Light-absorbing composition, method for producing light-absorbing composition, composition for light-absorbing film, and light-absorbing film
The light-absorbing composition with a copper and phosphorus-based compound addresses the issues of high solvent content and low copper concentration in existing compositions by optimizing the dry mass ratio, resulting in a stable and efficient film with enhanced absorption properties.
Patent Information
- Application Number
- PCT/JP2024/017865
- Authority / Receiving Office
- WO · WO
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2023-05-31
- Filing Date
- 2024-05-14
- Publication Date
- 2024-12-05
AI Technical Summary
Existing light-absorbing compositions for optical filters in imaging devices have high solvent content and low copper complex concentration, leading to uneven light-absorbing ability and the need for large quantities, which can result in aggregation issues during film formation.
A light-absorbing composition with a copper and phosphorus-based compound, where the ratio of dry mass to total mass is between 15% to 55%, is developed, allowing for improved dispersion and reduced solvent evaporation, thereby minimizing aggregation and achieving desired absorption properties.
The composition provides a stable and efficient light-absorbing film with improved transmittance characteristics, reducing the need for large quantities and minimizing uneven absorption issues, while maintaining effective infrared and ultraviolet shielding properties.
Smart Images

Figure JP2024017865_05122024_PF_FP_ABST
Abstract
Description
Light-absorbing composition, method for producing light-absorbing composition, composition for light-absorbing film, and light-absorbing film
[0001] The present invention relates to a light-absorbing composition, a method for producing a light-absorbing composition, a composition for a light-absorbing film, and a light-absorbing film.
[0002] In imaging devices or ambient light sensors using solid-state imaging elements such as CCDs (Charge Coupled Devices) or CMOSs (Complementary Metal Oxide Semiconductors), various optical filters are placed in front of the solid-state imaging elements to obtain images with good color reproducibility. Solid-state imaging elements generally have sensitivity over a wide wavelength range, from the ultraviolet to the infrared. Meanwhile, human visual sensitivity is limited to the visible light range. Therefore, in order to bring the sensitivity of the solid-state imaging elements in imaging devices closer to human visual sensitivity, a technique is known in which an optical filter is placed in front of the solid-state imaging element to block some infrared and ultraviolet light. Among these, light-absorbing optical filters having a film or layer containing a light absorber have attracted attention.
[0003] The transmittance characteristics of an optical filter having a film containing a light-absorbing compound are not easily affected by the angle of incidence, so even when light is incident obliquely on the optical filter in an imaging device, there is little change in color, and good images with good reproducibility and little color unevenness within the surface can be obtained. Furthermore, when using this type of optical filter that does not use a light-reflecting film, the occurrence of ghosts or flares caused by multiple reflections due to light reflection is suppressed, resulting in good images. In addition, optical filters having a film containing a light-absorbing compound are advantageous in terms of making imaging devices smaller and thinner.
[0004] Optical filters using a copper complex containing phosphonic acid as a light-absorbing compound are known. For example, Patent Document 1 describes an optical filter having a light-absorbing layer with a thickness of 80 μm or less and a maximum transmittance of 5% or less from 750 to 1080 nm. This light-absorbing layer contains copper phosphonate and an organic dye, and the organic dye has a maximum absorption wavelength of 720 nm to 780 nm. Patent Document 1 also describes a light-absorbing composition containing copper phosphonate and an organic solvent, in which the concentration of an acid, a by-product in the production of copper phosphonate, is 1.0 mass% or less. By using such a light-absorbing composition, copper phosphonate and the organic dye can coexist in a single light-absorbing layer.
[0005] International Publication No. 2020 / 071461
[0006] As described above, Patent Document 1 allows copper phosphonate and an organic dye to coexist in a single light-absorbing layer, thereby reducing the concentration of acid, a by-product, in the light-absorbing composition. However, the light-absorbing composition described in Patent Document 1 has a high solvent content and a low concentration of the copper complex component, i.e., the light-absorbing compound. It is understood that the concentration remains at 7% by mass or less. Therefore, a large amount of the light-absorbing composition is required to achieve the desired light absorption capacity. In addition, when preparing a light-absorbing film by solidifying the light-absorbing composition, a large amount of solvent must be evaporated, which may lead to problems such as bias or unevenness in the light absorption capacity on or within the film. Thus, the light-absorbing composition described in Patent Document 1 has room for reexamination from the perspective of addressing problems caused by its solvent content.
