Member for suppressing ice nucleation or suppressing icing
A member with a brush-like polymer chain aggregate and antifreeze water forming units on a cooling surface effectively suppresses ice nucleation and icing by maintaining a stable liquid layer, addressing the inefficiencies of existing methods and improving heat exchange efficiency.
Patent Information
- Application Number
- PCT/JP2024/017866
- Authority / Receiving Office
- WO · WO
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2023-05-24
- Filing Date
- 2024-05-14
- Publication Date
- 2024-11-28
AI Technical Summary
Existing methods for suppressing ice nucleation and icing on cooling surfaces in air conditioners and heat exchangers are inadequate, as they fail to effectively prevent the formation of frost and ice, leading to reduced heat exchange efficiency.
A member with a layer containing a brush-like polymer chain aggregate, where the polymer chain includes an antifreeze water forming unit and has a high proportion of antifreeze water, is used to suppress ice nucleation and icing. The polymer chain is bonded to a base material, forming a stable liquid layer that inhibits ice formation and allows water to remain in a supercooled or unfrozen state, even at low temperatures.
The solution effectively suppresses ice nucleation and icing by maintaining a stable liquid layer on the surface, preventing ice formation and allowing water to remain in a supercooled state, even at extremely low temperatures, thus enhancing heat exchange efficiency and preventing ice accumulation.
Smart Images

Figure JP2024017866_28112024_PF_FP_ABST
Abstract
Description
Ice nucleation suppression or anti-icing materials
[0001] The present invention relates to an ice nucleation or ice accretion suppression component.
[0002] In heat exchangers used in air conditioners and refrigerators, rapid cooling of air can cause water droplets to adhere to the surface of the cooling element in the heat exchanger, or frost to form, reducing the heat exchange efficiency. In particular, frost forms through the formation of ice on the surface of the cooling element or the formation and growth of ice nuclei. As a method for suppressing frost formation, a method of forming a resin film on the surface of the element is known, as described in Patent Document 1.
[0003] Japanese Patent Application Laid-Open No. 2019-158247
[0004] The method described in Patent Document 1 can control the shape of water droplets that adhere to the surface of a component and thereby delay the growth of frost, but it cannot sufficiently suppress ice nucleation or icing on the surface of the component, and further improvements were needed.
[0005] Therefore, an object of the present invention is to provide a member that can suppress ice nucleation and icing.
[0006] That is, the present invention is as follows: [1] A component for suppressing ice nucleation or icing, comprising a layer containing brush-like polymer chain assemblies composed of a plurality of polymer chains fixed to a substrate, the layer containing the polymer chain assemblies holding a liquid substance, at least a portion of the liquid substance being water, and the proportion of antifreeze water relative to the total mass of the water in the liquid substance being 15 mass% or more. [2] The component described in [1], wherein the polymer chains contain antifreeze-forming units composed of antifreeze-forming monomer units. [3] The component described in [1] or [2], wherein the ratio of the total molecular weight of antifreeze-forming structural moieties contained in the antifreeze-forming monomer units in the polymer chain to the molecular weight of the polymer chain (total molecular weight of antifreeze-forming structural moieties contained in the antifreeze-forming monomer units / molecular weight of the polymer chain) is 0.80 or more. [4] The component described in [1] or [2], wherein the substrate is a carrier made of a material different from the polymer chain assemblies, and the surface occupancy of the polymer chains on the substrate surface is 0.08 to 0.65. [5] The member according to [1] or [2], wherein the member has a bottle-brush structure in which the plurality of polymer chains are bonded as side chains to the base polymer chain, and the surface occupancy of the side chains is 0.08 to 0.65.
[0007] The member of the present invention has the above-described configuration, and therefore can suppress ice nucleation and icing.
[0008] FIG. 1 is a schematic diagram illustrating a test method for icing stress.
[0009] Hereinafter, an embodiment of the present invention (hereinafter referred to as "the present embodiment") will be described in detail. The present invention is not limited to the following description, and various modifications can be made within the scope of the present invention.
[0010] [Component] The component of this embodiment is a component for suppressing ice nucleation or icing, having a layer containing brush-like polymer chain assemblies composed of a plurality of polymer chains fixed to a substrate, the layer containing the polymer chain assemblies holding a liquid substance, at least a portion of which is water, and the proportion of antifreeze water relative to the total mass of the water in the liquid substance is 15 mass% or more. The component may consist only of the substrate and the layer containing the polymer chain assemblies, or may further contain other layers or materials. The layer containing the polymer chain assemblies may consist only of polymer chain assemblies and a liquid substance, or may further contain other substances. In this specification, a layer containing brush-like polymer chain assemblies may sometimes be referred to as a "layer containing polymer chain assemblies."
[0011] The member of this embodiment has excellent anti-icing and anti-ice nucleation effects. While the exact reasons for these effects are unclear, it is presumed that the following is the reason. In the member of this embodiment, the liquid substance is held by the polymer chain assemblies, forming a stable liquid layer that is less susceptible to irreversible liquid leakage within the layer containing the polymer chain assemblies. Furthermore, it is presumed that the mobility of the liquid substance held by the polymer chain assemblies is appropriately controlled by the polymer chain assemblies, making it more likely to create a supercooled or antifreeze state. Due to the presence of such a stable liquid layer, the member of this embodiment is presumed to have an interface with high mobility against ice, snow, frost, and the like. Furthermore, the presence of such a stable liquid layer allows thermal motion of water even below the freezing point without freezing, thereby further reducing the freezing temperature of water on the member surface. The present inventors further investigated the prevention of ice formation and surprisingly found that the proportion of non-freezing water that does not freeze even at temperatures below −90°C, which is significantly lower than the temperature at which icing occurs, is related to the prevention of ice nucleation and anti-icing. In the member of this embodiment, the liquid substance in the layer containing the polymer chain aggregate contains a large amount of antifreeze water, so water is less likely to freeze on the surface of the member even at low temperatures, and ice, snow, frost, etc. are less likely to form on the surface of the member, and further, because the member has an interface with high mobility for ice, snow, frost, etc., even if ice, snow, frost, etc. forms on the surface of the member, these particles slide off with excellent ease, and it is therefore presumed that the member has an extremely excellent anti-icing effect. Furthermore, the member of this embodiment can further lower the freezing temperature of water inside or on the surface of the member, thereby lowering the temperature at which ice nuclei form, and it is presumed that the member has an extremely excellent anti-icing effect.
[0012] The polymer chain assembly used in this embodiment refers to an assembly of multiple polymer chains that has a brush-like shape as a whole, and is completely different from an organic film formed by simply applying a polymer solution. In this specification, the term "brush-like" may refer to a structure in which multiple (e.g., two or more) polymer chains are present, at least one end of which is fixed to the surface of a substrate or a layer on the substrate, and which extend away from the substrate. When both ends of the polymer chain are fixed to the substrate, the structure may be U-shaped.
[0013] The retention of a liquid substance in the layer containing the polymer chain assembly can be confirmed by differential scanning calorimetry. Furthermore, if confirmation by differential scanning calorimetry is not possible, it can be confirmed by an indentation hardness test. Furthermore, the proportion of nonfreezing water in the layer containing the polymer chain assembly can be measured by the method described in the Examples below.
[0014] In the member of this embodiment, the liquid substance refers to a substance that is retained in the layer containing the polymer chain assembly and is liquid at room temperature. It is preferable that at least a portion of the liquid substance remains liquid even at temperatures below the freezing point (preferably −10°C or lower, more preferably −18°C or lower, even more preferably −20°C or lower, and particularly preferably −30°C or lower). Furthermore, the liquid substance is preferably water. From the viewpoint of excellent ice nucleation and icing suppression effects, the mass ratio of the substance confirmed to be in a liquid state at the above temperature to 100 parts by mass of polymer chains contained in the layer containing the polymer chain assembly at −18°C is preferably 50 parts by mass or more, more preferably 70 parts by mass or more, even more preferably 80 parts by mass or more, and particularly preferably 90 parts by mass or more. This ratio can be adjusted by, for example, combining the polymer chains with the liquid substance. Furthermore, this ratio can be measured using an atomic force microscope, ellipsometry, or the like. The member of the present embodiment preferably has a layer containing brush-like polymer chain assemblies composed of a plurality of polymer chains fixed to a substrate at −18° C., and the layer containing the polymer chain assemblies preferably holds a liquid substance.
[0015] The member of this embodiment contains antifreeze water in the layer containing the polymer chain assembly. Note that antifreeze water refers to water that is liquid at −90°C in the layer, and refers to water in the polymer (hydrated water) that does not freeze even at −90°C due to a strong interaction with the polymer. The amount of antifreeze water can be measured, for example, by the method described in the Examples below.
[0016] In the member of this embodiment, the thickness of the layer containing the polymer chain assembly is preferably 50 nm or more, more preferably 100 nm or more, even more preferably 350 nm or more, even more preferably 500 nm or more, and particularly preferably 1000 nm or more, because this makes it easier to obtain a better anti-icing effect and anti-ice nucleation effect. There is no particular upper limit, but it can be, for example, 100 μm or less, or even 50 μm or less. The thickness of the layer containing the polymer chain assembly can be measured by ellipsometry or the like. The film thickness may be a value measured at -18°C.
[0017] The components of this embodiment will be described in detail below.
[0018] [Polymer Chain Assembly] The polymer chain assembly in this embodiment is composed of multiple polymer chains and has a brush-like shape as a whole. In this specification, "polymer chain" refers to a molecule or a portion of a molecule having a structure in which multiple monomer units are linked in a chain. The multiple polymer chains that make up the polymer chain assembly may be the same or different from each other. Furthermore, the polymer chain may have a structure in which multiple identical or different monomer units are linked in a chain, and may be linear, have side chains, or have a branched structure. Crosslinked structures may be formed between the polymer chains or between the polymer chain and the substrate.
[0019] (Polymer Chain) The polymer chain may be a homopolymer obtained by polymerizing one type of monomer, or a copolymer obtained by polymerizing two or more types of monomers. Examples of the copolymer include random copolymers, block copolymers, gradient copolymers, and alternating copolymers. The monomer used to generate the polymer chain may be one type alone, or two or more types may be used in combination.
[0020] The polymer chain contains an antifreeze-forming unit. The polymer chain may consist solely of the antifreeze-forming unit, or may consist of the antifreeze-forming unit and units other than the antifreeze-forming unit (sometimes referred to as "other units"). The antifreeze-forming unit refers to a single monomer unit or a chain of multiple monomer units consisting solely of an antifreeze-forming monomer unit having an antifreeze-forming structural moiety, as described below. The mass ratio of the antifreeze-forming unit to 100 parts by mass of the polymer chain is preferably 40 to 100 parts by mass, more preferably 50 to 100 parts by mass, and even more preferably 80 to 100 parts by mass, from the viewpoint of being able to retain a large amount of antifreeze water in the layer containing the polymer chain assembly. The proportion of the antifreeze-forming unit in the polymer chain refers to the proportion of the antifreeze-forming monomer unit in the polymer chain. Furthermore, the other units refer to a chain of one or more monomer units consisting solely of monomer units other than the antifreeze-forming monomer unit.
[0021] The non-freezing water-forming structural moiety refers to a structural moiety within a monomer unit that has the property of being able to form and retain non-freezing water within the polymer chain, and examples thereof include functional groups capable of hydrogen bonding, and structures derived from (poly)alkylene glycol or alkoxy(poly)alkylene glycol. Note that the structure derived from (poly)alkylene glycol refers to all alkylene oxide units and terminal hydroxy groups, and the structure derived from alkoxy(poly)alkylene glycol refers to all alkylene oxide units and terminal alkoxy groups. The non-freezing water-forming monomer unit may have one or more non-freezing water-forming structural moieties.
[0022] Examples of the functional group capable of forming a hydrogen bond include a carboxy group, a group that can be converted into a salt of a carboxy group, a hydroxy group, a glycidyl group, a sulfonic acid group, a sulfonate salt, an amide group, a group containing quaternary ammonium, an imide group, a nitrile group, an alkoxy group, etc. The functional group capable of forming a hydrogen bond is preferably located at the end of the antifreeze-water-forming monomer.
[0023] Examples of monomers constituting the above-mentioned carboxyl group-containing antifreeze-forming monomer units include (meth)acrylic acid, maleic acid, fumaric acid, itaconic acid, and crotonic acid. Esters of the above-mentioned carboxyl group-containing monomers may also be used, such as monoalkyl esters of maleic acid and monoalkyl esters of fumaric acid. In this specification, the alkyl group may be an alkyl group having 1 to 10 carbon atoms (preferably 2 to 5 carbon atoms).
[0024] Examples of the monomer that constitutes the non-freezing water-forming monomer unit having a group that can be converted into a salt of a carboxy group include tert-butyl (meth)acrylate.
