Aluminum oxide film, method for producing same, and laminate
A dense and hard aluminum oxide film is used as a shielding layer between the substrate and epitaxial film to prevent defect transfer and impurity incorporation, addressing the issues of substrate defects and impurities, and enhancing the quality and performance of the epitaxial film for power semiconductors and MEMS applications.
Patent Information
- Application Number
- PCT/JP2024/016175
- Authority / Receiving Office
- WO · WO
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2023-04-27
- Filing Date
- 2024-04-24
- Publication Date
- 2024-10-31
AI Technical Summary
Conventional epitaxial film growth on substrates with crystal defects and impurities leads to defect transfer and impurity incorporation, resulting in poor film quality and performance.
A dense and hard aluminum oxide film with specific properties is interposed between the substrate and epitaxial film to act as a shielding layer, using an ion-assisted deposition method with controlled parameters to ensure low porosity, high Vickers hardness, and compressive stress, thereby preventing defect transfer and impurity incorporation.
The aluminum oxide film effectively shields the substrate defects and impurities, resulting in a high-quality epitaxial film with improved hardness, reduced porosity, and enhanced heat resistance, suitable for applications in power semiconductors and MEMS.
Smart Images

Figure JP2024016175_31102024_PF_FP_ABST
Abstract
Description
Aluminum oxide film, method for producing the same, and laminate
[0001] The present invention relates to an aluminum oxide film, a method for producing the same, and a laminate thereof.
[0002] 2. Description of the Related Art Conventionally, a laminate in which an epitaxial film (for example, a GaN film) is formed on a substrate such as a GaN substrate has been used, for example, as a part of a power semiconductor (see Patent Document 1).
[0003] Japanese Patent Application Publication No. 2021-020435
[0004] When forming an epitaxial film on a substrate by epitaxial growth, if the substrate has crystal defects, the crystal defects are likely to be transferred to the epitaxial film. Also, if the substrate contains impurities (such as moisture or oxygen), the impurities may also be mixed into the epitaxial film.
[0005] Therefore, the present inventors have investigated the possibility of providing an aluminum oxide film containing aluminum oxide between the substrate and the epitaxial film as a film with high shielding properties.
[0006] The present invention has been made in view of the above points, and an object of the present invention is to provide a novel aluminum oxide film.
[0007] As a result of extensive research, the present inventors have found that the above object can be achieved by employing the following configuration, and have thus completed the present invention. That is, the present invention provides the following [1] to
[24] . [1] An aluminum oxide film containing aluminum oxide, having a porosity of less than 0.5 vol %, and having a Vickers hardness of 1300 HV or more. [2] The aluminum oxide film according to [1] above, having a thickness of 0.1 μm or more. [3] The aluminum oxide film according to [1] or [2] above, having a thickness of 15 μm or less. [4] The aluminum oxide film according to any one of [1] to [3] above, having a thickness variation coefficient of 0.04 or less. [5] The number of hydrogen atoms is 10×10 20 pieces / cm 3[6] The aluminum oxide film according to any one of the above [1] to [4], having a compressive stress of 1 to 600 MPa. [7] The aluminum oxide film according to any one of the above [1] to [6], having an average secondary particle size of 100 nm or less. [8] The aluminum oxide film according to any one of the above [1] to [7], being an amorphous film. [9] The aluminum oxide film according to any one of the above [1] to [8], having a heat-resistant temperature of 500°C or higher.
[10] A laminate comprising a substrate and the aluminum oxide film according to any one of the above [1] to [9], in this order.
[11] The substrate is made of GaN, AlN, ZnO, SiC, LiTaO 3 , LiNbO 3 , PZT, Ga 2 O 3 The laminate according to
[10] above, which is composed of at least one selected from the group consisting of:
[12] The laminate according to
[10] or
[11] above, wherein the thickness of the substrate is 2.0 mm or less.
[13] The laminate according to any one of
[10] to
[12] above, wherein the substrate has a film-forming surface which is the surface on which the aluminum oxide film is to be disposed, and the surface roughness of the film-forming surface is 0.0005 μm or more and 0.2 μm or less in arithmetic mean roughness Ra.
[14] The laminate according to any one of
[10] to
[13] above, wherein the substrate has a film-forming surface which is the surface on which the aluminum oxide film is to be disposed, and the maximum length of the film-forming surface is 30 mm or more.
[15] The laminate according to any one of
[10] to
[14] above, which comprises one or more adhesion layers between the substrate and the aluminum oxide film.
[16] The laminate according to
[15] above, wherein the adhesion layer is an amorphous layer.
[17] The adhesion layer is made of SiO 2and SiC.
[18] The laminate according to any one of
[15] to
[17] above, wherein the adhesion layer has a thickness of 0.05 to 3.0 μm.
[19] The laminate according to any one of
[10] to
[18] above, wherein an epitaxial film is provided on the surface of the aluminum oxide film opposite to the substrate.
[20] The laminate according to any one of
[19] above, wherein the epitaxial film is a GaN film.
[21] The laminate according to any one of
[10] to
[20] above, which is a part of a power semiconductor, a piezoelectric element, or a MEMS.
[22] A method for producing the aluminum oxide film according to any one of [1] to [9] above, comprising evaporating an evaporation source to adhere to a substrate while irradiating the substrate with ions of at least one element selected from the group consisting of oxygen, argon, neon, krypton, and xenon in a vacuum, and 2 O 3
[23] A method for producing an aluminum oxide film according to
[22] above, wherein the temperature of the substrate when the evaporated evaporation source is attached is 270° C. or higher.
