is configured to transport the ion exchange material along the length of the column, to produce a lithiated ion exchange material; and b) treating the lithiated ion exchange material from a) with an acid solution to produce a salt solution comprising lithium ions.
[0342] An aspect described herein is a method of extracting lithium ions from a liquid resource, comprising: a) providing a system comprising an ion exchange material and a plurality of columns, wherein each of the plurality of columns is configured to transport the ion exchange material along the length of the column; b) flowing the liquid resource through a first one of the plurality of columns to produce a lithiated ion exchange material; c) flowing the lithiated ion exchange material from b) into a second one of the plurality of columns; and d) treating the lithiated ion exchange material from c) with an acid solution to produce a hydrogen-rich ion exchange material and a salt solution comprising lithium ions.
[0343] In some embodiments, the method further comprises, subsequent to b), flowing the lithiated ion exchange material into another one of the plurality of columns and washing the lithiated ion exchange material with an aqueous solution. In some embodiments, the method further comprises, subsequent to d), flowing the hydrogen-rich ion exchange material into another one of the plurality of columns and washing the hydrogen-rich ion exchange material with an aqueous solution.
[0344] An aspect described herein is a method of extracting lithium ion from a liquid resource, comprising: a) providing a system comprising an ion exchange material and a plurality of columns, wherein each of the plurality of columns is configured to transport the ion exchange material along the length of the column; b) flowing the liquid resource through a first one of the plurality of columns to produce a lithiated ion exchange material; c) flowing the lithiated ion exchange material from b) into a second one of the plurality of columns; d) washing the lithiatedion exchange material from c) with an aqueous solution; e) flowing the lithiated ion exchange material from d) into a third one of the plurality of columns; and f) treating the lithiated ion exchange material from e) with an acid solution to produce a hydrogen-rich ion exchange material and a salt solution comprising lithium ions.
[0345] In some embodiments, the method further comprises: g) flowing the hydrogen-rich ion exchange material into a fourth one of the plurality of columns; and h) washing the hydrogenrich ion exchange material with an aqueous solution. In some embodiments, each of the plurality of columns is configured to transport the ion exchange material by a pipe system or an internal conveyer system. In some embodiments, each of the plurality of columns is configured to transport the ion exchange material by a pipe system. In some embodiments, each of the plurality of columns is configured to transport the ion exchange material by an internal conveyer system.
[0346] In some embodiments of the methods described herein, the liquid resource is a natural brine, a dissolved salt flat, seawater, concentrated seawater, a desalination effluent, a concentrated brine, a processed brine, waste brine from a bromine-extraction process, an oilfield brine, a liquid from an ion exchange process, a liquid from a solvent extraction process, a synthetic brine, a leachate from an ore or combination of ores, a leachate from a mineral or combination of minerals, a leachate from a clay or combination of clays, a leachate from recycled products, a leachate from recycled materials, or combinations thereof. In some embodiments of the methods described herein, the liquid resource is a brine. In some embodiments of the methods described herein, the liquid resource comprises a natural brine, a synthetic brine, or a mixture of a natural and a synthetic brine. In some embodiments of the methods described herein, the liquid resource is a natural brine, a dissolved salt flat, seawater, concentrated seawater, a desalination effluent, a concentrated brine, a processed brine, waste brine from a bromine-extraction process, an oilfield brine, a liquid from an ion exchange process, or combinations thereof.
[0347] In some embodiments of the methods described herein, the acid solution comprises hydrochloric acid, sulfuric acid, phosphoric acid, hydrobromic acid, chloric acid, perchloric acid, nitric acid, formic acid, acetic acid, or combinations thereof. In some embodiments of the methods described herein, the acid solution comprises hydrochloric acid, sulfuric acid, phosphoric acid, nitric acid, or combinations thereof. In some embodiments of the methods described herein, the acid solution comprises hydrochloric acid, sulfuric acid, phosphoric acid, or combinations thereof. In some embodiments of the methods described herein the acid solution comprises hydrochloric acid. In some embodiments of the methods described herein the acidsolution comprises sulfuric acid. In some embodiments of the methods described herein the acid solution comprises phosphoric acid.Continuous Process for Lithium Extraction
[0348] Lithium is an essential element for batteries and other technologies. Lithium is found in a variety of liquid resources, including natural and synthetic brines and leachate solutions from minerals, clays, and recycled products. Lithium can be extracted from such liquid resources using an ion exchange process based on inorganic ion exchange materials. These inorganic ion exchange materials absorb lithium from a liquid resource while releasing hydrogen, and then elute lithium in acid while absorbing hydrogen. This ion exchange process can be repeated to extract lithium from a liquid resource and yield a synthetic lithium solution. The synthetic lithium solution can be further processed into chemicals for the battery industry or other industries.
[0349] Ion exchange materials are typically small particles, which together constitute a fine powder. Small particle size is required to minimize the diffusion distance that lithium must travel into the core of the ion exchange particles. In some cases, these particles are coated with protective surface coatings to minimize dissolution of the ion exchange materials while allowing efficient transfer of lithium and hydrogen to and from the particles, as disclosed in co-pending U.S. provisional application 62 / 421,934, filed on November 14, 2016, entitled “Lithium Extraction with Coated Ion Exchange Particles,” and incorporated in its entirety by reference.
[0350] One major challenge for lithium extraction using inorganic ion exchange particles is the loading of the particles into an ion exchange column in such a way that brine and acid can be pumped efficiently through the column with minimal clogging. The materials can be formed into beads, and the beads can be loaded into the column. This bead loading creates void spaces between the beads, and these void spaces facilitate pumping through the column. The beads hold the ion exchange particles in place and prevent free movement of the particles throughout the column. When the materials are formed into beads, the penetration of liquid resource and acid solutions into the beads can become slow and challenging. A slow rate of convection and diffusion of the acid and liquid resource solutions into the bead slows the kinetics of lithium absorption and release. Such slow kinetics can create problems for column operation. Slow kinetics can require slow pumping rates through the column. Slow kinetics can also lead to low lithium recovery from the liquid resource and inefficient use of acid to elute the lithium.
[0351] In one embodiment, an alternate phase is contacted with the ion exchange beads during on ore more of the steps of the process step. In some embodiments, the use of alternate phase speeds up the kinetics of ion exchange, enhances the forming of the ion exchange bed, controlsliquid level height in one or more process tanks, or a combination thereof. In some embodiments, contact between the ion exchange beads and the alternate phase is maximized and made possible by the design of this ion exchange device.
