Device, electrical device, substrate, and production method for device
The use of a Mo-containing barrier layer and Ni, Ag, or Au bonding layer with a β-Sn layer in the solder joint addresses the issue of interfacial strength degradation in electronic devices during high-temperature processes, ensuring reliable bonding and impact resistance.
Patent Information
- Application Number
- PCT/JP2024/001574
- Authority / Receiving Office
- WO · WO
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2023-05-25
- Filing Date
- 2024-01-22
- Publication Date
- 2024-11-28
AI Technical Summary
High-temperature processes such as reflow bonding can deteriorate the mechanical properties of solder joints in electronic devices, leading to reduced interfacial strength and reliability, especially when metal materials react with each other.
A substrate configuration with a barrier layer containing Mo and a bonding layer with Ni, Ag, or Au is used, which reduces the reaction between electrode metals and solder, maintaining interfacial strength and improving impact resistance through the inclusion of a β-Sn layer in the solder joint.
The solution ensures sufficient interfacial strength and bonding reliability even after high-temperature processes, while also enhancing impact resistance and maintaining solder wetting and spreading during reflow bonding.
Smart Images

Figure JP2024001574_28112024_PF_FP_ABST
Abstract
Description
Device, electrical device, substrate and method for manufacturing the device
[0001] FIELD OF THE DISCLOSURE The present disclosure relates to devices, electrical devices, substrates and methods for manufacturing devices.
[0002] Devices carrying electronic components are mounted on mounting boards of electrical devices by soldering.
[0003] For example, the acoustic wave device described in Patent Document 1 includes a pad (electrode) provided on a piezoelectric substrate, and an under-bump metal provided on the pad to facilitate bonding with solder.
[0004] Japanese International Publication No. WO2015 / 022931
[0005] A device according to one aspect of the present disclosure includes a substrate having a first surface, an electrode located on the first surface of the substrate, and a joint located on the electrode, the joint including, in order from the electrode side, a first layer, a second layer, and a third layer, the first layer including Mo as a main component, the second layer including β-Sn as a main component, and the third layer including solder.
[0006] An electrical device according to one aspect of the present disclosure includes the above-described device.
[0007] A substrate according to one aspect of the present disclosure includes a base body having a first surface, an electrode located on the first surface of the base body, a barrier layer located on the electrode, and a bonding layer located on the barrier layer, wherein the barrier layer contains Mo as a main component, and the bonding layer contains at least one of Ni, Ag, Au, and Cu.
[0008] A manufacturing method of a device according to one aspect of the present disclosure includes the steps of preparing the substrate and placing solder on the bonding layer and heating it to create a bonding portion on the electrode, the bonding portion including, in order from the electrode side, a first layer, a second layer, and a third layer, the first layer including Mo as a main component, the second layer including β-Sn as a main component, and the third layer including solder.
[0009] FIG. 1 is a cross-sectional structural diagram showing a portion of a substrate according to a first embodiment of the present disclosure. FIG. 2 is a cross-sectional structural diagram showing a portion of a device according to a first embodiment of the present disclosure. FIG. 3 is a micrograph of a cross section of an electrode and a joint according to a first embodiment of the present disclosure. FIG. 4 is a micrograph further enlarging the vicinity of a second layer in a cross section of an electrode and a joint according to a first embodiment of the present disclosure. FIG. 5 is a schematic diagram showing the atomic arrangement in the
[111] direction of β-Sn and the atomic arrangement in the
[121] direction of Mo in a joint according to a first embodiment of the present disclosure. FIG. 6 is a cross-sectional structural diagram showing a portion of an electronic module including a device according to a first embodiment of the present disclosure. FIG. 7 is a cross-sectional structural diagram of an acoustic wave device according to a second embodiment of the present disclosure. FIG. 8 is a micrograph of a joint of an electronic module according to a second embodiment of the present disclosure. FIG. 9 is a graph showing the results of evaluation of the bonding strength of a comparative example in demonstration test 2. FIG. 10 is a graph showing the results of evaluation of the bonding strength of a comparative example in demonstration test 2. FIG. 11 is a graph showing the results of evaluation of the bonding strength of an example in demonstration test 2. FIG. 12 is a graph showing the results of evaluation of the bonding strength of an example and a comparative example in demonstration test 3. FIG. 13 is a graph showing the results of evaluation of the bonding strength of an example in demonstration test 4. 1 is a graph showing the results of evaluating the bonding strength of Examples in Demonstration Test 5. FIG. 2 is a graph showing the results of evaluating the bonding strength of Examples in Demonstration Test 6. FIG. 3 is a graph showing the results of nanoindentation in Demonstration Test 8. FIG. 4 is a Weibull plot in Demonstration Test 9. FIG. 5 is a schematic diagram of an electrode structure produced in an additional test. FIG. 6 is a diagram showing an overview of a steel ball drop test. FIG. 7 is a graph showing the results of a steel ball drop test. FIG. 8 is a SEM observation result after a drop test of a comparative example. FIG. 9 is a SEM observation result after a drop test of an Example. FIG. 10 is an energy dispersive X-ray analysis (EDX) result of the Mo electrode side of the fracture surface of an Example electrode.
[0010] In the acoustic wave device described in Cited Document 1, when a high-temperature process such as reflow bonding is repeatedly performed or when the device is used at high temperatures for a long time, various metal materials, such as the under-bump metal, react with the metal contained in the solder, which may deteriorate the mechanical properties of the solder and reduce the interfacial strength of the soldered joint.
[0011] According to one aspect of the present disclosure, sufficient interfacial strength can be ensured at the solder joint even after undergoing high-temperature processes such as reflow bonding.
[0012] [Embodiment 1] One embodiment of the present disclosure will be described in detail below. Hereinafter, the device according to the present disclosure may be, for example, an electronic device including a substrate and electronic components such as electronic elements mounted on the substrate. An electronic module (electrical device) including the device is configured by mounting the device on a mounting substrate (module substrate).
[0013] Substrate An exemplary substrate 110 according to the present disclosure will now be described.
[0014] 1 is a cross-sectional structural view showing a part of a substrate 110 according to a first embodiment of the present disclosure. FIG. 1 is an enlarged cross-sectional structural view of a portion of the substrate 110 where an electrode 21 is located.
[0015] The substrate 110 includes a base 11, an electrode 21, a barrier layer 31, and a bonding layer 32. In the substrate 110, the barrier layer 31 and the bonding layer 32 are layered in this order from the electrode 21 side.
[0016] The substrate 110 is a substrate on which electronic components are mounted, and may include internal wiring located inside the substrate 110 and through conductors that vertically connect the internal wirings to each other.
[0017] The substrate 110 has a base 11 that may be composed of a single layer or multiple layers. The base 11 has a first surface 11a and a second surface 11b located on the opposite side of the first surface 11a. An electronic component such as an electronic element may be mounted on either the first surface 11a or the second surface 11b.
[0018] The substrate 11 has insulating properties. In this case, the material of the substrate 11 may be ceramic, such as an aluminum nitride sintered body, an aluminum oxide sintered body (alumina ceramics), a silicon nitride sintered body, a mullite sintered body, or a glass ceramic sintered body. Alternatively, the material of the substrate 11 may be resin, such as epoxy resin, polyimide resin, acrylic resin, phenolic resin, or fluorine-based resin. Examples of the fluorine-based resin include polyester resin and tetrafluoroethylene resin. Alternatively, the substrate 11 may be a Si substrate. Alternatively, the substrate 11 may be a substrate made of a support substrate made of Si and a lithium tantalate (LiTaO 3 :LT) or lithium niobate (LiNbO 3 The piezoelectric substrate may be formed by combining it with a piezoelectric substrate made of a single crystal material (also called LN).
