Preparation method for and application of crack-resistant nickel-based high-temperature alloy powder

Mixing nickel-based high-temperature alloy powder with carbide powder through a high-speed coulter mixer solves the problems of cracks and element burnout during laser forming of nickel-based high-temperature alloy, achieving precise regulation of alloy elements and crack elimination, and improving alloy mechanical properties and applicability of the processing process.

WO2024234436A1PCT designated stage expired Publication Date: 2024-11-21CHINA MASCH INST OF ADVANCED MATERIALS (ZHENGZHOU) CO LTD
View PDF 5 Cites 0 Cited by

Patent Information

Application Number
PCT/CN2023/100897
Authority / Receiving Office
WO · WO
Patent Type
Applications
Current Assignee / Owner
Priority Date
2023-05-17
Filing Date
2023-06-17
Publication Date
2024-11-21

AI Technical Summary

Technical Problem

During the laser forming process of nickel-based high-temperature alloys, crack problems are prone to occur. The prior art has problems of elemental burnout and impurities introduction when adjusting alloy composition or using ball milling processes, making it difficult to accurately regulate the alloy element content and uniform distribution.

Method used

Use a high-speed coulter mixer to mix nickel-based high-temperature alloy powder with carbide powder in a specific proportion to avoid high-temperature smelting, ensure uniform distribution of carbide fine crystal agent, and use it to induce ultrafine crystal structure generation during additive manufacturing to eliminate heat and the fine crystal carbide content is regulated during laser forming.

Benefits of technology

The precise component regulation of nickel-based high-temperature alloy powder is achieved, which avoids elemental burning and impurities introduction, significantly reduces the occurrence of cracks, improves the mechanical properties of the alloy and the simplicity of the processing process, and is suitable for large-scale industrial production.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN2023100897_21112024_PF_FP_ABST
    Figure CN2023100897_21112024_PF_FP_ABST
Patent Text Reader

Abstract

A preparation method for a crack-resistant nickel-based high-temperature alloy powder. The method comprises: loading into a high-speed coulter mixer and mixing a nickel-based high-temperature alloy powder and a carbide powder according to a mass ratio of 98.5-99.5 to 0.5-1.5; running the high-speed coulter mixer for 4-8 minutes and then stopping for 25-60 minutes, repeating 2-4 times, and obtaining a crack-resistant nickel-based high-temperature alloy powder; the blades of the high-speed coulter mixer rotating at 1000-3000 r / min.
Need to check novelty before this filing date? Find Prior Art

Description

Preparation method and application of crack-resistant nickel-based high-temperature alloy powder Technical Field

[0001] The present invention relates to the field of powder metallurgy, and in particular to a preparation method of crack-resistant nickel-based high-temperature alloy powder and applications thereof. Background Art

[0002] Nickel-based high-temperature alloys are widely used in structural or engineering applications due to their excellent mechanical properties and oxidation resistance at high temperatures, such as low-pressure turbines and combustion chambers in the hot end components of aircraft engines. However, due to their high hardness and high strength, high-temperature alloys are difficult to process using traditional casting, forging and welding methods.

[0003] Laser forming technology, such as selective laser melting (SLM), is an advanced manufacturing technology based on metal powder processing and is used to prepare complex structural components. This technology offers significant design flexibility and facilitates the customization of high-performance products. However, the laser forming process generates a high-temperature molten pool, which is subject to high thermal gradients, high cooling rates, and complex thermal cycles during solidification. The steep thermal gradient within the high-temperature molten pool leads to epitaxial grain growth, resulting in coarse columnar grains and strong texture orientation, ultimately resulting in anisotropic mechanical properties of the processed component. During laser deposition, the uneven heat distribution and high cooling rates within the build zone lead to high internal stresses. The interweaving of thermal stress and coarse columnar crystals can easily cause cracks in high-strength nickel-based superalloy materials.