[0352] In some embodiments, the alternate phase is a liquid or gas. In some embodiments, said alternate phase is a non-aqueous liquid. In some embodiments, the alternate phase is nonaqueous liquid. In some embodiments, the alternate phase is a non-aqueous solution. In some embodiments, the alternate phase is an organic liquid such as an alkane, alcohol, oil, bio-organic oil, ester, ether, hydrocarbon, or a combination thereof. In some embodiments, the alternate phase is butane, pentane, hexane, acetone, diethyl ether, butanol, or combinations thereof. In some embodiments, the alternate is a gas such as air, nitrogen, argon, or a combination thereof. In some embodiments, the alternate phase comprises a compressed or pressurized gas.
[0353] In some embodiments, the ion exchange beads are porous ion exchange beads with networks of pores that facilitate the transport into the beads of solutions that are pumped through an ion exchange column. Pore networks can be strategically controlled to provide fast and distributed access for the liquid resource and acid solutions to penetrate into the bead and deliver lithium and hydrogen to the ion exchange particles.
[0354] In some embodiments, the ion exchange beads are formed by mixing of ion exchange particles, a matrix material, and a filler material. These components are mixed and formed into a bead. Then, the filler material is removed from the bead to leave behind pores. The filler material is dispersed in the bead in such a way to leave behind a pore structure that enables transport of lithium and hydrogen with fast kinetics. This method can involve multiple ion exchange materials, multiple polymer materials, and multiple filler materials.
[0355] Another major challenge for lithium extraction using inorganic ion exchange materials is dissolution and degradation of the materials, especially during lithium elution in acid but also during lithium uptake in liquid resources. To yield a synthetic lithium solution from the ion exchange process, it is desirable to use a concentrated acid solution to elute the lithium. However, concentrated acid solutions dissolve and degrade inorganic ion exchange materials, which decreases the performance and lifespan of the materials. Therefore, the porous ion exchange beads can contain coated ion exchange particles for lithium extraction that are comprised of an ion exchange material and a coating material protecting the particle surface.The coating protects the ion exchange material from dissolution and degradation during lithium elution in acid, during lithium uptake from a liquid resource, and during other aspects of an ion exchange process. This coated particle enables the use of concentrated acids in the ion exchange process to yield synthetic lithium solutions.
[0356] In one aspect described herein, the ion exchange material is selected for high lithium absorption capacity, high selectivity for lithium in a liquid resource relative to other ions such as sodium and magnesium, strong lithium uptake in liquid resources including those with low concentrations of lithium, facile elution of lithium with a small excess of acid, and fast ionic diffusion. In one aspect described herein, a coating material is selected to protect the particle from dissolution and chemical degradation during lithium recovery in acid and also during lithium uptake in various liquid resources. In some embodiments, the coating material is selected to facilitate one or more of the following objectives: diffusion of lithium and hydrogen between the particles and the liquid resources, enabling adherence of the particles to a structural support, and suppressing structural and mechanical degradation of the particles.
[0357] When the porous ion exchange beads are used in an ion exchange column, the liquid resource containing lithium is pumped through the ion exchange column so that the ion exchange particles absorb lithium from the liquid resource while releasing hydrogen. After the beads have absorbed lithium, an acid solution is pumped through the column so that the particles release lithium into the acid solution while absorbing hydrogen. The column can be operated in co-flow mode with the liquid resource and acid solution alternately flowing through the column in the same direction, or the column can be operated in counter-flow mode with a liquid resource and acid solution alternately flowing through the column in opposite directions. Between flows of the liquid resource and the acid solution, the column can be treated or washed with water or other solutions for purposes such as adjusting pH in the column or removing potential contaminants. The beads can form a fixed or moving bed, and the moving bed can move in counter-current to the liquid resource and acid flows. The beads can be moved between multiple columns with moving beds where different columns are used for liquid resource, acid, water, or other flows. Before or after the liquid resource flows through the column, the pH of the liquid can be adjusted with NaOH or other chemicals to facilitate the ion exchange reaction as well as handling or disposal of the spent liquid resource. Before or after the liquid resource flows through the column, the liquid resource can be subjected to other processes including other ion exchange processes, solvent extraction, evaporation, chemical treatment, or precipitation to remove lithium, to remove other chemical species, or to otherwise treat the liquid resource.
[0358] When the ion exchange particles are treated with acid, a lithium solution is produced. This lithium solution can be further processed to produce lithium chemicals. These lithium chemicals can be supplied for an industrial application.
[0359] In some embodiments, an ion exchange material is selected from the following list: an oxide, a phosphate, an oxyfluoride, a fluorophosphate, or combinations thereof. In some embodiments, an ion exchange material is selected from the following list: I^MnsOn,Li4TisOi2, Li2MC>3 (M = Ti, Mn, Sn), LiMr^C , Li1.6Mn1.eO4, LiM02 (M = Al, Cu, Ti), Li4TiO4, Li7TiiiO24, Li3VO4, Li2Si3O7, LiFePO4, LiMnPO4, Li2CuP2O7, A1(OH)3, LiCl.xAl(OH)3.yH2O, SnO2.xSb2O5.yH2O, TiO2.xSb2O5.yH2O, solid solutions thereof, or combinations thereof. In some embodiments, an ion exchange material is selected from the following list: Li4MnsOi2, Li4TisOi2, Li1.6Mn1.eO4, Li2MO3(M = Ti, Mn, Sn), LiFePO4, solid solutions thereof, or combinations thereof.
[0360] In some embodiments, a coating material for protecting the surface of the ion exchange material is selected from the following list: a carbide, a nitride, an oxide, a phosphate, a fluoride, a polymer, carbon, a carbonaceous material, or combinations thereof. In some embodiments, a coating material is selected from the following list: TiCh, ZrCh, MoO2, SnCh, bt^Os, Ta20s, SiC>2, Li2TiO3, Li2ZrO3, Li2SiO3, Li2MnO3, Li2MoO3, LiNbO3, LiTaO3, AIPO4, LaPCL, ZrP2O7, MOP2O7, Mo2P3Oi2, BaSO4, A1F3, SiC, TiC, ZrC, Si3N4, ZrN, BN, carbon, graphitic carbon, amorphous carbon, hard carbon, diamond-like carbon, solid solutions thereof, or combinations thereof. In some embodiments, a coating material is selected from the following list: TiCh, ZrCh, MoO2, SiCh, Li2TiO3, Li2ZrO3, Li2SiO3, Li2MnO3, LiNbO3, A1F3, SiC, Si3N4, graphitic carbon, amorphous carbon, diamond-like carbon, or combinations thereof.
[0361] In some embodiments, the ion exchange particles have an average diameter that is selected from the following list: less than 10 nm, less than 100 nm, less than 1,000 nm, less than 10,000 nm, or less than 100,000 nm. In some embodiments, the ion exchange particles have an average size that is selected from the following list: less than 200 nm, less than 2,000 nm, or less than 20,000 nm.
