Optical fiber coating composition, optical fiber, and preparation method therefor

By using specific compounds of formula I as photoinitiators in the optical fiber coating composition, the initiation efficiency and environmental aging resistance of optical fiber coating are improved, and the efficiency and volatiles of optical fiber coating compositions in the prior art are solved. Problem, efficient fiber coating and healthy and safe production have been achieved.

WO2024235062A1PCT designated stage expired Publication Date: 2024-11-21SHANGHAI PHICHEM MATERIAL CO LTD

Patent Information

Application Number
PCT/CN2024/091524
Authority / Receiving Office
WO · WO
Patent Type
Applications
Current Assignee / Owner
Priority Date
2023-05-12
Filing Date
2024-05-07
Publication Date
2024-11-21

AI Technical Summary

Technical Problem

The existing fiber optic coating compositions have problems such as low efficiency, low chain radical reaction efficiency, low wire drawing efficiency and easy volatiles during curing, and may have an impact on life and health.

Method used

An optical fiber coating composition is employed which comprises 35-95% photocuring oligomer, 1-45% photocuring active monomer, 0.5-15% photoinitiator and 0.1-10% auxiliary agent, wherein Photoinitiators include specific compounds of formula I, which improve the wavelength sensitivity of chemical reactions and the efficiency of free chain reactions, improve the volatility and health hazards of the composition, and form a coating layer with high density crosslink density through ultraviolet curing.

Benefits of technology

It improves the initiation efficiency of fiber coating, reduces the generation of volatiles, improves the environmental aging resistance and signal transmission performance of the fiber, is suitable for high-speed wire drawing production, and is healthier and safer.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN2024091524_21112024_PF_FP_ABST
    Figure CN2024091524_21112024_PF_FP_ABST
Patent Text Reader

Abstract

The present application provides an optical fiber coating composition, and an optical fiber coated with the composition. The optical fiber coating composition comprises, by weight of the composition, 35-95wt% of a photocurable oligomer, 1-45wt% of a photocurable active monomer, 0.5-15wt% of a photoinitiator, and 0.1-10wt% of an auxiliary agent, wherein the photoinitiator comprises at least one compound as shown in general formula I. When the composition is applied to optical fiber coating, the initiation efficiency can be improved and volatiles can be reduced, and the optical fiber using the composition has good environmental aging resistance and signal transmission performance.
Need to check novelty before this filing date? Find Prior Art

Description

Optical fiber coating composition, optical fiber and preparation method thereof

[0001] This application claims priority to Chinese patent application No. 202310540156.8, filed on May 12, 2023, entitled “An optical fiber coating composition, an optical fiber, and a method for preparing the same,” the entire contents of which are incorporated herein by reference. Technical Field

[0002] The present application relates to a coating composition in the field of optical fiber communication, and in particular to a composition for optical fiber coating, an optical fiber prepared by coating the composition, and a method for preparing an optical fiber. Background Art

[0003] Optical fiber is a key material for the construction of information industry infrastructure, particularly as a critical transmission carrier and core component for fiber-optic communications, playing a vital supporting role in the national economy. Optical fiber is a dielectric cylindrical optical waveguide that confines and guides light waves and electromagnetic fields along its axis within or near its surface. Generally, an optical fiber consists of a glass core, a glass cladding, and an organic coating. The glass core and cladding of single-mode or multimode communication optical fibers are typically composed of high-purity silica and germanium dioxide doped in the glass. While the quartz glass fiber comprising the glass core and cladding possesses high longitudinal tensile strength, it is also brittle and easily breaks when bent. Furthermore, quartz glass fiber itself is not resistant to moisture and corrosive gases or liquids. To make quartz glass fiber practical, the outer surface of the glass fiber is typically coated with one or more layers of an organic polymer material to effectively protect it. This not only improves the fiber's environmental reliability but also enhances its optical performance.

[0004] Chinese patent CN202110299848 discloses a heat-resistant, light-cured optical fiber coating and its preparation method. The components of the optical fiber coating include alkoxylated nonylphenol acrylate, 2-hydroxy-2-methyl-1-phenyl-1-propanone, benzoin ethyl ether, 3-aminopropyltrimethoxysilane, polyether acrylate, modified polyurethane, and organic silica slurry. The organic silica particles are prepared from organosiloxane, trimethoxysilane, pentaerythritol tetra-3-mercaptopropionate, and diacrylamido-2-methylpropanesulfonic acid. The organosiloxane is one of methyltrimethoxysilane and hexadecyltrimethoxysilane. The main function of the optical fiber coating is to protect the optical fiber from the influence of the external environment and provide a certain degree of mechanical strength and optical performance. The technical solution of this patent has the problems of low initiation efficiency and the easy generation of volatile substances during the curing process.