[0019] (Electrode) The electrode 21 of the substrate 110 electrically connects the device 200 including the substrate 110 to a circuit board. The electrode 21 is located on the first surface 11a of the base 11. The substrate 110 may have a plurality of electrodes 21 on the first surface 11a.
[0020] The electrode 21 may include a wiring layer 21A that transmits signals and an adhesion layer 21B that improves adhesion between the wiring layer 21A and the barrier layer 31.
[0021] The wiring layer 21A may include, for example, at least one of a Ni layer mainly composed of Ni (nickel), a Cu layer mainly composed of Cu (copper), a layer made of an alloy containing Ni (nickel) and Cu (copper), an Al layer mainly composed of Al (aluminum), and a Ti layer mainly composed of Ti (titanium).
[0022] The adhesion layer 21B may include at least one of a layer mainly composed of Ti and a layer mainly composed of Cr. By including at least one of a layer mainly composed of Ti and a layer mainly composed of Cr in the adhesion layer 21B, it is possible to improve the adhesion between the wiring layer 21A and the barrier layer 31. The adhesion layer 21B may be composed only of a layer mainly composed of Ti.
[0023] The adhesion layer 21B may be in contact with the barrier layer 31. As will be described in detail in the <Device Configuration> section below, the barrier layer 31 is referred to as the first layer 301 in the device 200 (see FIG. 2 ). Therefore, in the device 200, the adhesion layer 21B may be in contact with the first layer 301. The electrode structure has a laminated structure composed of a wiring layer, an adhesion layer, and a protective layer that protects the electrode and acts as a base for the barrier layer. The protective layer may be composed of, for example, a single Ni layer or a multi-layer structure of Ni and Au layers. By using the barrier layer 31 according to the present disclosure, which contains Mo as a main component, the electrode 21 according to the present disclosure does not need to have a protective layer. By having the adhesion layer 21B in contact with the barrier layer 31, the cost of the electrode 21 can be reduced and the electrode 21 can be made thinner.
[0024] The substrate 110 may have a metallized layer on the surface of the base 11 in addition to the electrodes 21. The metallized layer includes, for example, a metallized layer that is provided in a mounting region of the base 11 where an electronic component is mounted and that can be electrically connected to the electronic component.
[0025] When the base 11 is made of an electrically insulating ceramic, the metallization layer may be made of, for example, any one of W (tungsten), Mo (molybdenum), Mn (manganese), Ag (silver), Ni, and Cu, or an alloy containing at least one of these. When the base 11 is made of a resin, the metallization layer may be made of, for example, any one of Cu, Au (gold), Al (aluminum), Ni, Mo, and Ti, or an alloy containing at least one of these. The internal wiring and through conductors may also have the same configuration as the metallization layer.
[0026] (Barrier Layer) The barrier layer 31 is a layer containing Mo as a primary component. The manufacturing process for devices and electronic modules including the substrate 110 includes a high-temperature soldering process. For example, when solder balls are placed and then heated, molten, high-temperature solder is applied to the electrodes 21. Furthermore, when reflow bonding is performed, the device 200 or electronic module 300 with the solder applied to the electrodes is heated in a reflow furnace. Furthermore, the soldered joints may be repeatedly or continuously exposed to high temperatures due to heat generation from the electronic module 300 during use. In such cases, without the barrier layer 31, electrode metals such as Cu and Ni contained in the electrodes 21 would melt and react with metals such as Sn (tin) and Cu contained in the solder, forming metal compounds. These metal compounds are hard and brittle, making them prone to crack initiation.
[0027] The barrier layer 31 located between the electrode 21 and the solder can reduce the possibility of reaction between the electrode metal contained in the electrode 21 and the metal contained in the solder. In other words, the diffusion of the electrode metal into the solder can be reduced. This can reduce the formation of metal compounds. The thickness of the barrier layer 31 may be, for example, 0.1 μm or more. By making the barrier layer 31 have a thickness of 0.1 μm or more, the possibility of reaction between the electrode metal and the metal of the solder layer can be significantly reduced. This can maintain the interface strength.
[0028] Although FIG. 1 shows an example in which the barrier layer 31 covers a portion of the electrode 21 , the barrier layer 31 may cover the entire exposed surface of the electrode 21 .
[0029] (Bonding Layer) The bonding layer 32 is located on the barrier layer 31 and is a layer containing at least one of Ni, Ag, Au, and Cu. The presence of the bonding layer 32 ensures the wettability of the solder, thereby improving the interfacial strength of the solder interface.
[0030] The bonding layer 32 may be composed of an underlayer located on the barrier layer 31 and a surface layer located on the underlayer.
[0031] For example, the bonding layer 32 may have a laminated structure including a Ni layer positioned as a base layer on the barrier layer 31 and an Au layer positioned on the base layer. This structure significantly improves wettability compared to, for example, a case where a single Au layer is used as the bonding layer 32.
[0032] Alternatively, the bonding layer 32 may include a layer made of a silver alloy primarily composed of Ag. For example, the bonding layer 32 may have a laminated structure consisting of a Ni layer positioned as an underlayer on the barrier layer 31 and a layer made of a silver alloy positioned on the underlayer. The silver alloy may be an alloy primarily composed of Ag, such as APC, commercially available from Furuya Metal. This configuration reduces costs compared to using an Au layer as the outermost layer of the bonding layer 32. Furthermore, using a silver alloy layer as the outermost layer of the bonding layer 32 further improves wettability compared to using an Au layer. Furthermore, a silver alloy layer dissolves slowly into the solder when it comes into contact with molten solder, thereby further reducing dissolution of the electrode metal, especially during repeated soldering.
[0033] The thickness of the bonding layer 32 may be smaller than the thickness of the electrode 21. For example, the thickness of the bonding layer 32 may be 0.1 μm or more and 1 μm or less, and may be 0.1 μm.
[0034] Under high temperature conditions, such as during soldering, the metal contained in the bonding layer 32 may react with the metal contained in the solder, forming a metal compound. By setting the thickness of the bonding layer 32 to the above-described thickness, the amount of metal eluted from the bonding layer 32 during soldering or other processes can be reduced, thereby reducing the amount of metal compounds formed. Furthermore, because the amount of metal eluted from a sufficiently thin bonding layer 32 is small, coarse particles of metal compounds are less likely to form, making the layer less brittle. In other words, a bonding portion 30 with excellent interfacial strength can be achieved while maintaining the wettability of the solder. The bonding portion 30 will be described later.
[0035] <Configuration of Device> The configuration of device 200 as an exemplary device according to the present disclosure will be described below. Fig. 2 is a cross-sectional structural view showing a portion of device 200 according to embodiment 1 of the present disclosure. Fig. 2 is an enlarged cross-sectional structural view of an electrode 21 portion provided in device 200, and does not show electronic components provided in device 200.
