Back transparent conductive film and preparation method therefor, and photovoltaic device

By adding cadmium elements to the transparent conductive film and optimizing the molar ratio of indium elements and cadmium elements, the problem of high cost of existing transparent conductive films is solved, and efficient photoelectric conversion and improved conductivity are achieved, which is suitable for photovoltaic devices.

WO2024234850A1PCT designated stage expired Publication Date: 2024-11-21LONGI GREEN ENERGY TECH CO LTD

Patent Information

Application Number
PCT/CN2024/085320
Authority / Receiving Office
WO · WO
Patent Type
Applications
Current Assignee / Owner
Priority Date
2023-05-15
Filing Date
2024-04-01
Publication Date
2024-11-21

AI Technical Summary

Technical Problem

The transparent conductive film on the existing back is relatively expensive, with the main component being indium oxide. Indium metal content is scarce and has high cost in the earth's crust, which limits its wide application.

Method used

Using a transparent conductive film of cadmium, oxygen and indium, the molar ratio of indium and cadmium is between 0.185% and 2.861%. It is prepared by reacting plasma deposition, sputtering or physical vapor deposition processes to increase cadmium to Reduce costs and optimize film mobility and square resistance.

Benefits of technology

The cost of the transparent conductive film on the back is reduced, the photoelectric conversion efficiency and conductivity of photovoltaic devices are improved, the filling factor and short-circuit current density are improved, and the transparency and conductivity of long-band light is ensured.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN2024085320_21112024_PF_FP_ABST
    Figure CN2024085320_21112024_PF_FP_ABST
Patent Text Reader

Abstract

The present application relates to the technical field of photovoltaics, and provides a back transparent conductive film and a preparation method therefor, and a photovoltaic device. The back transparent conductive film comprises: a cadmium element, an oxygen element, and an indium element; in the back transparent conductive film, the molar ratio of the indium element to the cadmium element is X, and X is greater than or equal to 0.185%, and less than or equal to 2.861%. The cadmium element is added to the back transparent conductive film, the indium element has a smaller content relative to the cadmium element, and the content of the cadmium element in the earth crust is far greater than the content of the indium element in the earth crust, thereby greatly reducing the cost of the back transparent conductive film. The back transparent conductive film has good light transmittance for light rays of long wave bands, thereby fully utilizing the light rays of long wave bands, and improving the photoelectric conversion efficiency of the photovoltaic device. The back transparent conductive film has high mobility, low sheet resistance and excellent conductive performance, thereby increasing the filling factor and the short-circuit current density of the photovoltaic device.
Need to check novelty before this filing date? Find Prior Art

Description

Back transparent conductive film and preparation method thereof and photovoltaic device

[0001] This application claims priority to the Chinese patent application filed with the China Patent Office on May 15, 2023, with application number 202310545381.0 and invention name “Transparent conductive film on the back, preparation method thereof and photovoltaic device”, the entire contents of which are incorporated by reference into this application. Technical Field

[0002] The present application relates to the field of photovoltaic technology, and in particular to a back-side transparent conductive film, a preparation method thereof, and a photovoltaic device. Background Art

[0003] Transparent conductive oxides (TCOs) are widely used in photovoltaic devices due to their high light transmittance and excellent electrical conductivity. For example, TCOs are used in solar cells to collect and transport charge carriers.

[0004] At present, the main component of the commonly used transparent conductive film on the back is indium oxide, which has the advantages of high mobility and low sheet resistance.

[0005] However, the content of metallic indium in the earth's crust is very low and its cost is relatively high, which limits the widespread use of transparent conductive films on the back.

[0006] Summary of the Invention

[0007] The present application provides a back transparent conductive film, a preparation method thereof, and a photovoltaic device, aiming to solve the problem of high cost of existing back transparent conductive films.

[0008] In a first aspect of the present application, there is provided a transparent conductive film for use on the back of a photovoltaic device, comprising: cadmium, oxygen, and indium;

[0009] In the transparent conductive film on the back side, the molar ratio of the indium element to the cadmium element is X, and X is greater than or equal to 0.185% and less than or equal to 2.861%.

[0010] In the embodiment of the present application, cadmium is added to the transparent conductive film on the back, and in the transparent conductive film on the back, the molar ratio of indium to cadmium is greater than or equal to 0.185% and less than or equal to 2.861%, indicating that the content of indium is very small relative to cadmium. At the same time, the content of cadmium in the earth's crust far exceeds the content of indium in the earth's crust, thereby greatly reducing the cost of the transparent conductive film on the back. At the same time, after light enters the light-facing side of the photovoltaic device, it will preferentially absorb short-wavelength light and reach the backlight side, leaving mainly long-wavelength light. The band gap of the transparent conductive film on the back is narrow, about 2.3 eV (electron volts), and has good transmittance for long-wavelength light, thereby making full use of long-wavelength light, which can improve the photoelectric conversion efficiency of the photovoltaic device. At the same time, the transparent conductive film on the back has a high mobility, low square resistance, and excellent conductivity, which can improve the fill factor and short-circuit current density of the photovoltaic device.

