Multi-coating terminal and conductive structure

By adopting a multi-plating structure on the aluminum terminal, including the first transition plating, nickel plating and contact plating, and filling the gaps with the second transition plating, the problems of terminal plating peeling off and poor bonding are solved, achieving better wear resistance. and corrosion resistance, extending service life and reducing electrochemical reactions.

WO2024222715A1PCT designated stage expired Publication Date: 2024-10-31CHANGZHOU JETTY AUTOMOTIVE PARTS CORP
View PDF 6 Cites 0 Cited by

Patent Information

Application Number
PCT/CN2024/089461
Authority / Receiving Office
WO · WO
Patent Type
Applications
Current Assignee / Owner
Priority Date
2023-04-24
Filing Date
2024-04-24
Publication Date
2024-10-31

AI Technical Summary

Technical Problem

The plating thickness of existing terminals is too thick, resulting in high internal stress and easy falling off. Moreover, the bonding between the plating layer and the base material is poor, resulting in insufficient wear resistance and corrosion resistance.

Method used

Adopting a multi-plated structure, including aluminum terminals, first transition plating, nickel plating and contact plating, the second transition plating is used to fill the gaps and holes on the surface to enhance the adhesion and flatness of the plating, and select the electrode potential to be between nickel and materials between contact plating to reduce electrochemical reactions.

Benefits of technology

It improves the adhesion and corrosion resistance of the coating, extends the service life of the terminal, and reduces the electrochemical reaction between metals, enhancing conductive efficiency and wear resistance.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN2024089461_31102024_PF_FP_ABST
    Figure CN2024089461_31102024_PF_FP_ABST
Patent Text Reader

Abstract

The invention relates to the technical field of electric connection. Provided are a multi-coating terminal and a conductive structure. The multi-coating terminal comprises an aluminum terminal and coatings, wherein the coatings are arranged on at least part of the surface of the aluminum terminal; and the coatings sequentially comprise a first transition coating, a nickel coating and a contact coating from the inside to the outside. The surface of the aluminum terminal is first provided with the first transition coating, such that the adhesiveness of the whole coating and the aluminum terminal can be improved, and the coating is prevented from falling off for quite a long time. The nickel coating has a very high stability in the air; and when the nickel coating covers the first transition coating, the whole aluminum terminal can be made to have a very strong passivation capability, a layer of an extremely thin passivation film can be rapidly generated on the surface, and corrosion by the atmosphere, alkalis and some acids can be resisted. The contact coating, as the outermost layer experiencing frequent plugging or rubbing, not only has a good conductivity, but also has a relatively good wear resistance and attractiveness, can greatly prolong the service life of the aluminum terminal, and can greatly improve the conductive efficiency of the aluminum terminal.
Need to check novelty before this filing date? Find Prior Art

Description

A multi-plating terminal and a conductive structure

[0001] Related applications

[0002] This application claims priority to Chinese patent application No. 202320948520.X filed on April 24, 2023, and cites the disclosed contents thereof as part of this application. Technical Field

[0003] The present disclosure relates to the technical field of electrical connection, and in particular to a multi-plating terminal and a conductive structure. Background Art

[0004] Currently, the application fields of electrical transmission equipment are becoming more and more extensive, especially the use of electric vehicles is becoming more and more common. In the design of electronic products, a large number of terminals are required to achieve circuit connection. The terminals often need to be plugged in, unplugged or welded, so the terminals are subject to greater wear and tear. The worn areas are easily oxidized and corroded, and poor electrical contact often occurs. In order to improve wear resistance, corrosion resistance, oxidation resistance and conductivity, many electronic interface terminals are currently electroplated with electroplating layers. The terminal plating generally contains a wear-resistant layer and an anti-oxidation corrosion layer. However, if the thickness of the current terminal plating is too thick, it will cause greater internal stress and easy to fall off, resulting in insufficient wear resistance and corrosion resistance of the terminal. Some electroplating layers ignore the bonding with the base material. After electroplating, the adhesion between the electroplating layer and the base material is poor, resulting in the electroplating layer falling off during later use. Therefore, a new solution is urgently needed in the existing technology to solve the above problems.