[0005] Chinese patent CN201980013837 discloses a coating composition and a cured product formed therefrom. The coating composition comprises an oligomer, an alkoxylated monofunctional acrylate monomer, and preferably, an N-vinylamide compound. However, the technical solution of this patent suffers from low chain radical reaction efficiency and low wire drawing efficiency.

[0006] Chinese patent CN201880036549 discloses a curable composition and its use, using one or more (meth)acrylate-functionalized compounds and one or more reactive comonomers, such as a mixture of 1,1-diester-1-ene (e.g., methylene malonate), 1,1-diketone-1-ene, 1-ester-1-keto-1-ene, and / or itaconate. The technical solution in this patent suffers from high energy consumption during the curing process and the generation of volatiles.

[0007] Chinese patent CN201780082334 discloses an optical fiber coating with low modulus and high critical stress. This coating achieves low Young's modulus, high tear strength, and / or high critical stress by using a coating composition comprising an oligomer material formed from an isocyanate, a hydroxy acrylate compound, and a polyol. The oligomer material comprises a polyether urethane acrylate and a diadduct compound. The technical solution in this patent suffers from low chain radical reaction efficiency and low fiber drawing efficiency.

[0008] Chinese patent CN201611141284 discloses a polyurethane acrylate prepolymer. The raw materials for this prepolymer include dihydroxy-terminated polysiloxane, isocyanate, hydroxy acrylate, a polymerization inhibitor, and a catalyst. This prepolymer increases the operating temperature of conventional polyurethane acrylate prepolymers. However, the technical solution in this patent suffers from low wire drawing efficiency and the generation of volatiles during the curing process.

[0009] In summary, existing coating compositions present industry technical challenges such as low initiation efficiency, low chain radical reaction efficiency, low fiber drawing efficiency, and the generation of high levels of volatiles during curing, as well as potential health risks. Therefore, a novel coating composition for optical fiber coating is urgently needed to address these existing challenges.

[0010] Public content

[0011] Purpose of the invention: The purpose of this application is to provide an optical fiber coating composition, which, when applied to optical fiber coating, can improve initiation efficiency and reduce volatiles.

[0012] Furthermore, the purpose of the present application is to provide an optical fiber comprising the composition coated thereon and a method for preparing the optical fiber, wherein the optical fiber has good environmental aging resistance and signal transmission performance.

[0013] Technical solution: An optical fiber coating composition comprising: based on the weight of the composition, 35-95 wt% of a photocurable oligomer, 1-45 wt% of a photocurable active monomer, 0.5-15 wt% of a photoinitiator, and 0.1-10 wt% of an auxiliary agent, wherein the photoinitiator comprises at least one compound represented by formula I:

[0014] wherein R1, R2, and R3 are the same or different and are each independently selected from a substituted or unsubstituted alkyl or alkoxy group of 1 to 5 carbon atoms, wherein the substituent is selected from an alkyl or alkoxy group of 1 to 3 carbon atoms;

[0015] n=1, 2 or 3; the alkyl group of 1-5 carbon atoms is selected from methyl, ethyl, propyl, isopropyl, n-butyl, isobutyl, sec-butyl, tert-butyl, n-pentyl, -CH(CH3)CH2CH2CH3, -CH2CH(CH3)CH2CH3, -CH2CH2CH(CH3)2, -CH(C2H5)CH2CH3, -C(CH3)2CH2CH3, -CH(CH3)CH(CH3)2 and -CH2C(CH3)3; the alkoxy group of 1-5 carbon atoms is selected from methoxy, ethoxy, propoxy, butoxy and pentoxy.

[0016] In some embodiments of the present application, R3 is selected from methyl, ethyl, propyl or isopropyl; in some embodiments of the present application, R3 is preferably methyl.

[0017] After the above-mentioned alkyl group is introduced into the structure, the thermal stability of the initiator is further improved, which can reduce the volatilization of the initiator during the photocuring process.

[0018] In some embodiments of the present application, the R3 substitution position may be the ortho position, the meta position, or the para position; in some embodiments of the present application, the R3 substitution position is preferably the ortho position and the para position.

[0019] In some embodiments of the present application, n is preferably 3.

[0020] In some embodiments of the present application, the photoinitiator preferably includes at least one compound of formula II:

[0021] In some embodiments of the present application, R1 and R2 are each independently selected from methyl, ethyl, propyl or isopropyl; in some embodiments of the present application, R1 and R2 are each independently preferably methyl.