[24] A method for producing an aluminum oxide film according to
[22] or
[23] above, wherein the film formation rate of the aluminum oxide film is more than 15 nm / min and less than 80 nm / min.
[0008] According to the present invention, a novel aluminum oxide film can be provided.
[0009] Fig. 1 is a schematic diagram showing an example of a laminate, and Fig. 2 is a schematic diagram showing an apparatus used for producing an aluminum oxide film.
[0010] The meanings of terms used in the present invention are as follows: A numerical range expressed using "to" means a range that includes the numerical values before and after "to" as the lower and upper limits.
[0011] [Aluminum Oxide Film] The aluminum oxide film of this embodiment (hereinafter also referred to as "the present aluminum oxide film") contains aluminum oxide, has a porosity of less than 0.5% by volume, and has a Vickers hardness of 1300 HV or more.
[0012] For example, the present aluminum oxide film is provided on a substrate, and then an epitaxial film is formed on the aluminum oxide film (i.e., the epitaxial film is formed on the substrate via the aluminum oxide film). The present aluminum oxide film has a porosity and Vickers hardness within the above-mentioned ranges, making it very dense and hard. Therefore, even if the substrate has crystal defects or is contaminated with a large amount of impurities (such as moisture), the present aluminum oxide film functions as a highly shielding film, and it is expected that defects in the substrate will not easily transfer to the epitaxial film.
[0013] The present aluminum oxide film will be described in more detail below.
[0014] <Vickers Hardness> The Vickers hardness of the present aluminum oxide film is 1300 HV or more, preferably 1500 HV or more, more preferably 1700 HV or more, even more preferably 1900 HV or more, particularly preferably 2100 HV or more, and most preferably 2300 HV or more. On the other hand, the Vickers hardness of the present aluminum oxide film is, for example, 3500 HV or less, preferably 3000 HV or less.
[0015] In order to set the Vickers hardness within the above range, it is preferable to produce the aluminum oxide film by the method (the present production method) described below.
[0016] The Vickers hardness of the aluminum oxide film is determined in accordance with JIS Z 2244. More specifically, it is the Vickers hardness (HV0.005) determined when a test force of 0.049 N is applied using a micro Vickers hardness tester (HM-220, manufactured by Mitutoyo Corporation) with a diamond indenter having a facing angle of 136°.
[0017] <Porosity> The porosity of the present aluminum oxide film is less than 0.5% by volume, preferably 0.3% by volume or less, more preferably 0.2% by volume or less, and even more preferably 0.1% by volume or less.
[0018] In order to set the porosity within the above range, it is preferable to produce the aluminum oxide film by the method (the present production method) described below.
[0019] The porosity of an aluminum oxide film is determined as follows. First, a focused ion beam (FIB) is used to perform a slope process in the thickness direction from the surface of the aluminum oxide film toward the substrate, at an angle of 52°, on a portion of the aluminum oxide film and a portion of the substrate (described later), to expose a cross section. The exposed cross section is observed at a magnification of 20,000 times using a field emission scanning electron microscope (FE-SEM), and cross-sectional images are taken. Cross-sectional images are taken at multiple locations. Specifically, for example, when the aluminum oxide film and substrate are circular, images are taken at five points: one point at the center of the surface of the aluminum oxide film (or the surface of the substrate) and four points 10 mm away from the periphery, with the size of the cross-sectional image being 6 μm × 5 μm. When the thickness of the aluminum oxide film is 5 μm or more, cross-sectional images are taken at multiple locations so that the entire cross section of the aluminum oxide film can be observed in the thickness direction. The cross-sectional image obtained is then analyzed using image analysis software (ImageJ, manufactured by the National Institute of Health) to identify the area of the pores in the cross-sectional image. The ratio of the area of the pores to the total cross-sectional area of the aluminum oxide film is calculated, and this is regarded as the porosity (unit: volume %) of the aluminum oxide film. Note that the area of pores that are too small to be detected by the image analysis software (pores with a pore diameter of 20 nm or less) is regarded as 0.
[0020] <Composition> The aluminum oxide film is made of aluminum oxide (Al 2 O 3 The aluminum oxide film contains Al. 2 O 3 The content is preferably 95% by mass or more, more preferably 98% by mass or more, and even more preferably 100% by mass. The aluminum oxide film produced by the method (the present production method) described later is substantially Al 2 O 3 It consists only of Al 2 O 3 The content satisfies the above range.
[0021] <Thickness> The thickness of the present aluminum oxide film is, for example, 0.1 μm or more, preferably 0.3 μm or more, more preferably 0.8 μm or more, even more preferably 1.5 μm or more, even more preferably 3 μm or more, particularly preferably 4 μm or more, and most preferably 5 μm or more. On the other hand, the thickness of the present aluminum oxide film is, for example, 15 μm or less, preferably 10 μm or less, and more preferably 6 μm or less.
[0022] The thickness of the aluminum oxide film is measured as follows (the same applies to the thickness of the substrate and adhesive layer described below): A cross section of the aluminum oxide film is observed using a scanning electron microscope (SEM), the thickness of the aluminum oxide film is measured at any five points, and the average value of the five measured points is regarded as the thickness (unit: μm) of the aluminum oxide film.