[0025] Examples of the monomer constituting the nonfreezing water-forming monomer unit having a hydroxy group include 2-hydroxyethyl (meth)acrylate, 2-hydroxypropyl (meth)acrylate, and hydroxy-substituted alkyl (meth)acrylates (for example, 2-hydroxyethyl (meth)acrylate, 2-hydroxypropyl (meth)acrylate, 2-hydroxypropyl (meth)acrylate, and 2,3-dihydroxypropyl (meth)acrylate).
[0026] Examples of the monomer that constitutes the glycidyl group-containing nonfreezing water-forming monomer unit include glycidyl (meth)acrylate.
[0027] Examples of the monomer that constitutes the sulfonic acid group-containing antifreeze-forming monomer unit include p-styrene chlorosulfonic acid and styrene sulfonic acid.
[0028] Examples of the monomer that constitutes the above-mentioned sulfonate-containing nonfreezing water-forming monomer unit include salts of the monomer that constitutes the above-mentioned sulfonic acid group-containing nonfreezing water-forming monomer unit, and anionic monomers such as 3-sulfopropyl potassium methacrylate.
[0029] Examples of the monomer that constitutes the non-freezing water-forming monomer unit having an amide group include acrylamide, methacrylamide, N-methylacrylamide, N,N-dimethylacrylamide, and N-methylmethacrylamide.
[0030] Examples of the monomer constituting the nonfreezing water-forming monomer unit having a group containing quaternary ammonium include ionic liquid type monomers, cationic type monomers such as N-vinylpyrrolidone, N,N-dimethylaminoethyl (meth)acrylate, and methacryloyloxyethyl trimethylammonium chloride. The ionic liquid type monomer is not particularly limited, but examples thereof include compounds represented by the following formula (1): In formula (1), m represents an integer of 1 to 10, and n represents an integer of 1 to 5. 1 represents a hydrogen atom or an alkyl group having 1 to 3 carbon atoms, R 2 , R 3 and R 4 each independently represents an alkyl group having 1 to 5 carbon atoms. 2 , R 3 and R 4 The alkyl group in R may have a carbon atom or a hydrogen atom substituted with one or more heteroatoms selected from oxygen atoms, sulfur atoms, and fluorine atoms. 2 , R 3 and R 4 Two or more of these may be linked to form a cyclic structure. Y represents a monovalent anion. Examples of the monovalent anion represented by Y include BF 4 - , P.F. 6 - , AsF 6 - , SbF 6 - , AlCl 4 -, NbF 6 - , HSO 4 - , ClO 4 - , C.H. 3 SO 3 - , C.F. 3 SO 3 - , C.F. 3 CO 2 - , (CF 3 SO 2 ) 2 N - , Cl - ,Br - , I - Considering the stability of the anion, BF 4 - , P.F. 6 - , (CF 3 SO 2 ) 2 N - , C.F. 3 SO 3 - , or CF 3 CO 2 - Of the compounds represented by formula (1), the ionic liquid type monomer is preferably a compound represented by any one of the following formulas (2) to (9). In formulas (2) to (9), m, n, R 1 , R 2 , Y is m, n, R in formula (1) 1 , R 2 , Y. Me represents a methyl group, and Et represents an ethyl group.
[0031] Examples of the monomer that constitutes the above-mentioned imide group-containing antifreeze-forming monomer unit include maleimide, methylmaleimide, ethylmaleimide, propylmaleimide, butylmaleimide, hexylmaleimide, octylmaleimide, dodecylmaleimide, stearylmaleimide, phenylmaleimide, and cyclohexylmaleimide.
[0032] Examples of the monomer that constitutes the nitrile group-containing antifreeze-forming monomer unit include acrylonitrile and methacrylonitrile.
[0033] Examples of the monomer that constitutes the alkoxy group-containing antifreeze-forming monomer unit include polyethoxyethyl (meth)acrylate and polyethoxypropyl (meth)acrylate.
[0034] Examples of the monomer that constitutes the alkylene glycol-containing antifreeze-forming monomer unit include nonionic monomers such as poly(alkylene glycol) mono(meth)acrylates (e.g., poly(ethylene glycol) monomethacrylate), alkoxypoly(alkylene glycol) (meth)acrylates (e.g., methoxypoly(ethylene glycol) methacrylate), phenoxypoly(alkylene glycol) (meth)acrylates (e.g., phenoxypoly(ethylene glycol) methacrylate), polyalkoxypoly(alkylene glycol) (meth)acrylate, 2-glucosyloxyethyl (meth)acrylate, and poly(ethylene glycol) monomethacrylate.
[0035] Examples of the monomer that constitutes the betaine-containing non-freezing water-forming monomer unit include (3-[(3-acrylamidopropyl)dimethylammonio]propane-1-sulfonic acid, etc.
[0036] Among these, as the antifreeze-forming monomer unit, from the viewpoint of being able to retain a larger amount of antifreeze water in the layer containing the polymer chain assembly, a monomer having an alkylene glycol is preferred, and polyalkoxypoly(alkylene glycol)(meth)acrylate is more preferred.
[0037] The monomer used to generate the polymer chain is preferably one that can bond the polymer chain obtained by its polymerization to the substrate as a graft chain. Examples of such monomers include monomers having at least one addition-polymerizable double bond, and monofunctional monomers having one addition-polymerizable double bond are preferred. Examples of monofunctional monomers having one addition-polymerizable double bond include (meth)acrylic acid-based monomers and styrene-based monomers. The monomer constituting the antifreeze-forming monomer unit is preferably a monofunctional monomer having an antifreeze-forming structural moiety and further having one addition-polymerizable double bond. Examples of monofunctional monomers having an antifreeze-forming structural moiety and further having one addition-polymerizable double bond include, for example, the monomers exemplified above as monomers having an antifreeze-forming structural moiety and also exemplified below as monofunctional monomers having one addition-polymerizable double bond.
[0038] Examples of (meth)acrylic acid-based monomers include (meth)acrylic acid, methyl (meth)acrylate, ethyl (meth)acrylate, propyl (meth)acrylate, isopropyl (meth)acrylate, butyl (meth)acrylate, isobutyl (meth)acrylate, tert-butyl (meth)acrylate, pentyl (meth)acrylate, hexyl (meth)acrylate, cyclohexyl (meth)acrylate, heptyl (meth)acrylate, octyl (meth)acrylate, 2-ethylhexyl (meth)acrylate, and nonyl (meth)acrylate. ) acrylate, decyl (meth)acrylate, dodecyl (meth)acrylate, tridecyl (meth)acrylate, phenyl (meth)acrylate, toluyl (meth)acrylate, benzyl (meth)acrylate, 2-methoxyethyl (meth)acrylate, 3-methoxypropyl (meth)acrylate, 3-methoxybutyl (meth)acrylate, 2-hydroxyethyl (meth)acrylate, 2-hydroxypropyl (meth)acrylate, stearyl (meth)acrylate, glycidyl (meth)acrylate, 3-ethyl-3-( Meth)acryloyloxymethyloxetane, 2-(meth)acryloyloxyethyl isocyanate, (meth)acrylate-2-aminoethyl, 2-(2-bromopropionyloxy)ethyl (meth)acrylate, 2-(2-bromoisobutyryloxy)ethyl (meth)acrylate, 1-(meth)acryloxy-2-phenyl-2-(2,2,6,6-tetramethyl-1-piperidinyloxy)ethane, 1-(4-((4-(meth)acryloxy)ethoxyethyl)phenylethoxy)piperidine, γ-(methacryloyloxypropyl) propyl)trimethoxysilane, 3-(3,5,7,9,11,13,15-heptaethylpentacyclo[9.5.1.13,9.15,15.17,13]octasiloxan-1-yl)propyl (meth)acrylate, 3-(3,5,7,9,11,13,15-heptaisobutyl-pentacyclo[9.5.1.13,9.15,15.17,13]octasiloxan-1-yl)propyl (meth)acrylate, 3-(3,5,7,9,11,13,15-heptaisooctylpentacyclo[9.5.1.13,9.15,15.17,13]octasiloxan-1-yl)propyl (meth)acrylate, 3-(3,5,7,9,11,13,15-heptacyclopentylpentacyclo[9.5.1.13,9.15,15.17,13]octasiloxan-1-yl)propyl (meth)acrylate, 3-(3,5,7,9,11,13,15-heptaphenylpentacyclo[9.5.1.13, 9.15,15.17,13]octasiloxan-1-yl)propyl (meth)acrylate, 3-[(3,5,7,9,11,13,15-heptaethylpentacyclo[9.5.1.13,9.15,15.17,13]octasiloxan-1-yloxy)dimethylsilyl]propyl (meth)acrylate, 3-[(3,5,7,9,11,13,15-heptaethylpentacyclo[9.5.1.13,9.15,15.17,13]octasiloxan-1-yloxy)dimethylsilyl]propyl (meth)acrylate 3-[(3,5,7,9,11,13,15-heptaisooctylpentacyclo[9.5.1.13,9.15,15.17,13]octasiloxan-1-yloxy)dimethylsilyl]propyl(meth)acrylate, 3-[(3,5,7,9,11,13,15-heptaisooctylpentacyclo[9.5.1.13,9.15,15.17,13]octasiloxan-1-yloxy)dimethylsilyl]propyl(meth)acrylate meth)acrylate, 3-[(3,5,7,9,11,13,15-heptacyclopentylpentacyclo[9.5.1.13,9.15,15.17,13]octasiloxan-1-yloxy)dimethylsilyl]propyl (meth)acrylate, 3-[(3,5,7,9,11,13,15-heptaphenylpentacyclo[9.5.1.13,9.15,15.17,13]octasiloxane-1-yloxy)dimethylsilyl]propyl (meth)acrylate, ethylene oxide adduct of (meth)acrylic acid, trifluoromethylmethyl (meth)acrylate, 2-trifluoromethylethyl (meth)acrylate, 2-perfluoroethylethyl (meth)acrylate, 2-perfluoroethyl-2-perfluorobutylethyl (meth)acrylate, 2-perfluoroethyl (meth)acrylate, trifluoromethyl (meth)acrylate, diperfluoromethylmethyl (meth)acrylate, 2-perfluoromethyl-2-perfluoroethylethyl (meth)acrylate, 2-perfluorohexylethyl (meth)acrylate, 2-perfluorodecylethyl (meth)acrylate, 2-perfluorohexadecylethyl (meth)acrylate, and the like.
[0039] Examples of styrene-based monomers include styrene, vinyltoluene, α-methylstyrene, p-chlorostyrene, p-chloromethylstyrene, m-chloromethylstyrene, o-aminostyrene, p-styrene chlorosulfonic acid, styrenesulfonic acid and its salts, vinylphenylmethyldithiocarbamate, 2-(2-bromopropionyloxy)styrene, 2-(2-bromoisobutyryloxy)styrene, 1-(2-((4-vinylphenyl)methoxy)-1-phenylethoxy)-2,2,6,6-tetramethylpiperidine, and 1-(4-vinylphenyl) -3,5,7,9,11,13,15-heptaethylpentacyclo[9.5.1.13,9.15,15.17,13]octasiloxane, 1-(4-vinylphenyl)-3,5,7,9,11,13,15-heptaisobutylpentacyclo[9.5.1.13,9.15,15.17,13]octasiloxane, 1-(4-vinylphenyl)-3,5,7,9,11,13,15-heptaisooctylpentacyclo[9.5.1.13,9.15,15.17,13]octasiloxane, 1-(4-vinylphenyl)-3,5,7,9,11,13,15-heptaisooctylpentacyclo[9.5.1.13,9.15,15.17,13]octasiloxane 5-heptacyclopentylpentacyclo[9.5.1.13,9.15,15.17,13]octasiloxane, 1-(4-vinylphenyl)-3,5,7,9,11,13,15-heptaphenylpentacyclo[9.5.1.13,9.15,15.17,13]octasiloxane, 3-(3,5,7,9,11,13,15-heptaethylpentacyclo[9.5.1.13,9.15,15.17,13]octasiloxane-1-yl)ethylstyrene, 3-(3,5,7,9,11,13,15-heptaisobutylpentacyclo[9.5.1.1 3,9.15,15.17,13]octasiloxan-1-yl)ethylstyrene, 3-(3,5,7,9,11,13,15-heptaisooctylpentacyclo[9.5.1.13,9.15,15.17,13]octasiloxan-1-yl)ethylstyrene, 3-(3,5,7,9,11,13,15-heptacyclopentylpentacyclo[9.5.1.13,9.15,15.17,13]octasiloxan-1-yl)ethylstyrene, 3-(3,5,7,9,11,13,15-heptaphenylpentacyclo[9.5.1.13,9.15,15.17,13]octasiloxan-1-yl)ethylstyrene, 3-((3,5,7,9,11,13,15-heptaethylpentacyclo[9.5.1.13,9.15,15.17,13]octasiloxan-1-yloxy)dimethylsilyl)ethylstyrene, 3-((3,5,7,9,11,13,15-heptaisobutylpentacyclo[9.5.1.13,9.15,15.17,13]octasiloxan-1-yloxy)dimethylsilyl)ethylstyrene, 3-((3,5,7,9,11,13,15-heptaisooctylpentacyclo [9.5.1.13,9.15,15.17,13]octasiloxan-1-yloxy)dimethylsilyl)ethylstyrene, 3-((3,5,7,9,11,13,15-heptacyclopentylpentacyclo[9.5.1.13,9.15,15.17,13]octasiloxan-1-yloxy)dimethylsilyl)ethylstyrene, 3-((3,5,7,9,11,13,15-heptaphenylpentacyclo[9.5.1.13,9.15,15.17,13]octasiloxan-1-yloxy)dimethylsilyl)ethylstyrene, and the like.