[0036] The device 200 according to the present disclosure can be obtained, for example, by placing solder balls on the substrate 110 shown in Fig. 1 and then heating the substrate. More specifically, a method for manufacturing the device 200 includes (1) a step of preparing the substrate 110, and (2) a step of placing solder on the bonding layer 32 of the substrate 110 and heating the solder to form a bonding portion 30 on the electrode 21. Hereinafter, for simplicity, the step (1) will be referred to as the substrate preparation step, and the step (2) will be referred to as the bonding portion formation step.
[0037] The device 200 has a substrate 11, an electrode 21, and a bonding portion 30. The bonding portion 30 is located on the electrode 21 and includes, in order from the electrode 21 side, a first layer 301, a second layer 302, and a third layer 303. FIG. 3 is a scanning transmission electron microscopy (STEM) photograph of a cross section of the electrode 21 and the bonding portion 30. FIG. 4 is a STEM photograph further enlarging the vicinity of the second layer 302 of the cross section of the electrode 21 and the bonding portion 30. The cross-sectional photographs of FIGS. 3 and 4 were obtained by cutting out a portion of the device 200 including the electrode 21 and the bonding portion 30 using a focused ion beam (FIB) and photographing it using STEM.
[0038] The first layer 301 is a layer containing Mo as a main component. The first layer 301 in the device 200 corresponds to the barrier layer 31 of the substrate 110. The barrier layer 31 remains substantially unchanged even after repeated heating and reflow bonding after placing the solder balls, and is located in the bonding portion 30 as the first layer 301.
[0039] The second layer 302 is a layer containing β-Sn as a main component. The second layer 302 is formed when the substrate 110 according to the present disclosure is solder-bonded. For example, the second layer 302 in the device 200 is formed in the above-described joint fabrication process.
[0040] In the joint forming step, when solder is placed on the joining layer 32 and heated, at least a part of the metal in the joining layer 32 reacts with the metal contained in the molten solder to form one or more metal compounds. The metal compound may be a Sn compound. For example, if the joining layer 32 before solder joining is mainly composed of Ni, Ni 3 Sn 4 , Ni 3 Sn 2 , Ni 3 Sn, (Cu, Ni) 3 Sn 4 , and (Cu, Ni) 6 Sn 5 At least one compound selected from the group consisting of the metal compounds mentioned above may be formed. The metal compound may be formed as a compound mass in the third layer 303 near the second layer 302 (see FIG. 3). In other words, the third layer 303 may contain a metal compound formed by a reaction between a metal contained in the bonding layer 32 and a metal contained in the solder.
[0041] Upon heating, at least a portion of the bonding layer 32 is incorporated into the third layer 303, forming a metal compound, while the second layer 302 is formed between the third layer 303 and the first layer 301. The second layer 302 is thought to be formed by the growth of oriented β-Sn crystals near the first layer 301 when the solder that forms the third layer 303 melts. The growth of the β-Sn crystals is due to the fact that the first layer 301 is a layer containing Mo as its main component. For example, the inventors have confirmed that when tungsten is used as the barrier layer, a layer containing β-Sn as its main component is not formed.
[0042] The second layer 302 may be located over the entire surface between the first layer 301 and the third layer 303. Alternatively, there may be a region between the first layer 301 and the third layer 303 where the second layer 302 is not present. Furthermore, a portion of the bonding layer 32 of the substrate 110 may remain between the first layer 301 and the third layer 303.
[0043] Here, the lattice structures of the first layer 301 and the second layer 302 will be described. In the bonding portion 30, the {111} plane of Mo contained in the first layer 301 and the {110} plane of β-Sn contained in the second layer 302 may be approximately parallel. "Approximately parallel" means that strict parallelism is not required; for example, a tilt of ±5° of one plane relative to the other plane is acceptable. FIG. 5 is a schematic diagram showing the arrangement of atoms in the
[111] direction of β-Sn and the arrangement of atoms in the
[121] direction of Mo. The interatomic distance d(β-Sn) in the {112} plane of β-Sn is 1.4843 Å, and the interatomic distance d(Mo) in the {110} plane of Mo is 2.2254 Å. The lengths of three interatomic distances of β-Sn and two interatomic distances of Mo are 3×d(β-Sn)=4.4529 Å and 2×d(Mo)=4.4508, which are almost equal.
[0044] The characteristic interatomic distance matching between the two layers, which occurs because the {111} plane of Mo and the {110} plane of β-Sn are approximately parallel to each other, allows the strength of the interface between the first layer 301 and the second layer 302 to be maintained.
[0045] Metal compounds formed near the solder joint surface due to the reaction between the electrode metal and the solder are often hard and brittle, but β-Sn, the main component of the second layer 302, is softer than these metal compounds. By including the second layer 302 on the solder joint surface, the device 200 according to the present disclosure can significantly improve impact resistance. This can improve the joint reliability of the electronic module.
[0046] Furthermore, a metal layer (e.g., Au) provided on the electrode to improve the solder wettability may form a metal compound when heated, which may repel the molten solder at the interface between the electrode and the solder during reflow bonding. By including the second layer 302, the device 200 according to the present disclosure can maintain the solder wettability even during reflow bonding.
[0047] The thickness of the second layer 302 may be 100 nm or more. When the thickness of the second layer 302 is 100 nm or more, the effects of maintaining the impact resistance and wettability during reflow bonding can be obtained with higher reliability.
[0048] The third layer 303 is a layer containing solder. The third layer 303 is mainly composed of Sn, and may contain metals other than Sn, such as Ag and Cu.
[0049] <Configuration of Electronic Module> Fig. 6 is a cross-sectional structural view showing a portion of an electronic module 300 including a device 200. As shown in Fig. 6, the electronic module 300 can be configured by mounting the device 200 on a mounting substrate (module substrate) 120. The electronic module 300 is an example of an electric device according to the present disclosure.
[0050] The electronic module 300 can be manufactured by reflow bonding the device 200 and the mounting substrate 120. That is, the electronic module 300 includes the device 200. The mounting substrate 120 is a circuit board mounted on the electronic module 300, and may include an electrical circuit inside and / or outside the mounting substrate 120. Before reflow bonding, the mounting substrate 120 includes a base 12, an electrode 22, a barrier layer 31, and a bonding layer 32, similar to the substrate 110. The electrode 22 of the mounting substrate 120 electrically connects the mounting substrate 120 to an electronic device or the like. The electrode 22 is located on the first surface 12a of the base 12. The base 12, the electrode 22, the barrier layer 31, and the bonding layer 32 of the mounting substrate 120 may have the same configurations as the base 11, the electrode 21, the barrier layer 31, and the bonding layer 32 of the substrate 110, respectively.
[0051] More specifically, electronic module 300 includes base 11 and electrode 21 of device 200, base 12 and electrode 22 of mounting substrate 120, and joint 30. In other words, electronic module 300 has a configuration in which electrode 21 of device 200 and electrode 22 of mounting substrate 120 are joined by joint 30. Joint 30 includes, in order from the side of electrodes 21 and 22, a first layer 301, a second layer 302, and a third layer 303. First layer 301, second layer 302, and third layer 303 have the configurations described above.
[0052] The electronic module 300 has the second layer 302, which provides excellent interfacial strength and allows the solder to maintain wet spread even after high-temperature processes such as reflow. This allows for an electronic module with excellent joint reliability and impact resistance.
[0053] As described above, by including the barrier layer 31 and the bonding layer 32, the substrate 110 can ensure the wettability of the solder during solder bonding, while reducing the amount of Sn-containing compounds formed near the interface between the solder layer 33 and the bonding layer 32. As a result, the substrate 100 can provide a device or electronic module that has sufficient interfacial strength at the soldered joints, even after undergoing high-temperature processes such as reflow bonding.
