Negative electrode material, negative electrode sheet and preparation method therefor, energy storage device and electric device

By controlling the matching of hard carbon particles with porous structures, the capacity and charging and discharging efficiency of hard carbon negative electrode materials are improved, and the low efficiency and low capacity of hard carbon materials in batteries are solved, thus achieving high energy density and long battery life. .

WO2024239691A1PCT designated stage expired Publication Date: 2024-11-28XIAMEN HITHIUM ENERGY STORAGE TECHNOLOGY CO LTD
View PDF 7 Cites 0 Cited by

Patent Information

Application Number
PCT/CN2024/073414
Authority / Receiving Office
WO · WO
Patent Type
Applications
Current Assignee / Owner
Priority Date
2023-05-19
Filing Date
2024-01-22
Publication Date
2024-11-28

AI Technical Summary

Technical Problem

The low first-week charge and discharge efficiency, low capacity and poor magnification characteristics of hard carbon negative electrode materials hinder their development in the battery field.

Method used

By controlling the ratio of the total volume of the Dv50 of the hard carbon particles to the porous structure within the range of 0.32≤Dv50/1000V≤2.40, match the hard carbon particle size and porous structure, improve ion storage and transmission efficiency, and prepare hard carbon negative electrode materials with porous structures in porous structures. , used to prepare negative electrode sheets and energy storage devices.

Benefits of technology

It achieves high capacity and high first-week charge and discharge efficiency, taking into account the energy density, rate performance and cycle performance of the battery, extending the battery life of the power consumption device and the battery life.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN2024073414_28112024_PF_FP_ABST
    Figure CN2024073414_28112024_PF_FP_ABST
Patent Text Reader

Abstract

A negative electrode material, a negative electrode sheet and a preparation method therefor, an energy storage device and an electric device. The negative electrode material comprises hard carbon, wherein the hard carbon has a porous structure, and satisfies: 0.32≤Dv50 / 1000V≤2.40, where the unit of the Dv50 of the hard carbon is μm, and the total volume of multiple pores in the hard carbon is V, with the unit thereof being cm 3 / g.
Need to check novelty before this filing date? Find Prior Art

Description

Negative electrode material, negative electrode sheet and preparation method, energy storage device and power device Technical Field

[0001] The present application belongs to the field of batteries, and specifically relates to negative electrode materials, negative electrode sheets and preparation methods, energy storage devices and power-consuming devices. Background Art

[0002] Compared with graphite negative electrodes, hard carbon has a rich disordered structure and a large interlayer spacing, which can accelerate ion diffusion. It is considered to be a very promising battery negative electrode material. However, hard carbon materials have low first-cycle charge and discharge efficiency, low capacity and poor rate characteristics, which hinder the development of hard carbon materials in the battery field.

[0003] Public content

[0004] This application is mainly based on the following questions and findings:

[0005] In order to improve the problems of low first-cycle charge and discharge efficiency, low capacity and poor rate characteristics of hard carbon negative electrode active materials, people have tried various methods to adjust the hard carbon structure. For example, hard carbon is coated with soft carbon to cover the micropores on the surface of the hard carbon, thereby reducing its specific surface area and reducing the side reactions between the hard carbon and the electrolyte, thereby improving the first-cycle charge and discharge efficiency of the battery. However, the method of coating hard carbon with soft carbon will reduce the active sites of ions (such as sodium ions), resulting in a decrease in battery capacity. For another example, atoms such as phosphorus, nitrogen, and sulfur are doped into hard carbon materials to improve the capacity and rate performance of hard carbon materials, but this method will reduce the first-cycle charge and discharge efficiency of the battery.

[0006] This application aims to at least partially address one of the technical problems in the related art. To this end, one objective of this application is to provide a negative electrode material, a negative electrode sheet, a preparation method, an energy storage device, and an electrical device. The negative electrode material has high capacity and first-cycle charge and discharge efficiency, while also exhibiting good kinetic performance, which is beneficial for balancing the energy density, rate capability, and cycle performance of the battery.

[0007] In a first aspect of the present application, a negative electrode material is provided. According to an embodiment of the present application, the negative electrode material includes hard carbon, the hard carbon having a porous structure, and the hard carbon satisfies: 0.32≤Dv50 / 1000V≤2.40, wherein the unit of Dv50 of the hard carbon is μm, and the total volume of the porous structure in the hard carbon is V, in cm 3 / g.

[0008] According to the negative electrode material of the above embodiment of the present application, it includes hard carbon with a porous structure, and at the same time, the ratio of Dv50 of the hard carbon particles to the total volume of the pores in the hard carbon is controlled within the above range to achieve matching between the particle size and the porous structure of the hard carbon material. This is not only beneficial to the storage of ions (such as sodium ions, etc.) and improving the capacity of the hard carbon material, but also beneficial to the transmission of ions (such as sodium ions, etc.) and accelerating the ion diffusion dynamics. When the particle size and porous volume of the hard carbon do not match, for example, when the total porous volume corresponding to the hard carbon material with large particle size is small, it is not conducive to the diffusion and transmission of ions, affecting the kinetic properties of the porous hard carbon, and causing the rate performance of the battery to decline; when the total porous volume corresponding to the hard carbon material with small particle size is large, the contact area between the porous hard carbon and the electrolyte will be increased, causing the side reactions between the hard carbon and the electrolyte to increase, affecting the first-week charge and discharge efficiency and cycle performance of the battery. The present application controls the Dv50 of the hard carbon and the total porous volume V to satisfy the above relationship, so that the negative electrode material has a higher capacity and first-week charge and discharge efficiency, and at the same time has better kinetic performance, which is beneficial to taking into account the energy density, rate performance and cycle performance of the battery.