[0011] Optionally, X is greater than or equal to 0.465% and less than or equal to 0.793%.

[0012] Optionally, in the transparent conductive film on the back side, the molar ratio of the oxygen element is 30% to 70%.

[0013] Optionally, the mobility of the transparent conductive film on the back side is 70 square centimeters per volt per second to 260 square centimeters per volt per second.

[0014] Optionally, the mobility of the transparent conductive film on the back side is 160 square centimeters per volt per second to 230 square centimeters per volt per second.

[0015] Optionally, the sheet resistance of the transparent conductive film on the back side is 10 ohms to 47 ohms.

[0016] Optionally, the sheet resistance of the transparent conductive film on the back side is 20 ohms to 26 ohms.

[0017] Optionally, in the transparent conductive film on the back side, the number of crystal grains along the 111 crystal plane direction is the largest.

[0018] Optionally, in the X-ray diffraction image, the ratio of the intensity of the strongest peak of the transparent conductive film on the back side to the intensity of the second strongest peak is greater than or equal to 50.

[0019] Optionally, within a wavelength range of 800 nm to 1200 nm, the effective total transmittance of the transparent conductive film on the back side is greater than or equal to 0.92.

[0020] Optionally, the thickness of the transparent conductive film on the back side is 50 nm to 110 nm.

[0021] Optionally, the transparent conductive film on the back side further contains hydrogen element, and the mass proportion of the hydrogen element is 0 to 0.1%.

[0022] A second aspect of the present application provides a method for preparing any of the aforementioned transparent conductive films for the back surface of a photovoltaic device, comprising:

[0023] Providing a target material; the target material comprises: cadmium element, oxygen element and indium element; in the target material, the molar ratio of the indium element to the cadmium element is Y, and the Y is greater than or equal to 0.185% and less than or equal to 2.861%;

[0024] Based on the target material, a transparent conductive film on the back side is prepared.

[0025] Optionally, preparing the transparent conductive film on the back side based on the target material includes:

[0026] The transparent conductive film on the back is prepared based on the target material by adopting one of reactive plasma deposition, sputtering and physical vapor deposition.

[0027] Optionally, the step of preparing the back transparent conductive film based on the target material by using one of reactive plasma deposition, sputtering, and physical vapor deposition includes:

[0028] During the entire preparation process of the transparent conductive film on the back, mixed gas is introduced; the mixed gas includes oxygen and inert gas; the ratio of the flow rate of the oxygen to the total flow rate of the mixed gas is 30% to 50%.

[0029] In a third aspect of the present application, a photovoltaic device is provided, comprising: any of the aforementioned transparent conductive films for use on the back side of the photovoltaic device.

[0030] Optionally, the photovoltaic device is a heterojunction solar cell, and in the heterojunction solar cell, the thickness of the transparent conductive film on the back side is 47 nm to 65 nm.

[0031] The above-mentioned photovoltaic device and the method for preparing the transparent conductive film on the back of the photovoltaic device have the same or similar beneficial effects as the transparent conductive film on the back of the photovoltaic device, and will not be described again here to avoid repetition.

[0032] The above description is only an overview of the technical solution of the present application. In order to more clearly understand the technical means of the present application, it can be implemented in accordance with the contents of the specification. In order to make the above and other purposes, features and advantages of the present application more obvious and easy to understand, the specific implementation methods of the present application are listed below. BRIEF DESCRIPTION OF THE DRAWINGS

[0033] In order to more clearly illustrate the embodiments of the present application or the technical solutions in the prior art, a brief introduction will be given below to the drawings required for use in the embodiments or the description of the prior art. Obviously, the drawings described below are some embodiments of the present application. For ordinary technicians in this field, other drawings can be obtained based on these drawings without any creative work.

[0034] FIG1 is a flowchart showing the steps of a method for preparing a transparent conductive film for the back side of a photovoltaic device according to an embodiment of the present application;

[0035] FIG2 shows a schematic structural diagram of a heterojunction solar cell according to an embodiment of the present application;

[0036] FIG3 shows a schematic diagram of the XRD pattern distribution of a back transparent conductive film in an embodiment of the present application;

[0037] FIG4 shows a schematic diagram of the effective total transmittance spectrum distribution of a back transparent conductive film in an embodiment of the present application;

[0038] FIG5 shows a schematic diagram of the electrical performance distribution of the heterojunction solar cell in an embodiment of the present application.

[0039] Description of the accompanying figures:

[0040] 1-back metal electrode, 2-back transparent conductive film, 3-back doped passivation layer, 4-back intrinsic passivation layer, 5-silicon substrate, 6-front intrinsic passivation layer, 7-front doped passivation layer, 8-front transparent conductive film, 9-front metal electrode. Specific embodiments

[0041] To make the purpose, technical solutions, and advantages of the embodiments of this application more clear, the technical solutions in the embodiments of this application will be clearly and completely described below in conjunction with the drawings in the embodiments of this application. Obviously, the described embodiments are part of the embodiments of this application, not all of the embodiments. Based on the embodiments in this application, all other embodiments obtained by ordinary technicians in this field without making creative efforts are within the scope of protection of this application.