[0054] Furthermore, by including the second layer 302, the device 200 and the electronic module 300 can maintain the wetting and spreading properties of the solder even after high-temperature processes such as reflow. This allows sufficient interfacial strength to be maintained, resulting in an electronic module with excellent bonding reliability. Furthermore, the properties of the second layer 302 allow an electronic module with excellent impact resistance to be realized.
[0055] [Embodiment 2] Another embodiment of the present disclosure will be described below. For convenience of explanation, the same reference numerals will be used to designate components having the same functions as those described in the above embodiment, and the description thereof will not be repeated.
[0056] In the second embodiment, an example will be described in which the device 200 is an acoustic wave device. Fig. 7 is a cross-sectional structural view of an acoustic wave device 210 in accordance with the second embodiment.
[0057] The acoustic wave device 210 includes a base 13, an electrode layer 23, and a joint 30. The acoustic wave device 210 can be mounted on a circuit board (mounting board) of a communication device.
[0058] The base 13 is an example of a base according to the present disclosure. The base 13 includes a piezoelectric layer 13A and a support substrate 13B that supports the piezoelectric layer 13A. The piezoelectric layer 13A has a first surface 13a located on the side opposite to the surface bonded to the support substrate 13B. The electrode layer 23 is provided on the first surface 13a of the piezoelectric layer 13A. The base 13 is not limited to the above configuration. For example, the base 13 does not need to include the support substrate 13B. In this case, the piezoelectric layer 13A itself also serves as the support substrate 13B.
[0059] The electrode layer 23 includes an IDT (Interdigital Transducer) electrode 231 and a pad portion 232. The pad portion 232 includes a first pad 232A and a second pad 232B. The pad portion 232 in this embodiment is an example of the electrode 21 according to the present disclosure. The first pad 232A and the second pad 232B are laminated in this order from the base 13 side. In other words, the pad portion 232 may include multiple layers. The first pad 232A may have the same thickness as the IDT electrode 231. The pad portion 232 has a laminated structure, which can reduce electrical resistance.
[0060] Acoustic wave device 210 is obtained by joining solder to substrate 130. Substrate 130 has a barrier layer and a bonding layer according to the present disclosure on pad portion 232. Substrate 130 is an example of a substrate according to the present disclosure.
[0061] By soldering, the barrier layer and the bonding layer, together with the solder, form a bonding portion 30. The bonding portion 30 is located on the pad portion 232 and includes, in order from the pad portion 232 side, a first layer 301, a second layer 302, and a third layer 303. In the acoustic wave device 210, the first layer 301, the second layer 302, and the third layer 303 are layered in this order from the pad portion 232 side. The first layer 301, the second layer 302, and the third layer 303 have the same configuration as described in the first embodiment.
[0062] The IDT electrode 231 is a comb-shaped electrode that generates an acoustic wave in the acoustic wave device. The IDT electrode 231 is composed of a pair of electrodes to which an AC voltage is applied. The IDT electrode 231 is electrically connected to a pad portion 232.
[0063] Compared to other electronic devices, acoustic wave device 210 has fewer joints via joints 30. Therefore, ensuring interfacial strength at joints 30 is even more important. Because acoustic wave device 210 includes substrate 130 and joints 30, sufficient interfacial strength can be ensured at the solder joints even after high-temperature processes such as reflow bonding. Furthermore, the inclusion of second layer 302 allows the solder to maintain wet spreading even after high-temperature processes such as reflow bonding. This allows for an acoustic wave device with excellent joint reliability. Furthermore, the properties of second layer 302 allow for an acoustic wave device with excellent impact resistance.
[0064] In the second embodiment, the acoustic wave device is described as being a surface acoustic wave (SAW) device, but is not limited to this. For example, the acoustic wave device may be a bulk acoustic wave (BAW) device.
[0065] [Demonstration Test] Below, a demonstration test that demonstrates the effects of the substrate, device, and electrical device of the present disclosure will be described.
[0066] (Demonstration Test 1: Comparison Using Microscope Photographs) FIG. 8 is a microscope photograph of a joint 30 of an electronic module. Reference numeral 8001 in FIG. 8 is a microscope photograph of the joint 30 in an electronic module 300 according to an example of the present disclosure. Reference numeral 8002 in FIG. 8 is a microscope photograph of a joint of an electronic module as a comparative example. The electronic module of the comparative example has a solder layer located between the electrodes on the electronic device side and the mounting substrate. In other words, it does not have the first layer 301 and second layer 302 according to the present disclosure. More specifically, the electronic module of the comparative example is formed by soldering an electronic device and a mounting substrate that do not have the barrier layer 31 and bonding layer 32 according to the present disclosure on the electrodes. The heating conditions during solder bonding were the same for both the example and the comparative example.
[0067] 8, a comparative example indicated by reference numeral 8002 has a region C near the interface of the joint that contains a large amount of compounds formed by a reaction between the electrode metal and the metal contained in the solder layer, and this region C is a coarse granular region. In addition, a large amount of the electrode metal has eluted toward the solder layer, forming a void P at the interface of the joint.
[0068] 8, the area C near the interface of the joint 30 is relatively small. Also, the void P observed in the comparative example was not observed.
[0069] A device manufactured using a substrate having a barrier layer 31 and a bonding layer 32 according to the present disclosure has a bonding portion including a first layer 301 and a second layer 302. It has been demonstrated that a device having a bonding portion including the first layer 301 and the second layer 302 can significantly reduce the formation of brittle compounds at the solder bonding portion, even after undergoing a high-temperature process such as reflow bonding. It has also been demonstrated that the barrier layer 31 reduces the elution of the electrode metal into the solder layer, thereby reducing the possibility of voids occurring at the interface between the electrode and the bonding portion.
[0070] From the above, it has been demonstrated that the substrate, device, and electrical device according to the present disclosure can ensure sufficient interfacial strength at the solder joints even after undergoing high-temperature processes.
[0071] (Demonstration Test 2: Bonding Strength Test 1 - Effect of Different Metals Used as Barrier Layer) Figures 9 to 12 are graphs showing the results of evaluating the bonding strength when the metal used for the barrier layer is changed. The bonding strength evaluation test was conducted in accordance with the JEDEC JESD22-B117 solder ball shear standard.
[0072] In Comparative Example 1, a Ni layer was laminated on a substrate as an electrode, a TaN (tantalum nitride) layer was laminated as a barrier layer, and a solder ball was placed on top of that. Figure 9 shows the results of tests conducted on the configuration of Comparative Example 1 after performing a reflow treatment once and after performing a reflow treatment three times.
[0073] In Comparative Example 2, a Ni layer was laminated on a substrate as an electrode, a TiN (titanium nitride) layer was laminated on a substrate as a barrier layer, and a solder ball was placed on top of that. Figure 10 shows the results for Comparative Example 2.
[0074] In Comparative Example 3, a Ni layer was laminated as an electrode on a substrate, a W (tungsten) layer was laminated as a barrier layer, and a solder ball was placed thereon. Figure 11 shows the results for Comparative Example 3.
[0075] In Example 1, a Ni layer was stacked on a substrate as an electrode, and a Mo (molybdenum) layer, which is the same as the barrier layer 31 of the present disclosure, was stacked as a barrier layer, and a solder ball was placed thereon. Figure 12 shows the results of this example.