[0005] Summary of the Invention

[0006] The object of the present disclosure is to provide a terminal having good plating adhesion, corrosion resistance, and good conductivity.

[0007] An embodiment of the present disclosure provides a multi-plated terminal, comprising an aluminum terminal and a plating layer. The plating layer is provided on at least a portion of the surface of the aluminum terminal; the plating layer comprises, from the inside to the outside, a first transition plating layer, a nickel plating layer, and a contact plating layer.

[0008] In some embodiments, a second transition plating layer is provided between the contact plating layer and the nickel plating layer.

[0009] In some embodiments, the electrode potential of the second transition coating material is between the electrode potential of nickel and the electrode potential of the contact coating material.

[0010] In some embodiments, the second transition coating is made of one or more of gold, silver, nickel, tin, tin-lead alloy, zinc, and a zinc alloy.

[0011] In some embodiments, the electrode potential of the first transition coating is between the electrode potentials of aluminum and nickel.

[0012] In some embodiments, the first transition coating is made of zinc or zinc alloy.

[0013] In some embodiments, the thickness of the first transition coating is 0.015 μm-2.5 μm.

[0014] In some embodiments, the material of the contact plating layer is one or a combination of gold, silver, hard silver, tin, tin-lead alloy, silver-antimony alloy, palladium, palladium-nickel alloy, graphite silver, graphene silver and silver-gold-zirconium alloy.

[0015] In some embodiments, the aluminum terminal is a flat terminal or one end of a solid aluminum wire.

[0016] In some embodiments, the aluminum terminal has a connection hole, and a surface of the connection hole has a conductive wear-resistant layer.

[0017] In some embodiments, the conductive wear-resistant layer is made of one or a combination of gold, tin, tin-lead alloy, silver-antimony alloy, palladium, palladium-nickel alloy, graphite silver, graphene silver, and silver-gold-zirconium alloy.

[0018] In some embodiments, the thickness of the contact plating layer is 0.012 μm-40 μm.

[0019] In some embodiments, the nickel plating layer has a thickness of 0.012 μm-15 μm.

[0020] An embodiment of the present disclosure further provides a conductive structure, comprising the aluminum terminal and the conductor as described above, wherein the aluminum terminal and the conductor are welded to form a weld, and a tin plating layer is provided on the surface of the weld.

[0021] In some embodiments, the thickness of the tin plating layer is not less than 8 μm.

[0022] In some embodiments, the weld is covered with an insulating protective layer.

[0023] In some embodiments, the insulating protective layer is made of a thermoplastic polymer material or a vulcanizable polymer material.

[0024] The present invention has the following beneficial effects: Applying a first transition coating to the surface of an aluminum terminal enhances the adhesion of the entire coating to the aluminum terminal, ensuring that the coating will not peel off for a considerable period of time. The nickel coating is highly stable in air, and covering it with the first transition coating imparts a strong passivation property to the entire aluminum terminal, rapidly forming an extremely thin passivation film on the surface that resists corrosion from the atmosphere, alkalis, and certain acids. The contact coating, as the outermost layer that is frequently plugged in, unplugged, or rubbed, not only has excellent conductivity but also good wear resistance and aesthetics, significantly increasing the service life and conductivity efficiency of multi-layered terminals. Applying a second transition coating to the surface of the nickel coating fills surface gaps and holes, making the terminal surface smooth and seamless. Applying the contact coating further strengthens the bond and creates a smoother, more even surface, further extending the terminal's service life. Selecting a second transition coating whose electrode potential lies between that of the nickel and contact coating material significantly reduces electrochemical reactions between the metals, reduces metal corrosion, and extends the terminal's service life. BRIEF DESCRIPTION OF THE DRAWINGS

[0025] The present disclosure is further described in detail below with reference to the accompanying drawings and specific embodiments.

[0026] FIG1 is a cross-sectional view of an embodiment of a multi-plated terminal of the present application.

[0027] FIG2 is a cross-sectional view of another embodiment of a multi-plated terminal of the present application.

[0028] FIG3 is a schematic structural diagram of an embodiment of a conductive structure of the present application.

[0029] FIG4 is a cross-sectional view of a conductive structure of the present application.