[0362] In some embodiments, the ion exchange particles are secondary particles comprised of smaller primary particles that have an average diameter selected from the following list: less than 10 nm, less than 100 nm, less than 1,000 nm, or less than 10,000 nm.
[0363] In some embodiments, the ion exchange particles have a coating material with a thickness selected from the following list: less than 1 nm, less than 10 nm, less than 100 nm, or less than 1,000 nm. In some embodiments, the coating material has a thickness selected from the following list: less than 1 nm, less than 10 nm, or less than 100 nm.
[0364] In some embodiments, the ion exchange material and a coating material form one or more concentration gradients where the chemical composition of the particle ranges between two or more compositions. In some embodiments, the ion exchange materials and the coating materials form a concentration gradient that extends over a thickness selected from the following list: less than 1 nm, less than 10 nm, less than 100 nm, less than 1,000 nm, less than 10,000 nm, or less than 100,000 nm.
[0365] In some embodiments, the ion exchange material is synthesized by a method selected from the following list: hydrothermal, solvothermal, sol-gel, solid state, molten salt flux, ion exchange, microwave, ball milling, precipitation, or vapor deposition. In some embodiments, the ion exchange material is synthesized by a method selected from the following list: hydrothermal, solid state, or microwave.
[0366] In some embodiments, a coating material is deposited by a method selected from the following list: chemical vapor deposition, atomic layer deposition, physical vapor deposition, hydrothermal, solvothermal, sol-gel, solid state, molten salt flux, ion exchange, microwave, wet impregnation, precipitation, titration, aging, ball milling, or combinations thereof. In some embodiments, the coating material is deposited by a method selected from the following list: chemical vapor deposition, hydrothermal, titration, solvothermal, wet impregnation, sol-gel, precipitation, microwave, or combinations thereof.
[0367] In some embodiments, a coating material is deposited with physical characteristics selected from the following list: crystalline, amorphous, full coverage, partial coverage, uniform, non-uniform, or combinations thereof.
[0368] In some embodiments, multiple coatings are deposited on the ion exchange material in an arrangement selected from the following list: concentric, patchwork, or combinations thereof.
[0369] In some embodiments, the matrix is selected from the following list: a polymer, an oxide, a phosphate, or combinations thereof. In some embodiments, a structural support is selected from the following list: polyvinyl fluoride, polyvinylidene difluoride, polyvinyl chloride, polyvinylidene dichloride, polyethylene, polypropylene, polyphenylene sulfide, polytetrafluoroethylene, polytetrafluoroethylene, sulfonated polytetrafluoroethylene, polystyrene, polydivinylbenzene, polybutadiene, sulfonated polymer, carboxylated polymer, Nafion, copolymers thereof, and combinations thereof. In some embodiments, a structural support is selected from the following list: polyvinylidene difluoride, polyvinyl chloride, sulfonated polytetrafluoroethylene, polystyrene, polydivinylbenzene, copolymers thereof, or combinations thereof. In some embodiments, a structural support is selected from the following list: titanium dioxide, zirconium dioxide, silicon dioxide, solid solutions thereof, or combinations thereof. In some embodiments, the matrix material is selected for thermal resistance, acid resistance, and / or other chemical resistance.
[0370] In some embodiments, the porous bead is formed by mixing the ion exchange particles, the matrix material, and the filler material together at once. In some embodiments, the porous bead is formed by first mixing the ion exchange particles and the matrix material, and then mixing with the filler material. In some embodiments, the porous bead is formed by first mixing the ion exchange particles and the filler material, and then mixing with the matrix material. Insome embodiments, the porous bead is formed by first mixing the matrix material and the filler material, and then mixing with the ion exchange particles.
[0371] In some embodiments, the porous bead is formed by mixing the ion exchange particles, the matrix material, and / or the filler material with a solvent that dissolves once or more of the components. In some embodiments, the porous bead is formed by mixing the ion exchange particles, the matrix material, and / or the filler material as dry powders in a mixer or ball mill. In some embodiments, the porous bead is formed by mixing the ion exchange particles, the matrix material, and / or the filler material in a spray drier.
[0372] In some embodiments, the matrix material is a polymer that is dissolved and mixed with the ion exchange particles and / or filler material using a solvent from the following list: n- methyl-2-pyrrolidone, dimethyl sulfoxide, tetrahydrofuran, dimethylformamide, dimethylacetamide, methyl ethyl ketone, or combinations thereof. In some embodiments, the filler material is a salt that is dissolved and mixed with the ion exchange particles and / or matrix material using a solvent from the following list: water, ethanol, iso-propyl alcohol, acetone, or combinations thereof.
[0373] In some embodiments, the filler material is a salt that is dissolved out of the bead to form pores using a solution selected from the following list: water, ethanol, iso-propyl alcohol, a surfactant mixture, an acid a base, or combinations thereof. In some embodiments, the filler material is a material that thermally decomposes to form a gas at high temperature so that the gas can leave the bead to form pores, where the gas is selected from the following list: water vapor, oxygen, nitrogen, chlorine, carbon dioxide, nitrogen oxides, organic vapors, or combinations thereof.
[0374] In some embodiments, the porous ion exchange bead is formed from dry powder using a mechanical press, a pellet press, a tablet press, a pill press, a rotary press, or combinations thereof. In some embodiments, the porous ion exchange bead is formed from a solvent slurry by dripping the slurry into a different liquid solution. The solvent slurry can be formed using a solvent of n-methyl-2-pyrrolidone, dimethyl sulfoxide, tetrahydrofuran, dimethylformamide, dimethylacetamide, methyl ethyl ketone, or combinations thereof. The different liquid solution can be formed using water, ethanol, iso-propyl alcohol, acetone, or combinations thereof.
[0375] In some embodiments, the porous ion exchange bead is approximately spherical with an average diameter selected from the following list: less than 10 pm, less than 100 pm, less than 1 mm, less than 1 cm, or less than 10 cm. In some embodiments, the porous ion exchange bead is approximately spherical with an average diameter selected from the following list: less than 200 pm, less than 2 mm, or less than 20 mm.
[0376] In some embodiments, the porous ion exchange bead is tablet-shaped with a diameter of less than 1 mm, less than 2 mm, less than 4 mm, less than 8 mm, or less than 20 mm and with a height of less than 1 mm, less than 2 mm, less than 4 mm, less than 8 mm, or less than 20 mm.