[0023] <Coefficient of Thickness Variation> The coefficient of variation of the thickness of the present aluminum oxide film is preferably 0.04 or less, more preferably 0.03 or less, even more preferably 0.02 or less, even more preferably 0.01 or less, particularly preferably 0.005 or less, and most preferably 0.001 or less. As described above, the coefficient of variation of the thickness is determined by measuring the thickness at five points on the surface of the aluminum oxide film, and dividing the standard deviation σ of the five points by the average value μ of the five points (σ / μ). The five points are one point (point P) on the surface of the aluminum oxide film, two points on a concentric circle with a radius of 50 mm centered on point P, and two points on a concentric circle with a radius of 95 mm centered on point P. However, if the surface size of the aluminum oxide film is so small that concentric circles with radii of 50 mm and 95 mm centered on point P cannot be drawn, measurements are made at any five points on the surface of the aluminum oxide film.
[0024] <Number of Hydrogen Atoms> The number of hydrogen atoms in the present aluminum oxide film is preferably small. Specifically, the number of hydrogen atoms in the present aluminum oxide film (number of hydrogen atoms in the film) is 10×10 20 pieces / cm 3 Preferably, 6 x 10 20 pieces / cm 3 Less than 4×10 is more preferable. 20 pieces / cm 3 More preferably, 2×10 20pieces / cm 3 The following is particularly preferred: 1 x 10 20 pieces / cm 3 The following are most preferred:
[0025] It is highly likely that the hydrogen atoms in the aluminum oxide film are due to the influence of moisture contained in the substrate, which will be described later. In particular, the number of hydrogen atoms in the aluminum oxide film can be reduced by heating the substrate (pre-heating) before forming the aluminum oxide film. Other methods for reducing the number of hydrogen atoms in the aluminum oxide film will be described later.
[0026] The number of hydrogen atoms in the aluminum oxide film was measured using a secondary ion mass spectrometer (model IMS-6f, manufactured by Ametec Co., Ltd.) to measure the number of hydrogen atoms in the aluminum oxide film using the primary ion species Cs + The measurement is performed under the conditions of a primary acceleration voltage of 15.0 kV, a detection area of φ8 μm, and a measurement depth of 500 nm.
[0027] <Compressive Stress> The stress (internal stress, residual stress) of the present aluminum oxide film is preferably compressive stress rather than tensile stress. The compressive stress of the present aluminum oxide film is preferably 1 MPa or more, more preferably 5 MPa or more, even more preferably 10 MPa or more, even more preferably 30 MPa or more, particularly preferably 50 MPa or more, and most preferably 80 MPa or more. On the other hand, the compressive stress of the present aluminum oxide film is preferably 600 MPa or less, more preferably 550 MPa or less, even more preferably 450 MPa or less, even more preferably 350 MPa or less, particularly preferably 250 MPa or less, and most preferably 150 MPa or less. In other words, the compressive stress of the present aluminum oxide film is preferably 1 to 600 MPa.
[0028] The compressive stress of an aluminum oxide film is determined as follows: An aluminum oxide film is formed on a quartz glass substrate, and the surface shape of the formed aluminum oxide film is measured using a surface shape measuring device (Surfcom NEX 241 SD2-13, manufactured by Tokyo Seimitsu Co., Ltd.), and the compressive stress (film stress σ) of the aluminum oxide film is determined from Stoney's equation (the following equation): σ=Yd 2 / (6c(1-ν)t) In the above formula, σ is film stress, Y is Young's modulus of the substrate, d is thickness of the substrate, ν is Poisson's ratio of the substrate, t is thickness of the aluminum oxide film, and c is radius of curvature.
[0029] <Average secondary particle diameter> The smaller the average secondary particle diameter of an aluminum oxide film, the denser it can be said to be. Therefore, the average secondary particle diameter of the present aluminum oxide film is preferably 100 nm or less, more preferably 70 nm or less, even more preferably 50 nm or less, even more preferably 30 nm or less, particularly preferably 20 nm or less, and most preferably 10 nm or less. In order to set the average secondary particle diameter within the above range, it is preferable to slow down the film formation rate of the aluminum oxide film in the method (present production method) described below.
[0030] On the other hand, the lower limit of the average secondary particle size is not particularly limited, and is, for example, 1 nm, preferably 2 nm, and more preferably 3 nm.
[0031] The aluminum oxide film is observed at a magnification of 100,000 times using a scanning electron microscope (SEM) to obtain a surface SEM photograph of the aluminum oxide film. Aggregates visible in the obtained surface SEM photograph are defined as "secondary particles," and the circle-equivalent diameter of each secondary particle is determined as the "secondary particle diameter." The average value of the secondary particle diameters in one field of view is determined as the "average secondary particle diameter."
[0032] <Crystallization> The present aluminum oxide film is preferably one in which crystallization is suppressed (i.e., an amorphous film). When an XRD (X-ray diffraction) measurement is performed on a test specimen in which an aluminum oxide film is formed on a substrate, and only the crystalline peaks of the material constituting the substrate are confirmed, the aluminum oxide film is considered to be one in which crystallization is suppressed and is an amorphous film.