[0030] FIG5 is a schematic structural diagram of another embodiment of a conductive structure of the present application.

[0031] The reference numerals in the figure are as follows: 1-aluminum terminal, 12-weld, 121-tin plating, 13-connection hole, 2-first transition plating, 3-nickel plating, 4-contact plating, 5-second transition plating, 6-conductor. DETAILED DESCRIPTION

[0032] The following will be combined with the accompanying drawings in the embodiments of the present disclosure to clearly and completely describe the technical solutions in the embodiments of the present disclosure. Obviously, the embodiments described are only part of the embodiments of the present disclosure, not all of the embodiments. Based on the embodiments of the present disclosure, all other embodiments obtained by ordinary technicians in this field without making any creative efforts are within the scope of protection of the present disclosure.

[0033] Referring to Figure 1 , an embodiment of the present disclosure provides a multi-plated terminal, comprising an aluminum terminal 1 and a plating layer. The plating layer is disposed on at least a portion of the surface of the aluminum terminal 1. The plating layer comprises, from the inside out, a first transition plating layer 2, a nickel plating layer 3, and a contact plating layer 4.

[0034] In the field of electrical connections, copper is used to conduct electric current. Copper has high conductivity and good ductility. However, as the price of copper continues to rise, the cost of using copper materials will become higher and higher. For this reason, people have begun to look for substitutes for metallic copper to reduce costs. The content of metallic aluminum in the earth's crust is about 7.73%. After the optimization of refining technology, the price is relatively low. In addition, compared with copper, aluminum is lighter and its conductivity is second only to copper. Aluminum can replace part of copper in the field of electrical connections. Therefore, replacing copper with aluminum is a development trend in the field of automotive electrical connections. However, the corrosion resistance and conductivity of aluminum terminals restrict their use. The aluminum terminal 1 provided in this application can overcome these problems. The material of the aluminum terminal 1 is aluminum or aluminum alloy, and high-hardness aluminum grades can be selected, such as grades AA6101, AA6061, AA6063 or AA8030. Plating the first transition coating 2 on the aluminum terminal 1 can increase the adhesion between the nickel coating 3 and the aluminum terminal 1. This is because if the nickel coating 3 is directly plated on the aluminum material, the adhesion between the aluminum material and the nickel coating 3 is poor, causing the nickel coating 3 to fall off very easily. If there are other coatings on the outside that increase the thickness, the coating on the aluminum terminal 1 will fall off even more easily. The present invention ensures that the coating will not fall off for a considerable period of time by providing the first transition coating 2 on the aluminum terminal 1 to increase the adhesion between the nickel coating 3 and the aluminum terminal 1. The nickel coating 3 has high stability in the air, and covering it on the first transition coating 2 can make the entire aluminum terminal 1 have a strong passivation ability, and can quickly form an extremely thin passivation film on the surface that can resist corrosion from the atmosphere, alkali and certain acids. The contact coating 4, as the outermost layer that needs to be frequently plugged in or rubbed, not only has good conductivity, but also has good wear resistance and aesthetics, which can greatly increase the service life and conductive efficiency of the aluminum terminal 1.

[0035] In the embodiment of FIG. 1 , the first transition plating layer 2 , the nickel plating layer 3 and the contact plating layer 4 all cover the entire outer surface of the aluminum terminal 1 , including the entire outer circumference and end surface of the aluminum terminal 1 .

[0036] In some embodiments, a second transition layer 5 is provided between the contact plating 4 and the nickel plating 3. As shown in FIG2 , after the aluminum terminal 1 is plated with the first transition layer 2 and the nickel plating 3, many gaps and holes still exist at the surface microscopic interface. These gaps and holes are still prone to wear and corrosion, and also easily make the contact plating 4 bonded loose. By providing a second transition layer 5 on the surface of the nickel plating 3 to smooth the surface of the nickel plating 3, the gaps and holes on the surface of the nickel plating 3 are filled, making the surface of the terminal flat and free of holes, and then plating the contact plating 4, the bonding will be more secure and flat, further extending the service life of the terminal.