[0004] In the existing technology, the problem of thermal cracking during the laser forming of nickel-based alloys is solved by adjusting the alloy composition during the smelting process, for example, increasing the proportion of solid solution strengthening and precipitation strengthening alloying elements, such as patent document CN202110345498.5 A crack-free nickel-based high-temperature alloy and its composition design method and preparation method, which increases the content of solid solution elements in GH3536 alloy and modifies the GH3536 alloy, and makes fuller use of the rapid solidification effect of laser selective melting forming technology, which can significantly improve the strength of GH3536 alloy and overcome the microcrack defects of traditional nickel-based high-temperature alloys in the laser selective melting forming process; however, in the process of forming the mixed alloy powder by laser selective melting, element burnout adds uncertainty to the results.

[0005] The ball milling process is also widely used in the field of alloy powder processing. For example, CN201911326194.3 discloses a composite powder for laser cladding and its preparation method. Nano-scale carbide cobalt powder is evenly coated on the surface of micron-scale low-carbon steel or nickel-based alloy spherical powder by ball milling. However, the ball milling process will cause powder work hardening, and impurities peeled off from the ball milling mixing balls will be introduced into the alloy powder produced. Technical issues

[0006] In view of this, the purpose of the present invention is to provide a method for preparing crack-resistant nickel-based high-temperature alloy powder and its application, which can prepare crack-resistant nickel-based high-temperature alloy powder with precisely controlled alloy element content. Technical Solutions

[0007] To achieve the above-mentioned objectives, the preparation method and application of the crack-resistant nickel-based high-temperature alloy provided by the present invention adopt the following technical scheme: a method for preparing crack-resistant nickel-based high-temperature alloy powder, wherein the nickel-based high-temperature alloy powder and the carbide powder are charged into a high-speed plowshare mixer and mixed in a mass ratio of 98.5~99.5:0.5~1.5; the high-speed plowshare mixer rotates for 4~8 minutes and then stops for 25~60 minutes, and repeats 2~4 times to obtain the crack-resistant nickel-based high-temperature alloy powder; the plowshare speed of the high-speed plowshare mixer is 1000-3000r / min.

[0008] Optionally, the carbide powder has a particle size of 1 μm to 5 μm.

[0009] Optionally, the nickel-based high-temperature alloy powder is prepared by atomizing gas, the atomizing gas is an inert gas, and the gas pressure is 10~20 MPa; the nickel-based high-temperature alloy powder has a particle size range of 0~63 μm and an oxygen content of 150~350 ppm.

[0010] Optionally, after obtaining the crack-resistant nickel-based high-temperature alloy powder, the powder is placed in a vacuum drying oven for drying at a temperature of 80-105°C.

[0011] Optionally, the loading capacity of the high-speed plowshare mixer is 1 to 5 tons.

[0012] Optionally, the high-speed plowshare mixer rolls the powder at the bottom of the mixing chamber from bottom to top and repeatedly performs a pouring motion.

[0013] A method for using crack-resistant nickel-based high-temperature alloy powder for additive manufacturing comprises placing the crack-resistant nickel-based high-temperature alloy powder in a powder bin of a laser forming device for additive manufacturing.

[0014] Optionally, when the laser forming equipment is a laser selective melting equipment, the printing parameters are: scanning spacing 35~45μm, substrate preheating temperature 90~110℃, powder thickness 25~35μm, laser power 35~40W, and scanning speed 800~1000mms.

[0015] Optionally, when the laser forming equipment is a laser cladding or laser metal deposition equipment, the process parameters are: laser power 2000~3000W, line speed 1~30m / min, powder feeding amount 20~30g / min, inert gas protection, powder carrier gas flow rate 6~10L / min, overlap rate 40%~60%. Beneficial effects

[0016] The beneficial effects of the present invention are as follows: since there are many alloying elements in the nickel-based high-temperature alloy system and their boiling points are different, the introduction of strengthening elements such as carbides during the early ingot melting or gas atomization powder making process will inevitably cause element burnout, and the target strengthening phase generated in situ in the molten liquid phase is difficult to accurately control the content; after the nickel-based high-temperature alloy powder is prepared, the present invention adds carbides, which, compared with the existing technology, does not require high-temperature melting, thus avoiding element burnout and achieving the purpose of accurately controlling the element content. In addition, the present invention uses a high-speed plow mixer to mix the materials, which can evenly disperse the carbide fine crystal agent in the nickel-based high-temperature alloy matrix, and then give full play to its role in promoting the formation of ultrafine grain structure in the subsequent additive manufacturing process, thereby achieving the purpose of eliminating thermal cracks.