[0033] The XRD pattern was obtained by XRD measurement in a micro-area 2D (two-dimensional) mode using an X-ray diffractometer (D8 DISCOVER Plus, manufactured by Bruker) under the following conditions: X-ray source: CuKα radiation (output: 45 kV, current: 120 mA) Scanning range: 2θ = 10° to 80° Step time: 0.2 s / step Scan speed: 10° / min Step width: 0.02° Detector: EIGER multimode detector (2D mode) Incident optical system: multilayer mirror + 1.0 mmφ microslit + 1.0 mmφ collimator Receiving optical system: OPEN
[0034] <Heat Resistance Temperature> The heat resistance temperature of the present aluminum oxide film is preferably 500°C or higher, more preferably 600°C or higher, even more preferably 700°C or higher, and particularly preferably 800°C or higher.
[0035] In order to set the heat resistance temperature within the above range, it is preferable to produce the aluminum oxide film by the method (the present production method) described below.
[0036] The heat resistance temperature of an aluminum oxide film is determined by conducting the following test (heat resistance test). First, a sample of a laminate having an aluminum oxide film is heated in an air-sintering furnace at a heating rate of 300°C / hr, heated at an arbitrary temperature T1 for 1 hour, and cooled at 50°C / hr before being removed. An optical microscope is then used to check for the presence or absence of cracks in the aluminum oxide film. This heat resistance test is conducted at temperatures T1 (in 50°C increments) from 100°C to 800°C, and the highest temperature T1 at which cracks do not occur is defined as the heat resistance temperature of the aluminum oxide film.
[0037] [Laminate] Fig. 1 is a schematic diagram showing an example of a laminate 1. The laminate 1 has a substrate 2 and an aluminum oxide film 4. As shown in Fig. 1, an adhesion layer 3 may be disposed between the substrate 2 and the aluminum oxide film 4. Furthermore, an epitaxial film 5 may be disposed on the surface of the aluminum oxide film 4 opposite to the substrate 2.
[0038] The laminate of this embodiment (hereinafter also referred to as "the present laminate") has the present aluminum oxide film as the aluminum oxide film. That is, the laminate of this embodiment includes a substrate and the above-mentioned aluminum oxide film in this order. Each component of the present laminate will be described in detail below.
[0039] <Substrate> The substrate has at least a surface on which an aluminum oxide film (or an adhesion layer, which will be described later) is formed. Hereinafter, this surface may be referred to as the "film formation surface" for convenience. In the laminate, the aluminum oxide film is disposed on the film formation surface side of the substrate.
[0040] The material of the substrate is appropriately selected depending on the application of the laminate. For example, the substrate may be made of GaN, AlN, ZnO, SiC, or LiTaO. 3 , LiNbO 3 , PZT, Ga 2 O 3 PZT is made of at least one material selected from the group consisting of lead zirconate titanate Pb(Zr,Ti)O 3 Refers to...
[0041] <<Shape>> The shape of the substrate is not particularly limited and may be, for example, a flat plate, a ring, a dome, a concave or a convex shape, and is appropriately selected depending on the use of the laminate, etc.
[0042] <<Thickness>> The thickness of the substrate is appropriately selected depending on the application of the laminate, etc. The thickness of the substrate is, for example, 2.0 mm or less, preferably 1.2 mm or less, more preferably 1.0 mm or less, even more preferably 0.8 mm or less, particularly preferably 0.6 mm or less, and most preferably 0.4 mm or less. The lower limit of the thickness of the substrate is not particularly limited, and is, for example, 0.1 mm, preferably 0.2 mm.
[0043] <<Surface Roughness of Film-Depositing Surface>> If the surface roughness (arithmetic mean roughness Ra) of the substrate film-depositing surface is too large, collisions between growing particles occur during the growth of the aluminum oxide film, and localized concentration of film stress may cause cracks to form in the resulting aluminum oxide film, resulting in a decrease in hardness. Therefore, the surface roughness (arithmetic mean roughness Ra) of the substrate film-depositing surface is preferably 0.2 μm or less, more preferably 0.1 μm or less, even more preferably 0.05 μm or less, particularly preferably 0.01 μm or less, and most preferably 0.005 μm or less, because this makes it easier to obtain a hard aluminum oxide film.
[0044] On the other hand, the surface roughness (arithmetic mean roughness Ra) of the substrate's film-forming surface is preferably 0.0005 μm or more, more preferably 0.001 μm or more, even more preferably 0.002 μm or more, particularly preferably 0.003 μm or more, and most preferably 0.004 μm or more. That is, the substrate has a film-forming surface, which is the surface on which the aluminum oxide film is disposed, and the surface roughness of the film-forming surface, in terms of arithmetic mean roughness Ra, is preferably 0.0005 μm or more and 0.2 μm or less. The surface roughness (arithmetic mean roughness Ra) of the film-forming surface is measured in accordance with JIS B 0601:2001.
[0045] <<Maximum Length of Film Formation Surface>> The maximum length of the film formation surface of the substrate is preferably 30 mm or more, more preferably 100 mm or more, even more preferably 200 mm or more, even more preferably 300 mm or more, particularly preferably 500 mm or more, very preferably 800 mm or more, and most preferably 1000 mm or more. Note that "maximum length" refers to the maximum length of the film formation surface. Specifically, for example, if the film formation surface is circular in plan view, it is its diameter; if it is ring in plan view, it is its outer diameter; and if it is rectangular in plan view, it is the length of the largest diagonal. On the other hand, the maximum length of the film formation surface is, for example, 2000 mm or less, preferably 1500 mm or less. That is, the substrate has a film formation surface, which is the surface on which the aluminum oxide film is disposed, and the maximum length of the film formation surface is preferably 30 mm or more.