[0040] Furthermore, examples of monofunctional monomers having one addition-polymerizable double bond per molecule include fluorine-containing vinyl monomers (perfluoroethylene, perfluoropropylene, vinylidene fluoride, etc.), silicon-containing vinyl monomers (vinyltrimethoxysilane, vinyltriethoxysilane, etc.), maleic anhydride, maleic acid, monoalkyl esters and dialkyl esters of maleic acid, fumaric acid, monoalkyl esters and dialkyl esters of fumaric acid, maleimide monomers (maleimide, methylmaleimide, ethylmaleimide, propylmaleimide, butylmaleimide, hexylmaleimide, octylmaleimide, dodecylmaleimide, stearylmaleimide, phenylmaleimide, cyclohexylmaleimide, etc.), and nitrile group-containing monomers. Monomers (such as acrylonitrile and methacrylonitrile), amide group-containing monomers (such as acrylamide and methacrylamide), vinyl ester monomers (such as vinyl acetate, vinyl propionate, vinyl pivalate, vinyl benzoate, and vinyl cinnamate), olefins (such as ethylene and propylene), conjugated diene monomers (such as butadiene and isoprene), vinyl halides (such as vinyl chloride), vinylidene halides (such as vinylidene chloride), allyl halides (such as allyl chloride), allyl alcohol, vinylpyrrolidone, vinylpyridine, N-vinylcarbazole, methyl vinyl ketone, vinyl isocyanate, and macromonomers whose main chains are derived from styrene, (meth)acrylic acid esters, siloxanes, and the like can also be used.
[0041] The polymer chain may be a polymer obtained by reacting polymers having reactive groups with each other. Examples of reactive groups include hydroxyl groups and isocyanate groups. Examples of polymers having reactive groups include polymers of polyethylene glycol and dimethylsiloxane, and a specific example is Silaplane FM-0421 (reactive silicone) (manufactured by Shin-Etsu Chemical Co., Ltd.). From the viewpoint of particularly excellent ice nucleation and icing suppression effects, methoxypoly(ethylene glycol) methacrylate or a mixture of dodecyl methacrylate and tridecyl methacrylate is preferred, and from the viewpoint of suppressing snow accumulation outdoors, a mixture of dodecyl methacrylate and tridecyl methacrylate is particularly preferred.
[0042] The polymer chain is preferably a hydrophilic polymer chain having affinity for a liquid substance to be held in the layer containing the polymer chain assembly. For example, when water or a hydrophilic liquid substance is to be held in the layer containing the polymer chain assembly, the polymer chain constituting the polymer chain assembly is preferably a hydrophilic polymer chain. The hydrophilic polymer chain may be synthesized using a hydrophilic monomer, or may be synthesized by synthesizing a polymer using a hydrophobic monomer and then introducing a hydrophilic group into the polymer. In this specification, a polymer chain having high compatibility with water may be referred to as a "compatible polymer chain," and a polymer chain having low compatibility with water may be referred to as a "non-compatible polymer chain." Note that a polymer chain having high compatibility with water refers to a polymer chain having a swelling index of 1.5 or more (preferably 2.0 or more, more preferably 2.5 or more), as measured and calculated by a film thickness measurement method using an atomic force microscope. A polymer chain having low compatibility with water refers to a polymer chain having a swelling index of less than 1.5 (preferably 1.3 or less, more preferably 1.1 or less, even more preferably 1.08 or less, and particularly preferably 1.05 or less). The swelling degree is a value measured by the following method: The test specimen for which the layer thickness is to be measured is scratched with the tip of tweezers or the like, and the boundary between the exposed substrate and the layer is measured using an atomic force microscope colloid probe method (contact mode) to estimate the height of the step (i.e., the thickness of the layer in the dry state). Next, the same test specimen is immersed overnight in a corresponding liquid substance (e.g., water), and then the height of the step (i.e., the thickness of the swollen layer) is estimated at the same location in the liquid using an atomic force microscope colloid probe method (contact mode). The swelling degree is then calculated from the thickness of the swollen layer divided by the thickness of the dry layer.
[0043] It is preferable to use a hydrophilic monomer for generating the polymer chain. That is, it is preferable that the polymer chain contains a monomer unit derived from a hydrophilic monomer. The monomer constituting the antifreeze-forming monomer unit is preferably a monomer having an antifreeze-forming structural moiety and further having hydrophilicity. Examples of monomers having an antifreeze-forming structural moiety and further having hydrophilicity include the monomers exemplified above as monomers having an antifreeze-forming structural moiety and also exemplified as hydrophilic monomers described below.
[0044] Preferred hydrophilic monomers include hydroxy-substituted alkyl(meth)acrylates (e.g., 2-hydroxyethyl(meth)acrylate, 2-hydroxypropyl(meth)acrylate, 2-hydroxypropyl(meth)acrylate, 2,3-dihydroxypropyl(meth)acrylate, polyethoxyethyl(meth)acrylate, polyethoxypropyl(meth)acrylate, etc.), poly(alkylene glycol) mono(meth)acrylates (e.g., poly(ethylene glycol) monomethacrylate, etc.), alkoxypoly(alkylene glycol)(meth)acrylates (e.g., methoxypoly(ethylene glycol) methacrylate, etc.), and phenoxypoly(alkylene glycol)(meth)acrylates (e.g., phenoxypoly(ethylene glycol) methacrylate, etc.), with polyalkoxypoly(alkylene glycol)(meth)acrylates being more preferred. Furthermore, examples of hydrophilic monomers that can be used include (meth)acrylamide, N-alkyl(meth)acrylamides (for example, N-methylacrylamide, N,N-dimethylacrylamide, and N-methylmethacrylamide), 2-glucosyloxyethyl(meth)acrylate, acrylic acid, methacrylic acid, fumaric acid, maleic acid, itaconic acid, crotonic acid, methacrylamide, N-vinylpyrrolidone, N,N-dimethylaminoethyl(meth)acrylate, and quaternary ammonium salts thereof.
[0045] To generate hydrophilic polymer chains, it is also preferable to use hydrophilic monomers having a group in the side chain that can be easily converted into a carboxy group or a salt of a carboxy group. Hydrophilicity can be imparted by converting the group in the side chain of the generated polymer chain into a carboxy group or a salt of a carboxy group. Examples of monomers having a group in the side chain that can be easily converted into a carboxy group or a salt of a carboxy group include tert-butyl(meth)acrylate.
[0046] In the member of this embodiment, at least a portion of the liquid substance is water, and from the viewpoint of excellent ice nucleation and icing suppression effects, the polymer chain is preferably a compatible polymer chain. The compatible polymer chain preferably contains a structural unit derived from at least one compatible monomer selected from the group consisting of nonionic monomers such as poly(ethylene glycol) monomethacrylate; anionic monomers such as 3-sulfopropyl potassium methacrylate; cationic monomers such as methacryloyloxyethyl trimethylammonium chloride; and betaine monomers such as 3-[(3-acrylamidopropyl)dimethylammonio]propane-1-sulfonic acid. Among these, monomers containing (poly)alkylene glycol are preferred from the viewpoint of particularly excellent ice nucleation and icing suppression effects. The compatible monomers may be used alone or in combination. The compatible polymer chain refers to a polymer chain in which the mass ratio of the structural unit derived from the compatible monomer relative to 100 parts by mass of the polymer chain is greater than 50 parts by mass (preferably 70 parts by mass or more, more preferably 80 parts by mass or more, even more preferably 90 parts by mass or more, and particularly preferably 100 parts by mass). The mass ratio of the structural unit derived from the betaine monomer relative to 100 parts by mass of the polymer chain is preferably 70 parts by mass or more, more preferably 80 parts by mass or more, even more preferably 90 parts by mass or more, and particularly preferably 100 parts by mass. The compatible monomer refers to a monomer whose swelling index when made into a homopolymer is 1.1 or more, and the incompatible monomer refers to a monomer whose swelling index when made into a homopolymer is less than 1.1. Some of the monomers constituting the compatible polymer chain may be incompatible monomers. When the polymer chain contains a monomer having a (poly)alkylene glycol, the mass ratio of the antifreeze-forming unit to 100 parts by mass of the polymer chain is preferably 80 to 100 parts by mass, from the viewpoint of being able to retain a large amount of antifreeze water in the layer containing the polymer chain assembly.
[0047] In the member of this embodiment, a part of the liquid substance may be a substance that is incompatible with water, as long as the effect of the present invention is not impaired.
[0048] The polymer chain assembly may have crosslinked structures formed between the polymer chains or between the polymer chain and the substrate. This allows the elastic modulus of the polymer chain assembly to be controlled. The crosslinked structures formed between the polymer chains may be either physical or chemical. The crosslinked structures may be formed simultaneously with the polymerization reaction to generate the polymer chains, or may be formed after the polymer chains are generated. The formation of crosslinked structures simultaneously with the polymerization reaction to generate the polymer chains can be achieved by adding an appropriate amount of a bifunctional monomer, such as a divinyl monomer such as ethylene glycol dimethacrylate, to the polymerization reaction solution in addition to the monofunctional monomer used to generate the polymer chains. Furthermore, the formation of crosslinked structures between the generated polymer chains or between the polymer chain and the substrate can be achieved by introducing a crosslinking group into the polymer chain using a monomer having a crosslinking group, and then reacting the crosslinking group with a reactive group on another polymer chain or with a reactive group on the substrate. Examples of crosslinking groups include azide groups, halogen groups (preferably bromo groups), alkoxysilyl groups, isocyanate groups, vinyl groups, and thiol groups. Furthermore, when polymer chains are produced by living radical polymerization, reactive groups remaining at the ends of graft chains can also be used as crosslinking groups.
[0049] In the member of this embodiment, the polymer chains that make up the polymer chain assembly are fixed to a substrate. The substrate may be a carrier made of a substance different from the polymer chain assembly, or may be a linear or branched polymer chain that is the same as or different from the polymer chain contained in the polymer chain assembly. In this specification, the polymer chain that serves as the substrate may be referred to as a "trunk polymer." When the substrate is a carrier, the polymer chain assembly constitutes a "polymer brush." The carrier may be a large surface area (e.g., 100 mm2) such as a flat, spherical, or porous carrier. 2The substrate may be a substrate having a surface area of 100 μm or more. Furthermore, when the substrate is a trunk polymer, the trunk polymer as the main chain and the polymer chains (side chains) attached to the main chain together constitute a "bottle brush structure." When the substrate is a trunk polymer, the component of this embodiment includes the bottle brush structure attached to the above-mentioned support. Furthermore, when the polymer chains constituting the polymer chain assembly are fixed to a support made of a material different from the polymer chain assembly, for example, when the polymer chain assembly constitutes a "polymer brush," only a portion of the polymer chain (e.g., one end or the center of the polymer chain) may be fixed to the substrate (support), or both ends of the polymer chain may be fixed to the substrate (support). When both ends of the polymer chain are fixed to the substrate (support), the polymer chain forms a loop structure, and such a polymer chain assembly constitutes a polymer brush with a loop structure. The brush-like polymer forming a loop structure may be a bottle brush. Here, "fixing" refers to direct chemical bonding between a polymer chain and a compound constituting the substrate or an initiator group introduced onto the substrate surface, or between a layer formed on the substrate surface and a polymer. In particular, direct chemical bonding between a polymer chain and a compound constituting the substrate or an initiator group introduced onto the substrate surface is preferred from the viewpoint of excellent ice nucleation suppression and icing suppression at low temperatures. In this specification, "substrate" refers to a substance to which a polymer chain is fixed. Furthermore, "support" refers to a substance that can have a layer on its surface containing a brush-like polymer chain assembly composed of multiple polymer chains. For example, in the member having the above-mentioned polymer brush structure, the substrate may be one to which the polymer chain is fixed, and the support may also be one to which the polymer chain is fixed. In the member having the above-mentioned bottle-brush structure, the substrate may be a trunk polymer, and the support may be one to which the trunk polymer is adhered.