[0017] The C, Cr, V and Zr elements in the carbides added by the present invention are also contained in the original nickel-based high-temperature alloy. Excessive external additives will not be introduced into the original alloy, causing damage to the original component system, and the performance can be improved without sacrificing the strengthening effect of the inherent elements of the alloy. The present invention performs component modification in the original powder post-processing process. Compared with the prior art, it does not involve a high-temperature smelting process. According to application requirements, the content of fine-grained carbides in the nickel-based high-temperature alloy powder system can be flexibly adjusted. The processing process is simple, the mixing batch is large, and it is suitable for large-scale industrial production. The present invention introduces a nano-scale carbide fine-grain agent to induce nickel-based alloy grain refinement during laser forming. The fine-grain agent itself can also be evenly dispersed in the matrix to play a role of dispersion strengthening, which has a dual hindering effect on crack growth and expansion during the molten pool solidification process.

[0018] The high-speed plowshare mixer employed in this invention achieves superior mixing performance compared to conventional high-energy ball milling processes. It prevents work hardening of the powder and eliminates the introduction of impurities from flaking mixing balls, ensuring uniform dispersion of the grain refiner throughout the nickel-based superalloy powder. Optionally, the carbide powder can be a mixture of one or more of Cr3C2, VC, and ZrC powders. BRIEF DESCRIPTION OF THE DRAWINGS

[0019] FIG1 is a scanning electron microscope image of a crack-resistant nickel-based high-temperature alloy powder 1000X prepared in Example 1 of the present invention;

[0020] FIG2 is a printed sample of the crack-resistant nickel-based high-temperature alloy powder prepared in Example 1 of the present invention placed in a selective laser melting device and a 1000X scanning electron microscope image of the printed sample;

[0021] Figure 3 is a diagram of a standard ˚5 tensile test bar;

[0022] FIG4 is a comparison diagram of strain test results of a standard tensile test bar made from the crack-resistant nickel-based superalloy powder prepared in Example 1 of the present invention and a standard tensile test bar made from the original nickel-based superalloy powder;

[0023] FIG5 is a 100X optical microscope image (a) of a workpiece processed from the crack-resistant GH3230 alloy powder prepared in Example 1 of the present invention and a 200X optical microscope image (b) of a workpiece processed from the original GH3230 alloy powder;

[0024] FIG6 is a 200X optical microscope image of a workpiece processed from the crack-resistant K418 alloy powder prepared in Example 2 of the invention (a) and a 200X optical microscope image of a workpiece processed from the original K418 alloy powder (b);

[0025] FIG7 is a 200X optical microscope image of a workpiece processed with the crack-resistant K418B alloy powder prepared in Example 3 of the invention (a) and a 200X optical microscope image of a workpiece processed with the original GH4169 alloy powder (b);

[0026] FIG8 is a 100X optical microscope image of a workpiece processed from the crack-resistant GH3230 alloy powder prepared in Example 4 of the present invention;

[0027] FIG9 is a 100X optical microscope image of a workpiece processed from the crack-resistant GH3230 alloy powder prepared in Example 5 of the present invention;

[0028] FIG10 is a 100X optical microscope image of a workpiece processed from the crack-resistant GH3230 alloy powder prepared in Comparative Example 1;

[0029] FIG11 is a 100X optical microscope image of a workpiece processed from the crack-resistant GH3230 alloy powder prepared in Comparative Example 2. Best Mode for Carrying Out the Invention

[0030] To make the objectives, technical solutions, and advantages of the embodiments of the present invention more clear, the technical solutions of the embodiments of the present invention will be clearly and completely described below in conjunction with the accompanying drawings of the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the described embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field are within the scope of protection of the present invention.