[0009] In its second aspect, this application provides a negative electrode plate. According to embodiments of this application, the negative electrode plate includes a negative electrode active material layer comprising the aforementioned negative electrode material. As a result, a battery equipped with this negative electrode plate exhibits excellent energy density, rate capability, and coulombic efficiency.

[0010] In a third aspect of the present application, a method for preparing the aforementioned negative electrode material is proposed. According to an embodiment of the present application, the method comprises:

[0011] (1) mixing a hard carbon precursor with a pore-forming agent to obtain a dispersion of the hard carbon precursor;

[0012] (2) The dispersion of the hard carbon precursor is dried and then carbonized, washed, crushed, and sieved to obtain the negative electrode material.

[0013] Therefore, this method can be used to prepare the above-mentioned negative electrode material with high capacity and first-cycle charge and discharge efficiency, as well as good kinetic performance, which is beneficial to taking into account the energy density, rate performance and cycle performance of the battery.

[0014] In its fourth aspect, this application proposes a method for preparing the aforementioned negative electrode sheet. According to an embodiment of the present application, a negative electrode active slurry is applied to at least one side of a current collector to produce a negative electrode sheet, wherein the negative electrode active slurry comprises the aforementioned negative electrode material or a negative electrode material obtained using the aforementioned method. This method not only simplifies the preparation process and facilitates industrial production, but also produces a negative electrode sheet with high capacitance, first-cycle charge-discharge efficiency, and excellent kinetic performance.

[0015] In a fifth aspect of the present application, an energy storage device is provided. According to an embodiment of the present application, the energy storage device includes the aforementioned negative electrode sheet. Compared with the prior art, the energy storage device has better overall performance, and can achieve higher energy density, better rate performance, and better cycle performance.

[0016] In a sixth aspect of the present application, an electric device is provided. According to an embodiment of the present application, the electric device includes the above-mentioned energy storage device. Compared with the prior art, the electric device has a longer battery life and a longer service life, and has a higher market satisfaction.

[0017] Additional aspects and advantages of the present application will be given in part in the description below, and in part will become obvious from the description below, or will be learned through practice of the present application. BRIEF DESCRIPTION OF THE DRAWINGS

[0018] The above and / or additional aspects and advantages of the present application will become apparent and easily understood from the description of the embodiments in conjunction with the following drawings, in which:

[0019] FIG1 is a flow chart of a method for preparing a negative electrode material according to one embodiment of the present application. DETAILED DESCRIPTION

[0020] The following describes embodiments of the present application in detail. Examples of the embodiments are shown in the accompanying drawings, wherein the same or similar reference numerals throughout represent the same or similar elements or elements having the same or similar functions. The embodiments described below are exemplary and are intended to be used to explain the present application and are not to be construed as limiting the present application.

[0021] In a first aspect of the present application, a negative electrode material is provided. According to an embodiment of the present application, the negative electrode material includes hard carbon, the hard carbon has a porous structure, and the hard carbon satisfies: 0.32≤Dv50 / 1000V≤2.40, wherein the unit of Dv50 of the hard carbon is μm, and the total volume of the porous structure in the hard carbon is V, which is in cm 3 / g.

[0022] According to the negative electrode material of the above embodiment of the present application, it includes hard carbon with a porous structure, and at the same time, the ratio of Dv50 of the hard carbon particles to the total volume of the pores in the hard carbon is controlled within the above range to achieve matching between the particle size and the porous structure of the hard carbon material. This is not only beneficial to the storage of ions (such as sodium ions, etc.) and improving the capacity of the hard carbon material, but also beneficial to the transmission of ions (such as sodium ions, etc.) and accelerating the ion diffusion dynamics. When the particle size and porous volume of the hard carbon do not match, for example, when the total porous volume corresponding to the hard carbon material with large particle size is small, it is not conducive to the diffusion and transmission of ions, affecting the kinetic properties of the porous hard carbon, and causing the rate performance of the battery to decline; when the total porous volume corresponding to the hard carbon material with small particle size is large, the contact area between the porous hard carbon and the electrolyte will be increased, causing the side reactions between the hard carbon and the electrolyte to increase, affecting the first-week charge and discharge efficiency and cycle performance of the battery. The present application controls the Dv50 of the hard carbon and the total porous volume V to satisfy the above relationship, so that the negative electrode material has a higher capacity and first-week charge and discharge efficiency, and at the same time has better kinetic performance, which is beneficial to taking into account the energy density, rate performance and cycle performance of the battery. It should be noted that the negative electrode material in the present application may include only the above-mentioned hard carbon, or may include other negative electrode materials, such as graphite, etc., wherein, based on the total mass of the negative electrode material, the mass proportion of hard carbon in the negative electrode material may be not less than 50wt%, for example, not less than 60wt%, not less than 70wt%, not less than 80wt%, not less than 85wt%, not less than 90wt% or not less than 95wt%, etc.

[0023] According to the embodiments of the present application, in the negative electrode material, the Dv50 of the hard carbon and the total volume V of the pores in the hard carbon can satisfy 0.42≤Dv50 / 1000V≤1.44. For example, Dv50 / 1000V can be 0.6, 0.8, 1.0, 1.2, 1.4, etc., which is more conducive to ensuring that the negative electrode material has a higher capacity, first-week charge and discharge efficiency and better kinetic performance, which can further improve the energy density, rate performance and cycle performance of the battery.

