Method and device for treating nickel laterite ore leaching residue

Through drying, granulation, roasting desulfurization and immersion reduction treatment of laterite nickel ore leaching residue, the problem of recovering iron and sulfur in the leaching residue is solved, energy consumption and environmental pollution are reduced, and resource utilization and economic benefits are achieved.

WO2024221684A1PCT designated stage expired Publication Date: 2024-10-31ZHEJIANG HUAYOU COBALT CO LTD

Patent Information

Application Number
PCT/CN2023/115895
Authority / Receiving Office
WO · WO
Patent Type
Applications
Current Assignee / Owner
Priority Date
2023-04-28
Filing Date
2023-08-30
Publication Date
2024-10-31

AI Technical Summary

Technical Problem

Laterite nickel ore leaching residue is rich in iron but of low grade and cannot be directly used as iron-making raw material, resulting in resource waste and environmental safety hazards. The pressurized wet leaching process requires high sulfur, causing energy consumption and environmental pollution problems.

Method used

The laterite nickel ore leaching slag is processed using steps such as drying, granulation, roasting desulfurization and immersion reduction. Drying tail gas and secondary combustion provide reaction heat, reduce energy consumption, and recover iron and sulfur to form high-grade molten iron and slag, reducing environmental impact. pollute.

Benefits of technology

It realizes the resource utilization of laterite nickel ore leaching residue, reduces energy consumption and environmental pollution, improves the recovery efficiency of iron and sulfur, solves the problem of leaching residue processing, and has economic benefits.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN2023115895_31102024_PF_FP_ABST
    Figure CN2023115895_31102024_PF_FP_ABST
Patent Text Reader

Abstract

A nickel laterite ore leaching residue treatment method, and a nickel laterite ore leaching residue treatment device. The treatment method comprises: providing a nickel laterite ore leaching residue; drying the nickel laterite ore leaching residue to obtain dry residue and drying tail gas; mixing the dry residue with a first reducing agent used for desulfurization, and granulating, to obtain a pellet; performing roasting and desulfurization of the pellet, to obtain hot baked sand and roasting tail gas; performing immersion reduction on the hot baked sand with a second reducing agent used for extracting iron and a flux, to obtain molten iron, slag and primary coal gas, and using escaped primary coal gas for immersion reduction and heat compensation by means of secondary combustion. The treatment apparatus mainly comprises a drying apparatus, a granulation apparatus, a desulfurization apparatus and a reduction apparatus. The treatment method can comprehensively recycle both iron and sulfur from the leaching residue of nickel laterite ore, reduce energy consumption, and effectively realize resource utilization of the leaching residue of nickel laterite ore.
Need to check novelty before this filing date? Find Prior Art

Description

Method and equipment for treating laterite nickel ore leaching residue

[0001] This application claims priority to the Chinese patent application filed with the China Patent Office on April 28, 2023, with application number 202310493474.3 and invention name “Method and equipment for treating laterite nickel ore leaching residue”, the entire contents of which are incorporated by reference into this application. Technical Field

[0002] The present application relates to the field of resource utilization of industrial solid waste, and in particular to a method and equipment for treating laterite nickel ore leaching residue. Background Art

[0003] Nickel has the characteristics of high mechanical strength, good ductility, high temperature resistance and high chemical stability. It is widely used in stainless steel, new energy and other fields. It is an indispensable metal material in the industrial field. Nickel resources are mainly distributed in laterite nickel ore and nickel sulfide ore, of which nickel sulfide ore accounts for about 40% and laterite nickel ore accounts for about 60%. However, nickel sulfide ore has been developed for hundreds of years. Long-term mining has led to a gradual decline in the resource reserves and ore grade of nickel sulfide ore. In addition, no large-scale nickel sulfide mines have been discovered in recent years. Therefore, the output of nickel sulfide ore has been on a downward trend, and laterite nickel ore has become the main raw material for extracting nickel resources.

[0004] The extraction of nickel and cobalt from laterite nickel ore typically involves pressurized wet leaching. However, this process produces a large amount of leaching residue. Although the leaching residue is rich in iron (over 30%), the iron in the residue is primarily in the form of hematite, and the residue has high water and sulfur contents and low grade. Therefore, the leaching residue cannot be used directly as an ironmaking raw material. Therefore, it is typically stockpiled for disposal, resulting in a significant waste of resources and a high environmental safety hazard. If not properly handled, this can become a bottleneck in the pressurized wet leaching process. Technical issues

[0005] Based on this, it is necessary to provide a method and equipment for treating laterite nickel ore leaching residue to address the above problems; the treatment method can not only comprehensively recover iron and sulfur in laterite nickel ore leaching residue, but also help reduce energy consumption, effectively realizing the resource utilization of laterite nickel ore leaching residue. Technical Solutions

[0006] A method for treating laterite nickel ore leaching residue, comprising:

[0007] Provide laterite nickel ore leaching residue;

[0008] Drying the laterite nickel ore leaching residue to obtain dry residue and dry tail gas;

[0009] mixing the dry slag with a first reducing agent for desulfurization and granulating the mixture to obtain pellets;

[0010] The pellets are roasted and desulfurized to obtain hot roasted sand and roasting tail gas;

[0011] The hot roasted sand is immersed in reduction with a second reducing agent and flux for iron extraction to obtain molten iron, slag and primary coal gas. The escaped primary coal gas is used for supplementary heat for immersion reduction through secondary combustion.

[0012] In one embodiment, the mass of the first reducing agent is α×(18.8%×W1+1.78%×W2) / FC, wherein α is an excess coefficient and α is selected from 1.05-1.20, W1 is the mass of sulfur in the dry slag, W2 is the mass of iron in the dry slag, and FC is the fixed carbon content of the first reducing agent.

[0013] In one embodiment, the moisture content of the dry residue is 15%-25%.

[0014] In one embodiment, the dry tail gas is subjected to dust removal treatment to obtain dry dust and dry flue gas, wherein the dry dust is mixed with the dry slag and the first reducing agent to be granulated, and the dry flue gas is subjected to desulfurization treatment.

[0015] In one embodiment, the particle size of the pellets is less than or equal to 8 mm, and the mass of the pellets with a particle size less than or equal to 3 mm accounts for more than 80% of the total mass of the pellets.

[0016] In one embodiment, the roasting tail gas is subjected to dust removal treatment to obtain roasting dust and roasting flue gas, wherein the roasting dust is immersed in reduction with the hot roasted sand, the second reducing agent, and the flux, and the roasting flue gas is used to produce acid.