[0377] In some embodiments, the porous ion exchange bead is embedded in a support structure, which can be a membrane, a spiral-wound membrane, a hollow fiber membrane, or a mesh. In some embodiments, the porous ion exchange bead is embedded on a support structure comprised of a polymer, a ceramic, or combinations thereof. In some embodiments, the porous ion exchange bead is loaded directly into an ion exchange column with no additional support structure.
[0378] In some embodiments, the liquid resource is selected from the following list: a natural brine, a dissolved salt flat, a geothermal brine, seawater, concentrated seawater, desalination effluent, a concentrated brine, a processed brine, liquid from an ion exchange process, liquid from a solvent extraction process, a synthetic brine, leachate from ores, leachate from minerals, leachate from clays, leachate from recycled products, leachate from recycled materials, or combinations thereof. In some embodiments, a liquid resource is selected from the following list: a natural brine, a dissolved salt flat, a concentrated brine, a processed brine, a synthetic brine, a geothermal brine, liquid from an ion exchange process, liquid from a solvent extraction process, leachate from minerals, leachate from clays, leachate from recycled products, leachate from recycled materials, or combinations thereof.
[0379] In some embodiments, the liquid resource is selected with a lithium concentration selected from the following list: less than 100,000 ppm, less than 10,000 ppm, less than 1,000 ppm, less than 100 ppm, less than 10 ppm, or combinations thereof. In some embodiments, a liquid resource is selected with a lithium concentration selected from the following list: less than 5,000 ppm, less than 500 ppm, less than 50 ppm, or combinations thereof.
[0380] In some embodiments, the acid used for recovering lithium from the porous ion exchange beads is selected from the following list: hydrochloric acid, sulfuric acid, phosphoric acid, hydrobromic acid, chloric acid, perchloric acid, nitric acid, formic acid, acetic acid, or combinations thereof. In some embodiments, the acid used for recovering lithium from the porous ion exchange beads is selected from the following list: hydrochloric acid, sulfuric acid, nitric acid, or combinations thereof.
[0381] In some embodiments, the acid used for recovering lithium from the porous ion exchange beads has a concentration selected from the following list: less than 0.1 M, less than 1.0 M, less than 5 M, less than 10 M, or combinations thereof.
[0382] In some embodiments, the porous ion exchange beads perform the ion exchange reaction repeatedly over a number of cycles selected from the following list: greater than 10 cycles,greater than 30 cycles, greater than 100 cycles, greater than 300 cycles, or greater than 1,000 cycles. In some embodiments, the porous ion exchange beads perform the ion exchange reaction repeatedly over a number of cycles selected from the following list: greater than 50 cycles, greater than 100 cycles, or greater than 200 cycles.
[0383] In some embodiments, the synthetic lithium solution that is yielded from the porous ion exchange beads is further processed into lithium raw materials using methods selected from the following list: solvent extraction, ion exchange, chemical precipitation, electrodialysis, el ectrowinning, evaporation with direct solar energy, evaporation with concentrated solar energy, evaporation with a heat transfer medium heated by concentrated solar energy, evaporation with heat from a geothermal brine, evaporation with heat from combustion, or combinations thereof.
[0384] In some embodiments, the synthetic lithium solution that is yielded from the porous ion exchange beads is further processed into lithium chemicals selected from the following list: lithium chloride, lithium carbonate, lithium hydroxide, lithium metal, lithium metal oxide, lithium metal phosphate, lithium sulfide, or combinations thereof. In some embodiments, the synthetic lithium solution that is yielded from the porous ion exchange beads is further processed into lithium chemicals that are solid, liquid, hydrated, or anhydrous.
[0385] In some embodiments, the lithium chemicals produced using the porous ion exchange beads are used in an industrial application selected from the following list: lithium batteries, metal alloys, glass, grease, or combinations thereof. In some embodiments, the lithium chemicals produced using the coated ion exchange particles are used in an application selected from the following list: lithium batteries, lithium-ion batteries, lithium sulfur batteries, lithium solid-state batteries, and combinations thereof.
[0386] In some embodiments, the ion exchange materials are synthesized in a lithiated state with a sublattice fully or partly occupied by lithium. In some embodiments, the ion exchange materials are synthesized in a hydrated state with a sublattice fully or partly occupied by hydrogen.Embodiments for Limiting or Eliminating Precipitation of Impurities in the Eluate Solution
[0387] In one embodiment, lithium and non-lithium impurities are absorbed from a lithium resource into an ion exchange material. In one embodiment, lithium and non-lithium impurities are eluted from an ion exchange material into an acidic solution. In one embodiment, lithium and non-lithium impurities are eluted from an ion exchange material into an acidic solution containing dissolved species that can precipitate at certain concentrations. In one embodiment,lithium and non-lithium impurities are eluted from an ion exchange material into an acidic solution containing dissolved species that are reduced in concentration to avoid precipitation. In one embodiment, lithium and non-lithium impurities are eluted from an ion exchange material into an acidic solution where said non-lithium impurities can precipitate at certain concentrations.
[0388] In one embodiment, lithium and multivalent impurities are absorbed from a lithium resource into an ion exchange material. In one embodiment, lithium and multivalent impurities are eluted from an ion exchange material into an acidic solution. In one embodiment, lithium and multivalent impurities are eluted from an ion exchange material into an acidic solution containing sulfate anions. In one embodiment, lithium and multivalent impurities are eluted from an ion exchange material into an acidic solution containing sulfate anions such that the multivalent impurities and sulfate anions can react to form insoluble salts that can precipitate. In one embodiment, lithium and multivalent impurities are eluted from an ion exchange material into a solution containing sulfate anions such that the multivalent impurities and sulfate anions that can react to form insoluble salts that can precipitate. In one embodiment, lithium and multivalent cations are eluted from an ion exchange material into a solution containing sulfate anions wherein the concentrations of sulfate anions and multivalent cations are limited to avoid precipitation of insoluble sulfate compounds.
[0389] In one embodiment, lithium and multivalent cations are eluted from an ion exchange material into a solution containing sulfate anions wherein the concentrations of multivalent cations are limited to avoid precipitation of insoluble sulfate compounds. In one embodiment, lithium and multivalent cations are eluted from an ion exchange material into a solution containing sulfate ...
Claims
CLAIMSWHAT IS CLAIMED IS:
1. A method of extracting lithium from a liquid resource, the method comprising: a) contacting a liquid resource to a lithium selective sorbent to yield an enriched lithium selective sorbent; b) contacting an eluent to the enriched lithium selective sorbent to generate a lithium eluate; c) adding a phosphate salt to the lithium eluate to precipitate a lithium phosphate salt and generate a depleted lithium eluate; d) separating the lithium phosphate salt and the depleted lithium eluate; and e) contacting a metathesis salt to the lithium phosphate salt; f) heating the metathesis salt and the lithium phosphate salt to generate an insoluble phosphate salt and a soluble lithium salt; wherein the insoluble phosphate salt comprises phosphate and has a solubility in water of at most 0.29 g / L, and wherein the soluble lithium salt comprises lithium and has a solubility in water of at least 0.41 g / L; g) adding water to the insoluble phosphate salt and the soluble lithium salt to dissolve the soluble lithium salt; and h) separating the insoluble phosphate salt and dissolved soluble lithium salt by filtration.