[0024] According to the embodiments of the present application, the Dv50 of the hard carbon can be 5μm-18μm, for example, it can be 6μm, 8μm, 10μm, 13μm, 15μm or 17μm, etc. If the Dv50 of the hard carbon is too small, it is easy to make its specific surface area too large, resulting in an increase in the side reactions between the negative electrode material and the electrolyte, which may increase the irreversible capacity of the battery and affect the first-week charge and discharge efficiency and cycle performance of the battery; if the Dv50 of the hard carbon is too large, it is not only easy to slow down the solid-phase diffusion rate of ions (such as sodium ions, etc.) in the hard carbon, increase the internal resistance of the battery, and affect the rate performance of the battery, but also is not conducive to improving the compaction density of the negative electrode active material layer, affecting the energy density of the battery. The present application is beneficial to taking into account the energy density, rate performance and cycle performance of the battery by controlling the Dv50 of the hard carbon within the above range. Furthermore, the Dv50 of the hard carbon can be 5μm-14μm, which is beneficial to further improve the energy density of the battery. It should be noted that Dv50 here refers to the particle size corresponding to when the cumulative volume distribution number of hard carbon reaches 50%.

[0025] According to an embodiment of the present application, the total volume V of the pores in the hard carbon can be 0.005 cm 3 / g-0.022cm 3 / g, for example, 0.006 cm 3 / g, 0.01cm 3 / g, 0.015cm 3 / g, 0.018cm 3 / g or 0.02cm 3 / g, etc. If the total volume of the hard carbon mesoporous structure is too large, it is easy to increase the side reactions between the negative electrode material and the electrolyte, reducing the first-week charge and discharge efficiency and cycle performance of the negative electrode plate; if the total volume of the hard carbon mesoporous structure is too small, it may reduce the number of ion active sites in the negative electrode material, affecting the capacity of the negative electrode plate. The present application controls the total volume V of the porous hard carbon within the above range, which is beneficial to taking into account the energy density, first-week charge and discharge efficiency and cycle performance of the battery. Furthermore, the total volume V of the porous hard carbon can be 0.008cm 3 / g-0.016cm 3 / g, thereby further ensuring that the battery has high energy density, first-cycle charge and discharge efficiency, and good cycle performance. It should be noted that the total volume V of the porous structure in the hard carbon can be obtained by nitrogen adsorption and desorption testing. By obtaining the isothermal adsorption and desorption curve, the total adsorption pore volume at a relative pressure P / P0 of 0.99 is obtained, which is the total volume V of the porous structure in the hard carbon.

[0026] According to the embodiments of the present application, the average pore size of the hard carbon can be 3nm-10nm, for example, 3nm, 5nm, 7nm or 9nm. If the average pore size of the hard carbon is too small, it will affect the transmission of ions, reduce the kinetic performance of the hard carbon, and affect the rate performance of the battery. If the average pore size of the hard carbon is too large, the metallic properties of the deposited sodium will be enhanced, which will bring the risk of short circuit to the battery. In addition, the excessively large pore size will reduce the specific surface area of ​​the material, resulting in a reduction in the sodium storage capacity. The present application controls the average pore size of the porous hard carbon within the above range, which is conducive to taking into account both the energy density and rate performance of the battery. It should be noted that the average pore size of the hard carbon can be tested by nitrogen adsorption and desorption method, and the isothermal adsorption and desorption curve is obtained to obtain the adsorption average pore size, which is the average pore size of the porous hard carbon.

[0027] In a second aspect of the present application, a method for preparing the above-mentioned negative electrode material is proposed. According to an embodiment of the present application, in conjunction with FIG1 , the method includes:

[0028] S100: Mixing the hard carbon precursor with the pore-forming agent to obtain a dispersion of the hard carbon precursor

[0029] According to an embodiment of the present application, a hard carbon precursor is mixed with a pore-forming agent so that a uniformly distributed porous structure is introduced into the hard carbon by decomposing the pore-forming agent during the subsequent carbonization process. According to some specific examples of the present application, the mixing ratio of the hard carbon precursor to the pore-forming agent can be 1: (0.02-0.2), for example, it can be 1 / 0.05, 1 / 0.1 or 1 / 0.15, etc. If the amount of the pore-forming agent is too much, the number of pores formed is too large and the total volume of the pores is too large, which will lead to an increase in the metallic properties of the deposited sodium and bring a risk of short circuit to the battery; if the amount of the pore-forming agent is too little, the number of pores formed is small and the total volume of the pores is too small, which is not conducive to ion transport and reduces the kinetic properties of the hard carbon. It should be noted that there is no particular restriction on the specific types of hard carbon precursors and pore-forming agents in this application, and those skilled in the art can flexibly choose according to actual conditions. For example, the hard carbon precursor may include but is not limited to phenolic resin, biomass, etc., and the pore-forming agent may include but is not limited to inorganic salts, such as at least one of sodium carbonate, sodium bicarbonate, potassium carbonate, potassium bicarbonate, and calcium bicarbonate.