[0037] In the embodiment of FIG. 2 , the first transition plating layer 2 , the nickel plating layer 3 , the contact plating layer 4 and the second transition plating layer 5 all cover the entire outer surface of the aluminum terminal 1 , including the entire outer circumference and end surface of the aluminum terminal 1 .

[0038] Furthermore, the electrode potential of the material of the second transition layer 5 is between that of nickel and that of the contact layer 4. Direct contact between metals with significantly different electrode potentials can result in electrochemical reactions. Under the influence of water and air, the metal with the lower electrode potential loses electrons, leading to metal corrosion and shortening the lifespan of the terminal. The connection between the nickel layer 3 and the contact layer 4 via the second transition layer 5 significantly reduces electrochemical reactions between the metals, reduces metal corrosion, and extends the lifespan of the terminal.

[0039] In some embodiments, the second transition layer 5 is made of one or more of gold, silver, nickel, tin, tin-lead alloy, zinc, and zinc alloy. These metals or alloys adhere more firmly to the nickel plating layer 3 and are more likely to fill surface gaps and holes.

[0040] In some embodiments, the electrode potential of the first transition layer 2 is between that of aluminum and nickel. As previously mentioned, direct contact between metals with significantly different electrode potentials can result in electrochemical reactions. Under the influence of water and air, the metal with the lower electrode potential loses electrons, leading to metal corrosion and shortening the lifespan of the terminal. The connection between the nickel coating 3 and the aluminum terminal 1 via the first transition layer 2 significantly reduces electrochemical reactions between the metals, minimizing metal corrosion and extending the terminal's lifespan.

[0041] In some embodiments, the first transition coating 2 is made of zinc or a zinc alloy. The inventors have concluded through experiments that applying zinc deposition to the first transition coating 2, i.e., using zinc or a zinc alloy, allows for excellent adhesion between the first transition coating 2 and the aluminum terminal 1, preventing the coating from detaching.

[0042] The thickness of the first transition coating 2 ranges from 0.015 μm to 2.5 μm. To determine the appropriate thickness of the first transition coating 2, the inventors conducted a salt spray test on aluminum terminals 1 having the first transition coating 2. The test involved applying zinc coatings of varying thicknesses to multiple aluminum terminals 1. Any coating damage or detachment during the salt spray test resulted in a failure. Table 1 shows the performance of zinc coatings of varying thicknesses in the salt spray test.

[0043] Table 1 Performance of zinc coatings of different thicknesses on multi-coated terminals in salt spray tests

[0044] As shown in Table 1, when the thickness of the zinc coating is less than 0.015 μm, the zinc coating will be damaged in the salt spray test, and when it is greater than 2.5 μm, it will fall off due to being too thick. Therefore, the inventors prefer that the thickness of the first transition coating 2 is 0.015 μm-2.5 μm.

[0045] In some embodiments, the contact plating layer 4 is made of one or a combination of gold, silver, hard silver, tin, tin-lead alloy, silver-antimony alloy, palladium, palladium-nickel alloy, graphite silver, graphene silver, and silver-gold-zirconium alloy. Using these materials as the contact plating layer 4 can provide the contact plating layer 4 with improved wear resistance and electrical conductivity.

[0046] In some embodiments, the aluminum terminal 1 is a flat terminal or one end of a solid aluminum conductor. The aluminum terminal 1 can be used in connection with a cable, or can be stamped from one end of a solid aluminum conductor such as an aluminum flat strip.

[0047] Furthermore, the aluminum terminal 1 has a connection hole 13, as shown in Figure 1. The surface of the connection hole 13 has a conductive, wear-resistant layer. Connection hole 13 can be a through hole or a threaded hole, used to connect the aluminum terminal 1 to a conductive member via bolts or other connectors. The inner wall of connection hole 13, as a metal contact subject to frequent friction, requires a highly wear-resistant metal as the conductive, wear-resistant layer to significantly extend its service life. Connection hole 13 also requires excellent electrical conductivity to meet the needs of power transmission.