2. A method of extracting lithium from a liquid resource, the method comprising: a) contacting a liquid resource to a lithium selective sorbent to yield an enriched lithium selective sorbent; b) contacting an eluent to the enriched lithium selective sorbent to generate a lithium eluate; c) adding a phosphate salt to the lithium eluate to precipitate a lithium phosphate salt and generate a depleted lithium eluate; d) separating the lithium phosphate salt and the depleted lithium eluate; and e) contacting a metathesis salt, an acid, or any combination thereof, to the lithium phosphate salt to generate a soluble lithium salt; wherein c) comprises: i. adding a first quantity of the phosphate salt to the lithium eluate to yield one or more metal phosphate precipitates comprising the one or more metals, ii. removing the one or more metal phosphate precipitates by filtration to yield a purified lithium solution, andiii. adding a second quantity of the phosphate salt to the purified lithium solution to yield the lithium phosphate salt.
3. A method of extracting lithium from a liquid resource, the method comprising: a) contacting a liquid resource to a lithium selective sorbent to yield an enriched lithium selective sorbent; b) contacting an eluent to the enriched lithium selective sorbent to generate a lithium eluate, wherein the pH of the eluent prior to contact with the enriched lithium selective sorbent is less than about 1; c) adding a phosphate salt to the lithium eluate to precipitate a lithium phosphate salt and generate a depleted lithium eluate; d) separating the lithium phosphate salt and the depleted lithium eluate; and e) contacting a metathesis salt, an acid, or any combination thereof, to the lithium phosphate salt to generate a soluble lithium salt.
4. A method of extracting lithium from a liquid resource, the method comprising: a) contacting a liquid resource to a lithium selective sorbent to yield an enriched lithium selective sorbent; b) contacting an eluent to the enriched lithium selective sorbent to generate a lithium eluate, wherein the concentration of lithium in the lithium eluate is less than about 1,500 mg / L; c) adding a phosphate salt to the lithium eluate to precipitate a lithium phosphate salt and generate a depleted lithium eluate; d) separating the lithium phosphate salt and the depleted lithium eluate; and e) contacting a metathesis salt, an acid, or any combination thereof, to the lithium phosphate salt to generate a soluble lithium salt.
5. The method of claim 4, wherein the pH of the eluent prior to contact with the enriched lithium selective sorbent is less than about 1.
6. The method of claim 1 or 2, wherein the pH of the eluent prior to contact with the enriched lithium selective sorbent is less than about 1.
7. The method of any one of claims 1 to 3, wherein the concentration of lithium in the lithium eluate is more than about 1,500 mg / L.
8. The method of any one of claims 1 or 2 or 6, wherein the concentration of lithium in the lithium eluate is less than about 1,500 mg / L.
9. The method of any one of claims 1 to 7, wherein the concentration of lithium in the lithium eluate is less than about 1,250 mg / L.
10. The method of claim 9, wherein the concentration of lithium in the lithium eluate is less than about 1,000 mg / L.
11. The method of any one of claims 1 to 10, further comprising generating a lithium phosphate slurry or lithium phosphate solution prior to step e), the lithium phosphate slurry or lithium phosphate solution comprising i) the lithium phosphate salt and ii) water or a non-aqueous solvent.
12. The method of any one of claims 1 to 11, further comprising increasing the pH of the lithium eluate after step b) and prior to step c).
13. The method of claim 12, wherein the pH of the lithium eluate is increased to 2 or more.
14. The method of claim 12, wherein the pH of the lithium eluate is increased to 3 or more.
15. The method of claim 12, wherein the pH of the lithium eluate is increased to between 3 and11.
16. The method of claim 12, wherein the pH of the lithium eluate is increased to between 4 and 9.
17. The method of any one of claims 12 to 16, wherein the pH of the lithium eluate is increased by the addition of a base to the lithium eluate.
18. The method of claim 17, wherein the base comprises NaOH, KOH, LiOH, NH4OH, or any combinations thereof.
19. The method of any one of claims 1 to 18, wherein the phosphate salt has a solubility of greater than 0.5 g / L in water at pH 7.
20. The method of any one of claims 1 to 19, wherein the phosphate salt comprises potassium, sodium, aluminum, zinc, ammonium, calcium, or any combination thereof.
21. The method of any one of claims 1 to 20, wherein the phosphate salt comprises Na3PO4, Na2HPO4, NaH2PO4, K3PO4, K2HPO4, KH2PO4, A1PO4, Zn3(PO4)2, (NH4PO3)n(OH)2(i.e. poly-ammonium phosphate), sodium-hexa-metaphosphate, Ca(H2PO4)2, CaHPO4, Ca3(PO4)2, or any combination thereof.
22. The method of any one of claims 1 to 21, wherein the metathesis salt comprises a cation selected from calcium, magnesium, lithium, sodium, potassium, strontium, barium, or any combination thereof.
23. The method of claim 22, wherein the metathesis salt comprises a cation selected from calcium, magnesium, or combinations thereof.
24. The method of claim 22, wherein the metathesis salt comprises a cation selected from lithium, sodium, or potassium, or combinations thereof.
25. The method of any one of claims 1 to 24, wherein the metathesis salt comprises an anion selected from oxide, hydroxide, sulfate, chloride, fluoride, nitrate, bromide, iodide, carbonate, or combinations thereof.
26. The method of claim 25, wherein the metathesis salt comprises an anion selected from oxide, hydroxide, sulfate, chloride, carbonate, or combinations thereof.
27. The method of any one of claims 1 to 26, wherein the metathesis salt is CaO, Mg(0H)2, CaSO4, MgCh, CaCh, MgSO4, A1(OH)3, Ca(OH)2, or Na2CO3.
28. The method of any one of claims 2 to 27, wherein the acid comprises an inorganic acid.
29. The method of claim 28, wherein the inorganic acid comprises hydrochloric acid, sulfuric acid, phosphoric acid, hydrobromic acid, chloric acid, perchloric acid, nitric acid, carbonic acid, or any combinations thereof.
30. The method of any one of claims 2 to 27, wherein the acid comprises an organic acid.
31. The method of claim 30, wherein the organic acid comprises formic acid, acetic acid, citric acid, propanoic acid, lactic acid, or combinations thereof.