[0017] In one embodiment, a second reducing agent containing at least 400 kg of fixed carbon is required to be provided for every 1 ton of molten iron obtained.

[0018] In one embodiment, at least one of the following conditions is met:

[0019] (1) The first reducing agent is selected from at least one of coke, coal, and blue carbon;

[0020] (2) The particle size of the first reducing agent is less than or equal to 1 mm;

[0021] (3) The second reducing agent is selected from at least one of coke, semi-coke, and anthracite;

[0022] (4) The fixed carbon content of the second reducing agent is greater than 70%;

[0023] (5) The water content of the second reducing agent is less than or equal to 2%;

[0024] (6) The particle size of the second reducing agent is 1 mm to 3 mm.

[0025] In one embodiment, the flux is selected from at least one of a calcined oxide of a magnesium-rich material and a calcined oxide of a calcium-rich material, the particle size of the flux is less than or equal to 1 mm, and the mass ratio of CaO to SiO2 in the slag is controlled by the flux to be (1.0-1.3):1, the mass fraction of MgO is 8%-10%, and the mass fraction of Al2O3 is 10%-20%.

[0026] In one embodiment, the combustion rate of the secondary combustion is 50%-60%.

[0027] In one embodiment, the escaped primary gas is subjected to secondary combustion to obtain raw gas, the raw gas is subjected to gas purification treatment to obtain clean gas and smelting dust, and the smelting dust is immersed in reduction with the hot roasted sand, the second reducing agent, and the flux.

[0028] In one embodiment, the clean coal gas is used as the first fuel for at least one of the steps of the drying process, the roasting desulfurization, and the immersion reduction.

[0029] In one embodiment, the roasting and desulfurization step also includes at least one of a second fuel and roasting combustion-supporting air, wherein the second fuel includes at least one of sulfur, coal powder, natural gas, and hydrogen, and the roasting combustion-supporting air includes oxygen-enriched air with an oxygen concentration of 21%-23%.

[0030] In one embodiment, at least one of the following conditions is met:

[0031] (1) The temperature of the immersion reduction is 1450°C-1550°C;

[0032] (2) Submerged combustion is performed by injecting a third fuel and a primary combustion-supporting air into the molten pool to supplement heat for submerged reduction, wherein the combustion oxygen excess coefficient of the submerged combustion is less than or equal to 0.6, the third fuel is selected from at least one of thermal coal, waste mineral oil, natural gas, coke oven gas, and hydrogen, and the primary combustion-supporting air is selected from oxygen-enriched air having an oxygen concentration greater than or equal to 40%;

[0033] (3) The primary coal gas undergoes secondary combustion under the action of secondary combustion-supporting air, wherein the secondary combustion-supporting air is selected from oxygen-enriched air with an oxygen concentration of 35%-50%, and the temperature of the secondary combustion-supporting air is 1000℃-1200℃.

[0034] In one embodiment, when the calcium content of the laterite nickel ore leaching residue is less than or equal to 1%, the temperature of the roasting desulfurization is 800° C.-900° C., and the temperature of the hot calcination is 500° C.-700° C.;

[0035] Alternatively, when the calcium content of the laterite nickel ore leaching residue is greater than 1%, the temperature of the roasting desulfurization is 1000°C-1100°C, and the temperature of the hot roasting is 800°C-900°C.

[0036] A processing device used in the above-mentioned method for treating laterite nickel ore leaching residue mainly includes:

[0037] A drying device is used to collect and dry the laterite nickel ore leaching residue to obtain dry residue and dry tail gas;

[0038] a granulation device for receiving the dry slag and mixing the dry slag with a first reducing agent for desulfurization to granulate the slag to obtain pellets;

[0039] A desulfurization device is used to receive the pellets and roast and desulfurize the pellets to obtain hot roasted sand and roasting tail gas;

[0040] The reduction device is used to receive the hot roasted sand and immerse the hot roasted sand with a second reducing agent and flux for iron extraction to obtain molten iron, slag and primary coal gas, and at the same time perform secondary combustion on the escaped primary coal gas.

[0041] The treatment method described in the present application first mixes the dried laterite nickel ore leaching residue with a first reducing agent and granulates it for roasting and desulfurization. The free water, crystal water and sulfur element in the dry residue are gradually removed through drying, decomposition, reduction desulfurization and other reactions. This not only allows the sulfur in the laterite nickel ore leaching residue to be recycled and utilized, and can especially be used to replenish the wet leaching process of laterite nickel ore, which is beneficial to significantly reduce the demand for sulfur in the wet leaching process, but also the obtained hot roasted sand has a low water content and sulfur content, which is beneficial to further refining and utilization of the hot roasted sand.

[0042] Furthermore, the hot roasted sand and the second reducing agent and flux rapidly undergo decomposition, pyrolysis, melting, reduction, slagging and carburizing reactions under high temperature conditions, and since the reaction products have different densities and forms, the molten iron, slag and primary gas can be easily separated. Among them, the molten iron can be used for steelmaking or casting raw materials, and the slag can be used as a building material raw material. The reaction heat generated by the primary gas and the secondary combustion air in the secondary combustion process provides the heat required for the immersion reduction reaction through radiation, convection, etc., thereby effectively reducing the energy consumption of the immersion reduction. Beneficial effects

[0043] Therefore, the present application utilizes roasting desulfurization and immersion reduction methods to collaboratively treat laterite nickel ore leaching residue, which can not only comprehensively recycle the iron and sulfur in the laterite nickel ore leaching residue, solving the treatment problem of laterite nickel ore leaching residue, but also helps to reduce energy consumption, generate certain economic benefits, and effectively realize the resource utilization of laterite nickel ore leaching residue. BRIEF DESCRIPTION OF THE DRAWINGS

[0044] FIG1 is a flow chart of a method for treating laterite nickel ore leaching residue in one embodiment of the present application. Modes for Carrying Out the Invention

[0045] To facilitate understanding of the present application, the present application will be described in more detail below. However, it should be understood that the present application can be implemented in many different forms and is not limited to the embodiments or examples described herein. On the contrary, the purpose of providing these embodiments or examples is to make the understanding of the disclosure of the present application more thorough and comprehensive.

[0046] Unless otherwise defined, all technical and scientific terms used herein have the same meaning as those commonly understood by those skilled in the art to which this application pertains. The terms used herein in the specification of this application are only for the purpose of describing specific embodiments or examples and are not intended to limit this application.