[0076] In Comparative Examples 1 and 2, the graphs show a sudden drop in load at a relatively small displacement in both the cases of one reflow treatment and three reflow treatments. This indicates that the interfacial strength is weak, and peeling occurs at the solder interface at the displacement where the load drops suddenly.
[0077] In Comparative Example 3, when the reflow process was performed once, the load did not drop sharply within the test range of displacement. The gradual drop in load indicates that bulk failure of the solder occurred, rather than peeling. However, when the reflow process was performed three times, the load also dropped sharply at small displacements. This indicates that the interfacial strength was weakened by repeated reflow processes.
[0078] On the other hand, in the examples, the load did not drop suddenly within the test range of displacement in either the case of one reflow treatment or three reflow treatments, demonstrating that the interfacial strength was maintained within the test range of displacement.
[0079] The above test results demonstrate that by using a barrier layer 31 containing Mo as its main component, sufficient interfacial strength can be ensured at the solder joint even after high-temperature processes such as reflow bonding.
[0080] (Demonstration Test 3: Bonding Strength Test 2 - Verification of Barrier Layer and Bonding Layer Configuration) Figure 13 is a graph showing the results of evaluating the bonding strength when the configuration of the barrier layer and bonding layer was changed using a model sample of the device. The bonding strength evaluation test was conducted in accordance with the solder ball shear standard of JEDEC JESD22-B117. The bonding strength evaluation test was conducted for each example or comparative example after three reflow treatments. The same test was also conducted six times for each example or comparative example.
[0081] Examples 2, 3, and 4 and Comparative Example 4 were prepared as follows as device samples used in Demonstration Test 3. All Examples and Comparative Examples shared a common substrate, a Si substrate. The electrodes were also common, with a layered structure consisting of an Al layer as a wiring layer, a Ti layer as an adhesion layer, and a Ni layer as a protective layer.
[0082] Example 2: Barrier layer - Mo layer (0.3 μm), bonding layer - Ni layer (0.2 μm) and Au layer (0.05 μm) laminated structure. Manufactured by placing a solder ball on the bonding layer.
[0083] Example 3: Barrier layer - Mo layer (0.1 μm), bonding layer - Ni layer (0.2 μm) and Au layer (0.05 μm) laminated structure. Manufactured by placing a solder ball on the bonding layer.
[0084] Example 4: Barrier layer - Mo layer (0.3 μm), bonding layer - Ni layer (0.1 μm) and Au layer (0.05 μm) laminated structure. Manufactured by placing a solder ball on the bonding layer.
[0085] Comparative Example 4: Barrier layer - none, bonding layer - laminated structure of Ni layer (0.6 μm) and Au layer (0.05 μm) A solder ball was placed on the bonding layer to produce the product.
[0086] Reference numeral 1301 in Fig. 13 indicates the results of Example 2. Reference numeral 1302 in Fig. 13 indicates the results of Example 3. Reference numeral 1303 in Fig. 13 indicates the results of Example 4. Reference numeral 1304 in Fig. 13 indicates the results of Comparative Example 4.
[0087] Examples 2 to 4 each have a configuration within the scope of the present disclosure. Comparative Example 4 does not include a barrier layer containing Mo as a main component, and therefore has a configuration outside the scope of the present disclosure.
[0088] In Comparative Example 4, the load dropped sharply at a displacement of less than 10 μm. On the other hand, in Examples 2 to 4, the load did not drop sharply within the test range of displacement, demonstrating that the interfacial strength was maintained within the test range of displacement.
[0089] The results of Example 3 demonstrate that the barrier layer according to the present disclosure, having a thickness of 0.1 μm or more, can ensure sufficient interfacial strength at the solder joint even after undergoing a high-temperature process such as reflow bonding. The results of Example 4 demonstrate that the bonding layer according to the present disclosure, having a thickness of 0.05 μm or more, can ensure sufficient interfacial strength at the solder joint even after undergoing a high-temperature process such as reflow bonding.
[0090] (Demonstration Test 4: Bonding Strength Test 3 - Verification of Bonding Strength with and without Protective Layer) Fig. 14 is a graph showing the results of evaluating the bonding strength of electrodes according to the present disclosure, with and without a protective layer. The bonding strength evaluation test was conducted in accordance with the JEDEC JESD22-B117 solder ball shear standard.
[0091] 14 indicates the results obtained using the sample of Example 2 in Demonstration Test 3. In Example 2, the electrode has a layered structure including an Al layer as a wiring layer, a Ti layer as an adhesion layer, and a Ni layer as a protective layer.
[0092] 14 indicates the results of Example 5, in which the electrode has a laminated structure consisting of an Al layer as a wiring layer and a Ti layer as an adhesion layer. In other words, Example 5 does not have a Ni layer as a protective layer, and has a configuration in which the adhesion layer and the barrier layer are in contact with each other. Example 5 is a configuration within the scope of the present disclosure.
[0093] In Example 5 as well, the load did not drop suddenly within the test range of displacement, demonstrating that the interfacial strength was maintained within the test range of displacement.
[0094] In other words, it has been demonstrated that in the substrate according to the present disclosure, when the adhesion layer and the barrier layer are in contact with each other, sufficient interfacial strength can be ensured at the solder joint even after undergoing high-temperature processes such as reflow bonding.
[0095] (Demonstration Test 5: Bonding Strength Test 4 - High-Temperature Test) A high-temperature test was conducted using a sample having a bond according to the present disclosure, and the cross-sectional structure after the high-temperature test was observed and the bonding strength was evaluated. FIG. 15 shows the results of the bonding strength evaluation test. The high-temperature test was conducted in accordance with the IEC 60068-2-2 standard at 150°C for 1000 hours. The bonding strength evaluation test was conducted in accordance with the JEDEC JESD22-B117 solder ball shear standard.
[0096] The samples used for observing the cross-sectional structure in Demonstration Test 5 were prepared by placing solder balls on the following substrate samples, and then reflow-bonding them to the following mother substrate samples.
[0097] Substrate sample: Base - Si substrate, electrode - laminated structure of Ni layer (0.6 μm) and Ti layer (0.05 μm), barrier layer - Mo layer (0.3 μm), bonding layer - laminated structure of Ni layer (0.2 μm) and Au layer (0.05 μm). Mother substrate sample: Base - Si substrate, electrode - laminated structure of Ni layer (0.6 μm) and Ti layer (0.05 μm), barrier layer - Mo layer (0.3 μm), bonding layer - laminated structure of Ni layer (0.2 μm) and Au layer (0.05 μm).
[0098] The sample fabricated as described above is within the scope of the present disclosure and includes an electrode and a joint located on the electrode, the joint including, from the electrode side, a first layer containing Mo as a main component, a second layer containing β-Sn as a main component, and a third layer containing solder.
[0099] The samples used to evaluate the bonding strength in Demonstration Test 5 were prepared by placing solder balls on the above-mentioned substrate samples. As shown in Figure 15, the samples within the scope of the present disclosure did not result in a sudden drop in load within the test range of displacement, demonstrating that the interfacial strength was maintained within the test range of displacement.
[0100] In other words, it was demonstrated that the substrate according to the present disclosure can ensure sufficient interface strength in a high-temperature test at 150° C. for 1000 hours.