32. The method of any one of claims 2 to 27, wherein the acid comprises hydrochloric acid, sulfuric acid, phosphoric acid, hydrobromic acid, chloric acid, perchloric acid, nitric acid, formic acid, acetic acid, citric acid, propanoic acid, lactic acid, carbonic acid, or combinations thereof.
33. The method of claim 32, wherein the acid comprises hydrochloric acid, sulfuric acid, phosphoric acid, hydrobromic acid, nitric acid, or combinations thereof.
34. The method of any one of claims 2 to 33, wherein the acid is generated in situ by the addition of a gas to an aqueous solution.
35. The method of claim 34, wherein the gas comprises HC1, CO2, SO2, SO3, H2S, NO, NO2or any combinations thereof.
36. The method of any one of claims 2 to 35, wherein a combination of the metathesis salt and the acid is used in step e).
37. The method of claim 36, wherein the combination is sulfuric acid and Ca(OH)2.
38. The method of claim 36, wherein the combination is hydrochloric acid and MgCh.
39. The method of claim 36, wherein the combination is phosphoric acid and Ca(OH)2.
40. The method of any one of claims 1 to 39, wherein the soluble lithium salt comprises LiCl,LiSO4, Li OH, LiHCO3, Li2CO3, LiNO3, LiBr, LiF, or any combinations thereof.
41. The method of any one of claims 1 to 40, wherein a solubilizing agent is added in combination with the metathesis salt, and wherein this agent enhances the rate of the metathesis reaction.
42. The method of claim 41, wherein the solubilizing agent comprises a chelator.
43. The method of claim 41, wherein the solubilizing agent comprises EDTA, glycerol, citric acid, or a combination thereof.
44. The method of claim 43, wherein the solubilizing agent comprises EDTA.
45. The method of any one of claims 11 to 44, wherein the lithium phosphate slurry or lithium phosphate solution comprises the lithium phosphate salt and water.
46. The method of any one of claims 11 to 45, wherein the lithium phosphate slurry or lithium phosphate solution is formed in supercritical water.
47. The method of any one of claims 11 to 45, wherein the lithium phosphate slurry or lithium phosphate solution comprises the lithium phosphate salt and the non-aqueous solvent.
48. The method of claim 47, wherein the non-aqueous solvent is an organic solvent comprising less than 20% of water.
49. The method of claim 48, wherein the non-aqueous solvent is an organic solvent comprising less than 10% of water.
50. The method of claim 49, wherein the non-aqueous solvent is an organic solvent comprising less than 5% of water.
51. The method of claim 50, wherein the non-aqueous solvent is an organic solvent comprising less than 1% of water.
52. The method of any one of claims 11 to 51, wherein the non-aqueous solvent comprises an organic solvent selected from methanol, ethanol, isopropanol, n-propanol, ammonia, methylamine, dimethyl amine, trimethylamine, glycerol, N-methyl-2-pyrrolidone, dimethyl sulfoxide, tetrahydrofuran, tetrahydropyran, dimethylformamide, dimethylacetamide, methyl ethyl ketone, acetone, supercritical CO2, and combinations thereof.
53. The method of claim 52, wherein the non-aqueous solvent comprises an organic solvent selected from methanol.
54. The method of claim 52, wherein the non-aqueous solvent comprises an organic solvent selected from glycerol.
55. The method of any one of claims 1 to 54, wherein the soluble lithium salt is generated by heating the metathesis salt and the lithium phosphate salt.
56. The method of claim 55, wherein the metathesis salt is a solid and the lithium phosphate salt is a solid.
57. The method of claim 55 or 56, wherein the metathesis salt and the lithium phosphate salt are heated to between 300 K and 3000 K.
58. The method of claim 57, wherein the metathesis salt and the lithium phosphate salt are heated to between 400 K and 2000 K.
59. The method of claim 58, wherein the metathesis salt and the lithium phosphate salt are heated to between 500 K and 1500 K.
60. The method of claim 55 or 56, wherein the metathesis salt and the lithium phosphate salt are heated to 650 K or more.
61. The method of claim 60, wherein the metathesis salt and the lithium phosphate salt are heated to 1000 K or more.
62. The method of claim 61, wherein the metathesis salt and the lithium phosphate salt are heated to 1200 K or more.
63. The method of any one of claims 1 to 62, wherein the metathesis salt and the lithium phosphate salt are heated with a facilitating agent to accelerate the metathesis reaction.
64. The method of claim 63, wherein the facilitating agent comprises P2O5, sodium triphosphate, an acid, an alkali, or any combinations thereof.
65. The method of any one of claims 55 to 64, wherein the metathesis salt at least partially melts when heated with the lithium phosphate salt.
66. The method of any one of claims 55 to 65, wherein the particle size of the lithium phosphate salt, the metathesis salt, or a combination thereof is reduced before, during, or before and during heating.
67. The method of claim 66, wherein the particle size reduction occurs through milling, fracturing, in a hammer mill, delumper, ball mill, attrition mill, jaw crusher, other mechanochemical methods, or a combination thereof.
68. The method of any one of claims 1 to 67, wherein the soluble lithium salt comprises LiOH and one or more additional monovalent hydroxide salts.
69. The method of claim 68, wherein the soluble lithium salt comprises LiOH, NaOH, and KOH.
70. The method of any one of claims 1 to 69, further comprising purifying the soluble lithium salt.
71. The method of any one of claims 68 to 70, wherein purifying the soluble lithium salt comprises selectively isolating LiOH by re-crystallization.
72. The method of any one of claims 1 to 71, further comprising adding a carbonate salt to a solution comprising the soluble lithium salt to yield lithium carbonate dissolved in solution.
73. The method of claim 72, wherein the carbonate salt is generated by addition of gaseous carbon dioxide.
74. The method of claim 72 or 73, wherein the lithium carbonate dissolved in solution is precipitated by heating the solution.
75. The method of any one of claims 1 to 74, wherein the soluble lithium salt is treated in an electrochemical system to generate an acidified solution and a basified solution.
76. The method of claim 75, wherein step e) is performed in water to generate the soluble lithium salt and a water-insoluble phosphate salt.
77. The method of any one of claims 2 to 76, wherein step e) additionally generates a waterinsoluble phosphate salt as a solid.
78. The method of claim 77, wherein the water-insoluble phosphate salt comprises phosphate and has a solubility in water of at most 0.29 g / L.
79. The method of any one of claims 2 to 78, wherein the soluble lithium salt comprises lithium and has a solubility in water of at least 0.41 g / L.
80. The method of any one of claims 1 to 79, wherein the phosphate salt of step c) comprises phosphate and has a solubility in water of at least 0.41 g / L.