[0022] In some embodiments of the present application, the substitution positions of R1 and R2 may be ortho, meta or para; in some embodiments of the present application, the substitution positions of R1 and R2 are preferably para.

[0023] In some embodiments of the present application, R1 and R2 are each a para-substituted methyl group, which can further improve the wavelength sensitivity of the chemical reaction, the efficiency of the free chain reaction, and improve the volatility and health hazards of the composition.

[0024] There are two more methyl groups at the para position of the two benzene rings connected to the phosphorus oxygen group. The methyl groups and the structure of the benzene ring form a σ-π hyperconjugated structure. Compared with the conjugated structure of the benzene ring, the σ-π hyperconjugated structure has lower conjugation energy and higher activity. Under the condition of free radical formation under light, it is easier to initiate polymerization, thereby increasing the cross-linking density of the system, thereby improving the curing efficiency and reducing the volatilization of small molecular monomers in the system.

[0025] The photoinitiator of the present application includes one or more compounds of formula I.

[0026] In some embodiments of the present application, the photoinitiator preferably includes at least one compound of formula II.

[0027] In some embodiments of the present application, the compound of formula I accounts for 0.5-15% by weight of the optical fiber coating composition. Specific examples may include 0.5%, 1%, 1.5%, 2%, 2.5%, 3%, 3.5%, 4%, 4.5%, 5%, 5.5%, 6%, 6.5%, 7%, 7.5%, 8%, 8.5%, 9%, 9.5%, 10%, 11%, 12%, 13%, 14%, 15% or a range between any two of these values.

[0028] In some embodiments of the present application, the weight percentage of the compound of formula I in the optical fiber coating composition is preferably 0.5-8%. Within this addition range, the compound of formula I can further improve the effect of residual free radicals on aging performance and improve yellowing performance.

[0029] In some embodiments of the present application, the compound of general formula I can also be used in combination with one or more of the following initiators, such as phenyl bis(2,4,6-trimethylbenzoyl)phosphine oxide, 1-hydroxycyclohexyl phenyl ketone, 2-hydroxy-2-methyl-1-phenyl-1-propanone, benzophenone, 2,2-dimethoxy-2-phenylacetophenone, 2-hydroxy-4'-(2-hydroxyethoxy)-2-methylpropiophenone, 2-isopropylthioxanthone, and 2,4-diethylthiazolone, and the combination can be one, two, three, or four of them.

[0030] In some embodiments of the present application, the amount of the initiator added together with the compound of formula I is no more than 5% by weight of the optical fiber coating composition.

[0031] In some embodiments of the present application, the coating composition includes 35-95% by weight of the optical fiber coating composition, based on the weight of the optical fiber coating composition. Specific examples can include 35%, 38%, 40%, 42%, 45%, 48%, 50%, 53%, 55%, 58%, 60%, 63%, 65%, 68%, 70%, 72%, 75%, 78%, 80%, 82%, 85%, 88%, 90%, 92%, 95%, or a range between any two of these values.

[0032] In some embodiments of the present application, the light-curable oligomer preferably accounts for 50-95% by weight of the optical fiber coating composition. Within the above addition range, a more suitable film thickness can be obtained, and environmental aging performance and volatility can be further improved.

[0033] In some embodiments of the present application, the photocurable oligomer includes at least one of a polyurethane acrylate oligomer and an epoxy acrylate oligomer.

[0034] In some embodiments of the present application, the polyurethane acrylate oligomer is one or more of a monofunctional polyurethane acrylate oligomer, a difunctional polyurethane acrylate oligomer, or a trifunctional polyurethane acrylate oligomer, preferably a difunctional polyurethane acrylate oligomer or a trifunctional polyurethane acrylate oligomer.

[0035] In some embodiments of the present application, the epoxy acrylate oligomer is one or more of a monofunctional epoxy acrylate oligomer, a difunctional epoxy acrylate oligomer, or a trifunctional epoxy acrylate oligomer, preferably a difunctional epoxy acrylate oligomer.

[0036] The polyurethane acrylate oligomer of the present application is prepared from diisocyanate and acrylate containing hydroxyl groups. During the preparation process, a chain extender is added to the reactants to increase the molecular chain length of the polyurethane acrylate oligomer.

[0037] In some embodiments of the present application, the chain extender is selected from at least one of polyester diols, alkyl diols, and polyether diols, preferably polyether diols.