[0048] Optionally, the connection hole 13 is provided between the two ends of the aluminum terminal 1. The connection hole 13 passes through the aluminum terminal 1, the first transition plating layer 2, the nickel plating layer 3, the contact plating layer 4, and the second transition plating layer 5 along the transverse direction of the aluminum terminal 1. The transverse direction is perpendicular to the axial direction of the aluminum terminal 1. When the cross-section of the aluminum terminal 1 is circular, the transverse direction may be the radial direction of the aluminum terminal 1; when the cross-section of the aluminum terminal 1 is square, the transverse direction may be the thickness direction of the aluminum terminal 1.

[0049] Furthermore, the conductive wear-resistant layer on the surface of connection hole 13 is made of one or a combination of gold, tin, tin-lead alloy, silver-antimony alloy, palladium, palladium-nickel alloy, graphite silver, graphene silver, and silver-gold-zirconium alloy. To demonstrate the impact of different conductive wear-resistant layer materials on the overall performance of connection hole 13, the inventors used aluminum terminal 1 samples with connection holes 13 of the same specifications and materials, but with different conductive wear-resistant layer materials, and conducted a series of screw connection times and corrosion resistance time tests using bolts of the same specifications. The experimental results are shown in Table 2.

[0050] The screw connection times in Table 2 were calculated by fixing multiple aluminum terminals 1 with different conductive wear-resistant layer materials on a test bench using the same bolts to simulate screw connection. After every 100 screw connections, the test was stopped to check for damage to the conductive wear-resistant layer on the surface of the connecting hole 13. If scratches appeared, exposing the material of the aluminum terminal 1, the test was stopped and the screw connection times at that time were recorded. In this example, a screw connection times of less than 8,000 was considered unqualified.

[0051] Table 2 Effects of different conductive wear-resistant layer materials on the connection holes of multi-plated terminals

[0052] The conductivity in Table 2 is measured after the aluminum terminal 1 is connected to a conductor and current is supplied. In this embodiment, a conductivity greater than 99% is considered acceptable.

[0053] As can be seen from Table 2, when the conductive wear-resistant layer is made of gold, tin, tin-lead alloy, silver-antimony alloy, palladium, palladium-nickel alloy, graphite silver, graphene silver, and silver-gold-zirconium alloy, the experimental results significantly exceed the standard values, and the performance is relatively stable. Therefore, the inventors selected the conductive wear-resistant layer on the connection hole 13 as one or a combination of gold, tin, tin-lead alloy, silver-antimony alloy, palladium, palladium-nickel alloy, graphite silver, graphene silver, and silver-gold-zirconium alloy.

[0054] In some embodiments, the thickness of the contact plating layer 4 ranges from 0.012 μm to 40 μm. To demonstrate the impact of varying the thickness of the contact plating layer 4 on the overall performance of the terminal, the inventors used aluminum terminals 1 of the same specifications, the same first transition plating layer 2 and nickel plating layer 3, and silver plating layers of varying thicknesses as the contact plating layer 4. Multiple samples were fabricated, each welded to the same aluminum conductor. The samples were subjected to a series of voltage drop and pull-out force tests. Tests with a voltage drop greater than 4 mV or a pull-out force less than 3000 N were considered unqualified. Table 3 shows the effects of varying silver plating thicknesses on voltage drop and pull-out force.

[0055] Table 3 Effect of different silver plating thickness on voltage drop and pull-out force of multi-plated terminals

[0056] As can be seen from Table 3, when the silver plating thickness is less than 0.012 μm, the pull-out force test is less than 3000 N, which is unqualified. When the silver plating thickness is greater than 40 μm, the voltage drop is greater than 4 mV, which is also unqualified. Therefore, the inventors prefer that the thickness of the contact plating layer 4 be 0.012 μm-40 μm. For example, it can be 1 μm, 5 μm, or 10 μm.

[0057] In some embodiments, the thickness of the nickel plating 3 is 0.012μm-15μm. The nickel plating 3 is easy to fall off from the first transition plating 2 if it is too thick or too thin. In order to find a suitable thickness of the nickel plating 3, the inventor conducted a salt spray test. A plurality of aluminum terminals 1 with a first transition plating 2 and a nickel plating 3 were placed in a salt spray test box. The thickness of the nickel plating 3 of each aluminum terminal 2 was different. Salt spray was sprayed on each position of all aluminum terminals 2. The surface nickel plating 3 was taken out for cleaning and observation every hour, which was a cycle. The test was stopped until the nickel plating 3 on the surface of a terminal fell off, and the number of cycles of the terminal at that time was recorded. In this embodiment, a cycle number less than 80 times was considered unqualified. The results are shown in Table 4.