[0042] The present application provides a transparent conductive film for use on the back side of a photovoltaic device. The photovoltaic device is a device capable of photoelectric conversion and carrier separation. The surface of the photovoltaic device that primarily absorbs light is the light-facing side, and the backlight side and the light-facing side are arranged opposite each other. The backside transparent conductive film is located on the backlight side of the photovoltaic device.

[0043] The transparent conductive film on the back side includes: cadmium element (Cd), oxygen element (O) and indium element (In), that is, cadmium element is added to the transparent conductive film on the back side of the present application. The molar ratio refers to the ratio of the amount of a substance, which can characterize the amount of a substance. In the transparent conductive film on the back side, the molar ratio of indium element (In) to cadmium element (Cd) is X, and X is greater than or equal to 0.185% and less than or equal to 2.861%, indicating that the content of indium element is very small relative to cadmium element. At the same time, the content of cadmium element in the earth's crust far exceeds the content of indium element in the earth's crust, thereby greatly reducing the cost of the transparent conductive film on the back side.

[0044] After the light enters the light-facing side of the photovoltaic device, it will preferentially absorb the light in the short-wave band and reach the backlight side, and the main remaining light is the long-wave band. For example, after the light enters the light-facing side of the photovoltaic device, it will preferentially absorb the light in the short-wave band and reach the backlight side, and the main remaining light is the light with a wavelength of 800nm ​​(nanometers) to 1200nm. The band gap of the transparent conductive film on the back is narrow, about 2.3eV (electron volts), and it has good light transmittance for the long-wave band, thereby making full use of the long-wave band light, which can improve the photoelectric conversion efficiency of the photovoltaic device. At the same time, the transparent conductive film on the back has a high mobility, low square resistance, and excellent conductive performance, which can improve the fill factor and short-circuit current density of the photovoltaic device.

[0045] For example, in the transparent conductive film on the back side, the above-mentioned X can be 0.185%, or 0.231%, or 0.31%, or 0.465%, or 0.52%, or 0.652%, or 0.674%, or 0.793%, or 0.813%, or 0.934%, or 1.111%, or 1.345%, or 1.789%, or 2.103%, or 2.451%, or 2.511%, or 2.861%.

[0046] It should be noted that the molar ratio of indium to cadmium in the transparent conductive film on the back can be measured by atomic spectroscopy, X-ray energy dispersive spectroscopy (EDX), EDS (Energy Dispersive Spectroscopy), XPS (X-ray photoelectron spectroscopy), ICP-OES (Inductively Coupled Plasma-Optical Emission Spectroscopy), etc. The specific method for measuring the molar ratio of indium to cadmium in the transparent conductive film on the back is not limited.

[0047] Optionally, the mobility of the transparent conductive film on the back is: 70 square centimeters per volt per second (cm 2 / V·S) to 260 square centimeters per volt per second. The back transparent conductive film has good electrical conductivity. If the back transparent conductive film is used in a solar cell, the back transparent conductive film has high mobility, carriers can be effectively collected laterally, and the metal grid spacing of the solar cell can be appropriately increased, reducing grid line obstruction, increasing the current of the solar cell, and reducing the amount of slurry used.

[0048] For example, the mobility of the transparent conductive film on the back is: 70cm 2 / V·S, or 90cm 2 / V·S, or 100cm 2 / V·S, or 110cm 2 / V·S, or 120cm 2 / V·S, or 130cm 2 / V·S, or 140cm 2 / V·S, or 150cm 2 / V·S, or 160cm 2 / V·S, or 170cm 2 / V·S, or 180cm 2 / V·S, or 200cm 2 / V·S.

[0049] Optionally, the sheet resistance of the transparent conductive film on the back side is 10 ohms (Ω) to 47 ohms. The sheet resistance of the transparent conductive film on the back side is small, and its electrical performance is good, which can improve the fill factor and short-circuit current density of the photovoltaic device.

[0050] For example, the square resistance of the transparent conductive film on the back is 10Ω, or 10.37Ω, or 13Ω, or 15.12Ω, or 20Ω, or 21.07Ω, or 23.01Ω, or 24Ω, or 25.51Ω, or 30Ω, or 34Ω, or 40Ω, or 45Ω, or 46.14Ω, or 47Ω.

[0051] Effective total transmittance = transmittance / (1-reflectivity). In the present application, the effective total transmittance is calculated by testing the transmittance spectrum and reflectance spectrum of the transparent conductive film on the back. Optionally, in the transparent conductive film on the back, the molar ratio of indium element (In) and cadmium element (Cd) is X, X is greater than or equal to 0.465% and less than or equal to 0.793%, and the molar ratio of indium element (In) and cadmium element (Cd) is X within this range. The transparent conductive film on the back has excellent effective total transmittance for long-wave bands such as 800nm ​​to 1200nm, and its corresponding mobility is higher and the square resistance is lower. At the same time, relative to cadmium element, the content of indium element is very small. At the same time, the content of cadmium element in the earth's crust far exceeds the content of indium element in the earth's crust, thereby greatly reducing the cost of the transparent conductive film on the back.