[0038] In some embodiments of the present application, the polyurethane acrylate oligomer may be a single oligomer or a combination of multiple oligomers.

[0039] In some embodiments of the present application, the polyurethane acrylate oligomer is a non-chain-extended polyurethane acrylate oligomer.

[0040] In some embodiments of the present application, the polyurethane acrylate oligomer is a combination of at least one unextended polyurethane acrylate oligomer and at least one extended polyurethane acrylate oligomer. The polyurethane acrylate oligomer can further coordinate and balance the strength and elongation of the coating composition after curing.

[0041] In some embodiments of the present application, the diisocyanate is selected from toluene diisocyanate (TDI), isophorone diisocyanate (IPDI), 4,4'-dicyclohexylmethane diisocyanate (HMDI), diphenylmethane diisocyanate (MDI), and hexamethylene diisocyanate (HDI) trimer.

[0042] In some embodiments of the present application, the acrylate containing a hydroxyl group is selected from at least one of hydroxyethyl acrylate (HEA), hydroxypropyl acrylate (HPA), hydroxyethyl methacrylate (HEMA), and hydroxypropyl methacrylate (HPMA).

[0043] In some embodiments of the present application, the epoxy acrylate oligomer is selected from the group consisting of bisphenol A epoxy resin and a photopolymerizable compound containing a carboxyl group.

[0044] The photopolymerizable compound containing a carboxyl group is a compound containing a carboxyl group at one end and a photoinitiable double bond at the other end.

[0045] In some embodiments of the present application, the compound containing a carboxyl group at one end and a photoinitiable double bond at the other end is acrylic acid, methacrylic acid, or a compound obtained by the reaction of an acid anhydride and a hydroxy acrylate.

[0046] The acid anhydride is selected from at least one of succinic anhydride, maleic anhydride, phthalic anhydride and tetrahydrophthalic anhydride.

[0047] The hydroxy acrylate compound is selected from hydroxyethyl acrylate (HEA), hydroxypropyl acrylate (HPA), hydroxyethyl methacrylate (HEMA), and hydroxypropyl methacrylate (HPMA).

[0048] In some embodiments of the present application, the coating composition includes 1-45% by weight of the optical fiber coating composition, based on the weight of the optical fiber coating composition. Specific examples may include 1%, 5%, 10%, 12%, 15%, 18%, 20%, 23%, 25%, 28%, 30%, 33%, 35%, 38%, 40%, 42%, 45% or a range between any two of these values.

[0049] The photocurable reactive monomer includes at least one of a monofunctional photocurable reactive monomer and a multifunctional photocurable reactive monomer. In some embodiments of the present application, the multifunctional photocurable reactive monomer is a difunctional photocurable reactive monomer and a trifunctional photocurable reactive monomer.

[0050] In some embodiments of the present application, the monofunctional monomer includes one or more combinations of: 2-phenoxyethyl acrylate (PHEA), isobornyl acrylate (IBOA), isodecyl acrylate, isooctyl acrylate, polyethylene glycol o-phenylphenyl ether acrylate (OPPEA), N-vinyl caprolactam, and nonylphenol polyoxyethylene ether acrylate.

[0051] In some embodiments of the present application, the coating composition includes 0-36% by weight of the monofunctional photocurable reactive monomer based on the weight of the optical fiber coating composition. Specific examples may include 0%, 1%, 5%, 10%, 12%, 15%, 18%, 20%, 23%, 25%, 28%, 30%, 33%, 36% or a range between any two of these values.

[0052] In some embodiments of the present application, the monofunctional photocurable monomer preferably accounts for 0-20% by weight of the optical fiber coating composition. If the monofunctional monomer is added in an excessive amount, the curing speed will be affected and the volatility will be higher.

[0053] The bifunctional photocurable reactive monomers include 1,6-hexanediol diacrylate (HDDA), tripropylene glycol diacrylate (TPGDA), and dipropylene glycol diacrylate (DPGDA).

[0054] The trifunctional photocurable reactive monomer includes trimethylolpropane triacrylate (TMPTA).

[0055] In some embodiments of the present application, the auxiliary agent is one or more combinations of a silane coupling agent, an active amine auxiliary agent, and a leveling agent; the silane coupling agent is one or more combinations of mercaptopropyltrimethoxysilane and 3-chloropropyltrioxysilane; the active amine auxiliary agent is one or more combinations of ethylenediamine and amine-modified acrylate; the leveling agent is one or more combinations of an organosilicon leveling agent and an acrylate leveling agent.