[0030] S200: drying the dispersion of the hard carbon precursor and then carbonizing it, washing, crushing, and screening it to obtain the negative electrode material

[0031] According to an embodiment of the present application, the dispersion of the hard carbon precursor is dried and then carbonized, so that the hard carbon precursor is pyrolyzed to obtain hard carbon, and the pore-forming agent is also thermally decomposed to form a porous structure inside the hard carbon. According to some specific examples of the present application, the carbonization treatment can be carried out under a protective atmosphere, and the temperature of the carbonization treatment can be 900°C-1100°C, for example, 920°C, 960°C, 1000°C, 1050°C, etc. The heating rate can be 0.5°C / min-10°C / min, for example, 1°C / min, 3°C / min, 5°C / min, 7°C / min or 8°C / min, etc., thereby facilitating the acquisition of a porous structure having the above-mentioned particle size matching the hard carbon. It should be noted that there is no particular restriction on the specific type of protective atmosphere in the present application, and those skilled in the art can flexibly select it according to actual conditions. For example, the carbonization treatment can be carried out under nitrogen and / or an inert atmosphere.

[0032] According to the embodiments of the present application, the hard carbon material obtained after carbonization treatment is washed, crushed, and sieved in sequence to achieve matching of the particle size and porous structure of the hard carbon material, so that the Dv50 of the hard carbon and the total porous volume V in the hard carbon satisfy 0.32≤Dv50 / 1000V≤2.40, so that the hard carbon meets the requirements of higher capacitance and first-cycle charge and discharge efficiency, while having better kinetic performance, which is beneficial to taking into account the energy density, rate performance, and cycle performance of the battery.

[0033] In general, this method not only has a simple preparation process and is conducive to industrial production, but also can obtain negative electrode materials with high capacity, first-cycle charge and discharge efficiency and good kinetic performance.

[0034] In its third aspect, this application proposes a negative electrode plate. According to embodiments of this application, this negative electrode plate includes a negative electrode active material layer comprising the aforementioned negative electrode material or a negative electrode material obtained using the aforementioned method. As a result, a battery equipped with this negative electrode plate exhibits excellent energy density, rate capability, and first-cycle charge and discharge efficiency.

[0035] According to the embodiments of the present application, the porosity of the negative electrode active material layer can be 28%-40%, for example, it can be 30%, 32%, 34%, 36% or 38%, etc. The porosity of the negative electrode active material layer will affect the electrolyte's ability to infiltrate and retain liquid in the negative electrode sheet, thereby affecting the transmission of ions. Specifically, if the porosity of the negative electrode active material layer is too large, it will lead to aggravated side reactions during the formation and circulation process, affecting the long cycle performance of the battery; if the porosity of the negative electrode active material layer is too small, it will affect the infiltration effect of the electrolyte in the negative electrode sheet, and at the same time, the liquid retention amount will decrease, which will easily increase the resistance to ion transmission and affect the battery's cycle performance and kinetic performance. The present application helps to improve the electrolyte's infiltration effect in the negative electrode sheet and reduce the sodium ion transmission resistance by controlling the porosity of the negative electrode active material layer within the above range, thereby improving the battery's cycle performance and kinetic performance. It should be noted that the porosity of the negative electrode active material layer can be obtained by mercury intrusion testing (also known as "mercury intrusion"), and the specific reference standard is GB / T 21650.1-2008 Mercury intrusion method and gas adsorption method for the determination of pore size distribution and porosity of solid materials Part 1: Mercury intrusion method.

[0036] According to an embodiment of the present application, the negative electrode active material layer may further include: a binder and / or a conductive agent. In the negative electrode active material layer, the amount of the negative electrode material may be 90 parts by weight to 98 parts by weight, for example, 95.5 parts by weight, etc. The amount of the binder may be 0.5 parts by weight to 5 parts by weight, for example, 1.5 parts by weight, etc. The amount of the conductive agent may be 1 part by weight to 5 parts by weight, for example, 3 parts by weight, etc. It should be noted that there is no particular limitation on the specific types of the binder and the conductive agent in the present application, and those skilled in the art may flexibly select them according to actual circumstances. For example, the binder may include at least one of styrene-butadiene rubber, polyvinylidene fluoride, polytetrafluoroethylene, polyvinyl alcohol, polyacrylonitrile, polyacrylic acid, polyacrylate, carboxymethyl cellulose, and sodium alginate; and the conductive agent may include at least one of acetylene black, Super-P, carbon nanotubes, carbon fibers, and graphene.

[0037] In the fourth aspect of the present application, the present application proposes a method for preparing the above-mentioned negative electrode sheet. According to an embodiment of the present application, a negative electrode active slurry is applied to at least one side of a current collector to obtain a negative electrode sheet, wherein the negative electrode active slurry includes the above-mentioned negative electrode material. This method not only has a simple preparation process and is conducive to industrial production, but also can obtain a negative electrode sheet with high capacity, first-cycle charge and discharge efficiency and good kinetic performance. It should be noted that there is no special restriction on the specific type of current collector in this application, and those skilled in the art can flexibly choose according to actual conditions. For example, the current collector may include at least one of copper foil, stainless steel foil, copper alloy foil, carbon-coated copper foil, aluminum foil, and carbon-coated aluminum foil.

[0038] In a fifth aspect of the present application, an energy storage device is provided. According to an embodiment of the present application, the energy storage device includes the aforementioned negative electrode sheet. Compared with the prior art, the energy storage device has better overall performance, and can achieve higher energy density, better rate performance, and better cycle performance.