[0047] As shown in FIG1 , the present application provides a method for treating laterite nickel ore leaching residue, comprising:

[0048] S1, providing laterite nickel ore leaching residue;

[0049] S2, drying the laterite nickel ore leaching residue to obtain dry residue and dry tail gas;

[0050] S3, mixing the dry slag with a first reducing agent for desulfurization and granulating the mixture to obtain pellets;

[0051] S4, roasting and desulfurizing the pellets to obtain hot roasted sand and roasting tail gas;

[0052] S5, immersing the hot roasted sand with a second reducing agent and flux for iron extraction to obtain molten iron, slag and primary gas, and the escaped primary gas is used for supplementary heat for immersion reduction through secondary combustion.

[0053] In step S1, the laterite nickel ore leaching residue is the leaching residue after nickel and cobalt are extracted from magnesia nickel ore type laterite nickel ore or limonite type laterite nickel ore by a wet leaching process. The laterite nickel ore leaching residue can be transported to the material preparation area by a car, a belt conveyor, etc., or the laterite nickel ore leaching residue produced by the wet leaching process can be directly transported to the material preparation area by pipeline transportation, etc.

[0054] Among them, the laterite nickel ore leaching residue produced by the wet leaching process is transported through pipelines and subjected to filter pressure treatment in the raw material warehouse. The filtrate can be used to replenish slag water or to replenish water for the wet leaching process, which not only helps to save the transportation cost of the laterite nickel ore leaching residue, but also improves the environment.

[0055] In step S2, the moisture content in the laterite nickel ore leaching residue can be further reduced by drying the laterite nickel ore leaching residue. Preferably, the moisture content of the dry residue obtained by drying is 15%-25%, which not only provides suitable conditions for the subsequent granulation of the dry residue, but also helps to reduce energy consumption in the subsequent roasting process.

[0056] The drying method includes but is not limited to steam drying, rotary kiln drying and the like.

[0057] Preferably, the drying treatment adopts a rotary kiln drying method. Further preferably, the fuel in the rotary kiln drying method can be the clean coal gas generated in the subsequent laterite nickel ore leaching slag treatment method of the present application, which is beneficial to saving fuel. Further, by indirectly exchanging heat between the drying combustion-supporting air and the roasting tail gas generated in step S3, the temperature of the drying combustion-supporting air is increased to 200°C-250°C, which is beneficial to saving fuel and thus reducing drying energy consumption.

[0058] Preferably, the dry tail gas is subjected to dust removal treatment to obtain dry dust and dry flue gas, wherein the dry dust can be mixed with the dry slag and the first reducing agent in the subsequent step for granulation, which is beneficial to improving the utilization rate of solid waste; the dry flue gas is subjected to desulfurization treatment, which is beneficial to avoiding environmental pollution problems caused by sulfur-containing gas emissions, thereby improving the environment.

[0059] In step S3, by mixing the dry slag with a specific amount of the first reducing agent for granulation, the sulfate in the dry slag can be prevented from generating sulfide during subsequent roasting and desulfurization, and the sulfate can be efficiently decomposed, so that the hot roasted sand obtained after desulfurization has a lower sulfur content.

[0060] Preferably, the mass of the first reducing agent is α×(18.8%×W1+1.78%×W2) / FC, wherein α is an excess coefficient and is selected from 1.05-1.20, W1 is the mass of sulfur in the dry slag, W2 is the mass of iron in the dry slag, and FC is the fixed carbon content of the first reducing agent, which can make the sulfur content of the hot roasted sand lower than 0.5%.

[0061] Further preferably, when the calcium content of the laterite nickel ore leaching residue is less than or equal to 1%, the mass of the first reducing agent is 1.5%-2.5% of the dry mass of the laterite nickel ore leaching residue; or, when the calcium content of the laterite nickel ore leaching residue is greater than 1%, the mass of the first reducing agent is 2.6%-4.5% of the dry mass of the laterite nickel ore leaching residue.

[0062] Wherein, the first reducing agent is selected from at least one of coke, coal, and blue carbon, and the particle size of the first reducing agent is less than or equal to 1 mm.

[0063] Preferably, the particle size of the pellets is less than or equal to 8 mm, and the mass of the pellets with a particle size less than or equal to 3 mm accounts for more than 80% of the total mass of the pellets, so that the obtained hot roasted sand is more suitable for pneumatic conveying, and the hot roasted sand can be pneumatically conveyed to the immersion reduction device.

[0064] In step S4, since the sulfur in the laterite nickel ore leaching residue mainly exists in the form of sulfate, and the main mineral phases are gypsum and bauxite, during the roasting desulfurization process, gypsum and bauxite first undergo a removal reaction of free water and crystallization water at low temperature, and then undergo a desulfurization reaction under the action of the first reducing agent, thereby efficiently removing the sulfur element in the dry slag, so that the obtained hot roasted sand has a lower water content and sulfur content, which is beneficial to the further refining and utilization of the hot roasted sand.

[0065] It should be noted that different desulfurization devices have different requirements for the moisture content of the feed pellets. When using a desulfurization device with a drying function, the pellets can be fed directly into the desulfurization device; when using other desulfurization devices, the pellets can be dried or air-dried until the moisture content of the pellets is less than 10%. This helps ensure that the pellets have sufficient strength and avoids pulverization during the roasting and desulfurization process, which affects the desulfurization effect. This application does not limit this, and those skilled in the art can make their own choices based on actual preparation requirements.

[0066] Preferably, a countercurrent roasting process is used during roasting and desulfurization, that is, the movement direction of the pellets is opposite to the movement direction of the high-temperature air blown in during roasting, so that the pellets can be dehydrated, desulfurized and reduced step by step during the slow heating process, avoiding the formation of sulfides caused by rapid heating.

[0067] Preferably, the roasting tail gas is subjected to dust removal treatment to obtain roasting dust and roasting flue gas, wherein the roasting dust can be immersed and reduced together with the hot roasted sand, the second reducing agent and the flux in the subsequent step, which is beneficial to improving the utilization rate of solid waste; the roasting flue gas is used for acid production, and more preferably, the roasting flue gas is returned to the sulfur-based acid production system of the wet process plant for acid production, so that the sulfur in the laterite nickel ore leaching residue can be recovered and utilized, which is beneficial to reducing the demand for sulfur in the wet leaching process.