[0056] In some embodiments of the present application, the optical fiber coating composition includes 0.1-10% (e.g., 0.1% to 5%, 0.5% to 10%, 0.5% to 5%, 1% to 5%, or a value within one of these ranges) of an adjuvant by weight of the optical fiber coating composition. Specific examples may include 0.1%, 0.25%, 0.5%, 0.75%, 1%, 2%, 3%, 4%, 5%, 6%, 7%, 8%, 9%, 10%, or a range between any two of these values.

[0057] The optical fiber coating composition described in the present application is suitable for ultraviolet curing at any wavelength within the range of 200-405 nm.

[0058] Another object of the present application is to provide an optical fiber comprising the optical fiber coating composition.

[0059] The optical fiber comprises a core, a cladding, a primary coating layer and a secondary coating layer. The cladding is wrapped around the outer layer of the core, the primary coating layer is wrapped around the outer layer of the cladding, and the secondary coating layer is wrapped around the outer layer of the primary coating layer.

[0060] The fiber core and cladding include silicon dioxide, germanium dioxide or materials doped with silicon dioxide and germanium dioxide.

[0061] At least one of the primary coating layer and the secondary coating layer is formed by ultraviolet curing of the optical fiber coating composition.

[0062] In some embodiments of the present application, the primary coating layer is formed by UV curing the optical fiber coating composition described in the present application.

[0063] In some embodiments of the present application, the secondary coating layer is formed by UV curing the optical fiber coating composition described in the present application.

[0064] In some embodiments of the present application, both the primary coating layer and the secondary coating layer are formed by ultraviolet curing of the optical fiber coating composition described in the present application.

[0065] Another object of the present application is to provide a method for preparing an optical fiber comprising the optical fiber coating composition. The preparation method comprises the following steps:

[0066] 1) Place the preform on the chuck of the feeding mechanism, put the preform into a high-temperature heating furnace to soften and melt, condense into a ball-shaped filament, and vertically thin under its own weight to form a bare optical fiber;

[0067] 2) The bare optical fiber passes through the mold soaked in the primary coating composition, the mold soaked in the secondary coating composition, the light curing furnace, bypasses the tension wheel, guide wheel, and traction wheel on the drawing, and is finally wound on the take-up drum.

[0068] In some embodiments of the present application, when the bare optical fiber passes through a mold dipped in a primary coating composition, it passes through a light-curing oven, then passes through a mold dipped in a secondary coating composition, and then passes through a light-curing oven to complete the curing.

[0069] In some embodiments of the present application, the speed at which the optical fiber passes through the light curing oven (hereinafter referred to as the drawing speed) is 2500 m / min-3500 m / min.

[0070] In some embodiments of the present application, the curing light source of the light curing oven is ultraviolet light, and the wavelength is any wavelength range of 200-405 nm.

[0071] Compared with the prior art, the advantages of this application are as follows:

[0072] (1) The present application provides an optical fiber coating composition comprising a compound of formula I, which solves the technical problems of low chemical reaction wavelength sensitivity, low free radical chain reaction efficiency, and high volatile matter of traditional photoinitiators, and avoids the health effects that may be caused by traditional photoinitiators such as photoinitiator TPO.

[0073] (2) The optical fiber coating composition provided in this application has high UV curing efficiency and is suitable for the production of optical fibers with high-speed drawing speeds of more than 2500 m / min.

[0074] (3) The coating layer formed by curing the optical fiber coating composition provided in the present application improves the environmental aging resistance of the optical fiber and has high strength, can protect the optical fiber cladding from damage, and reduce the attenuation of the optical signal, and has good application prospects in the optical fiber manufacturing industry.

[0075] (4) The optical fiber provided in this application improves the environmental reliability of the optical fiber, is green and environmentally friendly, and is healthier for life, and is suitable for large-scale production. BRIEF DESCRIPTION OF THE DRAWINGS

[0076] In order to more clearly illustrate the technical solutions in the embodiments of the present application, the following briefly introduces the drawings required for use in the description of the embodiments. Obviously, the drawings described below are only some embodiments of the present application. For ordinary technicians in this field, other drawings can be obtained based on these drawings without any creative work.

[0077] FIG1 is a schematic diagram of the structure of an optical fiber including a coating composition.

[0078] The reference numerals represent:

[0079] 1. Fiber core; 2. Cladding; 3. First coating layer; 4. Second coating layer. DETAILED DESCRIPTION

[0080] The present application is described in detail below in conjunction with the accompanying drawings and specific embodiments. The aspects described below in conjunction with the accompanying drawings and specific embodiments are merely exemplary and should not be understood as limiting the scope of protection of the present application.