[0101] (Demonstration Test 6: Bonding Strength Test 5 - High-Temperature, High-Humidity Test) A high-temperature, high-humidity test was conducted using a sample having a bond according to the present disclosure, and the cross-sectional structure after the high-temperature, high-humidity test was observed and the bonding strength was evaluated. FIG. 16 shows the results of the bonding strength evaluation test. The high-temperature, high-humidity test was conducted in accordance with the IEC 60068-2-78 standard at 85°C, 85 RH, and 1000 hours. The bonding strength evaluation test was conducted in accordance with the JEDEC JESD22-B117 solder ball shear standard.
[0102] The samples used for observing the cross-sectional structure in Demonstration Test 6 were prepared by placing solder balls on the following substrate samples, and then reflow-bonding them to the following mother substrate samples.
[0103] Substrate sample: Base - Si substrate, electrode - laminated structure of Ni layer (0.6 μm) and Ti layer (0.05 μm), barrier layer - Mo layer (0.3 μm), bonding layer - laminated structure of Ni layer (0.2 μm) and Au layer (0.05 μm). Mother substrate sample: Base - Si substrate, electrode - laminated structure of Ni layer (0.6 μm) and Ti layer (0.05 μm), barrier layer - Mo layer (0.3 μm), bonding layer - laminated structure of Ni layer (0.2 μm) and Au layer (0.05 μm).
[0104] The sample fabricated as described above is within the scope of the present disclosure and includes an electrode and a joint located on the electrode, the joint including, from the electrode side, a first layer containing Mo as a main component, a second layer containing β-Sn as a main component, and a third layer containing solder.
[0105] The samples used to evaluate the bonding strength in Demonstration Test 6 were prepared by placing solder balls on the above-mentioned substrate samples. As shown in Figure 16, the samples within the scope of the present disclosure did not result in a sudden drop in load within the test range of displacement, demonstrating that the interfacial strength was maintained within the test range of displacement.
[0106] In other words, it was demonstrated that the electronic module according to the present disclosure can ensure sufficient interface strength in a high-temperature, high-humidity test for 1000 hours under conditions of 85° C. and 85% RH.
[0107] (Demonstration Test 7: Temperature Cycle Test 1) A temperature cycle test was conducted using a model sample of an electronic module having a joint according to the present disclosure, and the cross sections of the example sample (Example 6) and the comparative example sample (Comparative Example 5) after the temperature cycle test were observed.
[0108] The temperature cycle test was conducted in accordance with the IEC 60068-2-14 standard, with 300 cycles of repeated temperature changes from -40°C to 85°C. The cross sections were observed using SEM photographs of samples taken every 50 cycles, embedded in resin, and polished.
[0109] The example sample (Example 6) and the comparative example sample (Comparative Example 5) used in Demonstration Test 7 were reflow-bonded to the following motherboard sample after solder balls were placed on the substrate sample.
[0110] Example 6: Substrate sample: Base—Si substrate, Electrode—Laminated structure of Ni layer (0.6 μm) and Ti layer (0.05 μm), Barrier layer—Mo layer (0.3 μm), Bonding layer—Laminated structure of Ni layer (0.2 μm) and Au layer (0.05 μm) Mother substrate sample: Base—LiTaO 3 Substrate, electrode - laminated structure of Ni layer (0.6 μm) and Ti layer (0.05 μm), barrier layer - Mo layer (0.3 μm), bonding layer - laminated structure of Ni layer (0.2 μm) and Au layer (0.05 μm).
[0111] Example 6, fabricated as described above, is within the scope of the present disclosure and includes an electrode and a joint located on the electrode. The joint includes, from the electrode side, a first layer containing Mo as a primary component, a second layer containing β-Sn as a primary component, and a third layer containing solder.
[0112] Comparative Example 5: Substrate sample: Base—Si substrate, Electrode—Laminated structure of Ni layer (0.6 μm) and Ti layer (0.05 μm), Barrier layer—None, Bonding layer—Laminated structure of Ni layer (0.6 μm) and Au layer (0.05 μm) Mother substrate sample: Base—LiTaO3 Substrate, electrode - laminated structure of Ni layer (0.6 μm) and Ti layer (0.05 μm), barrier layer - none, bonding layer - laminated structure of Ni layer (1.2 μm) and Au layer (0.05 μm).
[0113] The electronic module of Comparative Example 5, fabricated as described above, does not have the first and second layers according to the present disclosure and is outside the scope of the present disclosure.
[0114] In Demonstration Test 7, cracking of the substrate was observed in the comparative example after 50 cycles or more. On the other hand, fatigue was observed in the joint after 200 cycles or more in Example 6, but no cracking of the substrate was observed even after 300 cycles. This result is thought to be due to the fact that the flexible joint is able to absorb the difference in thermal expansion at the joint.
[0115] In other words, it was demonstrated that the electronic module according to the present disclosure can obtain sufficient bonding reliability in a temperature cycle test of 300 cycles from -40°C to 85°C.
[0116] (Demonstration Test 8: Hardness of Joint) In Demonstration Test 8, the hardness of the solder (joint) in a device within the scope of the present disclosure and the hardness of the solder in a device outside the scope of the present disclosure were evaluated by nanoindentation.
[0117] The example sample (Example 7) and the comparative example sample (Comparative Example 6) used in Demonstration Test 8 were prepared as follows.
[0118] Example 7: Substrate—Si substrate, electrode—layered structure of Ni layer (0.6 μm) and Ti layer (0.05 μm), barrier layer—Mo layer (0.3 μm), bonding layer—layered structure of Ni layer (0.2 μm) and Au layer (0.05 μm). Two substrates having this configuration were prepared and soldered together to produce the device.
[0119] The sample of Example 7 prepared as described above is within the scope of the present disclosure, and has a joint according to the present disclosure formed on an electrode. The joint has, from the electrode side, a first layer containing Mo as a main component, a second layer containing β-Sn as a main component, and a third layer containing solder.
[0120] Comparative Example 5: Substrate—Si substrate, electrode—layered structure of Ni layer (0.6 μm) and Ti layer (0.05 μm), barrier layer—none, bonding layer—layered structure of Ni layer (1.2 μm) and Au layer (0.05 μm). Two substrates having this configuration were prepared and solder-bonded together to produce the comparative example.
[0121] The device of Comparative Example 5, prepared as described above, does not have the first and second layers according to the present disclosure and is outside the scope of the present disclosure.
[0122] 17 is a graph showing the results of nanoindentation for Example 7 (Ni / Mo) and Comparative Example 6 (Ni (1.2 μm)). As can be seen from FIG. 17, the solder hardness is lower in Example 7. In other words, it was demonstrated that the joint according to the present disclosure has a lower hardness than a joint that does not include the first and second layers, such as Comparative Example 6, and can absorb differences in thermal expansion due to deformation, etc.
[0123] (Demonstration Test 9: Temperature Cycle Test 2) A temperature cycle test was conducted using a model sample of an electronic module, and Weibull plots were created for the example sample and the comparative example sample. The example sample and the comparative example sample were the same as Example 6 and Comparative Example 5 prepared in Demonstration Test 7. The temperature cycle test was conducted in accordance with the IEC 60068-2-14 standard, with repeated temperature changes from -55°C to 125°C for 1000 cycles.
[0124] Fig. 18 is a Weibull plot of Example 6 (Ni / Mo) and Comparative Example 5 (Ni (1.2 µm)). As can be seen from Fig. 18, it was demonstrated that Example 6 had a longer number of cycles to fracture. In other words, it was demonstrated that the electronic module according to the present disclosure has higher bonding reliability than the comparative example.