[0050] In the member of this embodiment, when the polymer chain assemblies constitute the polymer brush, the thickness of the polymer brush layer, i.e., the thickness of the layer containing the polymer chain assemblies, is preferably 10 nm or more, more preferably 50 nm or more, even more preferably 100 nm or more, even more preferably 300 nm or more, even more preferably 500 nm or more, and particularly preferably 1000 nm or more. There is no particular upper limit, but it can be, for example, 100 μm or less, or even 50 μm or less. When the polymer chain assemblies are formed by self-assembly, the layer thickness is preferably 1 nm or more, more preferably 5 nm or more, more preferably 10 nm or more, and even more preferably 100 nm or more. There is no particular upper limit, but it can be, for example, 1 μm or less, or even 10 μm or less. The formation of a polymer chain assembly by self-assembly means that individual polymer chains spontaneously form the polymer chain assembly.
[0051] Furthermore, in the member of this embodiment, when the polymer chain assembly has the bottle-brush structure, the thickness of the layer containing the polymer chain assembly is preferably 2 nm or more, more preferably 50 nm or more, even more preferably 100 nm or more, still more preferably 300 nm or more, even more preferably 500 nm or more, and particularly preferably 1000 nm or more. There is no particular upper limit, but it can be, for example, 100 μm or less, or 50 μm or less.
[0052] Hereinafter, methods for forming polymer chain assemblies will be described for each of the polymer brush and the member having a bottle-brush structure.
[0053] [A] Polymer Brush Polymer brush polymer chain assemblies can be obtained by, for example, graft polymerization, in which multiple polymer chains are bonded to a substrate, or a support, as graft chains. This graft polymerization can be performed by the grafting-from method or the grafting-to method, of which the grafting-from method is preferred. The grafting-from method involves introducing polymerization initiator groups into the substrate and growing graft chains from the polymerization initiator groups. The grafting-to method involves bonding pre-synthesized graft chains to reaction sites introduced into the substrate. Polymer chain assemblies can also be obtained by hydrophobically bonding the hydrophobic portion of a polymer (block copolymer) having hydrophobic and hydrophilic blocks to the surface of a hydrophobic substrate or a hydrophobized substrate. An example of a block copolymer is a copolymer having a polymethyl methacrylate (PMMA) structure as a hydrophobic block and a poly(sodium sulfonated glycidyl methacrylate) (PSGMA) structure as a hydrophilic block. Another polymer structure may be interposed between the PMMA structure and the PSGMA structure. For details of this method, see Nature, 425, 163-165 (2003), for example.
[0054] (Graft Polymerization Method) Hereinafter, a method for producing a polymer chain assembly by using graft polymerization method will be specifically described.
[0055] - Polymer Chain Production - The method for producing the polymer chains used in the graft polymerization method is not particularly limited, but radical polymerization is preferred, living radical polymerization (LRP) is more preferred, and atom transfer radical polymerization (ATRP) is even more preferred. Living radical polymerization has the advantage of being able to easily control the molecular weight and molecular weight distribution of the polymer chains and to produce various types of copolymers (e.g., random copolymers, block copolymers, compositionally gradient copolymers, etc.) as graft chains. Furthermore, living radical polymerization can be used under high pressure conditions or in an ionic liquid solvent to produce concentrated polymer brushes (described below) with precise control of their density and thickness. Here, when using living radical polymerization, the graft polymerization method may be either a grafting-from method or a grafting-to method, but the grafting-from method is preferred. For details of the graft polymerization method combining the living radical polymerization method and the grafting-from method, reference can be made to Japanese Patent Application Laid-Open No. 11-263819, etc. Furthermore, for details of the atom transfer radical polymerization method, reference can be made to J. Am. Chem. Soc., 117, 5614 (1995), Macromolecules, 28, 7901 (1995), Science, 272, 866 (1996), and Macromolecules, 31, 5934-5936 (1998). Furthermore, polymer chains can also be produced by nitroxide-mediated polymerization (NMP), reversible addition-fragmentation chain transfer (RAFT) polymerization, reversible transfer catalyzed polymerization (RTCP), reversible complexation-mediated polymerization (RCMP), etc.
[0056] The catalyst used in the radical polymerization method may be any catalyst capable of controlling radical polymerization, and is preferably a transition metal complex.Preferred examples of the transition metal complex include metal complexes having an element of Group 7, Group 8, Group 9, Group 10, or Group 11 of the periodic table as the central metal, and among these, copper complexes, ruthenium complexes, iron complexes, or nickel complexes are preferred, and copper complexes are more preferred.The copper complex preferably contains a complex of a monovalent copper compound and an organic ligand, and more preferably contains both a complex of a monovalent copper compound and an organic ligand and a complex of a divalent copper compound and an organic ligand.Examples of the monovalent copper compound include cuprous chloride, cuprous bromide, etc., and examples of the divalent copper compound include cupric chloride, cupric bromide, etc. Examples of the organic ligand include 2,2'-bipyridyl or a derivative thereof, 1,10-phenanthroline or a derivative thereof, polyamines (tetramethylethylenediamine, pentamethyldiethylenetriamine, hexamethyltris(2-aminoethyl)amine, etc.), and polycyclic alkaloids such as L-(-)-sparteine. When both a monovalent copper compound and a divalent copper compound are used, the proportion of non-freezing water in the layer containing the polymer chain aggregate can be further increased, and the molecular weight distribution index (Mw / Mn) can be well adjusted. Therefore, the molar ratio of the monovalent copper compound to the divalent copper compound is preferably 10 times or more, more preferably 20 times or more, and even more preferably 30 times or more. A divalent ruthenium chloride tristriphenylphosphine complex (RuCl 2 (PPh 3 ) 3 ) is also suitable as a catalyst. When a ruthenium compound is used as a catalyst, it is preferable to add an aluminum alkoxide as an activator. Bistriphenylphosphine complex of divalent iron (FeCl 2 (PPh 3 ) 2 ), bistriphenylphosphine complex of divalent nickel (NiCl 2 (PPh 3 ) 2 ), bistributylphosphine complex of divalent nickel (NiBr 2 (PBu 3 ) 2) are also suitable as catalysts. When a copper complex is added in radical polymerization, the copper complex may be formed in advance and then used in the radical polymerization, or the copper compound and the organic ligand may be added in a ratio that forms a copper complex and then radical polymerization may be carried out. The ratio of the copper compound and the organic ligand added in radical polymerization is preferably such that the number of moles of the organic ligand is 2 times or more, more preferably 2.1 times or more, and most preferably 2.2 times or more relative to the number of moles of the copper compound, so that the organic ligand is sufficiently coordinated to the copper compound and the copper complex is well dissolved.
[0057] The polymerization reaction is preferably carried out in a solvent. Examples of the solvent include hydrocarbon solvents (benzene, toluene, etc.), ether solvents (diethyl ether, tetrahydrofuran, diphenyl ether, anisole, dimethoxybenzene, etc.), halogenated hydrocarbon solvents (methylene chloride, chloroform, chlorobenzene, etc.), ketone solvents (acetone, methyl ethyl ketone, methyl isobutyl ketone, etc.), alcohol solvents (methanol, ethanol, propanol, isopropanol, butyl alcohol, t-butyl alcohol, etc.), nitrile solvents (acetonitrile, propionitrile, benzonitrile, etc.), ester solvents (ethyl acetate, butyl acetate, etc.), and carbonate solvents (ethylene carbonate, propylene carbonate, etc.). Examples of the solvent include amide solvents (N,N-dimethylformamide, N,N-dimethylacetamide, etc.), hydrochlorofluorocarbon solvents (1,1-dichloro-1-fluoroethane, dichloropentafluoropropane, etc.), hydrofluorocarbon solvents (hydrofluorocarbons having 2 to 5 carbon atoms, hydrofluorocarbons having 6 or more carbon atoms, etc.), perfluorocarbon solvents (perfluoropentane, perfluorohexane, etc.), alicyclic hydrofluorocarbon solvents (fluorocyclopentane, fluorocyclobutane, etc.), oxygen-containing fluorine-based solvents (fluoroethers, fluoropolyethers, fluoroketones, fluoroalcohols, etc.), water, etc. One of these solvents may be used alone, or two or more may be used in combination.
[0058] -Introduction of Polymerization Initiator Group- To produce a polymer chain assembly using, for example, a grafting-from method, a polymerization initiator group that serves as the initiation point for the polymerization reaction is introduced into a substrate, and polymer chains are grafted from this polymerization initiator group using the polymerization method described above. Examples of the polymerization initiator group include a halogenated alkyl group and a halogenated sulfonyl group. The polymerization initiator group is preferably physically or chemically bonded to the substrate surface, since this allows for accurate control of the density of the graft chains (graft density) and the primary structure (molecular weight, molecular weight distribution, monomer arrangement) of the polymer chains obtained by graft polymerization. Methods for introducing (bonding) a polymerization initiator group to the substrate surface include chemical adsorption and the Langmuir-Blodgett (LB) method. For example, chlorosulfonyl groups (polymerization initiator groups) can be introduced to the surface of a silicon wafer (substrate) by chemical bonding by reacting 2-(4-chlorosulfonylphenyl)ethyltrimethoxysilane or 2-(4-chlorosulfonylphenyl)ethyltrichlorosilane with the oxide layer on the silicon wafer surface.
[0059] To introduce polymerization initiator groups using the LB method, a film-forming material containing the polymerization initiator groups is dissolved in an appropriate solvent (e.g., chloroform, benzene, etc.). A small amount of this solution is then spread on a clean liquid surface, preferably pure water, and the solvent is evaporated or diffused into an adjacent aqueous phase to form a low-density film of film-forming molecules on the water surface. A partition plate is then mechanically swept across the water surface to reduce the surface area of the water surface on which the film-forming molecules are spread, thereby compressing the film and increasing its density, resulting in a dense monolayer on the water surface. Next, under appropriate conditions, while maintaining a constant surface density of the molecules constituting the monolayer on the water surface, the substrate on which the monolayer is to be deposited is immersed or withdrawn across the monolayer, transferring the monolayer onto the substrate and depositing the monolayer on the substrate. For details of the LB method, one can refer to "New Experimental Chemistry Lectures, Vol. 18 (Interfaces and Colloids), Chapter 6, by Fukuda Kiyonari et al., (1977), Maruzen," "LB Films and Electronics, edited by Fukuda Kiyonari, Sugi Michio, and Suzumebe Hiroyuki, (1986), CMC," or "Practical Techniques for Making Good LB Films, by Ishii Yoshio, (1989), Kyoritsu Shuppan."
[0060] When introducing a polymerization initiating group onto a substrate surface, it is preferable to treat the substrate surface with a surface treatment agent having at least one of a group that bonds to the substrate and a group that has affinity for the substrate, and at least one of a group that bonds to the polymerization initiating group and a group that has affinity for the polymerization initiating group. This surface treatment agent may be a low molecular weight compound or a high molecular weight compound. Examples of surface treatment agents include compounds represented by the following formula (10): In formula (10), n is an integer of 1 to 10, and preferably an integer of 3 to 8. 11 , R 12 and R 13 R each independently represents a substituent. 11 , R 12 and R 13 At least one of R is preferably an alkoxyl group or a halogen atom, 11 , R 12 and R 13 It is particularly preferred that all of R are methoxy groups or ethoxy groups. 14and R 15 R each independently represents a substituent. 14 and R 15 are preferably each independently an alkyl group having 1 to 3 carbon atoms or an aromatic functional group, and R 14 and R 15 Most preferably, both of X are methyl groups. 11 represents a halogen atom, preferably a bromine atom.
[0061] It is preferable to use a silane coupling agent containing a polymerization initiator group (polymerization initiator group-containing silane coupling agent) as the surface treatment agent. This allows surface treatment and introduction of the polymerization initiator group to be carried out simultaneously. Examples of the polymerization initiator group-containing silane coupling agent include compounds represented by the above formula (10). For a description of the polymerization initiator group-containing silane coupling agent and its production method, reference can be made to the description in International Publication No. 2006 / 087839. Specific examples of the polymerization initiator group-containing silane coupling agent include (2-bromo-2-methyl)propionyloxyhexyltrimethoxysilane (BHM) and (2-bromo-2-methyl)propionyloxypropyltrimethoxysilane (BPM).
[0062] From the viewpoint of adjusting the graft density, when a polymerization initiator group-containing silane coupling agent is used as a surface treatment agent, it is preferable to use a silane coupling agent that does not contain a polymerization initiator group, such as a known alkyl silane coupling agent. By adjusting the ratio of the polymerization initiator group-containing silane coupling agent to the silane coupling agent that does not contain a polymerization initiator group, the graft density can be freely changed. For example, when all of the silane coupling agents are polymerization initiator group-containing silane coupling agents, graft polymerization can be performed using the grafting-from method after the surface treatment, thereby growing polymer chains with a surface occupancy rate of more than 0.03. When a polymerization initiator group-containing silane coupling agent is used as a surface treatment agent, the polymerization initiator group-containing silane coupling agent may be hydrolyzed in the presence of water to form a silanol, which may then be partially condensed into an oligomer before being subjected to surface treatment. Specifically, this oligomer may be adsorbed onto a substrate, such as silica, via hydrogen bonding, and then dried to cause a dehydration condensation reaction, thereby introducing the polymerization initiator group into the substrate.