[0081] In this application, unless otherwise specified, all ratios are by weight and all temperatures are in degrees Celsius.

[0082] Test method:

[0083] Volatile emission test method: Place a glass slide in an oven and dry for 30 minutes. Then take it out of the oven and place it in a desiccator to cool to room temperature. The weight is recorded as M1. Apply the coating sample on the glass slide to form a coating film of appropriate thickness, and weigh the total weight of the glass slide + coating, recorded as M2. Place the glass slide in a container box with a high-purity quartz glass upper layer, pass nitrogen for 1 minute, exhaust the air in the container, and then place it under a UV light source for curing. The light source energy is set to 1500mJ / cm 2 The conveyor belt speed is set to 17m / min. After the curing is completed, nitrogen is passed for 1 minute to remove the volatile gas. The total weight of the glass slide + the cured coating is weighed and recorded as M3. At this time, the volatile amount of the sample = (M2-M3) / (M2-M1)*100%.

[0084] Example Curing speed test method: Coat the coating sample on a glass slide to form a coating film of appropriate thickness, and irradiate it under ultraviolet light for 1 second. Scan the irradiated sample surface with an infrared spectrometer to obtain the infrared spectrum of 1410 cm -1 Integrate the absorption peak of the standard absorption peak (such as 1730cm -1 The AU sample is determined by the integrated ratio of the two absorption peaks (S1410 / S1730). Uncured coating samples are tested in the same manner, with the integrated ratio of the two absorption peaks (L1410 / L1730) defined as the AU liquid. The degree of cure of the coating film can be calculated using the formula: ((AU liquid - AU sample) / AU liquid) * 100%. The cure rate is expressed as the degree of cure achieved within 1 second of irradiation.

[0085] Application Example Curing Degree Test Method:

[0086] 1) Use a dropper to take a small amount of the inner and outer layer liquid coating and drop it on the crystal surface, and measure the infrared spectrum of the liquid coating.

[0087] 2) Take the prepared optical fiber, stick the optical fiber surface to the crystal surface, press it tightly (note: the optical fiber must not spread out), and measure the infrared spectrum after the outer coating is cured.

[0088] 3) Take the optical fiber tested in step 2, cut off the coating layer of the optical fiber along the glass surface with a blade, and stick it on the crystal surface to measure the infrared spectrum after the inner coating is cured.

[0089] 4) 1410cm -1 Integrate the hydrocarbon absorption peak at 1730cm -1 The area integral ratio of the two absorption peaks is:

[0090] AU liquid = A liquid (1410cm -1 ) / A liquid (1730cm -1 ).

[0091] AU sample = A fiber sample (1410cm -1 ) / A optical fiber sample (1730cm -1 ).

[0092] Calculation: Degree of solidification = ((AU liquid - AU sample) / AU liquid) * 100%.

[0093] Optical fiber strength test method: Refer to GB / T15972.3-1998 Optical Fiber General Specification Part 3 Mechanical Properties Test Method.

[0094] Fiber attenuation test method: Refer to GB / T15972.4-1998 General Specification for Optical Fibers Part 4 Transmission Characteristics and Optical Characteristics Test Methods.

[0095] Fiber aging conditions: 85°C, 85% RH for 1 month.

[0096] The specific selection of compounds in the examples of this application is as follows:

[0097] Light-curing oligomers:

[0098] Oligomer 1: polyurethane acrylate oligomer, obtained by the direct end-capping reaction of hydroxyethyl methacrylate HEMA and toluene diisocyanate TDI.

[0099] Oligomer 2: Polyether polyurethane acrylate oligomer, obtained by reacting polyether diol with diphenylmethane diisocyanate MDI and then capping with hydroxypropyl methacrylate HPMA.

[0100] Oligomer 3: Epoxy acrylate oligomer, selected from Sanmu SM6104 epoxy acrylate.

[0101] Oligomer 4: modified epoxy acrylate oligomer, obtained by reacting phthalic anhydride with hydroxyethyl methacrylate (HEMA) and then with bisphenol A epoxy resin.

[0102] Photoinitiator:

[0103] Photoinitiator 1: a compound of formula I, wherein R1, R2, and R3 are methyl groups, and R1 and R2 are para-substituted; n=3, and the substitution positions are ortho and para.

[0104] Photoinitiator 2: Photoinitiator 2959.

[0105] Photoinitiator 3: Photoinitiator 184.

[0106] Photoinitiator 4: Photoinitiator TPO.

[0107] Additives:

[0108] Additive 1: silicone leveling agent Dow Corning DC-56.