81. The method of any one of claims 2 to 80, wherein step e) is performed in an aqueous solution and generates a water-insoluble phosphate salt as a solid and the soluble lithium salt dissolved in water.
82. The method of claim 81, further comprising separating the water-insoluble phosphate salt and the soluble lithium salt dissolved in water.
83. The method of claim 82, further comprising separating one or more of the water-insoluble phosphate salts and the soluble lithium salt dissolved in water in one or more particle traps.
84. The method of claim 83, wherein the one or more particle traps comprises a bag filter, a candle filter, a cartridge filter, a media filter, a depth filter, a sand filter, a membrane filter, an ultrafiltration system, a microfiltration filter, a nanofiltration filter, a cross-flow filter, a dead-end filter, a drum filter, a filter press, or a combination thereof.
85. The method of claim 84, wherein the one or more particle traps is a filter press.
86. The method of any one of claims 1 to 85, wherein e) comprises adding the lithium phosphate salt to a mixture comprising the metathesis salt and a liquid.
87. The method of claim 86, wherein the lithium phosphate salt is added as a mixture of lithium phosphate and a liquid.
88. The method of any one of claims 1 to 85, wherein e) comprises adding the metathesis salt to a mixture comprising the lithium phosphate salt and a liquid.
89. The method of claim 88, wherein the metathesis salt is added as a mixture of the metathesis salt and a liquid.
90. The method of any one of claims 1 to 89, further comprising contacting a carbonate salt to the soluble lithium salt dissolved in water to generate a lithium carbonate solution.
91. The method of claim 90, wherein the lithium carbonate solution is heated to yield solid lithium carbonate.
92. The method of claim 90 or 91, wherein the carbonate salt comprises sodium carbonate, potassium carbonate, calcium carbonate, magnesium carbonate, carbon dioxide dissolved in water, or a combination thereof.
93. The method of any one of claims 1 to 92, wherein the soluble lithium salt is processed into lithium carbonate to precipitate a majority of lithium as lithium carbonate, wherein the precipitated lithium carbonate is separated from the minority of lithium remaining in solution; wherein the minority of lithium remaining in solution is precipitated as lithium phosphate by addition of a phosphate salt.
94. The method of any one of claims 2 to 93, wherein sulfuric acid is contacted to the lithium phosphate salt to generate a solution of lithium sulfate and phosphoric acid.
95. The method of claim 94, wherein Ca(0H)2 is contacted with the solution of lithium sulfate to precipitate an insoluble salt of Ca and phosphate, thereby generating a purified lithium sulfate solution.
96. The method of claim 95, wherein the insoluble salt of Ca and phosphate and the lithium sulfate solution are separated.
97. The method of any one of claims 1 to 96, wherein the soluble lithium salt is processed in an electrochemical system to produce lithium hydroxide and an acid.
98. The method of claim 97, wherein said electrochemical system is a three compartment bipolar electrodialysis system.
99. The method of any one of claims 1 to 98, wherein the lithium eluate comprises lithium and one or more metals other than lithium.
100. The method of claim 99, wherein the one or more metals react with phosphate to form one or more metal phosphate precipitates.
101. The method any one of claims 99 or 100, further comprising, adding the phosphate salt of step c) in two or more portions to the lithium eluate, such that the first addition forms one or more metal phosphate precipitates.
102. The method of claim 101, further comprising removing the one or more metal phosphate precipitates by filtration.
103. The method of any one of claims 99 to 102, wherein the one or more metals are selected from calcium, magnesium, strontium, barium, zirconium, titanium, vanadium, iron, copper, manganese, molybdenum, aluminum, and niobium.
104. The method of claim 102 or 103, wherein the one or more metal phosphate precipitates are filtered by the use of one or more particle traps.
105. The method of claim 104, wherein the one or more particle traps comprises a bag filter, a candle filter, a cartridge filter, a media filter, a depth filter, a sand filter, a membrane filter, an ultrafiltration system, a microfiltration filter, a nanofiltration filter, a cross-flow filter, a dead-end filter, a drum filter, a filter press, or a combination thereof.
106. The method of claim 105, wherein the one or more particle traps comprises a filter press.
107. The method of any one of claims 1 to 106, wherein the liquid resource is a natural brine, a dissolved salt flat, seawater, concentrated seawater, brine concentrated by solar evaporation, a geothermal brine, a desalination effluent, a concentrated brine, a processed brine, an oilfield brine, a liquid from an ion exchange process, a liquid from a solvent extraction process, a synthetic brine, a leachate from an ore or combination of ores, a leachate from a mineral or combination of minerals, a leachate from a clay or combination of clays, a leachate from recycled products, a leachate from recycled materials, or combinations thereof.
108. The method of claim 107, wherein the liquid resource is a natural brine, a dissolved salt flat, concentrated seawater, brine concentrated by solar evaporation, a geothermal brine, a desalination effluent, an oilfield brine, a leachate from an ore or combination of ores, a leachate from a mineral or combination of minerals, a leachate from a clay or combination of clays, a leachate from recycled lithium batteries, or combinations thereof.
109. The method of claim 108, wherein the liquid resource is a leachate from an ore.
110. The method of claim 109, wherein the ore is spodumene rock.
111. The method of claim 109 or 110, wherein the leachate is generated by crushing the ore and contacting the crushed ore with an acid.
112. The method of claim 111, wherein the acid comprises hydrochloric acid, sulfuric acid, phosphoric acid, hydrobromic acid, chloric acid, perchloric acid, nitric acid, formic acid, acetic acid, or combinations thereof.
113. The method of claim 112, wherein the liquid resource is natural brine, a dissolved salt flat, or a geothermal brine.
114. The method any one of claims 1 to 113, wherein the eluent comprises hydrochloric acid, sulfuric acid, phosphoric acid, hydrobromic acid, chloric acid, perchloric acid, nitric acid, formic acid, acetic acid, or combinations thereof.
115. The method of any one of claims 1 to 114, wherein said lithium selective sorbent is selected from and ion exchange material and an adsorbent.
116. The method of claim 115, wherein said ion exchange material comprises LiFePCU, LiMnPCU, Li2TiOs, Li2MnOs, Li2SnOs, Li^isOn, I^MnsOn, LiMn2O4, Li1.6Mn1.eO4, LiA102, LiCuO2, LiTiO2, Li4TiO4, Li?TinO24, LisVO4, Li2SisO7, Li2CuP2O?, modifications thereof, solid solutions thereof, or a combination thereof.