[0052] For example, in the transparent conductive film on the back side, X may be 0.465%, 0.521%, 0.575%, 0.601%, 0.645%, 0.652%, 0.674%, 0.702%, 0.713%, 0.741%, 0.753%, 0.765%, 0.789%, or 0.793%.

[0053] Optionally, in the transparent conductive film on the back, the molar ratio of indium element (In) to cadmium element (Cd) is X, X is greater than or equal to 0.465% and less than or equal to 0.793%, and the mobility of the transparent conductive film on the back is: 160 (cm 2 / V·S) to 230 square centimeters per volt per second, and the transparent conductive film on the back has excellent electrical conductivity.

[0054] For example, in the transparent conductive film on the back, the molar ratio of indium element (In) to cadmium element (Cd) is X, X is greater than or equal to 0.465% and less than or equal to 0.793%, and the mobility of the transparent conductive film on the back is: 160cm 2 / V·S, or 170cm 2 / V·S, or 177cm 2 / V·S, or 180cm 2 / V·S, or 187.9cm 2 / V·S, or 189cm 2 / V·S, or 190cm 2 / V·S, or 192cm 2 / V·S, or 194.3cm 2 / V·S, or 196cm 2 / V·S, or 199cm 2 / V·S, or 200cm 2 / V·S.

[0055] Optionally, in the back transparent conductive film, the molar ratio of indium (In) to cadmium (Cd) is X, where X is greater than or equal to 0.465% and less than or equal to 0.793%, and the sheet resistance of the back transparent conductive film is 20 ohms to 26 ohms. The back transparent conductive film has a lower sheet resistance and good electrical performance, which can improve the fill factor and short-circuit current density of the photovoltaic device.

[0056] For example, the sheet resistance of the transparent conductive film on the back surface is 20Ω, or 20.37Ω, or 21.07Ω, or 22Ω, or 22.61Ω, or 23.01Ω, or 24Ω, or 25.51Ω, or 26Ω.

[0057] Optionally, the molar ratio of oxygen in the back transparent conductive film is 30% to 70%. The oxygen content in the back transparent conductive film is appropriate to avoid introducing too many defects and causing excessive recombination. The molar ratio of oxygen in this range can maintain a balance between mobility and carrier concentration.

[0058] For example, the molar ratio of oxygen element in the transparent conductive film on the back side can be 30%, or 34%, or 38%, or 39%, or 40%, or 43%, or 50%, or 56%, or 57%, or 60%, or 65%, or 70%.

[0059] It should be noted that in the present application, the mass ratio of hydrogen in the back transparent conductive film can be less than or equal to 0.1%. More specifically, the inventors have discovered that as the amount of hydrogen in the back transparent conductive film increases, the number of carriers first increases and then decreases, and the mobility decreases. When the mass ratio of hydrogen is less than or equal to 0.1%, it has little effect on the properties of the back transparent conductive film and can passivate any defects that may exist between and within the grains of the transparent conductive film, thereby improving the conductivity of the transparent conductive film.

[0060] For example, the mass proportion of hydrogen in the transparent conductive film on the back side can be 0, or 0.003%, or 0.008%, or 0.015%, or 0.022%, or 0.036%, or 0.047%, or 0.053%, or 0.079%, or 0.092%, or 0.1%.

[0061] Optionally, in the transparent conductive film on the back side, the number of crystal grains along the 111 crystal plane direction is the largest, so that the polycrystalline portion is larger, the crystallinity is higher, the defects are fewer, and the introduced recombination is less.

[0062] Optionally, in the X-ray diffraction image, the ratio of the intensity of the strongest peak of the transparent conductive film on the back to the intensity of the second strongest peak is greater than or equal to 50, indicating higher crystallinity, fewer defects, and less introduced recombination.

[0063] For example, in the X-ray diffraction image, the ratio of the intensity of the strongest peak of the transparent conductive film on the back side to the intensity of the second strongest peak is 50, or 53, or 59, or 60, or 62, or 63, or 64, or 67, or 70.

[0064] Optionally, within the wavelength range of 800 nm to 1200 nm, the effective total transmittance of the back transparent conductive film is greater than or equal to 0.92. In other words, the back transparent conductive film has a high effective total transmittance in the long-wavelength range, so the light reaching the backlight side of the photovoltaic device is primarily in the long-wavelength range, thereby improving the utilization rate of the long-wavelength range.

[0065] For example, in the wavelength range of 800 nm to 1200 nm, the effective total transmittance of the transparent conductive film on the back side can be 0.92, or 0.95, or 0.98, or 0.983, or 0.987, or 0.990, or 0.992, or 0.995, or 0.997, or 0.998.

[0066] Optionally, the thickness of the transparent conductive film on the back side is 50 nm to 110 nm. The thickness of the transparent conductive film on the back side is relatively appropriate, and the optical performance and the conductive performance are well balanced.

[0067] For example, the thickness of the transparent conductive film on the back surface may be 50 nm, or 60 nm, or 62 nm, or 70 nm, or 80 nm, or 90 nm, or 100 nm, or 110 nm.