[0109] Auxiliary agent 2: Active amine co-initiator: amine-modified acrylate, selected from Sartomer CN550.

[0110] Example 1:

[0111] The composition of the coating composition 1 is shown in Table 1 below:

[0112] Table 1

[0113] Example 2:

[0114] The composition of coating composition 2 is shown in Table 2 below:

[0115] Table 2

[0116] Example 3:

[0117] The composition of coating composition 3 is shown in Table 3 below:

[0118] Table 3

[0119] Example 4:

[0120] The composition of coating composition 4 is shown in Table 4 below:

[0121] Table 4

[0122] Example 5:

[0123] The composition of coating composition 5 is shown in Table 5 below:

[0124] Table 5

[0125] Example 6:

[0126] The composition of coating composition 6 is shown in Table 6 below:

[0127] Table 6

[0128] Example 7:

[0129] The composition of coating composition 7 is shown in Table 7 below:

[0130] Table 7

[0131] Comparative Example 1:

[0132] The composition of the comparative coating composition 1 is shown in Table 8 below:

[0133] Table 8

[0134] Comparative Example 2:

[0135] The composition of comparative coating composition 2 is shown in Table 9 below:

[0136] Table 9

[0137] Comparative Example 3:

[0138] The composition of comparative coating composition 3 is shown in Table 10 below:

[0139] Table 10

[0140] Comparative Example 4:

[0141] The composition of comparative coating composition 4 is shown in Table 11 below:

[0142] Table 11

[0143] The coating compositions of Examples 1-7 and Comparative Examples 1-4 were tested for curing speed and volatilization amount, respectively. The results are shown in Table 12 below:

[0144] Table 12

[0145] The coating compositions described in Examples 1-7 and Comparative Examples 1-2 were prepared according to the following method to form Application Examples 1-8 and Comparative Example 1, to complete optical fiber coating, and to characterize the optical fiber performance.

[0146] Preparation method: A preform rod is placed on the chuck of a feeding mechanism and placed in a high-temperature heating furnace to soften and melt. The preform then condenses into a ball-shaped filament, which then tapers vertically under its own weight to form a bare optical fiber. The bare optical fiber then passes through a mold impregnated with a primary coating composition, a mold impregnated with a secondary coating composition, and a light-curing furnace. It then passes over the tension pulley, guide pulley, and traction pulley on the drawing process, and is finally wound onto a take-up reel. The drawing speed is 3000 m / min, and the curing light source is an LED with a wavelength of 395 nm.

[0147] The difference between Application Examples 1-8 and Comparative Example 1 is that the coating compositions used in the first coating layer and the second coating layer are different, as shown in Table 13 below:

[0148] Table 13

[0149] The test results of the application example are shown in Table 14 below:

[0150] Table 14

[0151] The optical fiber coating was cured by adjusting the drawing speed to 2500 m / min and 3500 m / min in Application Example 1, Application Example 3, Application Example 8, and Application Comparative Example 1, respectively. The curing degree was tested. The results are shown in Table 15 below:

[0152] Table 15

[0153] The results of the above examples and comparative examples show that when the compound of formula I is added to the coating composition and optical fiber, the volatile matter is reduced, which can meet the requirements of high-speed optical fiber drawing. It effectively improves the curing speed of the coating layer and the curing degree of the optical fiber, reduces the signal attenuation of the fiber, improves the high temperature and high humidity resistance, and increases the environmental reliability of the optical fiber. Given the trend of increasing optical fiber drawing speeds, the coating composition has a good application prospect.

[0154] The above descriptions are merely some exemplary embodiments of the present application and are not intended to limit the present application. Any modifications, equivalent substitutions, improvements, etc. made within the spirit and principles of the present application shall be included in the scope of protection of the present application.

Claims

1. An optical fiber coating composition, wherein: The optical fiber coating composition comprises: based on the weight of the composition, 35-95 wt % of a photocurable oligomer, 1-45 wt % of a photocurable active monomer, 0.5-15 wt % of a photoinitiator, and 0.1-10 wt % of an auxiliary agent, wherein the photoinitiator comprises at least one compound represented by the general formula I: wherein R1, R2, and R3 are the same or different and are independently selected from substituted or unsubstituted alkyl or alkoxy groups of 1 to 5 carbon atoms, wherein the substituents are selected from alkyl or alkoxy groups of 1 to 3 carbon atoms; n=1, 2 or 3; the alkyl group of 1-5 carbon atoms is selected from methyl, ethyl, propyl, isopropyl, n-butyl, isobutyl, sec-butyl, tert-butyl, n-pentyl, -CH(CH3)CH2CH2CH3, -CH2CH(CH3)CH2CH3, -CH2CH2CH(CH3)2, -CH(C2H5)CH2CH3, -C(CH3)2CH2CH3, -CH(CH3)CH(CH3)2 and -CH2C(CH3)3; the alkoxy group of 1-5 carbon atoms is selected from methoxy, ethoxy, propoxy, butoxy and pentyloxy.