[0039] According to the embodiments of the present application, there is no particular restriction on the specific type of the energy storage device in the present application, and those skilled in the art can flexibly select according to actual conditions. For example, the energy storage device can be a battery, and the battery can include a positive electrode plate, a diaphragm and an electrolyte, wherein the positive electrode plate includes a positive electrode active material layer, and the positive electrode active material layer can include a positive electrode active material, a binder and a conductive agent. In the present application, there is no particular restriction on the specific types of the positive electrode active material, the binder and the conductive agent in the positive electrode active material layer. For example, for sodium ion batteries, the positive electrode active material can include at least one of a transition metal oxide, a polyanionic compound, an organic polymer, and a Prussian blue material; the present application also has no particular restriction on the specific composition of the diaphragm, for example, the diaphragm can include at least one of polypropylene (PP), polyethylene (PE), and a ceramic diaphragm; the electrolyte can include an electrolyte salt and an organic solvent, wherein the specific types and compositions of the electrolyte salt and the organic solvent are also not particularly restricted, and those skilled in the art can select according to actual needs.

[0040] In a sixth aspect of the present application, an electric device is provided. According to an embodiment of the present application, the electric device includes the above-mentioned energy storage device. Compared with the prior art, the electric device has a longer battery life and a longer service life, and has a higher market satisfaction.

[0041] The embodiments of the present application are described in detail below. The embodiments described below are exemplary and are only used to explain the present application, and should not be construed as limiting the present application. Where specific techniques or conditions are not specified in the embodiments, they are performed according to the techniques or conditions described in the literature in this area or according to the product specifications. Reagents or instruments used that do not specify the manufacturer are conventional products that can be obtained commercially.

[0042] Example 1

[0043] (1) The coconut shell powder that had been pre-treated before pulverization was mixed with potassium bicarbonate solution, wherein the mass ratio of coconut shell powder to potassium bicarbonate was 1:0.07, to obtain a dispersion of a hard carbon precursor; the dispersion of the hard carbon precursor was placed in a vacuum oven and dried for 20 h, and then heated to 1100°C at a heating rate of 5°C / min under nitrogen protection to obtain a carbonized product; the carbonized product was pulverized, washed with hydrochloric acid and deionized water in sequence, dried, and then sieved and demagnetized to obtain porous hard carbon, wherein the Dv50 of the porous hard carbon was 15 μm, the pore size of the single pore in the porous hard carbon was 8.8 nm, and the total volume V of the porous hard carbon was 0.007 cm 3 / g, Dv50 / 1000V is 2.14;

[0044] (2) Porous hard carbon, conductive carbon black, sodium hydroxymethyl cellulose, and styrene-butadiene rubber are mixed in a mass ratio of 95.5:1.5:1:2, the mixed powder is placed in a vacuum mixer, deionized water is added and stirred to obtain a negative electrode active slurry; the negative electrode slurry is evenly coated on the opposite sides of the negative electrode current collector to form a negative electrode active material layer, the negative electrode current collector coated with the negative electrode active slurry is transferred to an oven for drying, and then rolled and cut to obtain a negative electrode sheet, wherein the porosity of the negative electrode active material layer is 32%;

[0045] (3) Na3V2(PO4)3, conductive agent Super-P, and binder PVDF are mixed in a mass ratio of 95:2.5:2.5, the mixed powder is placed in a vacuum mixer, N-methylpyrrolidone is added, and the mixture is stirred evenly to obtain a positive electrode active slurry; the positive electrode active slurry is evenly coated on the opposite sides of the positive electrode current collector aluminum foil to form a positive electrode active material layer, the positive electrode current collector coated with the positive electrode slurry is transferred to an oven for drying, and then rolled and cut to obtain a positive electrode sheet;

[0046] (4) Ethylene carbonate (EC), ethyl methyl carbonate (EMC), and diethyl carbonate (DEC) were mixed in a volume ratio of 1:1:1 to obtain a mixed solution, dried sodium salt NaPF6 was added to the mixed solution to prepare an electrolyte with a concentration of 1 mol / L, and 2 wt% of fluoroethylene carbonate (FEC) as an additive was added to obtain an electrolyte;

[0047] (5) The positive electrode sheet, negative electrode sheet and polypropylene separator are stacked in order so that the separator is between the positive and negative electrode sheets, and then wound to obtain a bare cell. The bare cell is placed in an aluminum-plastic film soft package, and the electrolyte is injected after drying. After vacuum packaging, standing, forming, shaping and other processes, a secondary battery is obtained.

[0048] Example 2

[0049] The difference from Example 1 is that in step (1): the coconut shell powder that has been processed before crushing is mixed with potassium bicarbonate solution, wherein the mass ratio of coconut shell powder to potassium bicarbonate is 1:0.09, to obtain a dispersion of a hard carbon precursor; the dispersion of the hard carbon precursor is placed in a vacuum oven and dried for 20 hours, and then heated to 1100°C at a heating rate of 4°C / min under nitrogen protection for carbonization treatment to obtain a carbonized product; the carbonized product is crushed, washed with hydrochloric acid and deionized water in sequence, dried, and then sieved and demagnetized to obtain porous hard carbon, wherein the Dv50 of the porous hard carbon is 7 μm, the pore size of a single pore in the porous hard carbon is 7.3 nm, and the total volume V of the porous hard carbon is 0.010 cm 3 / g, Dv50 / 1000V is 0.7.