[0031] During mixing of the ultrafine carbide powder and nickel-based superalloy powder in a high-speed plowshare mixer, the powder is first evenly distributed into the matrix powder. It is then remelted and segregated at the grain boundaries during laser forming, inhibiting grain growth, inducing a fine equiaxed crystal structure, and eliminating thermal tearing. The alloy ingots and carbide powders used in the examples of the present invention are commercially available.

[0032] Example 1

[0033] The chemical composition of the GH3230 alloy ingot meets the following requirements (in mass percentage): Cr 22.18%, W 14.57%, Al 0.46%, C 0.08%, Co 1.73%, Fe 1.8%, La 0.02%, Mn 0.44%, Mo 2.29%, N 0.01%, O 0.0131%, S 0.0014%, Si 0.37%, Ti 0.09%. The specific preparation steps are as follows: Preparation of nickel-based high-temperature alloy powder: The GH3230 alloy ingot that meets the chemical composition requirements is placed in the crucible of a vacuum induction melting gas atomization device. The atomization medium is high-purity argon gas with a gas pressure of 10-20 MPa. High-purity GH3230 alloy powder is prepared by gas atomization powder making equipment; the above-obtained powder is air-selected and sieved to obtain an average particle size of 17.64 μm and a particle size range of 0-30 μm. The original powder has an oxygen content of 350ppm; the particle size range of 0-30 μm indicates that the particle size of the nickel-based high-temperature alloy powder is greater than 0 μm and less than or equal to 30 μm.

[0034] Preparation of the crack-resistant nickel-based high-temperature alloy powder of the present invention: The atomized nickel-based high-temperature alloy powder and Cr3C2 powder with a particle size of 1-5μm are loaded into a high-speed plowshare mixer at a mass ratio of 99:1 with a loading capacity of 1.5T. Subsequently, the materials are mixed at a speed of 2000r / min for 5 minutes and then paused for 30 minutes. This process is repeated three times to obtain the uniform crack-resistant nickel-based high-temperature alloy powder shown in Figure 1.

[0035] The crack-resistant nickel-based high-temperature alloy powder was vacuum-dried at 105° C. for 3 h to fully dry out the moisture in the material.

[0036] Printing trials for additive manufacturing

[0037] The dried pre-alloyed powder was placed in the powder chamber of a CAM-100 selective laser melting (SLM) machine for printing. The process parameters used in the experiment were as follows: scanning pitch (h) of 40 μm, substrate preheat temperature (T) of 100°C, powder layer thickness of 30 μm, laser power (P) of 30 W, 35 W, and 40 W, and scanning speed (v) of 800 mm / s, 1000 mm / s, and 1200 mm / s. P and v formed a 3×3 array for orthogonal experiments. The scanning strategy was checkerboard (67° rotation per layer). Argon gas was used throughout the process to keep the oxygen content in the printing chamber below 500 pmm.

[0038] The nine processes differed in laser power and scanning speed, while other printing parameters remained the same. The specific laser power and scanning speed are shown in the vertical and horizontal data corresponding to labels ①, ②, ③, ④, ⑤, ⑥, ⑦, ⑧, and ⑨ in Figure 2, where the horizontal direction represents laser power and the vertical direction represents scanning speed. Figure 2 shows 1000X scanning electron micrographs of samples printed using the nine processes on the left, and the printed samples and printed substrates using the nine processes on the right. The figure shows the surface quality of the samples printed using the nine processes. Processes ④, ⑤, ⑦, and ⑧ exhibit smooth prints with few holes, with process 5 being the best. The values ​​for ④, ⑤, ⑦, and ⑧ are 35W laser power and 800mm / s scanning speed, 35W laser power and 1000mm / s scanning speed, 40W laser power and 800mm / s scanning speed, and 40W laser power and 1000mm / s scanning speed, respectively.

[0039] Based on process No. 5, the crack-resistant GH3230 powder of the present invention and the original GH3230 powder were used to print the 10×10×75 mm cuboid shown on the printed substrate in Figure 2. After printing, the ˚5 tensile test bar shown in Figure 3 was processed by wire electrospark cutting. The performance parameters are shown in Table 1.