2. The optical fiber coating composition according to claim 1, wherein R1, R2 and R3 are each independently selected from methyl, ethyl, propyl or isopropyl.

3. The optical fiber coating composition according to claim 1, wherein The photocurable oligomer is selected from at least one of a polyurethane acrylate oligomer and an epoxy acrylate oligomer.

4. The optical fiber coating composition according to claim 3, wherein The polyurethane acrylate oligomer is one or more of a monofunctional polyurethane acrylate oligomer, a difunctional polyurethane acrylate oligomer or a trifunctional polyurethane acrylate oligomer.

5. The optical fiber coating composition according to claim 3, wherein The epoxy acrylate oligomer is one or more of a monofunctional epoxy acrylate oligomer, a difunctional epoxy acrylate oligomer or a trifunctional epoxy acrylate oligomer.

6. The optical fiber coating composition according to claim 1, wherein: The photocurable active monomer includes at least one of a monofunctional photocurable active monomer and a multifunctional photocurable active monomer.

7. The optical fiber coating composition according to any one of claims 1 to 6, wherein: The photoinitiator comprises one or more compounds of Formula I.

8. The optical fiber coating composition according to claim 7, wherein: The photoinitiator also includes one or more of the following substances: phenyl bis (2,4,6-trimethylbenzoyl) phosphine oxide, 1-hydroxycyclohexyl phenyl ketone, 2-hydroxy-2-methyl-1-phenyl-1-propanone, benzophenone, 2,2-dimethoxy-2-phenylacetophenone, 2-hydroxy-4'-(2-hydroxyethoxy)-2-methylpropiophenone, 2-isopropylthioxanthone, 2,4-diethylthiazolone.

9. The optical fiber coating composition according to claim 1, wherein: The auxiliary agent includes one or more combinations of a silane coupling agent, an active amine auxiliary agent, and a leveling agent.

10. An optical fiber comprising an optical fiber coating composition, wherein: The optical fiber coating composition is as shown in any one of claims 1 to 9, wherein the optical fiber comprises a core, a cladding, a primary coating layer, and a secondary coating layer, wherein the cladding is wrapped around the outer layer of the core, the primary coating layer is wrapped around the outer layer of the cladding, and the secondary coating layer is wrapped around the outer layer of the primary coating layer; At least one of the primary coating layer and the secondary coating layer is formed by ultraviolet curing of the optical fiber coating composition.

11. A method for preparing an optical fiber comprising an optical fiber coating composition, wherein: The optical fiber coating composition is as shown in any one of claims 1 to 9, and the preparation method comprises the following steps: 1) Place the preform on the chuck of the feeding mechanism, put the preform into a high-temperature heating furnace to soften and melt, condense into a ball-shaped filament, and thin vertically by its own weight to form a bare optical fiber; 2) The bare optical fiber passes through the mold soaked with the primary coating composition, the mold soaked with the secondary coating composition, and the light curing furnace in sequence, bypasses the tension wheel, guide wheel, and traction wheel on the drawing, and is finally wound on the take-up drum.

12. The preparation method according to claim 11, wherein When the bare optical fiber passes through the mold soaked with the primary coating composition, it passes through the light curing oven, then passes through the mold soaked with the secondary coating composition, and then passes through the light curing oven to complete the curing.

13. The preparation method according to claim 11, wherein: The speed of the optical fiber passing through the light curing oven is 1500m / min-3500m / min.

Citation Information

Patent Citations

  • Polyurethane-acrylate prepolymer as well as preparation and application of polyurethane-acrylate prepolymer

    CN106700025A

  • Fiber coatings with low modulus and high critical stress

    CN110167983A

  • Curable compositions and uses thereof

    CN110709436A

  • Fiber Optic Coating Composition with High Curing Speed

    CN111758054B

  • Heat-resistant light-cured optical fiber coating and preparation method thereof

    CN112920632A

Cited By

  • Glass fiber impregnating compound as well as preparation method, product and application thereof

    CN119707321A

  • Optical fiber colored secondary coating composition

    WO2026226384A1