[0050] Example 3

[0051] The difference from Example 1 is that in step (1): the coconut shell powder that has been pre-treated before crushing is mixed with a potassium bicarbonate solution, wherein the mass ratio of the coconut shell powder to the potassium bicarbonate is 1:0.15, to obtain a dispersion of a hard carbon precursor; the dispersion of the hard carbon precursor is placed in a vacuum oven and dried for 20 hours, and then heated to 1100°C at a heating rate of 2°C / min under nitrogen protection for carbonization treatment to obtain a carbonized product; the carbonized product is crushed, washed with hydrochloric acid and deionized water in sequence, dried, and then sieved and demagnetized to obtain porous hard carbon, wherein the Dv50 of the porous hard carbon is 7 μm, the pore size of a single pore in the porous hard carbon is 3.8 nm, and the total volume V of the porous is 0.022 cm 3 / g, Dv50 / 1000V is 0.32.

[0052] Example 4

[0053] The difference from Example 1 is that in step (1): the coconut shell powder that has been pre-treated before crushing is mixed with a potassium bicarbonate solution, wherein the mass ratio of the coconut shell powder to the potassium bicarbonate is 1:0.10, to obtain a dispersion of a hard carbon precursor; the dispersion of the hard carbon precursor is placed in a vacuum oven and dried for 20 hours, and then heated to 1100°C at a heating rate of 3°C / min under nitrogen protection for carbonization treatment to obtain a carbonized product; the carbonized product is crushed, washed with hydrochloric acid and deionized water in sequence, dried, and then sieved and demagnetized to obtain porous hard carbon, wherein the Dv50 of the porous hard carbon is 5 μm, the pore size of a single pore in the porous hard carbon is 6.4 nm, and the total volume V of the porous is 0.012 cm 3 / g, Dv50 / 1000V is 0.42.

[0054] Example 5

[0055] The difference from Example 1 is that in step (1): the coconut shell powder that has been processed before crushing is mixed with potassium bicarbonate solution, wherein the mass ratio of coconut shell powder to potassium bicarbonate is 1:0.08, to obtain a dispersion of a hard carbon precursor; the dispersion of the hard carbon precursor is placed in a vacuum oven and dried for 20 hours, and then heated to 1100°C at a heating rate of 4°C / min under nitrogen protection for carbonization treatment to obtain a carbonized product; the carbonized product is crushed, washed with hydrochloric acid and deionized water in sequence, dried, and then sieved and demagnetized to obtain porous hard carbon, wherein the Dv50 of the porous hard carbon is 9 μm, the pore size of a single pore in the porous hard carbon is 7.6 nm, and the total volume V of the porous is 0.009 cm 3 / g, Dv50 / 1000V is 1.0.

[0056] Example 6

[0057] The difference from Example 1 is that in step (1): the coconut shell powder that has been pre-treated before crushing is mixed with a potassium bicarbonate solution, wherein the mass ratio of the coconut shell powder to the potassium bicarbonate is 1:0.08, to obtain a dispersion of a hard carbon precursor; the dispersion of the hard carbon precursor is placed in a vacuum oven and dried for 20 hours, and then heated to 1100°C at a heating rate of 5°C / min under nitrogen protection for carbonization treatment to obtain a carbonized product; the carbonized product is crushed, washed with hydrochloric acid and deionized water in sequence, dried, and then sieved and demagnetized to obtain porous hard carbon, wherein the Dv50 of the porous hard carbon is 13 μm, the pore size of a single pore in the porous hard carbon is 8.1 nm, and the total volume V of the porous hard carbon is 0.009 cm 3 / g, Dv50 / 1000V is 1.44.

[0058] Example 7

[0059] The difference from Example 1 is that in step (1): the coconut shell powder that has been pre-treated before crushing is mixed with a potassium bicarbonate solution, wherein the mass ratio of coconut shell powder to potassium bicarbonate is 1:0.06, to obtain a dispersion of a hard carbon precursor; the dispersion of the hard carbon precursor is placed in a vacuum oven and dried for 20 hours, and then heated to 1100°C at a heating rate of 5°C / min under nitrogen protection for carbonization treatment to obtain a carbonized product; the carbonized product is crushed, washed with hydrochloric acid and deionized water in sequence, dried, and then sieved and demagnetized to obtain porous hard carbon, wherein the Dv50 of the porous hard carbon is 14 μm, the pore size of a single pore in the porous hard carbon is 8.3 nm, and the total volume V of the porous hard carbon is 0.006 cm 3 / g, Dv50 / 1000V is 2.33.

[0060] Comparative Example 1

[0061] The difference from Example 1 is that in step (2), commercially available hard carbon is used as the negative electrode active material, and the Dv50 of the hard carbon is 8 μm.

[0062] Comparative Example 2

[0063] The difference from Example 1 is that in step (1): the coconut shell powder that has been pre-treated before crushing is mixed with a potassium bicarbonate solution, wherein the mass ratio of coconut shell powder to potassium bicarbonate is 1:0.24, to obtain a dispersion of a hard carbon precursor; the dispersion of the hard carbon precursor is placed in a vacuum oven and dried for 20 hours, and then heated to 1100°C at a heating rate of 2°C / min under nitrogen protection for carbonization treatment to obtain a carbonized product; the carbonized product is crushed, washed with hydrochloric acid and deionized water in sequence, dried, and then sieved and demagnetized to obtain porous hard carbon, wherein the Dv50 of the porous hard carbon is 6 μm, the pore size of a single pore in the porous hard carbon is 3.2 nm, and the total volume V of the porous hard carbon is 0.021 cm 3 / g, Dv50 / 1000V is 0.29.