[0068] Taking into account the different calcium contents of laterite nickel ore leaching residues, the temperature of roasting and desulfurization has certain differences. In one embodiment, when the calcium content of the laterite nickel ore leaching residues is less than or equal to 1%, the temperature of the roasting and desulfurization is 800°C-900°C, and the temperature of the hot roasting is 500°C-700°C; when the calcium content of the laterite nickel ore leaching residues is greater than 1%, the temperature of the roasting and desulfurization is 1000°C-1100°C, which is conducive to fully roasting and desulfurizing the calcium sulfate in the laterite nickel ore leaching residues, and the temperature of the hot roasting is 800°C-900°C.

[0069] Preferably, the clean coal gas recovered in step S5 is used as the first fuel for roasting desulfurization. When the clean coal gas is insufficient to supply the roasting desulfurization, a second fuel can be added as a supplement, wherein the second fuel is selected from at least one of sulfur, coal powder, natural gas, and hydrogen. It is further preferred that the second fuel is sulfur, which not only increases the concentration of sulfur dioxide in the roasting tail gas, but also helps reduce the cost of sulfuric acid production in the wet process plant. When the fuel calorific value is insufficient, oxygen-enriched air with an oxygen enrichment concentration of 21%-23% can be further used as roasting combustion air to increase the flame temperature.

[0070] It should be noted that the roasting and desulfurization step may not use the clean coal gas recovered in step S5 as fuel, and this application does not limit this.

[0071] Preferably, the temperature of the hot baked sand is maintained at 600° C.-900° C., which is beneficial to reducing the heat required for subsequent immersion reduction and lowering energy consumption.

[0072] It should be noted that the hot roasted sand can be directly transported for immersion reduction or transferred to a buffer device. Preferably, the entire transportation process is in a closed state, which is beneficial to prevent the hot roasted sand from cooling and reoxidation.

[0073] In step S5, the hot roasted sand and the second reducing agent and flux rapidly undergo decomposition, pyrolysis, melting, reduction, slagging and carburizing reactions under high temperature conditions, so that the iron oxides in the hot roasted sand are reduced to metallic iron and carburized to obtain molten iron, and impurities such as calcium and silicon form slag. Since the reaction products have different densities and forms, the molten iron, slag and primary coal gas can be easily separated.

[0074] Preferably, when the mass of the first reducing agent is α×(18.8%×W1+1.78%×W2) / FC, where α is the excess coefficient and is selected from 1.05-1.20, W1 is the mass of sulfur in the dry slag, W2 is the mass of iron in the dry slag, and FC is the fixed carbon content of the first reducing agent, the sulfur content of the hot roasted sand after roasting and desulfurization is less than 0.5%, thereby making the iron content of the molten iron greater than or equal to 93%, the carbon content greater than or equal to 3.5%, and the sulfur content less than or equal to 1%. After a simple desulfurization treatment, the sulfur content in the molten iron is reduced to below 0.05%, and it can be used for steelmaking or ingot casting for sale. Preferably, by adding ferrosilicon, a foundry pig iron with a silicon content greater than 1.25% is produced, thereby increasing the added value of the product.

[0075] The slag mainly comprises calcium oxide, silicon dioxide, magnesium oxide and aluminum oxide, and contains iron less than or equal to 5%. It can be used as a raw material for building materials. The slag is preferably subjected to water crushing so that the slag can meet the needs of different building raw materials.

[0076] Fuel pyrolysis, reduction, and submerged combustion generate primary gas containing carbon monoxide, which escapes from the molten pool and undergoes secondary combustion. The reaction heat generated during the secondary combustion provides the heat required for the submerged reduction reaction through radiation and convection, effectively reducing the energy consumption of the submerged reduction process.

[0077] Preferably, the escaped primary coal gas is subjected to secondary combustion to obtain raw coal gas, and the raw coal gas is subjected to coal gas purification treatment to obtain clean coal gas. The clean coal gas can also be used as fuel supply in any step of the treatment method described in the present application to reduce costs. For example, the clean coal gas is used as the first fuel for at least one step of the drying treatment, the roasting desulfurization, and the immersion reduction, which is more conducive to saving fuel and thus reducing energy consumption.

[0078] In one embodiment, the raw coal gas is purified to obtain smelting dust, which can be immersed in the smelting dust, the hot roasted sand, the second reducing agent, and the flux for reduction, thereby improving the utilization rate of solid waste.

[0079] Preferably, when the combustion rate of the secondary combustion is 50%-60%, it is beneficial to reduce the iron content of the slag while controlling the fuel consumption, thereby making the laterite nickel ore leaching slag treatment method more economical.

[0080] It should be noted that the combustion rate of secondary combustion = (V1+V2) / (V1+V2+V3+V4)×100, wherein V1 represents the volume of CO2 in the raw gas, V2 represents the volume of H2O in the raw gas, V3 represents the volume of H2 in the raw gas, and V4 represents the volume of CO in the raw gas.

[0081] Preferably, for every 1 t of molten iron, a second reducing agent containing at least 400 kg of fixed carbon is provided, that is, the amount of the second reducing agent satisfies the fixed carbon ≥ 400 kg / (t of molten iron) to ensure the reduction and carburizing effects.

[0082] Specifically, the second reducing agent is selected from at least one of coke, semi-coke, and anthracite.

[0083] Preferably, the fixed carbon content in the second reducing agent is greater than 70%.

[0084] Preferably, the water content of the second reducing agent is less than or equal to 2%.

[0085] Preferably, the particle size of the second reducing agent is 1 mm-3 mm.

[0086] The slag is a quaternary slag system of CaO-SiO2-MgO-Al2O3. The addition of flux results in a CaO to SiO2 mass ratio of (1.0-1.3):1, a MgO mass fraction of 8%-10%, and an Al2O3 mass fraction of 10%-20%. Furthermore, the slag preferably has a melting point of less than or equal to 1500°C and a viscosity of less than or equal to 1 Pa·s at 1500°C, which facilitates slag discharge.

[0087] Preferably, the flux is selected from at least one of calcined oxides of magnesium-rich materials and calcined oxides of calcium-rich materials, and the particle size of the flux is less than or equal to 1 mm, which is conducive to shortening the slag making time.

[0088] The magnesium-rich material includes but is not limited to at least one of dolomite, magnesite, and magnesia, and the calcium-rich material includes but is not limited to at least one of limestone and steel slag.

[0089] Preferably, the temperature of the immersion reduction is 1450°C-1550°C.

[0090] It should be noted that, under the action of a sufficient amount of the second reducing agent, the hot roasted sand can undergo an immersion reduction reaction. Fuel can also be added to supplement the heat for the immersion reduction, thereby reducing the amount of the second reducing agent and helping to reduce costs.