[0040] Table 1

[0041]

[0042] Figure 4 shows a comparison of the room-temperature tensile properties of the crack-resistant GH3230 powder and the original GH323 powder. The SLM-molded crack-resistant GH3230 exhibited an approximately 20% increase in elongation, while its tensile strength, yield strength, and elongation were all higher than those of the original GH3230 powder, resulting in a high-performance nickel-based superalloy part. A comparative analysis of the workpiece microstructures under an optical microscope, as shown in Figures 5(a) and (b), reveals that microcracks in the workpieces produced using the crack-resistant GH3230 powder are virtually eliminated.

[0043] Example 2

[0044] The chemical composition of the K418 alloy ingot meets the following requirements (in mass percentage): Fe 0.6%, C 0.08%, Si 0.3%, Mn 0.1%, P 0.01%, S 0.006%, Cr 12.5%, Mo 3.88%, Ti 0.6%, Nb 2.0%, Zr 0.08%, B 0.01%, Al 5.8%, and Ni balance. The specific preparation steps are as follows: Preparation of nickel-based high-temperature alloy powder: The K418 alloy ingot that meets the chemical composition requirements is placed in the crucible of a vacuum induction melting gas atomization equipment. High-purity argon is used as the atomization medium, and the gas pressure is 10-20 MPa. High-purity K418 alloy powder is prepared by gas atomization powder making equipment; the above-obtained powder is air-selected and sieved to obtain an original powder with an average particle size of 32.5 μm and a particle size range of 15-53 μm, and the powder oxygen content is 150 ppm.

[0045] Preparation of the crack-resistant nickel-based high-temperature alloy powder of the present invention: atomized K418 high-temperature alloy powder and 1-5 μm VC powder are mixed in a mass ratio of 98.5:1.5 in a high-speed plowshare mixer, and then mixed at a speed of 3000 r / min for 8 minutes, paused for 60 minutes, and repeated three times to obtain a uniform crack-resistant alloy mixture; the pre-alloyed powder is vacuum-dried at 90°C for 3 hours to fully dry out the moisture in the material; the dried pre-alloyed powder is placed in the powder bin of a laser cladding (LC) equipment, the LC forming equipment model is CAM-EHLA1500, and a coating is clad on a 316L stainless steel shaft part. The process parameters selected are: laser power 2500W, linear speed 25m / min, powder feed rate 25g / min, inert shielding gas flow rate 10L / min, powder carrier gas flow rate 8L / min, overlap rate 50%, and the cladding is completed. After the cladding is completed, the powder is removed; based on the same cladding process parameters, crack-resistant K418 powder and original K418 are used respectively. The powder was clad, and a 10×10×5 mm square was cut from the clad shaft coating along with the substrate. The coating surface was sanded and polished to a mirror finish. The microstructure of the coating was compared and analyzed under a light microscope, as shown in Figure 6(a) and (b), respectively. In contrast, the microcracks in the coating prepared with the crack-resistant K418 powder were almost eliminated.