[0068] FIG1 shows a flow chart of steps of a method for preparing a transparent conductive film for the back of a photovoltaic device in an embodiment of the present application. The present application also provides a method for preparing any of the aforementioned transparent conductive films for the back of a photovoltaic device, as shown in FIG1 , the method comprising the following steps:

[0069] Step 101, providing a target material; the target material includes: cadmium element, oxygen element and indium element; in the target material, the molar ratio of the indium element to the cadmium element is Y, and the Y is greater than or equal to 0.185% and less than or equal to 2.861%.

[0070] Cadmium element is added to the target material. In the target material, the molar ratio of indium element (In) to cadmium element (Cd) is Y, and Y is greater than or equal to 0.185% and less than or equal to 2.861%. This means that the content of indium element is very small relative to cadmium element. At the same time, the content of cadmium element in the earth's crust far exceeds the content of indium element in the earth's crust, thereby greatly reducing the cost of the transparent conductive film on the back.

[0071] Step 102: preparing the transparent conductive film on the back side based on the target material.

[0072] The transparent conductive film on the back side can be prepared by sputtering, reactive plasma deposition, spin coating, spray pyrolysis and the like.

[0073] Optionally, step 102 may include: using one of reactive plasma deposition (RPD), sputtering and physical vapor deposition (PVD) to prepare a transparent conductive film on the back side based on the first target material. The above process is simple and can appropriately improve the mobility of the transparent conductive film on the back side.

[0074] Optionally, step 102 may include introducing a mixed gas throughout the entire process of preparing the backside transparent conductive film. The mixed gas may include oxygen and an inert gas, wherein the ratio of the oxygen flow rate to the total flow rate of the mixed gas is 30% to 50%. The inert gas provides a protective atmosphere, and the specific type of inert gas is not limited. For example, the inert gas may include argon. The oxygen replenishes oxygen lost during the process of preparing the backside transparent conductive film. During the entire process of preparing the backside transparent conductive film, the ratio of the oxygen flow rate to the total flow rate of the mixed gas is 30% to 50%, ensuring that the mass ratio of oxygen in the formed backside transparent conductive film meets the aforementioned requirements. During the entire process of preparing the backside transparent conductive film, the ratio of the oxygen flow rate to the total flow rate of the mixed gas is 30% to 50%, which is a wide range, thereby widening the process window for preparing the backside transparent conductive film. By appropriately adjusting this ratio, good optical and electrical properties can be achieved.

[0075] For example, during the preparation process of the entire transparent conductive film on the back side, the ratio of the oxygen flow rate to the total flow rate of the mixed gas is 30%, or 38%, or 39%, or 40%, or 43%, or 45%, or 46%, or 49%, or 50%.

[0076] It should be noted that the mixed gas may also include hydrogen, etc. In the case of including hydrogen, the flow ratio of hydrogen to the mixed gas is not specifically limited. During the process of preparing the back transparent conductive film, the back transparent conductive film can be further optimized by adjusting the total flow rate of the mixed gas and other process parameters, such as the plasma gun current. This is not specifically limited in the embodiments of the present application.

[0077] The present application also provides a photovoltaic device, including any of the aforementioned transparent conductive films on the back side, and the type of the photovoltaic device is not specifically limited. For example, the photovoltaic device may include a structure that separates and transmits carriers. For example, the photovoltaic device may be a solar cell, or the photovoltaic device may be a photovoltaic module, a photovoltaic power station, etc. For another example, the photovoltaic device may be a heterojunction solar cell (HJT).

[0078] Figure 2 shows a schematic structural diagram of a heterojunction solar cell in an embodiment of the present application. Optionally, referring to Figure 2, the photovoltaic device is a heterojunction solar cell. Referring to Figure 2, the heterojunction solar cell includes a back metal electrode 1, a back transparent conductive film 2, a back doped passivation layer 3, a back intrinsic passivation layer 4, a silicon substrate 5, a front intrinsic passivation layer 6, a front doped passivation layer 7, a front transparent conductive film 8, and a front metal electrode 9. The doping type of the silicon substrate 5 is not specifically limited. For example, the silicon substrate 5 can be nC-Si. Optionally, in the heterojunction solar cell, the thickness of the back transparent conductive film 2 is 47nm to 65nm. In the heterojunction solar cell, the thickness of the back transparent conductive film 2 is within this range, and the square resistance is low, which is more conducive to improving the performance of the heterojunction solar cell, for example, it is more conducive to improving the fill factor and conversion efficiency of the heterojunction solar cell.

[0079] For example, the photovoltaic device is a heterojunction solar cell, in which the thickness of the transparent conductive film 2 on the back is 47nm, or 49nm, or 50nm, or 52nm, or 53nm, or 57nm, or 60nm, or 61nm, or 64nm, or 65nm.

[0080] The preparation method of the transparent conductive film on the back and the photovoltaic device have the same or similar beneficial effects as any of the aforementioned transparent conductive films on the back, and the relevant parts among the three can be referenced to each other. In order to avoid repetition, they will not be described here.

[0081] The transparent conductive film on the back of the present application is further explained below with reference to specific embodiments.