[0058] Table 4 Performance of nickel plating of different thicknesses on multi-plated terminals in salt spray test

[0059] It can be seen from Table 4 that when the thickness of the nickel plating layer 3 is less than 0.012 μm or greater than 15 μm, it cannot meet the requirement of 80 cycles in the salt spray test. Therefore, the inventors prefer that the thickness of the nickel plating layer 3 is 0.012 μm-15 μm, which can make the nickel plating layer 3 more firmly bonded.

[0060] The present disclosure also provides a conductive structure, as shown in Figures 3 and 4, comprising a multi-plated terminal and a conductor 6 as described above. The aluminum terminal 1 and the conductor 6 are welded to form a weld 12, and a tin plating layer 121 is provided on the surface of the weld 12. After the weld 12 is formed, its surface has no plating and is easily corroded by moisture and impurities in the environment. Providing the tin plating layer 121 on the surface of the weld 12 can effectively improve the corrosion resistance and wear resistance of the weld 12.

[0061] In some embodiments, the thickness of the tin plating layer 121 is not less than 8 μm. In order to demonstrate the effect of different tin plating layer 121 thicknesses on corrosion resistance, the inventors used samples with the same specifications and materials, but with different tin plating layer 121 thicknesses on the weld 12, to conduct a corrosion resistance time test. The sample was placed in a salt spray test chamber, and salt spray was sprayed on various positions of the sample. The sample was taken out for cleaning and observation of surface corrosion every 20 hours, which was one cycle. When the surface corrosion area of ​​the weld 12 of the sample was greater than 10% of the total weld area, the test was stopped and the number of cycles at that time was recorded. In this embodiment, a cycle number less than 80 times was considered unqualified. The results are shown in Table 5.

[0062] Table 5 Performance of tin coatings of different thicknesses on conductive structures in salt spray tests

[0063] As can be seen from Table 5, when the thickness of the tin plating layer 121 is less than 8 μm, the number of cycles in the salt spray test is less than 80, which does not meet the requirements. Therefore, the inventors prefer that the thickness of the tin plating layer 121 is not less than 8 μm.

[0064] Optionally, the welded end faces of the aluminum terminal 1 and the conductor 6 are both beveled, and the width of the longitudinal cross-section of the weld 12 gradually decreases from one side of the aluminum terminal 1 toward the other side of the aluminum terminal 1. In the example of Figure 4, the width of the longitudinal cross-section of the weld 12 gradually decreases from top to bottom.

[0065] Optionally, the entire outer surface of the weld 12 is covered by the tin plating layer 121 .

[0066] Optionally, at least a portion of the tin plating layer 121 in the thickness direction is embedded in the contact plating layer 4. In other words, the tin plating layer 121 does not completely protrude from the outside of the contact plating layer 4. For example, the outer side surface of the tin plating layer 121 is flush with the outer side surface of the contact plating layer 4, or a portion of the tin plating layer 121 in the thickness direction protrudes from the outer side surface of the contact plating layer 4.

[0067] In some embodiments, as shown in FIG5 , the weld 12 is covered with an insulating protective layer 122. To further protect the weld 12 from corrosion and wear, the insulating protective layer 122 is preferably provided on the weld 12. The insulating protective layer 122 covers the tinned layer, which can isolate the weld 12 from air and water, reduce oxidation corrosion of the tinned layer, extend the service life, and greatly improve the safety performance.

[0068] Furthermore, the insulating protective layer 122 is made of a thermoplastic polymer material or a vulcanizable polymer material. Thermoplastic polymer materials can flow and deform when heated and maintain a certain shape after cooling, so they are easy to be molded by extrusion, injection or blow molding. The vulcanizable polymer material is preferably silicone rubber. Since silicone rubber has excellent heat resistance, cold resistance, dielectric properties, ozone resistance and atmospheric aging resistance, the outstanding performance of silicone rubber is that it has a wide operating temperature range and can be used for a long time at -60°C (or lower temperatures) to +250°C (or higher temperatures). Obviously, the above embodiments are only examples for clear explanation and are not limitations on the implementation methods. For ordinary technicians in the field, other different forms of changes or modifications can be made on the basis of the above description. It is not necessary and impossible to list all the implementation methods here. The obvious changes or modifications derived from this are still within the scope of protection of this disclosure.