[0046] Example 3

[0047] The chemical composition of the K418B alloy ingot meets the following requirements (in mass percentage): C 0.05%, Cr 12.5%, Fe 0.25%, Si 0.2%, Mn 0.1%, P 0.01%, S 0.01%, Cu 0.2%, Mo 4.6%, Ti 0.44%, Nb 2.0%, Zr 0.1%, B 0.01%, Co 0.5%, Al 6%, and the balance is Ni. The specific preparation steps are as follows: Preparation of nickel-based high-temperature alloy powder: The K418B alloy ingot that meets the chemical composition requirements is placed in the crucible of a vacuum induction melting gas atomization equipment. The atomization medium is high-purity argon gas with a gas pressure of 10-20 MPa. High-purity K418B alloy powder is prepared by gas atomization powder making equipment; the above-obtained powder is air-selected and sieved to obtain a powder with an average particle size of 25.3 μm and a particle size range of 15-53 μm. The original powder has an oxygen content of 200ppm; the preparation of the crack-resistant nickel-based high-temperature alloy powder of the present invention: atomized K418B alloy powder and 3μm ZrC powder are placed in a high-speed plowshare mixer at a mass ratio of 99:1, and then mixed at a speed of 3000r / min for 4 minutes, paused for 25 minutes, and repeated three times to obtain a uniform crack-resistant alloy mixture; the crack-resistant K418B alloy powder is vacuum-dried at 100℃ for 3h to fully dry the moisture in the material; the dried pre-alloyed powder is placed in the powder bin of the laser metal deposition (LMD) equipment, the LMD forming equipment model is CAM-ELMD1600, and the H13 The square samples were laser deposited on a steel substrate with the following process parameters: laser power 3000W, linear speed 1m / min, powder feeding rate 16.6g / min, shielding gas flow rate 8L / min, powder carrier gas flow rate 7L / min, overlap rate 45%. The samples were taken out after completion. Based on the same laser deposition process parameters, the crack-resistant K418B powder of the present invention and the original K418B powder were laser deposited to form three-dimensional squares. A 10×10×10mm sample was cut from the deposited sample. The coating surface was sanded and polished to a mirror effect. The microstructures of the samples were compared and analyzed under an optical microscope, as shown in Figures 7(a) and (b), respectively. The comparison found that the microcracks in the sample prepared by the crack-resistant K418B powder were almost eliminated.

[0048] Example 4

[0049] Example 4 Based on Example 1, the mass ratio of nickel-based high-temperature alloy powder to 1-5μm Cr3C2 powder was changed to a mass ratio of 99.5:0.5. The other preparation steps of the crack-resistant nickel-based high-temperature alloy powder were the same, and the printing parameters were the same as process ⑤. Figure 8 is a 100X optical microscope image of a workpiece processed with the crack-resistant GH3230 alloy powder prepared in Example 4; compared with Figure 5 (a), Figure 8 has sporadic cracks, but compared with Figure 5 (b), the cracks are much less.

[0050] Example 5

[0051] Example 5 Based on Example 1, the mass ratio of nickel-based high-temperature alloy powder to 1-5μm Cr3C2 powder was changed to a mass ratio of 98.5:1.5. The other preparation steps of the crack-resistant nickel-based high-temperature alloy powder were the same, and the printing parameters were the same as process 5. Figure 9 is a 100X optical microscope image of a workpiece processed with the crack-resistant GH3230 alloy powder prepared in Example 5. Compared with Figure 9 (a), the anti-crack effect is similar. Compared with Figure 5 (b), the cracks are almost gone.

[0052] Example 6

[0053] Example 6: Based on Example 1, the carbide composition was modified to use a 1:1 ratio of Cr3C2 and ZrC. The remaining steps for preparing the crack-resistant nickel-based superalloy powder were the same, and the printing parameters were the same as in Process 5. Printing of the prepared crack-resistant nickel-based superalloy powder revealed a near-elimination of cracks.

[0054] Example 7

[0055] Example 7: Based on Example 1, the carbide composition was changed to a combination of Cr3C2 and VC at a ratio of 3:7. Other preparation steps were the same, and the printing parameters were the same as in process 5. Printing of the crack-resistant nickel-based high-temperature alloy powder showed that cracks had almost disappeared.

[0056] Example 8

[0057] Example 8: Based on Example 1, the speed of the high-speed plowshare mixer was changed to 2500 rpm. After mixing for 8 minutes, the mixture was paused for 60 minutes, and this process was repeated twice to produce a crack-resistant nickel-based superalloy powder. The remaining preparation steps for the crack-resistant nickel-based superalloy powder were identical, and the printing parameters were the same as in process 5. Printing of the prepared crack-resistant nickel-based superalloy powder revealed sporadic cracks, but these cracks were nearly eliminated.