[0091] Preferably, the third fuel and the primary combustion-supporting air are injected into the molten pool for submerged combustion to supplement heat for submerged reduction, and the combustion oxygen excess coefficient of the submerged combustion is less than or equal to 0.6, thereby ensuring the reducing atmosphere required for the reduction reaction.

[0092] The third fuel is selected from at least one of thermal coal, waste mineral oil, natural gas, coke oven gas, and hydrogen. A low-cost fuel is preferred to reduce iron production costs. Furthermore, the thermal coal preferably has a particle size of 1 mm to 3 mm and a moisture content of less than or equal to 2%. The back pressure of the gas fuel is 0.1 MPa to 0.2 MPa, and the back pressure of the liquid fuel is 0.4 MPa to 0.6 MPa.

[0093] Preferably, the primary combustion-supporting air is selected from oxygen-enriched air with an oxygen concentration greater than or equal to 40%.

[0094] Preferably, the primary coal gas undergoes secondary combustion under the action of secondary combustion-supporting air, and the secondary combustion-supporting air is selected from oxygen-enriched air with an oxygen concentration of 35%-50%, and the temperature of the secondary combustion-supporting air is 1000℃-1200℃, which is beneficial to reducing fuel consumption and improving calorific value.

[0095] It should be noted that the coal gas and steam generated in step S5 account for more than 50% of the total heat generated by the entire treatment method. Since superheated steam power generation is more efficient than saturated steam power generation, this application preferably superheats the saturated steam generated in step S5 so that the obtained superheated steam can be used for power generation; using coal gas as fuel for drying and roasting can further reduce the fuel consumption in the previous steps and reduce costs.

[0096] Therefore, the present application utilizes roasting desulfurization and immersion reduction methods to collaboratively treat laterite nickel ore leaching residue, which can not only comprehensively recycle the iron and sulfur in the laterite nickel ore leaching residue, solving the treatment problem of laterite nickel ore leaching residue, but also helps to reduce energy consumption, generate certain economic benefits, and effectively realize the resource utilization of laterite nickel ore leaching residue.

[0097] The present application also provides a processing device for a method for treating laterite nickel ore leaching residue, which mainly includes:

[0098] A drying device is used to collect and dry the laterite nickel ore leaching residue to obtain dry residue and dry tail gas;

[0099] a granulation device for receiving the dry slag and mixing the dry slag with a first reducing agent for desulfurization to granulate the slag to obtain pellets;

[0100] A desulfurization device is used to receive the pellets and roast and desulfurize the pellets to obtain hot roasted sand and roasting tail gas;

[0101] The reduction device is used to receive the hot roasted sand and immerse the hot roasted sand with a second reducing agent and flux for iron extraction to obtain molten iron, slag and primary coal gas, and at the same time perform secondary combustion on the escaped primary coal gas.

[0102] Wherein, the drying device is preferably a rotary kiln.

[0103] The granulation device is preferably a disc granulator.

[0104] The desulfurization device is preferably a rotary kiln or a rotary hearth furnace, more preferably a countercurrent rotary kiln with chain grate drying.

[0105] The reduction device is preferably a Hismelt furnace, an oxygen-enriched side-blown furnace or one of other furnace types. The device preferably operates under positive pressure with a pressure of 25 kPa-150 kPa.

[0106] Specifically, the reduction device includes an iron zone, a slag zone and a furnace zone, wherein the iron zone adopts an insulating structure, the slag zone adopts a combined structure of a copper water jacket and refractory materials, and the furnace zone adopts a combined structure of hanging bricks and a water jacket.

[0107] Preferably, the reduction device is provided with two types of spray guns, including a mixing material spray gun and an immersion combustion spray gun, wherein the mixing material spray gun is a single-channel structure with an inner lining of wear-resistant ceramics; the immersion combustion spray gun is a double-channel structure with an inner channel for fuel and an outer channel for oxygen-enriched air; the spray gun is cooled by a copper water jacket and protected by slag.

[0108] More preferably, the tip of the lance is located about 500-1000 mm below the slag surface.

[0109] In one embodiment, at least one spray gun is used to inject secondary combustion-supporting air in the secondary combustion, and the spray gun is arranged on the side wall of the immersion reduction device and close to the slag surface. The spray gun adopts a water-cooling structure and a swirl blade is arranged inside the spray gun.

[0110] Hereinafter, the method and equipment for treating laterite nickel ore leaching residue will be further described through the following specific examples.

[0111] It should be noted that laterite nickel ore leaching residue is a wet basis, including dry basis and water, while dry residue includes dry basis and residual water after losing some water. Therefore, although the water content of laterite nickel ore leaching residue and dry residue is different, the mass of the dry basis and the components in the dry basis is the same.

[0112] Example 1

[0113] Provided is laterite nickel ore leaching residue, wherein the wet basis moisture content is 33%, the dry basis main element content is: 33% Fe, 5.11% Ca, 7% S, 4.42% Si, 0.31% Mg, 3.45% Al and the balance impurities.

[0114] A steam dryer was used to dry 200t of laterite nickel ore leaching residue on a dry basis to obtain dry residue with a moisture content of 18%, and the steam consumption was 50t.

[0115] Assuming the excess coefficient α is 1.2, the required amount of coke powder (particle size approximately 1 mm, fixed carbon content of 85%) is 5.4 tons, calculated as α × (18.8% × 7% × 200 tons + 1.78% × 33% × 200 tons) ÷ 85%. The dry slag and 5.4 tons of coke powder are mixed with water and pelletized in a disc pelletizer to produce pellets. The pellets have a particle size of ≤8 mm, and the mass of pellets with a particle size of ≤3 mm accounts for approximately 85% of the total mass. The pellets are then air-dried to a moisture content of 10%, yielding 228 tons of dry pellets.

[0116] The dry pellets were fed into a countercurrent rotary kiln for roasting and desulfurization. The feed rate of the dry pellets was controlled at 1 t / h, the roasting and desulfurization temperature was 1100°C, and the process took 2 hours from feed to discharge, producing 718.2 kg / h of hot roasted sand with an iron content of 44.65% and a sulfur content of 0.41%. The roasting and desulfurization process used 94.7 kg / h of pulverized coal as fuel, a high-temperature air flow of 1400°C, a roasting tail gas temperature of 300°C, and a SO2 concentration of 3.0%. After gravity and electrostatic dust collection, the roasting tail gas produced 22.2 kg / h of roasting dust, which was then used for wet acid production.