[0046] <Adhesion Layer> As described above, one or more adhesion layers may be provided between the substrate and the aluminum oxide film. By forming the adhesion layer, the tensile stress of the aluminum oxide film is alleviated to generate compressive stress, and the adhesion of the aluminum oxide film to the substrate is increased.
[0047] The upper limit of the number of adhesive layers is not particularly limited, but is preferably 5 layers or less, more preferably 4 layers or less, even more preferably 3 layers or less, particularly preferably 2 layers or less, and most preferably 1 layer.
[0048] The adhesion layer is preferably an amorphous layer. When an XRD (X-ray diffraction) measurement is performed on a test specimen having an adhesion layer formed on a substrate, and only a crystalline peak of the material constituting the substrate is confirmed, the adhesion layer is considered to be an amorphous layer.
[0049] The adhesive layer is SiO 2 and SiC. 2 The content of SiO and / or SiC is preferably 95 mass % or more, more preferably 98 mass % or more, and even more preferably 100 mass %. 2 and / or consists solely of SiC, the content of which satisfies the above range.
[0050] The thickness of the adhesive layer is preferably 0.05 μm or more, more preferably 0.5 μm or more, even more preferably 0.9 μm or more, and particularly preferably 1.0 μm or more. On the other hand, the thickness of the adhesive layer is preferably 3.0 μm or less, more preferably 2.0 μm or less, even more preferably 1.5 μm or less, and particularly preferably 1.3 μm or less. That is, the thickness of the adhesive layer is preferably 0.05 to 3.0 μm.
[0051] <Epitaxial Film> The laminate of this embodiment may include an epitaxial film on the surface of the aluminum oxide film opposite to the substrate. The epitaxial film is a film formed by epitaxial growth on the film formation surface of the substrate via an aluminum oxide film (or an adhesion layer and an aluminum oxide film). Specific examples of epitaxial films include films obtained by epitaxially growing nitride semiconductors such as AlN, GaN, and InN. For convenience, an epitaxial film obtained by epitaxially growing GaN is called a "GaN film." The epitaxial film is preferably a GaN film.
[0052] <Applications of Laminate> The laminate is used, for example, as a part of a power semiconductor, a piezoelectric element, or a MEMS (Micro Electro Mechanical Systems), although the applications are not limited thereto.
[0053] [Method for producing aluminum oxide film and laminate] Next, a method for producing the aluminum oxide film of this embodiment (hereinafter also referred to as "this production method") will be described. This production method is a method for producing the above-mentioned aluminum oxide film, and includes irradiating a substrate with ions of at least one element selected from the group consisting of oxygen, argon, neon, krypton, and xenon in a vacuum while evaporating an evaporation source to adhere to the substrate. 2 O 3 This production method is also a method for producing the present laminate described above.
[0054] This manufacturing method is a so-called ion-assisted deposition (IAD) method. Schematically, in a vacuum, an evaporation source (Al 2 O 3 ) is evaporated and deposited on the substrate, 2 O 3 According to this manufacturing method, it is possible to form an extremely dense and hard aluminum oxide film.
[0055] Incidentally, the thicker the aluminum oxide film, the more likely it is to crack. Furthermore, as the area of the deposition surface increases, the area of the aluminum oxide film formed on that deposition surface also increases. In this case, the aluminum oxide film is also prone to cracking. However, the aluminum oxide film obtained by this manufacturing method is very dense and hard, and when an adhesive layer is formed, the tensile stress is alleviated. Therefore, even if the aluminum oxide film is thicker or has a larger area, it is less likely to crack.
[0056] Furthermore, the surface roughness (arithmetic mean roughness Ra) of the substrate surface on which the film is to be formed is preferably in the above-mentioned range, so that the aluminum oxide film formed is denser and harder, and less susceptible to cracking.
[0057] It should be noted that methods such as ALD (Atomic Layer Deposition) tend to result in an aluminum oxide film with insufficient hardness.
[0058] <Apparatus Configuration> This manufacturing method will be described in more detail with reference to FIG. 2 . FIG. 2 is a schematic diagram showing an apparatus used to manufacture an aluminum oxide film. The apparatus shown in FIG. 2 includes a chamber 11. The interior of the chamber 11 can be evacuated by driving a vacuum pump (not shown). Inside the chamber 11, crucibles 12 and 13 and an ion gun 14 are disposed, and a holder 17 is disposed above these. The holder 17 is integrated with a support shaft 16 and rotates with the rotation of the support shaft 16. A heater 15 is disposed around the holder 17. The holder 17 holds the substrate 2 described above with its film-forming surface facing downward. The substrate 2 held by the holder 17 rotates with the rotation of the holder 17 while being heated by the heater 15. Furthermore, quartz-crystal film thickness monitors 18 and 19 are attached to the chamber 11.