[0064] Comparative Example 3

[0065] The difference from Example 1 is that in step (1): the coconut shell powder that has been pre-treated before crushing is mixed with a potassium bicarbonate solution, wherein the mass ratio of coconut shell powder to potassium bicarbonate is 1:0.05, to obtain a dispersion of a hard carbon precursor; the dispersion of the hard carbon precursor is placed in a vacuum oven and dried for 20 hours, and then heated to 1100°C at a heating rate of 5°C / min under nitrogen protection for carbonization treatment to obtain a carbonized product; the carbonized product is crushed, washed with hydrochloric acid and deionized water in sequence, dried, and then sieved and demagnetized to obtain porous hard carbon, wherein the Dv50 of the porous hard carbon is 16 μm, the pore size of a single pore in the porous hard carbon is 9.2 nm, and the total volume V of the porous is 0.006 cm 3 / g, Dv50 / 1000V is 2.67.

[0066] Comparative Example 4

[0067] The difference from Example 1 is that in step (1): the coconut shell powder that has been pre-treated before crushing is mixed with a potassium bicarbonate solution, wherein the mass ratio of the coconut shell powder to the potassium bicarbonate is 1:0.16, to obtain a dispersion of a hard carbon precursor; the dispersion of the hard carbon precursor is placed in a vacuum oven and dried for 20 hours, and then heated to 1100°C at a heating rate of 3°C / min under nitrogen protection for carbonization treatment to obtain a carbonized product; the carbonized product is crushed, washed with hydrochloric acid and deionized water in sequence, dried, and then sieved and demagnetized to obtain porous hard carbon, wherein the Dv50 of the porous hard carbon is 4 μm, the pore size of a single pore in the porous hard carbon is 4.5 nm, and the total volume V of the porous is 0.016 cm 3 / g, Dv50 / 1000V is 0.25.

[0068] Comparative Example 5

[0069] The difference from Example 1 is that in step (1): the coconut shell powder that has been processed before crushing is mixed with potassium bicarbonate solution, wherein the mass ratio of coconut shell powder to potassium bicarbonate is 1:0.09, to obtain a dispersion of a hard carbon precursor; the dispersion of the hard carbon precursor is placed in a vacuum oven and dried for 20 hours, and then heated to 1100°C at a heating rate of 5°C / min under nitrogen protection for carbonization treatment to obtain a carbonized product; the carbonized product is crushed, washed with hydrochloric acid and deionized water in sequence, dried, and then sieved and demagnetized to obtain porous hard carbon, wherein the Dv50 of the porous hard carbon is 20 μm, the pore size of a single pore in the porous hard carbon is 8.3 nm, and the total volume V of the porous hard carbon is 0.007 cm 3 / g, Dv50 / 1000V is 2.86.

[0070] Comparative Example 6

[0071] The difference from Example 1 is that in step (1): the coconut shell powder that has been pre-treated before crushing is mixed with a potassium bicarbonate solution, wherein the mass ratio of the coconut shell powder to the potassium bicarbonate is 1:0.30, to obtain a dispersion of a hard carbon precursor; the dispersion of the hard carbon precursor is placed in a vacuum oven and dried for 20 hours, and then heated to 1100°C at a heating rate of 2°C / min under nitrogen protection for carbonization treatment to obtain a carbonized product; the carbonized product is crushed, washed with hydrochloric acid and deionized water in sequence, dried, and then sieved and demagnetized to obtain porous hard carbon, wherein the Dv50 of the porous hard carbon is 7 μm, the pore size of a single pore in the porous hard carbon is 2.4 nm, and the total volume V of the porous is 0.027 cm 3 / g, Dv50 / 1000V is 0.26.

[0072] Comparative Example 7

[0073] The difference from Example 1 is that in step (1): the coconut shell powder that has been pre-treated before crushing is mixed with a potassium bicarbonate solution, wherein the mass ratio of coconut shell powder to potassium bicarbonate is 1:0.03, to obtain a dispersion of a hard carbon precursor; the dispersion of the hard carbon precursor is placed in a vacuum oven and dried for 20 hours, and then heated to 1100°C at a heating rate of 6°C / min under nitrogen protection for carbonization treatment to obtain a carbonized product; the carbonized product is crushed, washed with hydrochloric acid and deionized water in sequence, dried, and then sieved and demagnetized to obtain porous hard carbon, wherein the Dv50 of the porous hard carbon is 15 μm, the pore size of a single pore in the porous hard carbon is 11.7 nm, and the total volume V of the porous hard carbon is 0.004 cm 3 / g, Dv50 / 1000V is 3.75.

[0074] The differences between the above Examples 1 to 7 and Comparative Examples 1 to 7 are shown in Table 1.

[0075] Table 1 Experimental parameters of Examples 1 to 7 and Comparative Examples 1 to 7

[0076] Testing and Analysis

[0077] Under the same conditions, the batteries prepared in Examples 1 to 7 and Comparative Examples 1 to 7 were tested for energy density, cycle performance, and kinetic performance. The specific testing methods are as follows:

[0078] Energy density: Weigh the battery using an electronic balance at 25°C. Charge and discharge the battery at a 1.5C rate at 25°C, and record the actual discharge energy. The ratio of the actual discharge energy to the battery weight is the battery's energy density.

[0079] Cycle performance: The battery is charged at a 2C rate and discharged at a 1C rate for a full charge and discharge cycle test. The battery capacity retention rate after 1000 cycles is recorded to characterize the battery's cycle performance.