[0063] (Substrate) In a polymer brush-type polymer chain assembly, the material constituting the substrate (support) to which the polymer chains are fixed is not particularly limited. It can be appropriately selected from organic materials, inorganic materials, metal materials, etc. The substrate is preferably a support made of a material different from the polymer chain assembly.
[0064] The organic material is not particularly limited, and various resins and rubbers can be used without limitation. The resin may be either a thermosetting resin or a thermoplastic resin. Examples of thermosetting resins include epoxy resins, phenolic resins, amino resins, unsaturated polyester resins, polyurethane resins, urea resins, melamine resins, thermosetting polyimide resins, and diallyl phthalate resins. Examples of thermoplastic resins include polyolefin-based resins such as polyethylene, polypropylene, polystyrene, and polycycloolefin; vinyl-based resins such as polystyrene, acrylic resins, polyvinyl chloride resins, and polyvinyl alcohol; fluorine-based resins such as polytetrafluoroethylene; polyester-based resins such as polyethylene terephthalate, polybutylene terephthalate, polytrimethylene terephthalate, and polyethylene naphthalate; and silicone resins such as polydimethylsiloxane. Examples of rubber include diene-based rubbers such as butadiene rubber, styrene-butadiene rubber, chloroprene rubber, isoprene rubber, natural rubber, nitrile rubber, and butyl rubber; and rubbers other than diene-based rubbers such as ethylene propylene rubber, acrylic rubber, polyether rubber, polyurethane rubber, fluororubber, and silicone rubber.
[0065] The substrate may be a polymer monolith. Here, the polymer monolith refers to a polymeric porous body having a three-dimensional co-continuous structure formed by three-dimensionally interconnected pores and a polymer skeleton. The polymer skeleton of the polymer monolith is preferably a polymer of a polymerizable compound and a crosslinking agent.
[0066] The polymerizable compound may be any compound capable of forming a polymer skeleton by polymerization with a crosslinking agent, and examples thereof include epoxy compounds, (meth)acrylate compounds, and styrene compounds. Of these, epoxy compounds are preferred because they are highly flexible and can easily form a polymer monolith with a fine porous structure. Examples of the epoxy compounds include bisphenol A epoxy resins, brominated bisphenol A epoxy resins, bisphenol F epoxy resins, bisphenol AD epoxy resins, stilbene epoxy resins, biphenyl epoxy resins, bisphenol A novolac epoxy resins, cresol novolac epoxy resins, diaminodiphenylmethane epoxy resins, polyphenyl-based epoxy resins such as tetrakis(hydroxyphenyl)ethane-based epoxy resins, fluorene-containing epoxy resins, and 2,2,2-tri-(2,3-epoxypropyl)-isocyanate. Examples of such epoxy compounds include epoxy resins containing heteroaromatic rings, such as triglycidyl isocyanurate and triazine ring-containing epoxy resins; aromatic epoxy compounds containing carbon atoms derived from aromatic rings, such as N,N,N',N'-tetraglycidyl-m-xylylenediamine; and aliphatic epoxy compounds not containing carbon atoms derived from aromatic rings, such as aliphatic glycidyl ether epoxy resins, aliphatic glycidyl ester epoxy resins, alicyclic glycidyl ether epoxy resins, alicyclic glycidyl ester epoxy resins, and 1,3-bis(N,N'-diglycidylaminomethyl)cyclohexane. Among these, bifunctional or higher functional epoxy compounds are preferred, and compounds having two or more glycidyl groups in the molecule are more preferred. A preferred example is 1,3-bis(N,N'-diglycidylaminomethyl)cyclohexane.
[0067] Examples of the crosslinking agent include amine compounds, acid anhydrides, phenol compounds, hydrazide compounds, etc. Examples of the amine compound include aromatic amine compounds such as m-phenylenediamine, p-phenylenediamine, o-phenylenediamine, 4,4'-diaminodiphenylsulfone, 4,4'-methylene-bis(2-chloroaniline), benzyldimethylamine, and dimethylaminomethylbenzene; aromatic amine compounds having a heteroaromatic ring such as a triazine ring; ethylenediamine, diethylenetriamine, triethylenetetramine, tetraethylenepentamine, iminobispropylamine, bis(hexamethylene)triamine, 1,3,6-trisaminomethylhexane, and polyamines. Examples of suitable amine compounds include alicyclic amine compounds such as t-butyl methyl methyl diamine, trimethylhexamethylene diamine, polyether diamine, isophorone diamine, menthane diamine, N-aminoethylpiperazine, 3,9-bis(3-aminopropyl)2,4,8,10-tetraoxaspiro(5,5)undecane adduct, bis(4-aminocyclohexyl)methane, and modified products thereof; aliphatic polyamine hydrazide compounds such as 1,6-hexamethylenebis(N,N-dimethylsemicarbazide); and aliphatic polyamidoamines and polyaminoamides formed from polyamines and dimer acids. Examples of suitable acid anhydrides include aromatic acid anhydrides such as phthalic anhydride, trimellitic anhydride, and pyromellitic anhydride. Examples of suitable phenolic compounds include novolac phenolic resins. Examples of the hydrazide compound include aromatic hydrazide compounds such as isophthalic acid dihydrazide; and aliphatic hydrazide compounds such as adipic acid dihydrazide, sebacic acid dihydrazide, and dodecanedioic acid dihydrazide.
[0068] It is preferable to select a crosslinking agent appropriately depending on the type of polymerizable compound. When an epoxy compound is used as the polymerizable compound, the crosslinking agent is preferably an amine compound, and more preferably a bifunctional or higher functional amine compound having two or more amino groups in the molecule. The bifunctional or higher functional amine compound is preferably an alicyclic amine compound. A preferred specific example is bis(4-aminocyclohexyl)methane.
[0069] The polymer backbone of the polymer monolith is preferably a polymer of a difunctional or higher epoxy compound and a difunctional or higher amine compound, and more preferably a polymer of a difunctional or higher aliphatic epoxy compound and a difunctional or higher alicyclic amine compound, in view of the ease of forming the polymer monolith.
[0070] The blending ratio of the polymerizable compound and the crosslinking agent may be determined in consideration of the crosslinking density, etc. For example, when the polymerizable compound is a bifunctional or higher epoxy compound and the crosslinking agent is a bifunctional or higher amine compound, it is preferable to adjust the amine equivalent of the crosslinking agent to be in the range of 0.6 to 1.5 per equivalent of the epoxy group of the polymerizable compound.
[0071] The polymer monolith can be formed, for example, from a polymer monolith-forming composition containing a polymerizable compound, a crosslinker, and a pore-forming agent. More specifically, the polymer monolith-forming composition is applied to a substrate as a carrier to form a coating film, and the coating film is cured. Polymerization of the polymerizable compound increases the polymer component, causing spinodal decomposition and the development of a co-continuous structure. The pore-forming agent is then removed from the cured film to form the polymer monolith.
[0072] The surface on which the polymer monolith is to be formed may be treated with a known coupling agent such as a silane coupling agent, or may be subjected to plasma treatment in order to improve affinity with the polymer monolith-forming composition.
[0073] The inorganic material is not particularly limited, and examples thereof include ceramics (e.g., alumina ceramics, bioceramics, composite ceramics such as zirconia-alumina composite ceramics, etc.), metals (e.g., iron, cast iron, steel, stainless steel, carbon steel, iron alloys such as high carbon chromium bearing steel (SUJ2), non-ferrous metals and non-ferrous alloys such as aluminum, zinc, copper, and titanium, etc.), silicon such as polycrystalline silicon, silicon oxide, silicon nitride, various types of glass, quartz, and composite materials thereof.
[0074] The type of substrate is not particularly limited. Examples include tubes, sheets, fibers, strips, films, plates, foils, membranes, pellets, powders, particles, molded products (e.g., extrusion molded products, cast molded products, etc.), etc. Furthermore, the article to which the member of this embodiment is applied may itself be used as the substrate.
[0075] (Other Manufacturing Methods) Polymer brush polymer chain assemblies can also be produced by the following manufacturing method. That is, they can be produced by a manufacturing method comprising the steps of: mixing, in a solvent, an organic material constituting a substrate (hereinafter also referred to as substrate polymer) with a plurality of block copolymers comprising polymer block A and polymer block B having a lower affinity for the substrate polymer than polymer block A, and having polymer block A at at least two locations, to prepare a mixed solution; and removing the solvent from the mixed solution to cause phase separation. This manufacturing method makes it possible to produce polymer chain assemblies of polymer brushes with a loop structure, in which both ends of the polymer chains constituting the polymer chain assembly are each fixed to a substrate, which is a carrier.
[0076] The organic material constituting the base material, which is a base polymer, is not particularly limited, and examples thereof include those mentioned above.
[0077] The block copolymer is not particularly limited as long as it comprises a polymer block A and a polymer block B that has a lower affinity for the base polymer than the polymer block A, and has the polymer block A at at least two locations. However, from the viewpoint of favorable formation of a loop structure, it is preferable to use a polymer block B that is incompatible with the base polymer, and a combination in which the polymer block B is incompatible with the base polymer and the polymer block A is compatible with the base polymer is more preferable.
[0078] Here, the term "compatible" of the polymer block A with the base polymer refers to the following state: That is, when a polymer consisting only of the polymer block A is mixed with the base polymer by hot melt mixing, co-solution mixing, or the like, and the resulting mixture is solidified by cooling or solvent evaporation, or the like, and the glass transition temperature (Tg) of the obtained sample is measured, it is determined that the polymer is compatible if a Tg different from the Tg of the polymer consisting only of the polymer block A and the Tg of the base polymer is observed in a temperature range between these two. On the other hand, the term "incompatible" of the polymer block B with the base polymer refers to the following state: That is, when a polymer consisting only of the polymer block B is mixed with the base polymer by hot melt mixing, co-solution mixing, or the like, and the resulting mixture is solidified by cooling or solvent evaporation, or the like, and the glass transition temperature (Tg) of the obtained sample is measured, it is determined that the polymer is incompatible if no Tg different from the Tg of the polymer consisting only of the polymer block B and the Tg of the base polymer is observed.
[0079] The polymer block A and the polymer block B may be those having the above-mentioned compatibility with the base polymer. From the viewpoint of favorably forming a loop structure, the difference in SP value (solubility parameter) between the polymer block A and the polymer block B is 1.5 (MPa). 0.5 It is preferable that the pressure is 3 (MPa) or more. 0.5 More preferably, it is 5 (MPa) or more. 0.5Furthermore, with regard to the SP value of the polymer block A, it is more preferable that the difference between the SP value of the polymer block A and the SP value of the base polymer is 0.5 (MPa) or more. 0.5 It is preferable that the pressure is 0.3 (MPa) or less. 0.5 More preferably, it is 0.2 (MPa) or less. 0.5 With respect to the SP value of the polymer block B, it is more preferable that the difference between the SP value of the polymer block B and the SP value of the base polymer is 1.5 (MPa) or less. 0.5 It is preferable that the pressure is 3 (MPa) or more. 0.5 More preferably, it is 5 (MPa) or more. 0.5 The SP values of polymer block A and polymer block B may be, for example, values disclosed in Polymer Handbook (4th edition, Wiley-Interscience).
[0080] The polymer block A is not particularly limited as long as it satisfies the above-mentioned properties and may be selected in relation to the base polymer to be used. Specific examples include polymer blocks composed of polymer segments that constitute the resins or rubbers exemplified above as the resins or rubbers that constitute the base polymer.
[0081] The molecular weight (weight average molecular weight (Mw)) of the polymer block A portion of the block copolymer is not particularly limited, but from the viewpoint of exhibiting sufficient interaction with the base polymer and thereby more appropriately supporting the loop structure formed by the polymer block B, thereby further enhancing durability, the molecular weight is preferably 1,000 to 100,000, more preferably 1,000 to 50,000, even more preferably 1,000 to 20,000, still more preferably 2,000 to 20,000, and particularly preferably 2,000 to 6,000.
[0082] As the polymer block B, of the polymer chains described above, those which satisfy the above-mentioned properties with respect to the base polymer are preferably used.