[0082] Example 1

[0083] A transparent conductive film on the back surface was prepared using RPD. During the preparation process, the ratio of the oxygen flow rate to the total flow rate of the mixed gas was 39%. The resulting transparent conductive film had a molar ratio of indium to cadmium of 0.185%. The film had a thickness of 110 nm and was deposited on a 2 mm thick glass substrate.

[0084] Example 2

[0085] In Example 2, the molar ratio of indium to cadmium in the transparent conductive film formed on the back surface is 0.465%. The rest of Example 2 is the same as Example 1.

[0086] Example 3

[0087] In Example 3, the molar ratio of indium to cadmium in the transparent conductive film formed on the back surface is 0.652%. The rest of Example 3 is the same as Example 1.

[0088] Example 4

[0089] In Example 4, the molar ratio of indium to cadmium in the transparent conductive film formed on the back surface is 0.793%. The rest of Example 4 is the same as Example 1.

[0090] Example 5

[0091] In Example 5, the molar ratio of indium to cadmium in the transparent conductive film formed on the back surface is 0.934%. The rest of Example 5 is the same as Example 1.

[0092] Example 6

[0093] In Example 6, the molar ratio of indium to cadmium in the transparent conductive film formed on the back surface is 2.861%. The rest of Example 6 is the same as Example 1.

[0094] The electrical properties of the transparent conductive films on the back side of Examples 1 to 6, which were disposed on a glass substrate with a thickness of 2 mm, were measured. The results are shown in Table 1 below.

[0095] Table 1: Comparison of electrical properties of the transparent conductive films on the back side of Examples 1 to 6

[0096] From Table 1 above, it can be concluded that as X increases, the carrier concentration of the transparent conductive film on the back increases, the migration increases first and then decreases, and the square resistance decreases. In general, the carrier concentration of the transparent conductive film on the back in Examples 1 to 6 is approximately 9.80×10 19 cm-3 to 4.81×10 20 cm -3 The migration rate is 72cm 2 / V·S to 194.3cm 2 / V·S, and the square resistance is between 10.37Ω and 46.14Ω. Table 1 shows that the electrical performance of the back transparent conductive film of the present application is superior to that of the back transparent conductive film of the prior art whose main component is indium oxide. In other words, the electrical performance of the back transparent conductive film of the present application is superior to that of the back transparent conductive film of the prior art whose main component is indium oxide.

[0097] In particular, in the present application, when X is greater than or equal to 0.465% and less than or equal to 0.793%, the electrical properties of the transparent conductive film on the back are better, more specifically, the carrier concentration is lower, the mobility is higher, and the sheet resistance is smaller.

[0098] XRD (Diffraction of x-rays) spectrum measurement was performed on the transparent conductive film on the back side of Example 1, Example 3, Example 5, and Example 6, which were arranged on a glass substrate with a thickness of 2 mm, and the results are shown in Figure 3. Figure 3 shows a schematic diagram of the XRD spectrum distribution of a transparent conductive film on the back side in an embodiment of the present application. The four spectra from top to bottom in Figure 3 correspond to the transparent conductive film on the back side in Example 1, Example 3, Example 5, and Example 6, respectively. In order to reduce the overlap of the spectra corresponding to different embodiments and clearly see the differences between the various embodiments, the remaining embodiments except Example 6 are the result of shifting the spectra upward. Specifically, Example 5 is the result of shifting the spectrum on the vertical axis by approximately 75 in intensity. Example 3 is the result of shifting the spectrum on the vertical axis by approximately 150 in intensity. Example 1 is the result of shifting the spectrum on the vertical axis by approximately 260 in intensity. As can be seen from Figure 3, the number of crystal grains along the 111 crystal plane is the largest in the back transparent conductive films of Examples 1, 3, 5, and 6, and the ratio of the intensity of the strongest peak to the intensity of the second strongest peak of the back transparent conductive film is greater than or equal to 50. Furthermore, in Figure 3, as X increases, the crystallinity of the back transparent conductive film deteriorates.

[0099] The effective total transmittance (TTE) spectra of the back-side transparent conductive films of Examples 1 to 6, which were disposed on a 2mm thick glass substrate, were measured, and the results are shown in Figure 4. Figure 4 shows a schematic diagram of the effective total transmittance spectrum distribution of a back-side transparent conductive film in an embodiment of the present application. As can be seen from Figure 4, when X is greater than or equal to 0.465% and less than or equal to 0.793%, the effective total transmittance of the back-side transparent conductive film within the wavelength range of 800nm ​​to 1200nm is greater than or equal to 0.98.

[0100] In summary, based on the electrical properties of the back transparent conductive film shown in Table 1 and the effective total transmittance spectrum distribution of the back transparent conductive film shown in FIG4 , after light enters the light-facing side of the photovoltaic device, it preferentially absorbs short-wavelength light and reaches the backlight side, leaving mainly long-wavelength light. Therefore, in the transparent conductive film on the back of the photovoltaic device, the more preferred X is greater than or equal to 0.465% and less than or equal to 0.793%.

[0101] The photovoltaic device using the transparent conductive film on the back of the present application will be further explained below with reference to specific embodiments.