Claims

1. A multi-plated terminal, characterized in that: Includes aluminum terminals and plating; The plating layer is disposed on at least a portion of the surface of the aluminum terminal; The plating layers include, from the inside to the outside, a first transition plating layer, a nickel plating layer and a contact plating layer.

2. A multi-plated terminal according to claim 1, characterized in that: A second transition plating layer is arranged between the contact plating layer and the nickel plating layer.

3. A multi-plated terminal according to claim 2, characterized in that: The electrode potential of the second transition coating material is between the electrode potentials of nickel and the contact coating material.

4. A multi-plated terminal according to claim 2, characterized in that: The material of the second transition plating layer is one or more combinations of gold, silver, nickel, tin, tin-lead alloy, zinc and zinc alloy.

5. The multi-plated terminal according to claim 1, characterized in that: The electrode potential of the first transition coating is between the electrode potentials of aluminum and nickel.

6. The multi-plated terminal according to claim 1, characterized in that: The material of the first transition coating is zinc or zinc alloy.

7. The multi-plated terminal according to claim 1, characterized in that: The thickness of the first transition coating is 0.015 μm-2.5 μm.

8. The multi-plated terminal according to claim 1, characterized in that: The material of the contact plating layer is one or a combination of gold, silver, hard silver, tin, tin-lead alloy, silver-antimony alloy, palladium, palladium-nickel alloy, graphite silver, graphene silver and silver-gold-zirconium alloy.

9. The multi-plated terminal according to claim 1, characterized in that: The aluminum terminal is a flat terminal or one end of a solid aluminum wire.

10. The multi-plated terminal according to claim 1, characterized in that: The aluminum terminal has a connection hole, and a surface of the connection hole has a conductive wear-resistant layer.

11. The multi-plated terminal according to claim 10, characterized in that: The conductive wear-resistant layer is made of one or a combination of gold, tin, tin-lead alloy, silver-antimony alloy, palladium, palladium-nickel alloy, graphite silver, graphene silver and silver-gold-zirconium alloy.

12. The multi-plated terminal according to claim 1, characterized in that: The thickness of the contact plating layer is 0.012 μm-40 μm.

13. The multi-plated terminal according to claim 1, characterized in that: The thickness of the nickel plating layer is 0.012 μm-15 μm.

14. The multi-plated terminal according to claim 1, characterized in that: The plating layer is arranged on the entire surface of the aluminum terminal.

15. A conductive structure, characterized in that: It comprises the aluminum terminal and the conductor as described in any one of claims 1 to 14, wherein the aluminum terminal and the conductor are welded to form a weld, and a tin plating layer is provided on the surface of the weld.

16. A conductive structure according to claim 15, characterized in that: The thickness of the tin plating layer is not less than 8 μm.

17. A conductive structure according to claim 15, characterized in that: The weld is covered with an insulating protective layer.

18. A conductive structure according to claim 17, characterized in that: The insulating protective layer is made of a thermoplastic polymer material or a vulcanizable polymer material.

19. A conductive structure according to claim 15, characterized in that: The welded end surfaces of the aluminum terminal and the conductor are both inclined surfaces, and the width of the longitudinal section of the weld gradually decreases from one side of the aluminum terminal to the other side of the aluminum terminal.

20. The conductive structure according to claim 15, characterized in that: At least a portion of the tin plating layer in a thickness direction is embedded in the contact plating layer of the aluminum terminal.

Citation Information

Patent Citations

  • Connector of copper terminal and aluminum wire

    CN108418001A

  • Novel aluminum terminal

    CN115799855A

  • Novel copper-aluminum composite terminal

    CN115954689A

  • A electroplate cladding material and terminal for handing electronic device interface terminal

    CN207632906U

  • Multi-plating terminal and conductive structure

    CN220474949U