[0083] The solvent used when mixing the base polymer and the plurality of block copolymer chains in a solvent is not particularly limited, and any solvent that can dissolve or disperse the base polymer and the block copolymer chains may be used. alicyclic hydrocarbons such as cyclopentane, cyclohexane, methylcyclohexane, dimethylcyclohexane, trimethylcyclohexane, ethylcyclohexane, diethylcyclohexane, decahydronaphthalene, bicycloheptane, tricyclodecane, hexahydroindene, and cyclooctane; aromatic hydrocarbons such as benzene, toluene, xylene, and mesitylene; nitrogen-containing hydrocarbons such as nitromethane, nitrobenzene, acetonitrile, propionitrile, and benzonitrile; ethers such as diethyl ether, tetrahydrofuran, and dioxane; ketones such as acetone, ethyl methyl ketone, methyl isobutyl ketone, cyclopentanone, and cyclohexanone; esters such as methyl acetate, ethyl acetate, ethyl propionate, and methyl benzoate; halogenated hydrocarbons such as chloroform, dichloromethane, 1,2-dichloroethane, chlorobenzene, dichlorobenzene, and trichlorobenzene; and alcohols such as methanol and ethanol.
[0084] A mixture can be obtained by mixing a base polymer and multiple block copolymer chains in such a solvent and dissolving or dispersing them. The resulting mixture is then used to form a film by a casting method, spin coating method, or the like, and the solvent is then removed from the resulting mixture. By removing the solvent, some of the multiple block copolymer chains dispersed in the base polymer undergo phase separation from the base polymer, with the polymer block A remaining in a compatible state with the base polymer, while the polymer block B constituting the block copolymer chain undergoes phase separation from the base polymer, resulting in a state in which the polymer block A is present in the base polymer and the polymer block B is exposed from the base polymer. This allows the formation of a loop structure in which both ends of the polymer chains constituting the polymer chain assembly are each fixed to a support.
[0085] The method for removing the solvent is not particularly limited and may be selected depending on the type of solvent used, but a method of heating at 50 to 100°C is preferred, and a method of heating at 70 to 80°C is more preferred.
[0086] Furthermore, polymer brush polymer chain assemblies can also be produced by the following production method: That is, they can be produced by a production method comprising the steps of: mixing, under heating, a base polymer with a plurality of block copolymers, each block copolymer comprising a polymer block A and a polymer block B having a lower affinity for the base polymer than the polymer block A, and each block copolymer having the polymer block A at at least two locations, to prepare a molten mixture; and cooling the molten mixture to cause phase separation. This production method also makes it possible to produce polymer chain assemblies of polymer brushes with a loop structure, in which both ends of the polymer chains that make up the polymer chain assembly are fixed to a substrate, which is a carrier.
[0087] The heating temperature when the base polymer and the plurality of block copolymers are mixed under heating to prepare a molten mixture is not particularly limited and may be a temperature at which the base polymer or the block copolymers melt, preferably a temperature at which both the base polymer and the block copolymer chains melt, and is preferably 40 to 300°C, more preferably 80 to 200°C.
[0088] The resulting molten mixture is used to form a film by casting, spin coating, dip coating, or the like, and then cooled to cause phase separation during the solidification process. As a result of the melt-mixing, some of the block copolymers dispersed in the base polymer change from a molten state to a solid state, and while polymer block A remains in a compatible state with the base polymer, polymer block B constituting the block copolymer undergoes phase separation from the base polymer, resulting in a change in the state where polymer block A is present in the base polymer and polymer block B is exposed from the base polymer, thereby forming a loop structure.
[0089] The method for cooling the molten mixture is not particularly limited, but examples include a method in which the molten mixture formed into a film is allowed to stand at room temperature, or a method in which the molten mixture is heated to a temperature lower than the melting temperature of each component constituting the molten mixture and then allowed to stand.
[0090] (Number-Average Molecular Weight and Molecular Weight Distribution Index of Polymer Chains) The number-average molecular weight (Mn) of the polymer chains constituting the polymer chain assembly is preferably 500 to 10,000,000, more preferably 100,000 to 10,000,000. The molecular weight distribution index (Mw / Mn) of the polymer chain assembly is preferably 1.0 to 2.0, more preferably 1.0 to 1.5, from the viewpoint of retaining a larger amount of antifreeze water in the layer containing the polymer chain assembly. When the molecular weight distribution index (Mw / Mn) is within the above range, it is expected that the polymer chains constituting the polymer chain assembly can maintain a high density state up to the outermost surface. The molecular weight distribution index (Mw / Mn) can be adjusted, for example, by the ratio of the monovalent copper compound to the divalent copper compound in the copper catalyst used in the radical polymerization to form the polymer chain assembly, the number of moles of the organic ligand relative to the copper compound, or the like. The number average molecular weight (Mn) and molecular weight distribution index (Mw / Mn) of a polymer chain assembly can be measured by cutting out polymer chains from a substrate by hydrofluoric acid treatment and performing molecular weight analysis of the cut polymer chains using size exclusion chromatography such as gel permeation chromatography. Furthermore, when a polymer chain assembly is formed using graft polymerization, it is assumed that the free polymer produced during the polymer chain polymerization reaction has the same molecular weight as the polymer chain fixed to the substrate. The number average molecular weight (Mn) and molecular weight distribution index (Mw / Mn) of the free polymer can be measured using size exclusion chromatography, and these values can be used directly as the number average molecular weight (Mn) and molecular weight distribution index (Mw / Mn) of the polymer chain. It has been confirmed that the number average molecular weight (Mn) and molecular weight distribution index (Mw / Mn) are approximately equal between the polymer chain fixed to the substrate and the free polymer produced during the polymerization reaction.
[0091] A method for measuring molecular weight using a free polymer will be specifically described. When polymer chains are synthesized by surface-initiated living radical polymerization, adding a free initiator to the polymerization solution can produce a free polymer having a molecular weight and molecular weight distribution equivalent to that of the polymer chains constituting the polymer chain assembly. The free polymer is analyzed by size exclusion chromatography to determine the number average molecular weight (Mn) and molecular weight distribution index (Mw / Mn).
[0092] The analysis by size exclusion chromatography involves calibration using available, homogeneous, monodisperse standard samples with known molecular weights, and absolute molecular weight evaluation using a multi-angle light scattering detector. In the examples herein, the number-average molecular weight (Mn) and weight-average molecular weight (Mw) values are shown as absolute values appropriately calculated using a multi-angle light scattering detector and molecular weight calibration curves of various standard samples. Examples of standard samples include polystyrene standard samples, polymethyl methacrylate standard samples, and polyethylene glycol standard samples.
[0093] The density of polymer chains on the substrate surface is 0.01 chains / nm 2 It is preferable that the number of chains is 0.05 chains / nm or more. 2 More preferably, it is 0.1 chains / nm or more. 2 More preferably, it is 0.2 chains / nm or more. 2 The upper limit is not particularly limited, but is preferably 1.0 chain / nm. 2 and can be less than or equal to 0.9 chains / nm 2 It can also be the following:
[0094] The density of the polymer chains can be calculated by measuring the graft amount (W) per unit area and the number average molecular weight (Mn) of the polymer chain aggregate, using the following formula: 2 ) = W (g / nm 2) / Mn×(Avogadro's number) In the formula, W represents the graft amount per unit area, and Mn represents the number average molecular weight of the polymer chain assembly. When the substrate is a flat substrate such as a silicon wafer, the graft amount per unit area (W) can be determined by measuring the total thickness in a dry state by ellipsometry, i.e., the thickness of the polymer chain assembly layer in a dry state, and calculating the graft amount per unit area (W) using the density of the bulk film. The number average molecular weight (Mn) of the polymer chain assembly can be measured by the method described above.
[0095] The surface occupancy of the polymer chains on the substrate surface (cross-sectional area of the polymer × density of the polymer chains) is preferably 0.01 or more, more preferably 0.05 or more, and even more preferably 0.10 or more. The surface occupancy refers to the proportion of the substrate surface occupied by grafting points (first structural units), and is 1 in closest packing. The density of the polymer chains can be calculated using the method described above. The cross-sectional area of the polymer can be determined using the repeating unit length in the extended form of the polymer and the bulk density of the polymer. When the polymer is a copolymer, it can be determined as a number average value depending on the ratio of the constituent monomers. The surface occupancy of the polymer chains on the substrate surface is preferably 0.08 to 0.65, more preferably 0.10 to 0.40, and even more preferably 0.15 to 0.25 from the viewpoint of suppressing snow accumulation outdoors.
[0096] When the member of this embodiment has a polymer brush structure, from the viewpoint of obtaining an excellent ice formation suppression effect over a wide temperature range of 0°C to -18°C, it is preferable that the substrate is a carrier made of a substance other than the polymer chain assembly, and that the surface occupancy of the polymer chains on the substrate surface is 0.08 to 0.65 (preferably 0.10 to 0.40, more preferably 0.15 to 0.40). In particular, when the member has a polymer brush structure, if the surface occupancy is within the above range, the brush density falls within an appropriate range, improving the retention of liquid substances (especially for liquid substances that are not phase with water, the retention is greatly improved), and further improving the suppression of ice nucleation due to the size exclusion effect.
[0097] [B] Member Having Bottle Brush Structure Next, a member having a bottle brush structure will be described. A bottle brush structure refers to a branched polymer structure in which multiple side chains branch off from a main chain, forming a bottle brush-like shape as a whole. In a bottle brush structure, the main chain constitutes the base material, and the side chains constitute a polymer chain assembly. Furthermore, the bottle brush structure may be adhered to a support to form a member having a bottle brush structure. Examples of the support include those described above. In this case, both the bottle brush and the polymer brush may be fixed or adhered to the support. In this case, the polymer brush is preferably a dense polymer brush. The member of this embodiment is preferably a member having a bottle brush structure in which the multiple polymer chains are attached as side chains to the base polymer chain.
[0098] Members having a bottle brush structure can also be obtained by graft polymerization. This graft polymerization can be carried out using a grafting-to method in which a pre-synthesized reactive side chain (graft chain) is bonded to a trunk polymer that serves as the main chain, a grafting-from method in which a side chain (graft chain) grows from the polymerization initiation group of a macroinitiator (a trunk polymer into which a polymerization initiation group has been introduced), or a grafting-through method in which a macromonomer (a polymer having a polymerizable functional group at the end of a side chain constituent polymer) is polymerized. In addition, living anionic polymerization, ring-opening metathesis polymerization (ROMP), or the highly versatile living radical polymerization method (LRP) can be used to synthesize these side chains and trunk polymers. A preferred example of a member having a bottle brush structure can be a compound represented by formula (11). In formula (11), R 1 and R 2 each independently represents a hydrogen atom or a methyl group, R 3 represents a substituent, and is preferably an alkyl group having 1 to 10 carbon atoms. 4 and R 5represents an end group consisting of an atom or atomic group, and examples thereof include a hydrogen atom, a halogen, and a functional group derived from a polymerization initiator. X represents O or NH, Y represents a divalent organic group, n represents an integer of 10 or more, and Polymer A represents a polymer chain. In the compound represented by formula (11), the repeating structure of the structural units bounded by n corresponds to the main chain of the bottle brush structure, and Polymer A corresponds to the side chain of the bottle brush structure.
[0099] Examples of the organic group represented by Y include an alkylene group having 1 to 10 carbon atoms, an oxyalkylene group (RO) having 1 to 5 carbon atoms (R represents an alkylene group having 1 to 5 carbon atoms), a linked structure in which multiple oxyalkylene groups are linked, and a divalent organic group formed by combining at least two of these organic groups (alkylene groups having 1 to 10 carbon atoms, oxyalkylene groups having 1 to 5 carbon atoms, and linked structures of oxyalkylene groups). Here, the alkylene group and the alkylene group of the oxyalkylene group may be linear or branched, or may have a cyclic structure. Specific examples of the alkylene group include an ethylene group, a propylene group, a butylene group, and a cyclohexylene group. The alkylene group and the alkylene group of the oxyalkylene group may be substituted with a substituent. Examples of the substituent include an alkyl group having 1 to 10 carbon atoms, an aryl group having 6 to 40 carbon atoms, and a heteroaryl group having 3 to 40 carbon atoms, and these substituents may be further substituted with a substituent. For an explanation of Polymer A, a preferred range, and specific examples, please refer to the polymer chain described above. Polymer A may be the same or different from each other in the structural units of the main chain.
[0100] For a component having a bottle-brush structure, when the main chain is the central axis, the side chains (graft chains) are linearly extended from the central axis, and a surface (virtual periphery) including the tips of the side chains is imagined, the outer shape of the component can be considered as a cylinder with the surface including the tips as the side. In a component having such an outer shape, the longer the side chains (graft chains), the lower the density of the side chains (graft chains) on the side, and the greater the structural freedom of the side chains (graft chains). As a result, the side chains (graft chains) can be freely folded.