[0102] Example 7

[0103] The backside transparent conductive film was prepared using RPD. During the preparation process, the ratio of the oxygen flow rate to the total flow rate of the mixed gas was 39%. The resulting backside transparent conductive film had a molar ratio of indium to cadmium of 0.185%. The backside transparent conductive film had a thickness of 65 nm and was deposited on a 2 mm thick glass substrate.

[0104] A 65 nm thick transparent conductive film 2 on a 2 nm thick glass substrate and on the back side of the glass substrate is provided in the heterojunction solar cell shown in FIG. 2 .

[0105] Example 8

[0106] In Example 8, the molar ratio of indium to cadmium in the transparent conductive film on the back surface is 0.465%. The rest of Example 8 is the same as Example 7.

[0107] Example 9

[0108] In Example 9, the molar ratio of indium to cadmium in the transparent conductive film on the back surface is 0.652%. The rest of Example 9 is the same as Example 7.

[0109] Example 10

[0110] In Example 10, the molar ratio of indium to cadmium in the transparent conductive film on the back surface is 0.793%. The rest of Example 10 is the same as Example 7.

[0111] Example 11

[0112] In Example 11, the molar ratio of indium to cadmium in the transparent conductive film on the back surface is 0.934%. The rest of Example 11 is the same as Example 7.

[0113] Example 12

[0114] In Example 12, the molar ratio of indium to cadmium in the transparent conductive film on the back surface is 2.861%. The rest of Example 12 is the same as Example 7.

[0115] The electrical performance tests were conducted on the heterojunction solar cells in Examples 7 to 12, and the test structure was referred to FIG5 . FIG5 shows a schematic diagram of the electrical performance distribution of the heterojunction solar cells in the embodiments of the present application. In FIG5 , the electrical performance of the existing heterojunction solar cells manufactured using the same process is set to 1. The structure of the existing heterojunction solar cell is the same as that in FIG2 , with the only difference being that the transparent conductive film 2 on the back of the existing heterojunction solar cell is the existing transparent conductive film 2 on the back, the main component of which is indium oxide, and the rest are the same.

[0116] Figure 5 contains four sub-figures. The upper left sub-figure is a schematic diagram of the conversion efficiency (Eff) distribution of a heterojunction solar cell; the upper right sub-figure is a schematic diagram of the short-circuit current (Isc) distribution of a heterojunction solar cell; the lower left sub-figure is a schematic diagram of the open-circuit voltage (Voc) distribution of a heterojunction solar cell; and the lower right sub-figure is a schematic diagram of the fill factor (FF) distribution of a heterojunction solar cell. Each sub-figure in Figure 5, from left to right, shows the cell performance parameters of the heterojunction solar cell corresponding to X = 0.185%, X = 0.465%, X = 0.652%, X = 0.793%, X = 0.934%, and X = 2.861%, respectively. In other words, each sub-figure in Figure 5, from left to right, shows the cell performance parameters of the heterojunction solar cell corresponding to Examples 1 to 6, respectively. Figure 5 shows that by using the transparent conductive film 2 on the back side of the present application, the cell performance of existing heterojunction solar cells is essentially achieved. Moreover, when X is greater than or equal to 0.465% and less than or equal to 0.793%, the FF of the heterojunction solar cell of the embodiment of the present application is superior to the FF of the existing heterojunction solar cell. Furthermore, compared to the transparent conductive film on the back side of the prior art, the present application adds cadmium. Furthermore, the content of indium in the transparent conductive film on the back side is very low compared to cadmium. Furthermore, the content of cadmium in the earth's crust far exceeds that of indium, thereby significantly reducing the cost of the transparent conductive film on the back side.

[0117] It should be noted that in Figure 5, when X is 0.185%, the reason for the low FF may be due to the large square resistance of the transparent conductive film 2 on the back. When X is 2.861%, the reason for the low FF is that the contact resistance between the transparent conductive film 2 on the back and the doped passivation layer 3 on the back is too large. As X increases, the battery Isc becomes smaller and smaller, which is related to the change in the effective total transmittance of the transparent conductive film 2 on the back in the long wavelength band. The contact resistivity between the transparent conductive film 2 on the back and the metal electrode 1 on the back in this application is less than 0.02Ω·cm 2 .

[0118] It should be noted that, for the sake of simplicity, the method embodiments are described as a series of action combinations, but those skilled in the art should be aware that the embodiments of the present application are not limited by the order of the actions described, because according to the embodiments of the present application, certain steps can be performed in other orders or simultaneously. Secondly, those skilled in the art should also be aware that the embodiments described in the specification are all preferred embodiments, and the actions involved are not necessarily required by the embodiments of the present application.

[0119] References herein to "one embodiment," "an embodiment," or "one or more embodiments" mean that a particular feature, structure, or characteristic described in connection with the embodiment is included in at least one embodiment of the present application. Furthermore, please note that instances of the phrase "in one embodiment" do not necessarily all refer to the same embodiment.

[0120] In the description provided herein, a large number of specific details are described. However, it is understood that the embodiments of the present application can be practiced without these specific details. In some instances, well-known methods, structures, and techniques are not shown in detail so as not to obscure the understanding of this description.