[0058] Embodiment 9

[0059] Example 9: Based on Example 1, the speed of the high-speed plowshare mixer was changed to 2800 rpm. After mixing for 4 minutes, the mixture was paused for 25 minutes, and this process was repeated four times to produce a crack-resistant nickel-based superalloy powder. The remaining preparation steps for the crack-resistant nickel-based superalloy powder were identical, and the printing parameters were the same as in process 5. Printing of the prepared crack-resistant nickel-based superalloy powder revealed sporadic cracks, but these cracks were nearly eliminated.

[0060] Example 10

[0061] Example 10 Based on Example 1, another specification of commercially available Cr3C2 was used with a particle size range of 0.2μm~1μm. Other preparation methods were the same, and printing parameters were the same as process ⑤. The crack-resistant nickel-based high-temperature alloy powder prepared was printed, showing sporadic cracks, but they were almost gone.

[0062] Example 11

[0063] Example 11 Based on Example 1, another specification of Cr3C2 available on the market was used, with a particle size range of 5μm~10μm. Other preparation methods were the same, and printing parameters were the same as process ⑤. The crack-resistant nickel-based high-temperature alloy powder prepared was printed, showing sporadic cracks, but they were almost gone.

[0064] Example 12

[0065] Example 12 Based on Example 2, another commercially available VC powder with a particle size range of 0.2 μm to 1 μm was used. Other preparation methods and printing parameters were the same. The crack-resistant nickel-based high-temperature alloy powder was printed, showing sporadic cracks, but almost disappeared.

[0066] Example 13

[0067] Example 13 Based on Example 2, another commercially available VC powder with a particle size range of 5μm-10μm was used. Other preparation methods and printing parameters were the same as process ⑤. The crack-resistant nickel-based high-temperature alloy powder was printed, showing sporadic cracks, but almost disappeared.

[0068] Example 14

[0069] Example 14 Based on Example 3, the carbide powder is a combination of Cr3C2, VC and ZrC powders in a ratio of 1:1:1. Other preparation methods and printing parameters are the same as process ⑤. The crack-resistant nickel-based high-temperature alloy powder prepared is printed, and the cracks are almost eliminated.

[0070] Comparative Example 1

[0071] Comparative Example 1: Based on Example 1, the ratio of nickel-based high-temperature alloy powder to carbide powder was changed to 98:2. Other preparation methods and printing parameters were the same. The crack-resistant nickel-based high-temperature alloy powder was printed as shown in Figure 10. Compared with Figures 5(a), 8, and 9, Comparative Example 1 has more cracks, while Figures 5(a), 8, and 9 have almost no cracks.

[0072] Comparative Example 2

[0073] Comparative Example 2: Based on Example 1, the ratio of nickel-based high-temperature alloy powder to carbide powder was changed to 96:4. Other preparation methods and printing parameters were the same. The crack-resistant nickel-based high-temperature alloy powder was printed as shown in Figure 11. Compared with Figures 5(a), 8, and 9, Comparative Example 2 has more cracks, and compared with Figure 10 of Comparative Example 1, there are even more cracks.

[0074] Comparative Example 3

[0075] Comparative Example 3 Based on Example 1, the speed of the high-speed plowshare mixer was changed to 3500 r / min and stopped after rotating for 2 minutes. Other preparation methods and printing parameters were the same. The crack-resistant nickel-based high-temperature alloy powder prepared showed many cracks and holes when printed.

[0076] Comparative Example 4

[0077] Comparative Example 4 Based on Example 1, the speed of the high-speed plowshare mixer was changed to 1500 r / min, and it was stopped after rotating for 10 minutes. Other preparation methods and printing parameters were the same. The crack-resistant nickel-based high-temperature alloy powder prepared showed many cracks and holes when printed.

[0078] Comparative Example 5

[0079] Comparative Example 5: Based on Comparative Example 4, the speed of the high-speed plowshare mixer was changed to 1500 r / min, and the mixture was rotated for 10 minutes and then stopped for 20 minutes, which was repeated 5 times. Other preparation methods and printing parameters were the same. The crack-resistant nickel-based high-temperature alloy powder prepared by printing showed more cracks.