[0059] <Formation of Aluminum Oxide Film> A case where an aluminum oxide film (not shown in FIG. 2) is formed on a substrate 2 in the apparatus shown in FIG. 2 will be described. First, an evaporation source Al is placed in one or both of the crucibles 12 and 13. 2 O3 After the substrate 2 is held by the holder 17, the inside of the chamber 11 is evacuated to a vacuum. Next, the heater 15 is driven while the holder 17 is rotated. This causes the substrate 2 to rotate while being heated. In this state, ion-assisted deposition is performed to form a film on the substrate 2. That is, while ions (ion beam) are irradiated from the ion gun 14, the evaporation source Al filled in one or both of the crucibles 12 and 13 is evaporated. 2 O 3 The evaporation source is melted and evaporated by irradiating it with an electron beam (not shown). In this way, the evaporated evaporation source adheres to the film formation surface of the substrate 2, and an aluminum oxide film is formed.
[0060] <Pressure in the Chamber> Film formation is performed in a vacuum. Specifically, the pressure reached in the chamber 11 at the start of film formation is 1×10 -4 Pa (0.01 × 10 -2 Pa) or less, and 2 × 10 -5 Pa (0.002×10 -2 The pressure inside the chamber 11 during film formation is preferably 6×10 Pa or less. -2 Pa or less is preferable, and 5 × 10 -2 Pa or less is more preferable, and 3×10 -2 On the other hand, from the viewpoint of mass productivity, the ultimate pressure inside the chamber 11 at the start of film formation is preferably 1×10 Pa or less. -6 Pa (0.0001×10 -2 Pa) or more, and 1 × 10 -5 Pa (0.001×10 -2 Pa) or more is more preferable.
[0061] <<Substrate Temperature>> The temperature of the substrate 2 during film formation (the temperature of the substrate 2 when the evaporated evaporation source is attached) is preferably 200° C. or higher, more preferably 250° C. or higher, even more preferably 270° C. or higher, even more preferably 320° C. or higher, particularly preferably 370° C. or higher, and most preferably 400° C. or higher. On the other hand, this temperature is preferably 600° C. or lower, more preferably 500° C. or lower, and even more preferably 450° C. or lower.
[0062] <<Film Formation Rate>> The rate at which the evaporation sources in the crucibles 12 and 13 evaporate and an aluminum oxide film is formed (film formation rate) is monitored using quartz film thickness monitors 18 and 19. The film formation rate is adjusted by controlling the conditions of the electron beam irradiated onto the evaporation sources and the conditions of the ion beam from the ion gun 14 (current value, current density, etc.). During the formation of the aluminum oxide film, the film formation rate (unit: nm / min) of each evaporation source is adjusted to a desired value.
[0063] The deposition rate of the aluminum oxide film is preferably less than 80 nm / min, more preferably 70 nm / min or less, even more preferably 50 nm / min or less, particularly preferably 30 nm / min or less, and most preferably 20 nm / min or less, because a dense aluminum oxide film is easily obtained. Note that a slower deposition rate makes it easier to suppress crystallization of the resulting aluminum oxide film (making it easier to obtain an amorphous film). On the other hand, the deposition rate of the aluminum oxide film is preferably more than 15 nm / min, more preferably 16 nm / min or more, and even more preferably 17 nm / min or more, because a dense aluminum oxide film is easily obtained. That is, the deposition rate of the aluminum oxide film is preferably more than 15 nm / min and less than 80 nm / min.
[0064] <Ion Irradiation Conditions> A gas (e.g., oxygen gas) is supplied to the ion gun 14. The ion gun 14 ionizes the supplied gas and emits ions (an ion beam). The ions emitted from the ion gun 14 are irradiated onto the evaporated evaporation source, the film formation surface of the substrate 2, and the like.
[0065] The flow rate of the gas supplied to the ion gun 14 is preferably 1 sccm or more, more preferably 1.5 sccm or more, and even more preferably 3 sccm or more. On the other hand, the flow rate of the gas supplied to the ion gun 14 is preferably 80 sccm or less, more preferably 70 sccm or less, and even more preferably 60 sccm or less.
[0066] The ions emitted from the ion gun 14 are preferably ions of at least one element selected from the group consisting of oxygen, argon, neon, krypton, and xenon, more preferably ions of at least two elements selected from the group consisting of oxygen, argon, neon, krypton, and xenon, and even more preferably a combination of oxygen and argon ions.
[0067] For example, when oxygen and argon ions are to be emitted from the ion gun 14, argon gas (Ar) and oxygen gas (O 2 At this time, argon gas (Ar) and oxygen gas (O 2 ) and the flow rate ratio (Ar / O 2 ) (volume ratio) is preferably 1 / 50 or more, more preferably 1.5 / 50 or more, and even more preferably 2 / 50 or more. 2 ) is preferably 4 / 50 or less, more preferably 3.5 / 50 or less, and even more preferably 3 / 50 or less.
[0068] This increases the hardness of the aluminum oxide film that is formed. The reason for this is not clear, but it is presumed that the strength with which the evaporated evaporation source is implanted into the substrate 2 is greater when argon (Ar), which has high kinetic energy, is used in combination with oxygen (O) ions than when oxygen (O) ions alone are used.
[0069] The distance between the ion gun 14 and the substrate 2 is preferably 700 mm or more, more preferably 900 mm or more. On the other hand, this distance is preferably 1500 mm or less, more preferably 1300 mm or less. The current value of the ion beam is preferably 1000 mA or more, more preferably 1500 mA or more. On the other hand, the current value of the ion beam is preferably 3000 mA or less, more preferably 2500 mA or less.