117. The method of claim 115, wherein the adsorbent comprises a crystalline lithium salt aluminate, a lithium aluminum intercalate, LiCT2Al(OH)3, crystalline aluminum trihydroxide (Al(0H)3), gibbsite, beyerite, nordstrandite, alumina hydrate, bauxite, amorphous aluminum trihydroxide, activated alumina layered lithium-aluminum double hydroxides, Li Ah(OH)6Cl, combinations thereof, compounds thereof, or solid solutions thereof.
118. The method of claim 115, wherein the adsorbent comprises a lithium aluminum intercalate.
119. The method of any one of claims 1 to 118, wherein said lithium selective sorbent is coated with a coating that is selected from an oxide, a polymer, or combinations thereof.
120. The method of claim 119, wherein said lithium selective sorbent is coated with a coating that is selected from SiCh, TiCL, ZrCL, polyvinylidene difluoride, polyvinyl chloride, polystyrene, polybutadiene, polydivinylbenzene, or combinations thereof.
121. A method of extracting lithium from a liquid resource, the method comprising: a) contacting a liquid resource to a lithium selective sorbent to yield an enriched lithium selective sorbent; b) contacting an eluent to the enriched lithium selective sorbent to generate a lithium eluate; c) adding a phosphate salt to the lithium eluate to precipitate a lithium phosphate salt and generate a depleted lithium eluate; d) separating the lithium phosphate salt and the depleted lithium eluate; e) generating a lithium phosphate slurry comprising the lithium phosphate salt and adding an acid to generate an acidified lithium phosphate slurry or solution; f) adding a metathesis salt to acidified lithium phosphate slurry or solution to generate a water-insoluble phosphate salt and a water-soluble lithium salt; and g) separating the water-insoluble phosphate salt and the water-soluble lithium salt.
122. A method of preparing a water-soluble lithium salt, the method comprising: a) generating a lithium phosphate salt; b) contacting a metathesis salt to the lithium phosphate salt to yield a salt mixture; c) heating the salt mixture to generate a water-insoluble phosphate salt and the water-soluble lithium salt; wherein the water-insoluble phosphate salt comprises phosphate and has a solubility in water of at most 0.29 g / L, and wherein the water-soluble lithium salt comprises lithium and has a solubility in water of at least 0.41 g / L;d) adding water to the water-insoluble phosphate salt and the water-soluble lithium salt to dissolve the water-soluble lithium salt; and e) separating the water-insoluble phosphate salt and dissolved water-soluble lithium salt by filtration.
123. The method of claim 122, wherein the metathesis salt comprises a cation selected from calcium, magnesium, or combinations thereof.
124. The method of claim 122 or 123, wherein the metathesis salt comprises a cation selected from lithium, sodium, or potassium, or combinations thereof.
125. The method of any one of claims 122 to 124, wherein the metathesis salt comprises an anion selected from oxide, hydroxide, sulfate, chloride, carbonate, or combinations thereof.
126. The method of claim 125, wherein the metathesis salt is CaO, Mg(OH)2, CaSCU, CaCO3, or Ca(OH)2.
127. The method of any one of claims 122 to 126, wherein the metathesis salt and the lithium phosphate salt are heated to between 300 K and 3000 K.
128. The method of claim 127, wherein the metathesis salt and the lithium phosphate salt are heated to between 400 K and 2000 K.
129. The method of claim 127, wherein the metathesis salt and the lithium phosphate salt are heated to between 500 K and 1500 K.
130. The method of any one of claims 122 to 126, wherein the metathesis salt and the lithium phosphate salt are heated to 650 K or more.
131. The method of claim 130, wherein the metathesis salt and the lithium phosphate salt are heated to 1000 K or more.
132. The method of claim 131, wherein the metathesis salt and the lithium phosphate salt are heated to 1200 K or more.
133. The method of any one of claims 122 to 132, further comprising ball milling the salt mixture prior to c).
134. A method of preparing a water-soluble lithium salt, the method comprising: a) generating an impure lithium solution, wherein the impure lithium solution comprises lithium and one or more metals other than lithium, wherein the one or more metals join with phosphate to form one or more metal precipitates, and wherein one or more metal precipitates each have a solubility of at most 0.29 g / L;b) adding a phosphate salt to the impure lithium solution to yield one or more metal precipitates and a purified lithium solution; c) adding additional phosphate salt to the purified lithium solution to yield a lithium phosphate salt; d) contacting a metathesis salt to generate a water-insoluble phosphate salt and the water- soluble lithium salt; wherein the water-insoluble phosphate salt comprises phosphate and has a solubility in water of at most 0.29 g / L, and wherein the water-soluble lithium salt comprises lithium and has a solubility in water of at least 0.41 g / L.
135. The method of claim 134, wherein the one or more metals are selected from calcium, magnesium, strontium, barium, zirconium, titanium, vanadium, iron, copper, manganese, molybdenum, aluminum, niobium.
136. The method of claim 134 or 135, wherein the metathesis salt and the lithium phosphate salt are heated to generate the water-insoluble phosphate salt and the water- soluble lithium salt in step d).
137. The method of any one of claims 134 to 136, further comprising separating the water-insoluble phosphate salt and the water-soluble lithium salt.
138. The method of claim 137, further comprising adding water to the water-insoluble phosphate salt and the water-soluble lithium salt to dissolve the water-soluble lithium salt; and separating the water insoluble phosphate salt and dissolved water-soluble lithium salt by filtration.
139. The method of claim 134 or 135, wherein the metathesis salt and the lithium phosphate salt are slurried in water to generate the water-insoluble phosphate salt and the water-soluble lithium salt in step d), wherein the water-soluble lithium salt is dissolved in the water.
140. The method of claim 139, wherein the metathesis salt is a carbonate salt, the water-soluble lithium salt is lithium carbonate, and the water-soluble lithium salt dissolved in water is a solution of lithium carbonate in water.
141. The method of claim 140, further comprising precipitation of solid lithium carbonate by heating the lithium carbonate in water.
142. The method of claim 139, wherein the metathesis salt is a hydroxide salt, the water-soluble lithium salt is lithium hydroxide, and the water-soluble lithium salt dissolved in water is a solution of lithium hydroxide in water.
Citation Information
Patent Citations
Method for preparing high-purity lithium sulfate from waste liquid recovered from hydrothermal method based lithium iron phosphate production
CN107915239A
Manufacturing method of lithium hydroxide and lithium carbonate with high purity from brine
KR1020120063069A
Lithium extraction in the presence of scalants
US20220348475A1
Lithium extraction process
WO2021212214A1
Cited By
US12257529B2
Lithium extraction enhanced by an alternate phase
US12370468B2
Ion exchange system for lithium extraction
US12374679B2
Methods and systems for the extraction of lithium and production of lithium compounds
WO2026111968A1