[0080] Kinetic performance: At 25°C, the battery is fully charged at nC and fully discharged at 1C. After repeating the charge and discharge cycle 10 times, the battery is then charged to a full charge state at an nC rate (n>0). The negative electrode is then disassembled and the sodium precipitation on the surface of the negative electrode is observed. If the area of ​​sodium precipitation on the surface of the negative electrode is less than 2%, it is considered that there is no sodium precipitation. The sodium precipitation rate refers to the rate at which, if there is no sodium precipitation on the surface of the negative electrode, the charging rate is increased from nC by a gradient of 0.1C and the test is repeated until sodium precipitation occurs on the surface of the negative electrode. The charging rate at this time, nC minus 0.1C, is the maximum charging rate of the battery without sodium precipitation.

[0081] The test results are shown in Table 2.

[0082] Table 2 Test results of Examples 1 to 7 and Comparative Examples 1 to 7

[0083] Results and Discussion

[0084] It can be seen from Tables 1 to 2 that, compared with Comparative Examples 1 to 7, the sodium ion batteries prepared in Examples 1 to 7 of the present application have higher first-week charge and discharge efficiency, energy density, and better rate performance and cycle performance, indicating that by adopting the porous hard carbon of the above-mentioned embodiments of the present application and controlling the ratio of the particle size of the hard carbon particles to the total porous volume of the hard carbon within the above-mentioned range, the particle size and porous structure of the hard carbon material can be matched, so that the porous hard carbon has a higher capacity and first-week charge and discharge efficiency, and at the same time has better kinetic performance, thereby taking into account the energy density, rate performance and cycle performance of the battery.

[0085] In the description of this specification, the description with reference to the terms "one embodiment", "some embodiments", "example", "specific example", or "some examples" means that the specific features, structures, materials or characteristics described in conjunction with the embodiment or example are included in at least one embodiment or example of the present application. In this specification, the schematic representations of the above terms do not necessarily refer to the same embodiment or example. Moreover, the specific features, structures, materials or characteristics described can be combined in any one or more embodiments or examples in a suitable manner. In addition, those skilled in the art can combine and combine different embodiments or examples described in this specification and features of different embodiments or examples without contradiction.

[0086] Although the embodiments of the present application have been shown and described above, it can be understood that the above embodiments are exemplary and cannot be understood as limitations on the present application. Ordinary technicians in this field can change, modify, replace and modify the above embodiments within the scope of the present application.

Claims

1. A negative electrode material, wherein: The negative electrode material includes hard carbon, and the hard carbon has a porous structure. The hard carbon satisfies: 0.32≤Dv50 / 1000V≤2.40, wherein the unit of Dv50 of the hard carbon is μm, and the total volume of the porous in the hard carbon is V, and the unit is cm 3 / g.

2. The negative electrode material according to claim 1, wherein The hard carbon satisfies: 0.42≤Dv50 / 1000V≤1.

44.

3. The negative electrode material according to claim 1 or 2, wherein Satisfies at least one of the following conditions: Dv50 of the hard carbon is 5 μm-18 μm; The total volume V of the pores in the hard carbon is 0.005 cm 3 / g-0.022cm 3 / g; The average pore size of the pores in the hard carbon is 3nm-10nm.

4. The negative electrode material according to any one of claims 1 to 3, wherein Satisfy at least one of the following conditions: The Dv50 of the hard carbon is 5 μm-14 μm; The total volume V of the pores in the hard carbon is 0.008 cm 3 / g-0.016cm 3 / g.

5. A negative electrode sheet, wherein: The negative electrode sheet includes a negative electrode active material layer, and the negative electrode active material layer includes the negative electrode material according to any one of claims 1 to 4.

6. The negative electrode sheet according to claim 5, wherein: The porosity of the negative electrode active material layer is 28%-40%.

7. The negative electrode sheet according to claim 5 or 6, wherein: The negative electrode active material layer also includes: a binder and / or a conductive agent. In the negative electrode active material layer, the amount of the negative electrode material is 90 parts by weight to 98 parts by weight, the amount of the binder is 0.5 parts by weight to 5 parts by weight, and the amount of the conductive agent is 1 part by weight to 5 parts by weight.

8. A method for preparing the negative electrode material according to any one of claims 1 to 4, wherein: include: (1) mixing a hard carbon precursor with a pore-forming agent to obtain a dispersion of the hard carbon precursor; (2) The hard carbon precursor dispersion is dried and then carbonized, washed, crushed and sieved to obtain the negative electrode material.

9. The method according to claim 8, wherein: In step (1), the mass ratio of the hard carbon precursor to the pore-forming agent is 1:(0.02-0.3).

10. A method for preparing a negative electrode sheet according to any one of claims 5 to 7, wherein: A negative electrode active slurry is applied to at least one side of the current collector to obtain a negative electrode sheet, wherein the negative electrode active slurry comprises the negative electrode material according to any one of claims 1 to 4 or the negative electrode material obtained by the method according to claim 8 or 9.

11. An energy storage device, wherein: The invention comprises the negative electrode sheet according to any one of claims 5 to 7.

12. An electrical device, wherein: Includes the energy storage device as claimed in claim 11.

Citation Information

Patent Citations

  • Hard carbon negative electrode material for lithium ion secondary battery and preparation method of hard carbon negative electrode material

    CN113113602A

  • Hard carbon negative electrode composite material and preparation method and application thereof

    CN113184828A

  • Electrochemical device and electronic device

    CN113437250A

  • Negative active material, negative pole piece comprising same, electrochemical device and electric device

    CN115458723A

  • Negative electrode material, negative electrode plate, preparation method of negative electrode plate, energy storage device and power utilization device

    CN116706063A