[0070] The ion beam current density is set to 40 μA / cm because the resulting aluminum oxide film becomes harder. 2 More than 65 μA / cm is preferable. 2 More preferably, 75 μA / cm 2 More preferably, 77 μA / cm 2On the other hand, the ion beam current density is preferably 140 μA / cm 2 Preferably, 120 μA / cm or less 2 More preferably, 100 μA / cm or less 2 The following is even more preferred:
[0071] <<Preheating of the substrate>> The moisture contained in the substrate is unlikely to be incorporated into the aluminum oxide film. 2 O 3 is attached to the film-forming surface of the substrate (i.e., before forming an aluminum oxide film), the substrate is preferably heated (preheated) at a high temperature. The preheating temperature is preferably 300°C or higher, more preferably 400°C or higher, even more preferably 450°C or higher, and particularly preferably 500°C or higher. On the other hand, the preheating temperature is, for example, 800°C or lower, preferably 750°C or lower, and more preferably 700°C or lower.
[0072] The preheating time is preferably 60 minutes or more, more preferably 120 minutes or more, even more preferably 240 minutes or more, and particularly preferably 480 minutes or more, while the preheating time is preferably 1200 minutes or less, more preferably 1000 minutes or less, even more preferably 800 minutes or less, and particularly preferably 600 minutes or less.
[0073] The pre-heating atmosphere is, for example, the air atmosphere.
[0074] <Formation of Adhesion Layer> Before forming the aluminum oxide film, it is preferable to form the above-mentioned adhesion layer (not shown in FIG. 2 ) on the film-forming surface of the substrate 2. This covers at least the film-forming surface of the substrate, making it difficult for moisture contained in the substrate to be absorbed into the aluminum oxide film that is formed.
[0075] The adhesion layer is formed by ion-assisted deposition in the same manner as the aluminum oxide film. 2 When forming an adhesive layer made of 2The evaporation source is evaporated while irradiating ions (ion beam) from the ion gun 14, and is adhered to the film formation surface of the substrate 2. The conditions for forming the adhesion layer are the same as those for forming the aluminum oxide film.
[0076] SiO 2 When forming an adhesion layer made of silicon carbide, the ions emitted from the ion gun 14 may be, for example, oxygen ions. On the other hand, when forming an adhesion layer made of silicon carbide, the ions emitted from the ion gun 14 are preferably ions of an element other than oxygen (for example, argon).
[0077] <Formation of Epitaxial Film> The epitaxial film is a film (e.g., a GaN film) formed by epitaxial growth on an aluminum oxide film. After the aluminum oxide film (or an adhesion layer and an aluminum oxide film) is formed on the film formation surface of the substrate 2, it is removed from the chamber 11 and epitaxial growth is carried out separately. The epitaxial growth method is not particularly limited, and a conventionally known method such as MOCVD (Metal Organic Chemical Vapor Deposition) can be appropriately adopted.
[0078] The present invention will be specifically described below with reference to examples. However, the present invention is not limited to the examples described below. Examples 1 to 33 are examples, and Examples 34 to 37 are comparative examples.
[0079] Examples 1 to 36 Using the apparatus described with reference to FIG. 2 , an aluminum oxide film (or an adhesion layer and an aluminum oxide film) was formed on the deposition surface of a substrate by the IAD method under the conditions shown in Table 1 below. All of the formed adhesion layers were amorphous. When no adhesion layer was formed, a "-" was entered in the "Adhesion Layer" column in Table 1 below. A circular substrate (thickness: 0.5 mm) having a deposition surface with a maximum length (diameter) shown in Table 1 below was used as the substrate. This substrate was preheated in an air atmosphere while held in a holder in a chamber. The preheating temperature was 550°C, and the preheating time was 600 minutes. Other manufacturing conditions not listed in Table 1 below included a distance between the ion gun and the substrate of 1100 mm, and an ion beam current of 2000 mA. Note that the term "base material" in Table 1 is synonymous with "substrate."
[0080] Example 37: An aluminum oxide film was formed on the deposition surface of a substrate by ALD instead of IAD. In this case, "-" is entered in the "Manufacturing conditions" column in Table 1 below.
[0081] <Physical Properties of Aluminum Oxide Film> The formed aluminum oxide film was measured for Vickers hardness, porosity, thickness, thickness variation coefficient, number of hydrogen atoms, compressive stress, average secondary particle size, and heat resistance temperature using the methods described above. The results are shown in Table 1 below. When no measurement was performed, a "-" is entered in the corresponding field. Note that the compressive stress value is entered as a negative number.
[0082] Regarding the formed aluminum oxide film, if no crystallization was observed and it was an amorphous film, it was recorded as "absent," and if crystallization was observed, it was recorded as "present" in the "Crystallization" column in Table 1 below.
[0083] Furthermore, the surface roughness (arithmetic mean roughness Ra) of the formed aluminum oxide film (surface opposite to the substrate) was measured, and this is shown in the "Ra after film formation" column in Table 1. The surface roughness (arithmetic mean roughness Ra) of the aluminum oxide film surface was also measured in accordance with JIS B 0601:2001, similar to the film-formed surface of the substrate.
[0084] <Appearance> The appearance of the formed aluminum oxide film was visually inspected to check for the presence or absence of cracks (including wrinkles; the same applies below). If a crack of 1.0 mm or more was found, it was marked with "X", and if a crack of less than 1.0 mm or no crack was found, it was marked with "O", as shown in Table 1 below. If it was marked with "O", it could be evaluated as having excellent appearance.