[0101] In the bottle-brush structure, the surface occupancy of the side chains (σ * ) can be calculated by the following formula: In the above formula, DP n,graft is the number-average degree of polymerization of the graft chains, x is the number of graft chains per unit length of the backbone polymer (number / nm), r is the radius of the backbone polymer (nm) (for example, 0.8 nm for PBIEM), a 2 is the cross-sectional area of the monomer (nm 2 ) (e.g., 3.3 nm for PEGMA) 2 ), l is the total length of the repeating unit of the polymer chain (nm) (e.g., 0.25 for polymethacrylate), and 2π(DP n,graft l + r) is the circumference (nm) of the cross section of the bottle brush, and l / x is the distance (nm) between adjacent graft chains. For the above method, see Biomacromolecules, 2021, 22, 2505-14. The surface occupancy of the side chains indicates a value between 0 and 1, and the larger the value, the greater the proportion of the side chain tips on the polymer side, limiting the degree of freedom of the side chains. In other words, the surface occupancy of the side chains is a value that reflects the degree of freedom of the side chains, and the surface occupancy of the side chains (σ * The higher the σ is, the more restricted the structural freedom of the side chains. As a result, the side chains can maintain a state of extending in a direction approximately perpendicular to the main chain, which is thought to result in the properties specific to that structure.
[0102] The surface occupancy of the side chains of the member having a bottle-brush structure is preferably 0.01 or more, more preferably 0.05 or more, and even more preferably 0.10 or more. The surface occupancy of the side chains is preferably 0.08 to 0.65, more preferably 0.10 to 0.50, and even more preferably 0.20 to 0.40.
[0103] The density of the side chains of the member having the bottle brush structure is 0.01 chains / nm 2 It is preferable that the number of chains is 0.05 chains / nm or more. 2 More preferably, it is 0.1 chains / nm or more. 2 More preferably, it is 0.2 chains / nm or more. 2The upper limit is not particularly limited, but is preferably 1.0 chain / nm. 2 and can be less than or equal to 0.9 chains / nm 2 It can also be the following:
[0104] The number average molecular weight of the member having a bottle-brush structure is preferably 1,000 to 10,000,000, more preferably 1,000 to 1,000,000, and even more preferably 5,000 to 500,000.
[0105] The molecular weight distribution index (Mw / Mn) of the member having a bottle-brush structure is preferably 1.0 to 2.0, more preferably 1.0 to 1.5. When the molecular weight distribution index is within the above range, it can be expected that the polymer chains constituting the polymer chain assembly can maintain a high density state up to the outermost surface.
[0106] When the member of this embodiment is a member having a bottle brush structure, the member has a bottle brush structure in which the plurality of polymer chains are bonded as side chains to a polymer chain that is the base material, and the member having the bottle brush structure preferably has a surface occupancy rate of the side chains of 0.08 to 0.50 (more preferably 0.10 to 0.50, and even more preferably 0.15 to 0.50).
[0107] [Liquid Substance] The layer containing the polymer chain assembly of the member of this embodiment holds a liquid substance, and the liquid substance contains at least water. The liquid substance may be water alone, or may further contain other liquid substances. The liquid substance other than water is preferably a hydrophilic liquid substance. Examples of hydrophilic liquid substances include hydrophilic ionic liquids, low-molecular-weight alcohols such as methanol and ethanol, acetonitrile, acetone, and ethylene glycol. The liquid substance may contain an additive.
[0108] Ionic liquids, also known as ionic liquids or room-temperature molten salts, are ionically conductive salts with low melting points. Many ionic liquids have relatively low melting points obtained by combining an organic onium ion as the cation with an organic or inorganic anion as the anion. The melting point of an ionic liquid is usually 100°C or lower, preferably room temperature (25°C) or lower. The melting point of an ionic liquid can be measured using a differential scanning calorimeter (DSC) or the like.
[0109] The ionic liquid may be a compound represented by the following formula (20): The melting point of this ionic liquid is preferably 50° C. or lower, more preferably 25° C. or lower. In formula (20), R 21 , R 22 , R 23 and R 24 are each independently an alkyl group having 1 to 5 carbon atoms, or R'-O-(CH 2 ) n -, R' represents a methyl group or an ethyl group, and n is an integer of 1 to 4. 21 , R 22 , R 23 and R 24 may be the same or different. 21 , R 22 , R 23 and R 24 Any two of R may be bonded to each other to form a cyclic structure. 21 , R 22 , R 23 and R 24 At least one of X is an alkoxyalkyl group. 21 represents a nitrogen atom or a phosphorus atom, and Y represents a monovalent anion.
[0110] R 21 , R 22 , R 23 and R 24 Examples of the alkyl group having 1 to 5 carbon atoms in R include a methyl group, an ethyl group, an n-propyl group, a 2-propyl group, an n-butyl group, and an n-pentyl group. 21 , R22 , R 23 and R 24 In the formula, R'-O-(CH 2 ) n As the alkoxyalkyl group represented by -, a methoxymethyl group or an ethoxymethyl group, a 2-methoxyethyl group or a 2-ethoxyethyl group, a 3-methoxypropyl group or a 3-ethoxypropyl group, a 4-methoxybutyl group or a 4-ethoxybutyl group, etc. are preferred. 21 , R 22 , R 23 and R 24 Compounds in which any two of the above are bonded to form a cyclic structure include X 21 When a nitrogen atom is used for X, a quaternary ammonium salt having an aziridine ring, an azetidine ring, a pyrrolidine ring, a piperidine ring, or the like is preferred. 21 When a phosphorus atom is used in Y, a quaternary phosphonium salt having a pentamethylenephosphine (phosphorinane) ring or the like is preferred. Furthermore, as the quaternary ammonium salt, one having a methyl group for R' and at least one 2-methoxyethyl group with n being 2 as a substituent is preferred. Examples of monovalent anions in Y include BF 4 - , P.F. 6 - , AsF 6 - , SbF 6 - , AlCl 4 - , NbF 6 - , HSO 4 - , ClO 4 - , C.H. 3 SO 3 - , C.F. 3 SO 3 - , C.F. 3 CO 2 - , (CF 3 SO 2 ) 2 N - , Cl - ,Br- , I - BF 4 - , P.F. 6 - , (CF 3 SO 2 ) 2 N - , C.F. 3 SO 3 - , or CF 3 CO 2 - It is preferable that:
[0111] The ionic liquid may be a compound represented by the formula (20): 21 is a methyl group, and R 23 and R 24 is an ethyl group, and R 24 is R'-O-(CH 2 ) n Compounds having a structure in which the alkoxyalkyl group is represented by - are preferably used.
[0112] Among the compounds represented by formula (20), specific examples of the quaternary ammonium salt and quaternary phosphonium salt that can be suitably used include the compounds shown below.
[0113] Furthermore, as the ionic liquid, an ionic liquid containing an imidazolium ion or an ionic liquid containing an aromatic cation can also be used.
[0114] The method for retaining a liquid substance in the layer containing polymer chain assemblies is not particularly limited. Examples include a method in which a liquid substance is applied to the surface of the layer containing polymer chain assemblies and then allowed to stand to retain the liquid substance, and a method in which a substrate on which a layer containing polymer chain assemblies has been formed is immersed in a liquid substance. Alternatively, the polymer chain assemblies may absorb moisture from the atmosphere to retain water as a liquid substance in the layer containing polymer chain assemblies.
[0115] The mass proportion of water relative to 100 parts by mass of the liquid substance is preferably 80 parts by mass or more, more preferably 90 parts by mass or more, even more preferably 95 parts by mass or more, and particularly preferably 100 parts by mass. The water as the liquid substance includes antifreeze water. The mass proportion of antifreeze water relative to the total mass of water in the liquid substance has a lower limit of 15% by mass or more, preferably 20% by mass or more, more preferably 25% by mass or more, and an upper limit of 50% by mass or less, preferably 40% by mass or less, and more preferably 30% by mass or less. The mass proportion of antifreeze water relative to the total mass of water in the liquid substance can be adjusted by the monomer composition of the polymer chains, etc. Water in a layer containing polymer chain assemblies includes bulk water and hydrated water (e.g., water in polymer chains) contained in the layer. Examples of the hydrated water include free water and intermediate water that freeze at -90°C, and antifreeze water that does not freeze at -90°C. The mass proportion of antifreeze water can be measured by the method described in the Examples below.
[0116] [Characteristics of Member] The member of this embodiment has an icing stress at -18°C of 150 kPa or less, preferably 100 kPa or less, more preferably 80 kPa or less, more preferably 65 kPa or less, even more preferably 50 kPa or less, still more preferably 35 kPa or less, and particularly preferably 20 kPa or less. The icing stress at -18°C can be measured by the method described in the examples below. The icing stress at -18°C can be adjusted by the type of polymer chain, the type of liquid substance, the surface occupancy of the polymer chain, etc.
[0117] The ice adhesion stress of the member of this embodiment at -8°C is preferably 10 to 50 kPa, more preferably 10 to 30 kPa, and even more preferably 0 to 20 kPa. When the ice adhesion stress at -8°C is within this range, an excellent ice adhesion suppression effect can be obtained over a wide range of temperatures from 0°C to -18°C. The ice adhesion stress at -8°C can be adjusted by the type of polymer chain, the type of liquid substance, the surface occupancy of the polymer chain, etc.
[0118] The difference between the icing stress of the member of this embodiment at -18°C and that at -8°C is preferably 100 kPa or less, more preferably 90 kPa or less, even more preferably 80 kPa or less, even more preferably 50 kPa or less, even more preferably 30 kPa or less, and particularly preferably 10 kPa or less. When the difference is within the above range, an excellent anti-icing effect can be obtained over a wide range of temperatures from 0°C to -18°C. In particular, when a compatible polymer chain is used as the polymer chain, an especially excellent anti-icing effect can be obtained at 0°C to -20°C. The member of this embodiment preferably has an icing stress at -18°C that is higher than that at -8°C. In this specification, the difference between the icing stress at -18°C and that at -8°C refers to the absolute value of the difference.
[0119] In this embodiment, the contact angle of the component surface with water at 25°C is preferably 10° or more, more preferably 20° or more, even more preferably 45° or more, even more preferably 48° or more, and particularly preferably 48 to 80°. A contact angle within the above range provides a more excellent effect in suppressing water droplet adhesion, icing, and ice nucleation. In this specification, the value of the contact angle of the component surface with water is determined by dropping 1 μL of water onto the component surface at 23°C and measuring the contact angle of water on the component surface one second after the drop has landed.
[0120] In order to retain a larger amount of antifreeze water in the layer containing the polymer chain assemblies, the member of this embodiment preferably has a ratio of the sum of the molecular weights of the antifreeze-forming structural moieties contained in each antifreeze-forming monomer unit contained in the polymer chain to the number-average molecular weight of the polymer chain in the layer containing the polymer chain assemblies (total molecular weights of the antifreeze-forming structural moieties contained in the antifreeze-forming monomer unit / number-average molecular weight of the polymer chain) of 0.75 or more, more preferably 0.80 or more, and even more preferably 0.80 to 0.95. This ratio can be adjusted by the mass proportion of the antifreeze-forming monomer unit. This ratio can be measured by the method described in the Examples below.
[0121] [Shape of Member] The shape of the member of the present embodiment is not particularly limited, and examples thereof include a tube, sheet, fiber, strip, film, plate, foil, membrane, pellet, powder, and particle shape.
[0122] [Applications of the Member] The member of this embodiment can be applied to a variety of articles. Examples include window glass, vehicle glass, mirrors, piping, and containers. The member of this embodiment does not change significantly in ice formation stress in the temperature range of 0°C to -20°C, and therefore can be suitably used in applications where ice formation must be suppressed over a wide temperature range of 0°C to -20°C.
[0123] The present invention may also be a member capable of retaining a liquid substance containing at least water in a layer containing polymer chain assemblies, and capable of making the proportion of antifreeze water relative to the total amount of water in the liquid substance 15 mass % or more. For example, the member obtained by the above-mentioned method can be produced by drying the member and then immersing it in water. Since the penetrated water is likely to strongly interact with the polymer in the layer containing the polymer chain assemblies, much of the penetrated water becomes antifreeze water that does not freeze even at -90°C.
[0124] The present invention will be described in more detail below based on examples, but the present invention is not limited to these examples.