[0125] (Demonstration Test 10: Drop Impact Test) A drop impact test was conducted using a model sample of an electronic module, and the example sample and the comparative example sample were compared. The drop impact test was conducted in accordance with the JEITA ET-7409 / 107 standard, in which a 4.1 g iron ball was dropped from heights of 0.5 m and 1.0 m, and the cross section of the solder joint was observed to check for fracture. The cross section was observed using SEM photographs.
[0126] Examples 8 and 9 and Comparative Examples 7 and 8 were prepared as model samples of the electronic module used in Demonstration Test 10 as follows. In each example and comparative example, solder balls were placed on each substrate sample, and then reflow-bonded to each mother substrate sample. Six samples were prepared for each example and comparative example and tested.
[0127] Example 8: Substrate sample: Base—Si substrate, electrode—laminated structure of Ti layer (0.015 μm) and Ni layer (0.3 μm), barrier layer—Mo layer (0.3 μm), bonding layer—laminated structure of Ni layer (0.1 μm) and Au layer (0.05 μm). Mother substrate sample: Base—Si substrate, electrode—laminated structure of Ti layer (0.015 μm) and Ni layer (0.3 μm), barrier layer—Mo layer (0.3 μm), bonding layer—laminated structure of Ni layer (0.1 μm) and Au layer (0.05 μm).
[0128] Example 9: Substrate sample: Base—Si substrate, electrode—Ti layer (0.015 μm), barrier layer—Mo layer (0.3 μm), bonding layer—Ni layer (0.2 μm) and Au layer (0.05 μm) laminated structure. Mother substrate sample: Base—Si substrate, electrode—Ti layer (0.015 μm), barrier layer—Mo layer (0.3 μm), bonding layer—Ni layer (0.2 μm) and Au layer (0.05 μm) laminated structure.
[0129] Comparative Example 8: Substrate sample: base—Si substrate, electrode—Ti layer (0.050 μm), bonding layer—Ni layer (1.2 μm) and Au layer (0.05 μm) laminated structure Mother substrate sample: base—Si substrate, electrode—Ti layer (0.050 μm), bonding layer—Ni layer (1.2 μm) and Au layer (0.05 μm) laminated structure.
[0130] Comparative Example 9: Substrate sample: laminated structure of base—Si substrate, electrode—Ti layer (0.050 μm), bonding layer—Ni layer (0.6 μm) and APC layer (0.1 μm). Mother substrate sample: laminated structure of base—Si substrate, electrode—Ti layer (0.050 μm), bonding layer—Ni layer (0.6 μm) and APC layer (0.1 μm).
[0131] When the drop distance was 0.5 m, no breakage was observed in four out of six samples for each of Examples 8 and 9, even after 100 or more drops. On the other hand, breakage was observed after an average of 6.7 drops for Comparative Example 8 and an average of 7.1 drops for Comparative Example 9.
[0132] In other words, it was demonstrated that the electronic module according to the present disclosure has superior impact resistance to the comparative example.
[0133] Furthermore, in order to investigate the above experimental results in more detail, the following additional experiments were carried out.
[0134] (Fabrication of Multilayer Electrodes) An electrode pattern was formed on a 4-inch Si wafer with a thickness of 525 μm using a photolithography process, and different configurations were deposited by sputtering on a Ti seed layer (0.05 μm). This Si wafer is an example of a substrate according to the present disclosure. A schematic diagram of the fabricated electrode structure is shown in FIG. 19. Reference numeral 1901 in FIG. 19 indicates a general-purpose Ni / Au electrode as a comparative example. The Ni thickness was set to 1.2 μm to prevent Ni loss due to dissolution. Reference numeral 1902 in FIG. 19 indicates a Ni / Mo / Ni / Au electrode as an example of the present disclosure, in which a Mo barrier layer was deposited on the 0.6 μm-thick Ni. This Mo barrier layer is an example of a barrier layer according to the present disclosure. Reference numeral 1903 in FIG. 19 indicates an electrode in which Mo / Ni / Au was deposited directly on a Ti seed layer as an example of the present disclosure. The Mo layer shown in the example of reference numeral 1903 is also an example of a barrier layer according to the present disclosure.
[0135] A 90 μm diameter Sn-3.0 mass% Ag-0.5 mass% Cu solder ball was mounted on a chip that had been diced into 1.5 mm x 1.5 mm and 2.5 mm x 1.5 mm pieces. Next, the solder balls were melted in a formic acid reducing atmosphere with a peak temperature of 260 ° C., and a simple bonded sample was produced in which the upper and lower chips were bonded with four 100 μm diameter electrodes. Reflow was repeated three times to simulate the thermal history during assembly.
[0136] (Impact Resistance Evaluation) Shear testing machines are often used to evaluate the strength of electrode parts. However, if the strength is above a certain level and the breakage occurs inside the solder, it is difficult to determine the superiority or inferiority of the electrode parts. Therefore, in this experiment, a repeated steel ball drop test was used. Figure 20 shows an overview of the steel ball drop test. As shown in Figure 20, an aluminum plate to which a bonded sample was attached with a cyanoacrylate adhesive was fixed at both ends, and a steel ball with a diameter of 10 mm and a mass of 4.1 g was dropped from a height of 500 mm aimed at the center of the back surface of the sample. The number of times the upper chip fell was compared. There were five samples for each.
[0137] (Results and Discussion) Figure 21 is a graph showing the results of a steel ball drop test. Figure 21 shows the results of comparing the number of steel ball drops required before the upper chip fell between electrode structures. The Ni / Au electrode, which is a comparative example, broke after an average of seven drops. On the other hand, the Ni / Mo / Ni / Au electrode and Mo / Ni / Au electrode, which are examples of the present disclosure and include a Mo barrier layer, saw a significant increase in the number of repeated drops required before breaking, exceeding 100. In a general-purpose bump shear test, both electrodes broke inside the solder, but a clear difference was apparent in the steel ball drop test.
[0138] To clarify the cause of the difference between electrodes with different configurations, scanning electron microscope (SEM) observations were performed. Figure 22 shows the SEM observation results of a comparative Ni / Au electrode after a drop test (five drops). As shown in the diagrams denoted by reference numerals 2201 and 2202 in Figure 22, the Ni in this electrode dissolved and disappeared over a width of approximately 5 μm from the outer periphery of the electrode, which is believed to be the origin of the fracture. It is presumed that cracks generated from this Ni-disappeared portion as an initial defect propagated through the Si interface, leading to the fracture of the Si chip. The dissolution and disappearance of the Ni electrode occurs because the outer periphery is thin after film formation, but this is due to the shadow of the resist during sputtering, making it difficult to avoid in the process.
[0139] On the other hand, Figure 23 shows the SEM observation results of a Ni / Mo / Ni / Au electrode according to an embodiment of the present disclosure after a drop test (289 drops). Striations, indicated by reference numeral 2302 in Figure 23, were observed from the outer periphery of the fractured surface of the solder bump indicated by reference numeral 2301 in Figure 23 to the dashed line region. The striation spacing was approximately 50 nm, and the maximum distance from the outer periphery to the dashed line was 20 μm. This suggests that repeated steel ball drops caused fatigue cracks to propagate to the dashed line region, resulting in macroscopic fracture. Reference numeral 2303 in Figure 23 is a cross-sectional photograph of the electrode. It can be seen that Mo covers even the thin portion of the Ni layer on the periphery, preventing Ni dissolution. It is believed that the absence of Ni and initial defects in the electrode of the embodiment significantly increased the number of drops required before fracture. The suppression of electrode dissolution by the introduction of a Mo barrier layer is also effective in improving impact resistance.