[0080] Comparative Example 6

[0081] Comparative Example 6 Based on Comparative Example 3, the speed of the high-speed plowshare mixer was changed to 3500 r / min, and it was rotated for 2 minutes and then stopped for 70 minutes, and repeated 5 times. Other preparation methods and printing parameters were the same. The crack-resistant nickel-based high-temperature alloy powder prepared by printing showed more cracks.

[0082] The above is a preferred embodiment of the present invention. It should be pointed out that for ordinary technicians in this technical field, several improvements and modifications can be made without departing from the principles of the present invention. These improvements and modifications should also be regarded as within the scope of protection of the present invention.

Claims

1. A method for preparing crack-resistant nickel-based high-temperature alloy powder, characterized in that: The nickel-based high-temperature alloy powder and the carbide powder are mixed in a high-speed plowshare mixer at a mass ratio of 98.5-99.5:0.5-1.5; the high-speed plowshare mixer rotates for 4-8 minutes and then stops for 25-60 minutes, and repeats 2-4 times to obtain the crack-resistant nickel-based high-temperature alloy powder; the plowshare speed of the high-speed plowshare mixer is 1000-3000r / min.

2. The method for preparing crack-resistant nickel-based high-temperature alloy powder according to claim 1, characterized in that: The carbide powder is one of Cr3C2, VC, and ZrC powders or a mixture of two or more thereof.

3. The method for preparing crack-resistant nickel-based high-temperature alloy powder according to claim 2, characterized in that: The carbide powder has a particle size of 0.2 μm to 10 μm.

4. The method for preparing crack-resistant nickel-based high-temperature alloy powder according to claim 1, characterized in that: The nickel-based high-temperature alloy powder is prepared by atomizing gas, the atomizing gas is an inert gas, and the gas pressure is 10-20 MPa; the nickel-based high-temperature alloy powder has a particle size range of 0-63 μm and an oxygen content of 150-350 ppm.

5. The method for preparing crack-resistant nickel-based high-temperature alloy powder according to claim 1, characterized in that: After the crack-resistant nickel-based high-temperature alloy powder is obtained, it is moved into a vacuum drying oven for drying at a temperature of 80-105°C.

6. The method for preparing crack-resistant nickel-based high-temperature alloy powder according to claim 1, characterized in that: The loading capacity of the high-speed plowshare mixer is 1-5 ton.

7. The method for preparing crack-resistant nickel-based high-temperature alloy powder according to claim 6, characterized in that: The high-speed plowshare mixer rolls the powder at the bottom of the mixing chamber upward and repeatedly performs pouring motions.

8. A method for using the crack-resistant nickel-based high-temperature alloy powder prepared according to any one of claims 1 to 7 for additive manufacturing, characterized in that: The crack-resistant nickel-based high-temperature alloy powder is placed in a powder bin of a laser forming device for additive manufacturing.

9. The method for using the crack-resistant nickel-based high-temperature alloy powder for additive manufacturing according to claim 8, characterized in that: When the laser forming equipment is a laser selective melting equipment, the printing parameters are: scanning spacing 35-45 μm, substrate preheating temperature 90-110° C., powder thickness 25-35 μm, laser power 35-40 W, and scanning speed 800-1000 mms.

10. According to the method for using crack-resistant nickel-based high-temperature alloy powder for additive manufacturing as described in claim 8, when the laser forming equipment is a laser cladding type or laser metal deposition equipment, the process parameters are: laser power 2000~3000W, line speed 1~30m / min, powder feeding amount 20~30g / min, inert gas protection, powder carrier gas flow rate 6~10L / min, overlap rate 40%~60%.

Citation Information

Patent Citations

  • Preparation method of composite rare-earth tungsten powder

    CN109014231A

  • Composite powder for laser cladding and preparation method thereof

    CN110846537A

  • Method for reducing additive manufacturing cracks of nickel-based superalloy and nickel-based superalloy

    CN114480893A

  • Preparation method and application of anti-crack nickel-based superalloy powder

    CN116618666A

  • Ni ALLOY POWDER FOR ADDITIVE MANUFACTURING AND ADDITIVELY MANUFACTURED ARTICLE

    JP2023064068A