[0125] Example 1 A silicon wafer and a DSC pan (made of aluminum) were ultrasonically cleaned in acetone for 30 minutes, chloroform for 30 minutes, and 2-propanol for 30 minutes, respectively, and then both surfaces of the silicon wafer and DSC pan were irradiated with UV ozone for 30 minutes. Next, only the DSC pan was coated with silica. Next, the silicon wafer and the silica-coated DSC pan were ultrasonically cleaned in ethanol for 30 minutes, and then immersed in a mixed solution of (2-bromo-2-methyl)propionyloxypropyltrimethoxysilane (BPM) / ethanol / aqueous ammonia = 1 / 89 / 10 (mass ratio) for 24 hours to introduce polymerization initiation groups into the silicon wafer and DSC pan. Next, methoxypoly(ethylene glycol) methacrylate (manufactured by Aldrich, code 10 ... 447943, number average molecular weight = 500) (hereinafter referred to as PEGMA), 50 parts by mass of a mixture of ethyl 2-bromo-2-methylpropionate (hereinafter referred to as EBIB), cuprous bromide (hereinafter referred to as CuBr(I)), cupric bromide (hereinafter referred to as CuBr(II)), and 4,4'-dinonyl-2,2'-bipyridine (hereinafter referred to as diNbip) (PEGMA / EBIB / CuBr(I) / CuBr(II) / diNbip = 200,000 / 0.1 / 1036.8 / 28.8 / 2344 (molar ratio)), and 50 parts by mass of anisole. The silicon wafer and DSC pan with the polymerization initiator groups introduced therein were placed in a fluororesin container containing the polymer chain assemblies. The container was sealed, covered with an aluminum bag, and placed in a high-pressure reactor, where a polymerization reaction was carried out at 400 MPa and 60°C for 4 hours. After the polymerization reaction was completed, the silicon wafer and DSC pan were removed from the container and washed with tetrahydrofuran using a shaker. The sample was then dried to form a brush-like polymer chain assembly (polymer brush layer) composed of multiple polymer chains on the silicon wafer surface, yielding a test specimen. The layer thickness of the obtained test specimen was measured using an atomic force microscope in both a dry state and a water-immersed state. The mass ratio of water was 50 parts by mass per 100 parts by mass of polymer chains contained in the layer containing the polymer chain assembly. Subsequent analysis revealed that the polymer brush layer formed on the silicon wafer surface had a thickness of 1102 nm and a number-average molecular weight of 6.2 × 10 6, molecular weight distribution index (Mw / Mn) is 1.4, polymer conversion is 3%, and polymer chain density is 0.12 chains / nm 2 The surface occupancy of the polymer chains was 0.33. The film thickness of the polymer brush layer was measured by ellipsometry. The number-average molecular weight and molecular weight distribution index of the polymer brush layer were calculated by gel permeation chromatography using dimethylformamide containing 10 mM lithium bromide as the developing solvent and a multi-angle light scattering detector as the detector. The polymer polymerization rate was 1 Measurement was performed by H-NMR. The obtained DSC pan was dried under reduced pressure at 40°C for 24 hours. Thereafter, it was moistened with 0.03 mg of water (an amount of water exceeding the water content (Wmax) in the layer in a saturated swollen state). It was confirmed by the method described below that the layer containing the polymer chain assemblies contained 20% by mass of non-freezing water. Furthermore, differential scanning calorimetry was performed, and it was confirmed that water was retained in a liquid state in the layer containing the polymer chain assemblies even at -18°C.
[0126] Example 2 A member was obtained in the same manner as in Example 1, except that methoxypoly(ethylene glycol) methacrylate (manufactured by Aldrich, code (447951), number average molecular weight = 950) was used instead of methoxypoly(ethylene glycol) methacrylate (manufactured by Aldrich, code 447943, number average molecular weight = 500).
[0127] Example 3 A member was obtained in the same manner as in Example 1, except that a mixture of 50 parts by mass of methoxypoly(ethylene glycol) methacrylate (manufactured by Aldrich, code 447943, number average molecular weight = 500) and 50 parts by mass of methoxypoly(ethylene glycol) methacrylate (manufactured by Aldrich, code (447951), number average molecular weight = 950) was used instead of methoxypoly(ethylene glycol) methacrylate (manufactured by Aldrich, code 447943, number average molecular weight = 500).
[0128] Example 4 A member was obtained in the same manner as in Example 1, except that a mixture of 50 parts by mass of methoxypoly(ethylene glycol) methacrylate (manufactured by Aldrich, code (447935), number average molecular weight = 300) and 50 parts by mass of methoxypoly(ethylene glycol) methacrylate (manufactured by Aldrich, code (447951), number average molecular weight = 950) was used instead of methoxypoly(ethylene glycol) methacrylate (manufactured by Aldrich, code 447943, number average molecular weight = 500).
[0129] Example 5 A member was obtained in the same manner as in Example 1, except that a mixture of 50 parts by mass of methoxypoly(ethylene glycol) methacrylate (manufactured by Aldrich, code 447943, number average molecular weight = 500) and 50 parts by mass of methoxypoly(ethylene glycol) methacrylate (manufactured by Aldrich, code (447935), number average molecular weight = 300) was used instead of methoxypoly(ethylene glycol) methacrylate (manufactured by Aldrich, code 447943, number average molecular weight = 500).
[0130] Comparative Example 1 A member was obtained in the same manner as in Example 1, except that methoxypoly(ethylene glycol) methacrylate (manufactured by Aldrich, code (447935), number average molecular weight = 300) was used instead of methoxypoly(ethylene glycol) methacrylate (manufactured by Aldrich, code 447943, number average molecular weight = 500).
[0131] [Evaluation] The members obtained in the above examples were subjected to the following measurements.
[0132] (Surface Coverage Ratio) Calculated by the above-mentioned method.
[0133] (Mass Proportion of Water in Layer Containing Polymer Chain Assembly) When members were produced in the Examples and Comparative Examples, the thickness of the layer containing polymer chain assemblies after drying under reduced pressure at 40°C for 24 hours was measured in contact mode using an atomic force microscope (trade name: NanoWizard 3, manufactured by JPK Instruments) to measure the difference in level between areas where the layer was present and areas where the layer was not present. The thickness of the layer containing polymer chain assemblies in a saturated swollen state, i.e., immersed in ion-exchanged water at room temperature, was then measured in the same manner. The amount of water (Wmax, unit: mg) contained in the layer containing polymer chain assemblies in a saturated swollen state was then calculated from the difference between the layer thickness in the saturated swollen state and the layer thickness in the dry state. Furthermore, a layer containing polymer chain assemblies of a dry member produced in the same manner as above was wetted by adding ion-exchanged water in an amount exceeding Wmax (Wcal, unit: mg), to obtain a wet member. The wet member was covered and sealed with a lid (Tzero Hermetic Lid, manufactured by TA Instruments), and differential scanning calorimetry was performed using a Discovery DSC 2500 differential scanning calorimeter (manufactured by TA Instruments) by cooling from 25°C to -90°C at a cooling rate of 3°C / min, followed by heating to 50°C at a heating rate of 3°C / min. The amount of frozen water (Wice, unit (mg)) in the layer containing the wet polymer chain assembly was determined by dividing the heat of fusion calculated from the DSC curve by the latent heat of fusion of ice (334 J / g). The amount of non-freezed water Wf (unit (mg)) was then obtained by subtracting Wice from the amount of ion-exchanged water Wcal added to the layer containing the polymer chain assembly, and the proportion of non-freezed water Wf / Wmax × 100 (unit (% by mass)) was calculated. When an excess amount of water is added to a layer containing polymer chain assemblies, it becomes bulk water and hydrated water (water in the polymer). The hydrated water includes free water that freezes at 0°C, intermediate water that does not freeze at 0°C but freezes when cooled to -90°C, and non-freezing water that does not freeze even at -90°C. The free water and intermediate water are hydrated water in the polymer chains that freezes at -90°C. In this specification, when measuring the mass proportion of water in a layer containing polymer chain assemblies, the total mass of water in the liquid substance may be the total mass of hydrated water excluding bulk water.
[0134] (Molecular Weight Proportion of Nonfreeze-Forming Structural Moiety) Polymer chains were cut out from the substrate of a layer containing polymer chain assemblies by treatment with hydrofluoric acid, and the number average molecular weight (Mn) of the cut polymer chains was measured by molecular weight analysis using size exclusion chromatography. The structure of the nonfreeze-forming monomer units contained in the polymer chain assemblies was analyzed, and the molecular weight was calculated from the composition of the nonfreeze-forming structural moieties within the monomer units. The molecular weight analysis using size exclusion chromatography was performed as follows. The size exclusion chromatography analysis was performed using a multi-angle light scattering detector (product name (see Examples)) and a molecular weight calibration curve created using a polymethyl methacrylate standard sample, which is a homogeneous monodisperse standard sample with a known molecular weight. The size exclusion chromatography analysis was performed under the following conditions. Name and model number of apparatus used: GPC-101, manufactured by Shodex Corporation; Product name and model number of column: LF-804, KF-06L, manufactured by Shodex Corporation; Eluent: DMF / LiBr (10 mM); Flow rate of eluent: 0.8 mL / min; Column temperature: 40°C; Name and model number of detector: DAWN-HELLO, manufactured by Wyatt Technology Corporation. The number average molecular weight Mn of the polymer chains cut out from the layer containing the polymer chain aggregate, and the weight average molecular weight (Mw) / number average molecular weight (Mn) are shown in Table 1. Furthermore, the ratio of the total molecular weight of the nonfreezable water-forming structural moieties contained in the nonfreezable water-forming monomer units constituting the nonfreezable water-forming units to the molecular weight of the polymer chain was calculated from the following formula (1): Sum of molecular weights of the antifreeze-forming structural moieties contained in each monomer unit constituting the antifreeze-forming unit / Sum of molecular weights of the monomer units constituting the polymer chain (1)
[0135] (Icing Stress) The members obtained in the Examples and Comparative Examples were placed on a microscope-equipped stretching stage (manufactured by Japan High-Tech Co., Ltd.) with a cooling function, and icing stress measurements were performed. Icicles were prepared by pouring 60 μL of pure water into an aluminum cylinder (inner diameter 6 mm) with silicone grease applied to the edges, cooling it to −20°C at a rate of 5°C / min, and holding it for 30 minutes. The stage temperature was then raised to −18°C at a rate of 5°C / min and held for 30 minutes before testing. The L-shaped jig attached to the stage was set to push against the aluminum cylinder as the stretching stage moved, and the icing stress (kPa) was calculated from the load applied to the load cell of the stretching stage when the icicle peeled off (Figure 1). Evaluation was performed according to the following criteria. The stage movement speed was 10 mm / min. ◎ (Excellent): Ice adhesion stress is less than 50 kPa ○ (Excellent): Ice adhesion stress is 50 kPa or more and less than 100 kPa △ (Good): Ice adhesion stress is 100 kPa or more and less than 150 kPa × (Poor): Ice adhesion stress is 150 kPa or more
[0136] (Thickness of Layer Containing Polymer Chain Assembly) Measured at room temperature by spectroscopic ellipsometry (MASS-105 manufactured by Five Labs). Optical constants, etc., were measured using files prepared using each test specimen according to the manufacturer's procedures.
[0137] (Swelling Degree) The members prepared in the Examples and Comparative Examples were dried under reduced pressure at 40°C for 24 hours. The layer containing the polymer chain assemblies of the members was scratched with the tip of tweezers. The boundary between the exposed substrate and the layer containing the polymer chain assemblies was measured for the height of the step (i.e., the thickness of the layer containing the polymer chain assemblies in a dry state) using an atomic force microscope colloidal probe method (contact mode). The same test specimens were then immersed in ion-exchanged water at room temperature, and the height of the step in the swollen state was measured at the same location in the liquid using an atomic force microscope colloidal probe method (contact mode). The swelling degree was calculated from the ratio of the layer thickness of the swollen body to the layer thickness in a dry state.
[0138]
[0139] The member of the present embodiment can suppress ice nucleation and icing. The member of the present embodiment can be applied to various articles, such as window glass, vehicle glass, mirrors, piping, and containers.
Claims
1. A component for inhibiting ice nucleation or icing, comprising a layer containing brush-like polymer chain assemblies composed of a plurality of polymer chains fixed to a substrate, the layer containing the polymer chain assemblies retaining a liquid substance, at least a portion of the liquid substance being water, and the proportion of antifreeze water relative to the total mass of the water in the liquid substance being 15 mass% or more.
2. The member according to claim 1, wherein the polymer chain contains an antifreeze-forming unit consisting of an antifreeze-forming monomer unit.
3. A member according to claim 1 or 2, wherein the ratio of the sum of the molecular weights of the nonfreeze-water-forming structural moieties contained in the nonfreeze-water-forming monomer units in the polymer chain to the molecular weight of the polymer chain (the sum of the molecular weights of the nonfreeze-water-forming structural moieties contained in the nonfreeze-water-forming monomer units / the molecular weight of the polymer chain) is 0.80 or more.
4. The member according to claim 1 or 2, wherein the substrate is a carrier made of a material different from the polymer chain assembly, and the surface occupancy of the polymer chains on the substrate surface is 0.08 to 0.
65.
5. The member according to claim 1 or 2, wherein the member has a bottle-brush structure in which the plurality of polymer chains are bonded as side chains to the base polymer chain, and the surface occupancy rate of the side chains is 0.08 to 0.65.
Citation Information
Patent Citations
Preparation and application of super-smooth coating with long-acting ice dredging characteristic
CN113528010A
Heat exchanger and refrigeration cycle device
JP2022020472A
Snow slip film or sheet
WO2019181216A1
Member for fogging prevention, suppression of water droplet adhesion, suppression of icing, or suppression of ice nucleus formation
WO2021117537A1