[0085]
[0086]
[0087]
[0088]
[0089] <Summary of Evaluation Results> As shown in Table 1 above, the aluminum oxide films of Examples 1 to 33 had a porosity of less than 0.5% by volume and a Vickers hardness of 1,300 HV or more. Comparing Examples 1 to 30 and Examples 32 to 33 with Example 31, the aluminum oxide films obtained in Examples 1 to 30 and Examples 32 to 33, which were irradiated with argon and oxygen ions from the ion gun, had higher Vickers hardness values than Example 31, which was irradiated with only oxygen ions.
[0090] In Example 34 (an example in which the Ra of the substrate surface on which the film was formed was greater than in Examples 1 to 33), the Vickers hardness of the aluminum oxide film was less than 1300 HV. In Example 35 (an example in which the film formation rate was faster than in Examples 1 to 33), the porosity of the aluminum oxide film was 0.5 vol% or more. In Example 36 (an example in which the film formation rate was slower than in Examples 1 to 33), the porosity of the aluminum oxide film was 0.5 vol% or more. In Example 37 (an example in which the ALD method was used), the Vickers hardness of the aluminum oxide film was less than 1300 HV.
[0091] According to the present invention, a novel aluminum oxide film can be provided.
[0092] Although the present invention has been described in detail and with reference to specific embodiments, it will be apparent to those skilled in the art that various changes and modifications can be made without departing from the spirit and scope of the present invention. This application is based on a Japanese patent application (Patent Application No. 2023-072873) filed on April 27, 2023, the contents of which are incorporated herein by reference.
[0093] 1: Laminate 2: Substrate 3: Adhesion layer 4: Aluminum oxide film 5: Epitaxial film 11: Chamber 12, 13: Crucible 14: Ion gun 15: Heater 16: Support shaft 17: Holder 18, 19: Quartz film thickness monitor
Claims
1. An aluminum oxide film containing aluminum oxide, having a porosity of less than 0.5 volume percent, and having a Vickers hardness of 1,300 HV or more.
2. The aluminum oxide film according to claim 1, having a thickness of 0.1 μm or more.
3. The aluminum oxide film according to claim 1, having a thickness of 15 μm or less.
4. The aluminum oxide film according to claim 1, having a thickness variation coefficient of 0.04 or less.
5. The number of hydrogen atoms is 10 x 10 20 pieces / cm 3 2. The aluminum oxide film according to claim 1, wherein:
6. The aluminum oxide film according to claim 1, having a compressive stress of 1 to 600 MPa.
7. The aluminum oxide film according to claim 1, having an average secondary particle size of 100 nm or less.
8. The aluminum oxide film according to claim 1, which is an amorphous film.
9. The aluminum oxide film according to claim 1, having a heat-resistant temperature of 500° C. or higher.
10. A laminate comprising, in this order, a substrate and the aluminum oxide film according to any one of claims 1 to 9.
11. The substrate is made of GaN, AlN, ZnO, SiC, LiTaO 3 , LiNbO 3 , PZT, Ga 2 O 3 The laminate according to claim 10, which is composed of at least one selected from the group consisting of:
12. The laminate according to claim 10, wherein the thickness of the substrate is 2.0 mm or less.
13. The laminate according to claim 10, wherein the substrate has a film-forming surface which is the surface on which the aluminum oxide film is disposed, and the surface roughness of the film-forming surface is, in arithmetic mean roughness Ra, 0.0005 μm or more and 0.2 μm or less.
14. The laminate according to claim 10, wherein the substrate has a film-forming surface which is the surface on which the aluminum oxide film is disposed, and the maximum length of the film-forming surface is 30 mm or more.
15. The laminate according to claim 10, further comprising one or more adhesion layers between the substrate and the aluminum oxide film.
16. The laminate according to claim 15, wherein the adhesion layer is an amorphous layer.
17. The adhesion layer is made of SiO 2 The laminate according to claim 15, comprising at least one selected from the group consisting of SiC and SiC.
18. The laminate according to claim 15, wherein the adhesive layer has a thickness of 0.05 to 3.0 μm.
19. The laminate according to claim 10, further comprising an epitaxial film on a surface of the aluminum oxide film opposite to the substrate.
20. The stack of claim 19, wherein the epitaxial film is a GaN film.
21. The laminate according to claim 10, which is part of a power semiconductor, a piezoelectric element or a MEMS.
22. A method for producing an aluminum oxide film according to any one of claims 1 to 9, comprising irradiating a substrate with ions of at least one element selected from the group consisting of oxygen, argon, neon, krypton and xenon in a vacuum while evaporating an evaporation source to adhere to the substrate, and using Al as the evaporation source. 2 O 3 A method for producing an aluminum oxide film using the above method.
23. The method for producing an aluminum oxide film according to claim 22, wherein the temperature of the substrate when the evaporated evaporation source is attached is 270° C. or higher.
24. The method for producing an aluminum oxide film according to claim 22, wherein the deposition rate of the aluminum oxide film is more than 15 nm / min and less than 80 nm / min.
Citation Information
Patent Citations
Electrophotographic sensitive body
JP1990208660A
Formation of thin hard alumina film
JP1992099862A
Multilayer coating with diffusion barrier layer and erosion prevention layer - Patent Application 20070122997
JP2019522104A