[0117] The hot roasted sand and roasted dust at 850℃ were mixed at a flow rate of 794.5kg / h, and 80.9kg / h of light-burned dolomite (particle size about 1mm), 30.7kg / h of lime (particle size about 0.5mm), 174.7kg / h of coke powder (fixed carbon 400kg / t molten iron, water content ≤2%, particle size about 1mm), and 83.5Nm 3 / h nitrogen is used as the conveying gas, which is sprayed into the furnace molten pool below 500mm through the material gun, and 185kg / h of coal powder and 371Nm 3 / h of oxygen-enriched air (oxygen concentration of 40%, combustion oxygen excess coefficient of 0.6), submerged combustion at 1470℃, to obtain 334.7kg / h of molten iron (iron content of 93.64%, sulfur content of 0.35%), 423.6kg / h of slag and primary gas. 3 / h of oxygen-enriched air (oxygen concentration 40%) and primary gas for secondary combustion, and the secondary combustion rate is controlled at 50%. The raw gas is cooled by waste heat boiler and dust-collected by bag to obtain 1218Nm 3 / h of clean coal gas (CO concentration 22.25%, calorific value 3001kJ / Nm 3 ).

[0118] After carburizing, the molten iron is discharged through the iron tapping port at a temperature of 1420°C. A mixture of passivated magnesium (0.6 kg / t) and lime (6.1 kg / t) is sprayed into the molten iron for desulfurization, reducing its sulfur content to 0.05%. 75% ferrosilicon (20.5 kg / t) is then added to increase the silicon content to 1.8%. Finally, the molten iron is cast into pig iron blocks at a rate of 349.4 kg / h. The slag is separated by sedimentation and discharged through the slag outlet at a temperature of 1470°C. The main components of the slag are CaO, SiO2, MgO, and Al2O3. The mass ratio of CaO to SiO2 is 1.3, the MgO content is 8.1%, the Al2O3 content is 17.4%, and the iron content is ≤5%. The slag melting point is 1435°C, and the slag viscosity at 1470°C is ≤1 Pa•s.

[0119] Example 2

[0120] Provided is laterite nickel ore leaching residue, wherein the wet basis moisture content is 33%, the dry basis main element content is: 42% Fe, 0.5% Ca, 3% S, 5.53% Si, 0.39% Mg, 4.31% Al and the balance impurities.

[0121] A steam dryer was used to dry 200t of laterite nickel ore leaching residue on a dry basis to obtain dry residue with a moisture content of 18%, and the steam consumption was 50t.

[0122] Assuming the excess coefficient α is 1.05, the required amount of coke powder (particle size approximately 0.5 mm, fixed carbon content 85%) is 3.3 tons, calculated as α × (18.8% × 3% × 200 tons + 1.78% × 42% × 200 tons) ÷ 85%. The dry slag and 3.3 tons of coke powder are mixed with water and pelletized in a disc pelletizer to produce pellets. The pellets have a particle size of ≤8 mm, and the mass of pellets with a particle size of ≤3 mm accounts for approximately 85% of the total mass. The pellets are then air-dried to a moisture content of 10%, yielding 226 tons of dry pellets.

[0123] The dry pellets were fed into a countercurrent rotary kiln for roasting and desulfurization. The feed rate of the dry pellets was controlled at 1 t / h, the roasting and desulfurization temperature was 850°C, and the time from feed to discharge was 2 hours, producing 849.9 kg / h of hot roasted sand with an iron content of 47.95% and a sulfur content of 0.19%. The roasting and desulfurization process used 78 kg / h of pulverized coal as fuel, a high-temperature air flow of 1400°C, and a roasting exhaust temperature of 300°C. The SO2 concentration in the roasting exhaust was 1.58%. After gravity and electrostatic dust collection, the roasting exhaust produced 26.3 kg / h of roasting dust, which was then used for wet acid production.

[0124] The 600℃ hot calcined sand and calcined dust were mixed at a flow rate of 942.4kg / h, and 102.9kg / h of light-burned dolomite (particle size of about 0.5mm), 116.8kg / h of lime (particle size of about 0.5mm), 277.6kg / h of coke powder (fixed carbon 500kg / t molten iron, water content ≤2%, particle size of about 2mm), and 102.8Nm 3 / h of compressed air is used as the conveying gas, which is sprayed into the molten pool 500mm below the furnace through the material gun, and the immersion combustion gun is blown into 116.2kg / h of coal powder and 180Nm 3 / h of oxygen-enriched air (oxygen concentration of 45%, combustion oxygen excess coefficient of 0.5), submerged combustion at 1450℃, to obtain 424.6kg / h of molten iron (iron content of 93.9%, sulfur content of 0.12%), 536.6kg / h of slag and primary gas. 3 / h of oxygen-enriched air (oxygen concentration 35%) and primary gas for secondary combustion, and the secondary combustion rate is controlled at 55%. The raw gas is cooled by waste heat boiler and dust-collected by bag to obtain 1372Nm 3 / h of clean coal gas (CO concentration 19.9%, calorific value 2674kJ / Nm 3 ).

[0125] After carburizing, the molten iron is discharged through the iron tapping port at a temperature of 1400°C. A mixture of passivating magnesium (0.2 kg / t) and lime (1.9 kg / t) is sprayed into the molten iron for desulfurization, reducing the sulfur content to 0.03%. 75% ferrosilicon (12.9 kg / t) is then added to increase the silicon content to 1.25%. Finally, pig iron blocks are cast at a rate of 432.3 kg / h. The slag is separated by sedimentation and discharged through the slag outlet at a temperature of 1450°C. The main components of the slag are CaO, SiO2, MgO, and Al2O3. The mass ratio of CaO to SiO2 is 1.2, the MgO content is 8.9%, the Al2O3 content is 17.0%, and the iron content is ≤5%. The slag melting point is 1410°C, and the slag viscosity at 1450°C is ≤1 Pa•s.

[0126] Example 3

[0127] The same laterite nickel ore leaching residue as in Example 1 was used, and the same drying treatment and granulation were performed to obtain 228 tons of dry pellets.