[0121] In the claims, any reference signs placed between brackets shall not be construed as limiting the claims. The word "comprising" does not exclude the presence of elements or steps not listed in the claims. The word "a" or "an" preceding an element does not exclude the presence of a plurality of such elements. The use of the words first, second, and third, etc. in this application does not indicate any order. These words may be interpreted as names. Finally, it should be noted that the above embodiments are only used to illustrate the technical solutions of the present application, not to limit them; although the present application has been described in detail with reference to the aforementioned embodiments, those skilled in the art should understand that they can still modify the technical solutions described in the aforementioned embodiments, or make equivalent replacements for some of the technical features therein; and these modifications or replacements do not deviate the essence of the corresponding technical solutions from the spirit and scope of the technical solutions of the various embodiments of the present application.

Claims

1. A transparent conductive film for the back of a photovoltaic device, in, include: Cadmium, oxygen and indium; In the transparent conductive film on the back side, the molar ratio of the indium element to the cadmium element is X, and X is greater than or equal to 0.185% and less than or equal to 2.861%.

2. The transparent conductive film for the back of a photovoltaic device according to claim 1, in, The X is greater than or equal to 0.465% and less than or equal to 0.793%.

3. The transparent conductive film for the back side of a photovoltaic device according to claim 1, in, In the transparent conductive film on the back side, the molar ratio of the oxygen element is 30% to 70%.

4. The transparent conductive film for the back side of a photovoltaic device according to claim 1, in, The mobility of the transparent conductive film on the back side is 70 square centimeters per volt per second to 260 square centimeters per volt per second.

5. The transparent conductive film for the back side of a photovoltaic device according to claim 2, in, The mobility of the transparent conductive film on the back side is 160 square centimeters per volt per second to 230 square centimeters per volt per second.

6. The transparent conductive film for the back side of a photovoltaic device according to claim 1, in, The sheet resistance of the transparent conductive film on the back side is 10 ohms to 47 ohms.

7. The transparent conductive film for the back of a photovoltaic device according to claim 2, in, The sheet resistance of the transparent conductive film on the back side is 20 ohms to 26 ohms.

8. The transparent conductive film for the back side of a photovoltaic device according to any one of claims 1 to 7, in, In the transparent conductive film on the back side, the number of crystal grains along the 111 crystal plane direction is the largest.

9. The transparent conductive film for the back side of a photovoltaic device according to any one of claims 1 to 7, in, In the X-ray diffraction image, the ratio of the intensity of the strongest peak of the transparent conductive film on the back side to the intensity of the second strongest peak is greater than or equal to 50.

10. The transparent conductive film for the back side of a photovoltaic device according to any one of claims 1 to 7, in, In a wavelength band of 800 nm to 1200 nm, the effective total transmittance of the transparent conductive film on the back side is greater than or equal to 0.

92.

11. The transparent conductive film for the back side of a photovoltaic device according to any one of claims 1 to 7, in, The thickness of the transparent conductive film on the back side is 50nm to 110nm.

12. The transparent conductive film for the back side of a photovoltaic device according to any one of claims 1 to 7, in, The transparent conductive film on the back side further contains hydrogen element, and the mass proportion of the hydrogen element is 0 to 0.1%.

13. A method for preparing a transparent conductive film for the back side of a photovoltaic device according to any one of claims 1 to 12, in, include: Providing target materials; The target material comprises: cadmium element, oxygen element and indium element; in the target material, the molar ratio of the indium element to the cadmium element is Y, and the Y is greater than or equal to 0.185% and less than or equal to 2.861%; Based on the target material, a transparent conductive film on the back side is prepared.

14. The preparation method according to claim 13, in, The method of preparing the transparent conductive film on the back side based on the target material comprises: A transparent conductive film on the back is prepared based on the target material by adopting one of reactive plasma deposition, sputtering and physical vapor deposition.

15. The preparation method according to claim 14, in, The method of using one of reactive plasma deposition, sputtering and physical vapor deposition to prepare a transparent conductive film on the back based on the target material comprises: During the entire preparation process of the transparent conductive film on the back side, a mixed gas is introduced; the mixed gas includes oxygen and inert gas; the ratio of the flow rate of the oxygen to the total flow rate of the mixed gas is 30% to 50%.

16. A photovoltaic device, in, include: A transparent conductive film for the back side of a photovoltaic device as claimed in any one of claims 1 to 12.

17. The photovoltaic device according to claim 16, in, The photovoltaic device is a heterojunction solar cell. In the heterojunction solar cell, the thickness of the transparent conductive film on the back side is 47 nm to 65 nm.

Citation Information

Patent Citations

  • Method for preparing transparent low resistance / high resistance composite membrane used for thin-film solar cell

    CN101447533A

  • Preparation method for electroconductive film with cadmium oxide base light-transmitting waveband adjustable

    CN103107244A

  • Conductive film, and making method and application thereof

    CN103963367A

  • Conductive film as well as preparation method and application thereof

    CN104674173A

  • Thin film infrared transparent conductor

    US20020146599A1

Cited By

  • Back contact cell and manufacturing method thereof, laminated cell and photovoltaic module

    CN122396113A