[0140] Figure 24 shows the results of energy dispersive X-ray analysis (EDX) of the Mo layer side of the fracture surface of a Ni / Mo / Ni / Au electrode, an example of the present disclosure. Previous research has shown that the internal structure after fusion bonding is a Mo / β-Sn / solder layer structure. EDX mapping revealed that a Sn layer was widely distributed on the Mo layer, but only a small amount of Ag was detected. The layer remaining on the Mo layer was primarily a β-Sn layer, suggesting that the crack propagated at the interface between the solder and β-Sn.
[0141] The fracture morphology of the Mo / Ni / Au electrode, which is an example of the present disclosure, was similar to that of the Ni / Mo / Ni / Au electrode. By removing the Ni layer, it is expected that the electrode can be made even thinner and the deposition time can be shortened, thereby improving productivity.
[0142] From the above, it was found that in the Ni / Au electrode used as a comparative example, the thin, outer periphery of the electrode, approximately 5 μm thick, melted and became an initial defect, leading to chip failure, but the Mo barrier layer prevented melting, improving impact resistance. After soldering, the electrode structure including the Mo barrier layer experienced ductile fracture, mainly at the β-Sn / solder interface.
[0143] [Summary] (1) A device according to a first aspect of the present disclosure includes a substrate having a first surface, an electrode located on the first surface of the substrate, and a joint located on the electrode, the joint including, in order from the electrode side, a first layer, a second layer, and a third layer, the first layer including Mo as a main component, the second layer including β-Sn as a main component, and the third layer including solder.
[0144] (2) In a device according to a second aspect of the present disclosure, in the above-described first aspect, the electrode includes a wiring layer that transmits signals and an adhesion layer that improves adhesion between the wiring layer and the first layer, and the adhesion layer is in contact with the first layer.
[0145] (3) A third aspect of the present disclosure provides the device according to the second aspect, wherein the adhesion layer includes at least one of a layer containing Ti as a main component and a layer containing Cr as a main component.
[0146] (4) A fourth aspect of the present disclosure is directed to a device according to any one of the above aspects 1 to 3, wherein the thickness of the second layer is 100 nm or more.
[0147] (5) A device according to a fifth aspect of the present disclosure is any one of the aspects 1 to 4 above, wherein the {111} plane of Mo contained in the first layer and the {110} plane of β-Sn contained in the second layer are approximately parallel to each other.
[0148] (6) A sixth aspect of the present disclosure is directed to a device according to any one of the first to fifth aspects, wherein the substrate includes a piezoelectric layer, and the electrode is provided on the piezoelectric layer and connected to an IDT electrode.
[0149] (7) An electric device according to a seventh aspect of the present disclosure includes the device according to any one of aspects 1 to 6 above.
[0150] (8) A substrate according to an eighth aspect of the present disclosure includes a base having a first surface, an electrode located on the first surface of the base, a barrier layer located on the electrode, and a bonding layer located on the barrier layer, wherein the barrier layer contains Mo as a main component, and the bonding layer contains at least one of Ni, Ag, Au, and Cu.
[0151] (9) A ninth aspect of the present disclosure provides a substrate according to the eighth aspect, wherein the bonding layer includes a layer made of a silver alloy containing Ag as a main component.
[0152] (10) A method for manufacturing a device according to a tenth aspect of the present disclosure includes the steps of preparing a substrate according to aspect 8 or 9 above, and placing solder on the bonding layer and heating it to form a bonding portion on the electrode, wherein the bonding portion includes, in order from the electrode side, a first layer, a second layer, and a third layer, the first layer containing Mo as a main component, the second layer containing β-Sn as a main component, and the third layer containing solder.
[0153] [Additional Notes] The invention according to the present disclosure has been described above based on the drawings and examples. However, the invention according to the present disclosure is not limited to the above-described embodiments. In other words, the invention according to the present disclosure can be modified in various ways within the scope of the present disclosure, and embodiments obtained by appropriately combining the technical means disclosed in different embodiments are also included in the technical scope of the invention according to the present disclosure. In other words, it should be noted that a person skilled in the art could easily make various modifications or corrections based on the present disclosure. It should also be noted that these modifications or corrections are included in the scope of the present disclosure.
[0154] DESCRIPTION OF SYMBOLS 110: Substrate 11: Base 21: Electrode 21A: Wiring layer 21B: Adhesion layer 31: Barrier layer 32: Bonding layer 120: Mounting substrate 12: Base 22: Electrode 200: Device 30: Bonding portion 301: First layer 302: Second layer 303: Third layer 300: Electronic module (electrical device) 210: Acoustic wave device (device) 130: Substrate 13: Base 13A: Piezoelectric layer (base) 13B: Support substrate (base) 23: Electrode layer 231: IDT electrode 232: Pad portion (electrode)
Claims
1. A device comprising: a base having a first surface; an electrode located on the first surface of the base; and a joint located on the electrode, the joint including, in order from the electrode side, a first layer, a second layer, and a third layer, the first layer including Mo as a main component, the second layer including β-Sn as a main component, and the third layer including solder.
2. The device according to claim 1, wherein the electrode includes a wiring layer for transmitting signals and an adhesion layer for improving adhesion between the wiring layer and the first layer, the adhesion layer being in contact with the first layer.
3. The device according to claim 2, wherein the adhesion layer includes at least one of a layer mainly composed of Ti and a layer mainly composed of Cr.
4. A device according to any one of claims 1 to 3, wherein the second layer has a thickness of 100 nm or more.
5. The device according to any one of claims 1 to 4, wherein the {111} plane of Mo contained in said first layer and the {110} plane of β-Sn contained in said second layer are approximately parallel to each other.
6. A device according to any one of claims 1 to 5, wherein the substrate comprises a piezoelectric layer, and the electrodes are provided on the piezoelectric layer and connected to IDT electrodes.
7. An electrical device comprising a device according to any one of claims 1 to 6.
8. A substrate comprising: a base having a first surface; an electrode located on the first surface of the base; a barrier layer located on the electrode; and a bonding layer located on the barrier layer, wherein the barrier layer contains Mo as a main component, and the bonding layer contains at least one of Ni, Ag, Au, and Cu.
9. The substrate according to claim 8, wherein the bonding layer includes a layer made of a silver alloy containing Ag as a main component.
10. A method for manufacturing a device, comprising: a step of preparing a substrate as described in claim 8 or 9; and a step of placing solder on the bonding layer and heating it to create a bonding portion on the electrode, wherein the bonding portion includes, from the electrode side, a first layer, a second layer, and a third layer, wherein the first layer includes Mo as a main component, the second layer includes β-Sn as a main component, and the third layer includes solder.
Citation Information
Patent Citations
Semiconductor device
JP1992180230A
Semiconductor light emitting device
JP2000332343A
Semiconductor device and its manufacturing method
JP2006108604A
Gallium nitride-based compound semiconductor and light emitting device
JP2007115941A
Elastic wave device, electronic component and method for manufacturing elastic wave device