[0128] The dry pellets were fed into a countercurrent rotary kiln for roasting and desulfurization. The feed rate of the dry pellets was controlled at 1 t / h, the roasting and desulfurization temperature was 1000°C, and the process took 2 hours from feed to discharge, producing 717.5 kg / h of hot roasted sand with an iron content of 44.68% and a sulfur content of 0.42%. The roasting and desulfurization process used 78 kg / h of pulverized coal and 50 kg / h of liquid sulfur at 150°C and 1400°C, respectively. The high-temperature air flow was 300°C, and the SO2 concentration in the roasting exhaust gas was 5.27%. Gravity and electrostatic dust collection produced 21 kg / h of roasting dust, which was then used for wet acid production.

[0129] The hot roasted sand and roasted dust at 850℃ were mixed at a flow rate of 791.1kg / h, and 115.1kg / h of light-burned dolomite (particle size about 1mm), 262.1kg / h of coke powder (fixed carbon 600kg / t molten iron, water content ≤2%, particle size about 3mm), and 86Nm 3 / h of oxygen-enriched air (oxygen concentration is 50%) is used as the conveying gas, which is sprayed into the furnace molten pool below 500mm through the material gun, and 10.5kg / h of pulverized coal and 11.6Nm 3 / h of oxygen-enriched air (oxygen concentration of 50%, combustion oxygen excess coefficient of 0.4), submerged combustion at 1500℃, to obtain 335kg / h of molten iron (iron content of 93.7%, sulfur content of 0.36%), 427kg / h of slag and primary gas. 3 / h of oxygen-enriched air (oxygen concentration 50%) and primary coal gas for secondary combustion, and the secondary combustion rate is controlled at 60%. The raw coal gas is cooled by waste heat boiler and dust-collected by bag to obtain 735Nm 3 / h of clean coal gas (CO concentration 22.8%, calorific value 3020kJ / Nm 3 ).

[0130] After carburizing, the molten iron is discharged through an iron tapping port at a temperature of 1450°C. A mixture of passivated magnesium (0.7 kg / t) and lime (6.6 kg / t) is sprayed into the molten iron for desulfurization, reducing its sulfur content to 0.01%. 75% ferrosilicon (30.3 kg / t) is then added to increase the silicon content to 2.5%. Finally, the molten iron is cast into pig iron blocks at a rate of 359.3 kg / h. The slag is separated by sedimentation and discharged through a slag outlet at a temperature of 1500°C. The main components of the slag are CaO, SiO2, MgO, and Al2O3. The mass ratio of CaO to SiO2 is 1.2, the MgO content is 10%, the Al2O3 content is 17.3%, and the iron content is ≤5%. The slag melting point is 1447°C, and the slag viscosity at 1500°C is ≤1 Pa•s.

[0131] Example 4

[0132] The difference between Example 4 and Example 1 is that the dry slag and 20 tons of coke powder are mixed with water and then granulated in a disc granulator, and reduction roasted at 1050°C for 1 hour to obtain hot roasted sand with a sulfur content of 2.5%.

[0133] Comparative Example 1

[0134] The same laterite nickel ore leaching residue as in Example 1 was used.

[0135] 30% of coal powder and 6% of lime powder were added to 200g of laterite nickel ore leaching residue, the prepared raw materials were mixed evenly, and an appropriate amount of water was added to granulate to obtain pellets, which were then dried.

[0136] The dried pellets were placed in a gold assay furnace, heated to 1300°C, and calcined for 30 minutes to obtain hot calcined sand.

[0137] The hot calcined sand was cooled, dried and ground in water, and then magnetically separated at a magnetic field strength of 2650 Gs to obtain an iron concentrate with an iron grade of 52.05%.

[0138] Comparative Example 2

[0139] The same laterite nickel ore leaching residue as in Example 1 was used.

[0140] The laterite nickel ore leaching residue is washed with a filter press, and ammonia water and sodium metabisulfite are added to the washed laterite nickel ore leaching residue for slurry pre-treatment, and then slurry treatment is performed to obtain ore pulp, wherein the mass ratio of the laterite nickel ore leaching residue to ammonia water and sodium metabisulfite is 1:0.5:1, the slurry ratio in the slurry pre-treatment is 5:1, the pre-slurrying temperature is 100°C, and the pre-slurrying time is 1.5 hours.

[0141] The slurry was added into an autoclave and pressurized at 200°C for 2 h.

[0142] The pressurized pulp was subjected to wet magnetic separation to obtain magnetite slag with a hematite conversion rate of 74%.

[0143] As can be seen from Examples 1-4 above, the method for treating laterite nickel ore leach residue provided by this application can recover high-grade molten iron and simultaneously recycle sulfur, effectively realizing resource utilization of laterite nickel ore leach residue and reducing energy consumption, thereby resolving the treatment challenges of laterite nickel ore leach residue. In Example 4, due to the addition of a large amount of coke powder, the dry residue is partially converted to form sulfides such as iron sulfide, aluminum sulfide, and calcium sulfide during the roasting and desulfurization process, resulting in a higher sulfur content in the hot roasted sand than in Examples 1-3.

[0144] Comparative Example 1 only performed primary purification on the laterite nickel ore leach residue. Since the laterite nickel ore leach residue is a secondary crystallization product with a small particle size, the magnetic separation effect after roasting is poor, resulting in a low-grade concentrate and low added value. Comparative Example 2 used a wet process to treat the laterite nickel ore leach residue. However, the tailings after magnetic separation are still hazardous waste and pose a high environmental safety hazard.

[0145] The technical features of the above-mentioned embodiments can be combined arbitrarily. In order to make the description concise, not all possible combinations of the technical features in the above-mentioned embodiments are described. However, as long as there is no contradiction in the combination of these technical features, they should be considered to be within the scope of this specification.

[0146] The above-described embodiments merely represent several implementation methods of the present application. While the descriptions are relatively specific and detailed, they should not be construed as limiting the scope of the present invention. It should be noted that a person skilled in the art could make various modifications and improvements without departing from the spirit of the present application, all of which fall within the scope of protection of the present application. Therefore, the scope of protection of the present patent application shall be determined by the appended claims.

Claims

1. A method for treating laterite nickel ore leaching residue, characterized in that: include: Provide laterite nickel ore leaching residue; Drying the laterite nickel ore leaching residue to obtain dry residue and dry tail gas; The dry slag is mixed with a first reducing agent for desulfurization to form pellets; The pellets are roasted and desulfurized to obtain hot roasted sand and roasting tail gas; The hot roasted sand is immersed in reduction with a second reducing agent and flux for iron extraction to obtain molten iron, slag and primary coal gas. The escaped primary coal gas is used for supplementary heat for immersion reduction through secondary combustion.

2. The method for treating laterite nickel ore leaching residue according to claim 1, characterized in that: The mass of the first reducing agent is α×(18.8%×W1+1.78%×W2) / FC, wherein α is the excess coefficient and α is selected from 1.05-1.20, W1 is the mass of sulfur in the dry slag, W2 is the mass of iron in the dry slag, and FC is the fixed carbon content of the first reducing agent.

3. The method for treating laterite nickel ore leaching residue according to claim 1, characterized in that: The moisture content of the dry slag is 15%-25%.

4. The method for treating laterite nickel ore leaching residue according to claim 1, characterized in that: The dry tail gas is subjected to dust removal treatment to obtain dry dust and dry flue gas, wherein the dry dust is mixed with the dry slag and the first reducing agent to be granulated, and the dry flue gas is subjected to desulfurization treatment.

5. The method for treating laterite nickel ore leaching residue according to claim 1, characterized in that: The particle size of the pellets is less than or equal to 8 mm, and the mass of the pellets with a particle size less than or equal to 3 mm accounts for more than 80% of the total mass of the pellets.

6. The method for treating laterite nickel ore leaching residue according to claim 1, characterized in that: The roasting tail gas is subjected to dust removal treatment to obtain roasting dust and roasting flue gas, wherein the roasting dust is immersed in reduction with the hot roasted sand, the second reducing agent and the flux, and the roasting flue gas is used to produce acid.

7. The method for treating laterite nickel ore leaching residue according to claim 1, characterized in that: For every ton of molten iron obtained, a second reducing agent containing at least 400 kg of fixed carbon is required.

8. The method for treating laterite nickel ore leaching residue according to claim 1, characterized in that: At least one of the following conditions is met: (1) The first reducing agent is selected from at least one of coke, coal, and blue carbon; (2) The particle size of the first reducing agent is less than or equal to 1 mm; (3) The second reducing agent is selected from at least one of coke, semi-coke and anthracite; (4) The fixed carbon content of the second reducing agent is greater than 70%; (5) The water content of the second reducing agent is less than or equal to 2%; (6) The particle size of the second reducing agent is 1 mm-3 mm.

9. The method for treating laterite nickel ore leaching residue according to claim 1, characterized in that: The flux is selected from at least one of the calcined oxide of magnesium-rich material and the calcined oxide of calcium-rich material. The particle size of the flux is less than or equal to 1 mm. The mass ratio of CaO to SiO2 in the slag is controlled by the flux to be (1.0-1.3):1, the mass fraction of MgO is 8%-10%, and the mass fraction of Al2O3 is 10%-20%.

10. The method for treating laterite nickel ore leaching residue according to claim 1, characterized in that: The combustion rate of the secondary combustion is 50%-60%.

11. The method for treating laterite nickel ore leaching residue according to claim 1, characterized in that: The escaped primary coal gas is subjected to secondary combustion to obtain raw coal gas, the raw coal gas is subjected to gas purification treatment to obtain clean coal gas and smelting dust, and the smelting dust is subjected to immersion reduction with the hot roasted sand, the second reducing agent, and the flux.

12. The method for treating laterite nickel ore leaching residue according to claim 11, characterized in that: The clean coal gas is used as the first fuel for at least one step of the drying process, the roasting desulfurization, and the immersion reduction.

13. The method for treating laterite nickel ore leaching residue according to claim 1 or 12, characterized in that: The roasting and desulfurization step also includes at least one of a second fuel and roasting combustion-supporting air, wherein the second fuel includes at least one of sulfur, coal powder, natural gas, and hydrogen, and the roasting combustion-supporting air includes oxygen-enriched air with an oxygen concentration of 21%-23%.

14. The method for treating laterite nickel ore leaching residue according to claim 1, characterized in that: At least one of the following conditions is met: (1) The temperature of the immersion reduction is 1450°C-1550°C; (2) injecting a third fuel and a primary combustion-supporting air into the molten pool for submerged combustion to supplement heat for submerged reduction, wherein the combustion oxygen excess coefficient of the submerged combustion is less than or equal to 0.6, the third fuel is selected from at least one of electric coal, waste mineral oil, natural gas, coke oven gas, and hydrogen, and the primary combustion-supporting air is selected from oxygen-enriched air having an oxygen concentration greater than or equal to 40%; (3) The primary coal gas undergoes secondary combustion under the action of secondary combustion-supporting air, wherein the secondary combustion-supporting air is selected from oxygen-enriched air with an oxygen concentration of 35%-50%, and the temperature of the secondary combustion-supporting air is 1000°C-1200°C.

15. The method for treating laterite nickel ore leaching residue according to claim 1, characterized in that: When the calcium content of the laterite nickel ore leaching residue is less than or equal to 1%, the temperature of the roasting desulfurization is 800°C-900°C, and the temperature of the hot roasting is 500°C-700°C; Alternatively, when the calcium content of the laterite nickel ore leaching residue is greater than 1%, the temperature of the roasting desulfurization is 1000°C-1100°C, and the temperature of the hot roasting is 800°C-900°C.

16. A processing device used in the method for processing laterite nickel ore leaching residue according to any one of claims 1 to 15, characterized in that: The processing device mainly includes: A drying device, used for collecting and drying the laterite nickel ore leaching residue to obtain dry residue and dry tail gas; A granulation device, used for receiving the dry slag, and mixing the dry slag with a first reducing agent for desulfurization to granulate to obtain pellets; A desulfurization device, used for receiving the pellets, and roasting and desulfurizing the pellets to obtain hot roasted sand and roasting tail gas; The reduction device is used to receive the hot roasted sand and immerse and reduce the hot roasted sand with a second reducing agent and flux for iron extraction to obtain molten iron, slag and primary coal gas, and at the same time perform secondary combustion on the escaped primary coal gas.

Citation Information

Patent Citations

  • Novel technique for comprehensively recovering nickel-cobalt-iron from nickel laterite ore through low-temperature acidification and acidolysis

    CN105907949A

  • Method for recovering iron from pressurized leachate of laterite

    CN106498148A

  • Method for recovering valuable metals from nickel-containing leaching residues

    CN111534703A

  • Method for producing high-grade matte nickel by reducing, vulcanizing and smelting laterite-nickel ore

    CN115386738A

  • Treatment method of laterite-nickel ore acid leaching residues

    CN116004936A

Cited By

  • Method for preparing high-metallization-ratio reduced iron block with low energy consumption by using laterite-nickel ore high-pressure acid leaching residues

    CN121428258A