[0007] Therefore, the present invention provides a light-absorbing composition that contains a light-absorbing compound having phosphorus and copper, and is advantageous in terms of addressing the problems caused by the solvent content.
[0008] The present invention provides a light-absorbing composition comprising: a light-absorbing compound having phosphorus and copper; and a solvent, wherein the ratio of the dry mass of the light-absorbing composition to the mass of the light-absorbing composition is 15% to 55%.
[0009] The present invention also provides a method for producing a light-absorbing composition, comprising: mixing a phosphorus-containing compound and a copper salt in a first solvent; separating the first solvent to obtain a solid having phosphorus and copper; and adding the solid to a second solvent and adjusting by distillation a ratio of the dry mass of the light-absorbing composition to the mass of the light-absorbing composition to be 15% to 55%.
[0010] Furthermore, the present invention provides a composition for a light-absorbing film, comprising: a light-absorbing compound having phosphorus and copper; a solvent; and a resin, wherein the ratio of the dry mass of the composition for a light-absorbing film to the mass of the composition for a light-absorbing film is 10% to 55%.
[0011] The present invention further provides a light-absorbing film comprising a light-absorbing compound containing phosphorus and copper and a resin, having a thickness of 300 μm or less, and exhibiting a transmission spectrum having the following characteristics (I) to (IV) when light having a wavelength of 300 nm to 1200 nm is incident at an incident angle of 0°. (I) The average transmittance in the wavelength range of 800 nm to 1100 nm is 10% or less. (II) The average transmittance in the wavelength range of 460 nm to 580 nm is 80% or more. (III) The first cutoff wavelength at which the transmittance is 50% in the wavelength range of 300 nm to 400 nm is in the wavelength range of 320 nm to 400 nm. (IV) The second cutoff wavelength at which the transmittance is 50% in the wavelength range of 600 nm to 800 nm is in the wavelength range of 650 nm to 750 nm.
[0012] The composition for a light-absorbing film described above is advantageous in that it contains a light-absorbing compound having phosphorus and copper, while addressing the problems caused by the content of a solvent.
[0013] FIG. 1A is a cross-sectional view of an optical filter according to an example embodiment of the present invention. FIG. 1B is a cross-sectional view of an optical filter according to another example embodiment of the present invention. FIG. 1C is a cross-sectional view of an optical filter according to yet another example embodiment of the present invention. FIG. 1D is a cross-sectional view of an optical filter according to yet another example embodiment of the present invention. FIG. 1E is a cross-sectional view of an optical filter according to yet another example embodiment of the present invention. FIG. 1F is a cross-sectional view of an optical filter according to yet another example embodiment of the present invention. FIG. 2 is a transmission spectrum of a light-absorbing composition according to Example 1. FIG. 3 is a transmission spectrum of a light-absorbing composition according to Example 4. FIG. 4 is a transmission spectrum of a light-absorbing composition according to Example 9. FIG. 5 is a transmission spectrum of a light-absorbing composition according to Example 11. FIG. 6 is a transmission spectrum of a light-absorbing composition according to Example 15. FIG. 7 is a transmittance spectrum of an optical filter according to Example 22. FIG. 8 is a transmittance spectrum of D263 T eco (manufactured by SCHOTT) used as a support. FIG. 9 is a transmittance spectrum of an optical filter according to Example 23. Fig. 10 is a transmittance spectrum of the optical filter according to Example 24. Fig. 11 is a transmittance spectrum of the optical filter according to Example 25. Fig. 12 is a transmittance spectrum of the optical filter according to Example 26. Fig. 13 is a transmittance spectrum of the optical filter according to Example 27.
[0014] Hereinafter, embodiments of the present invention will be described. Note that the following description relates to examples of the present invention, and the present invention is not limited to these.
[0015] The light-absorbing composition according to the present invention comprises a light-absorbing compound and a solvent. The light-absorbing compound can absorb light of a specific wavelength. The solvent disperses or dissolves the light-absorbing compound in the light-absorbing composition. The light-absorbing compound contains phosphorus and copper. The ratio r1 of the dry mass of the light-absorbing composition to the mass of the light-absorbing composition is 15% to 55%. The dry mass of the light-absorbing composition is the mass of the residue remaining after removing liquid components such as the solvent from the light-absorbing composition by evaporation, for example, by heating. The mass of the light-absorbing composition is the mass of the light-absorbing composition provided as a product before the solvent is removed.
[0016] Furthermore, the concentration of the specific acid in the light-absorbing composition according to the present invention may be 0.2 mass % or less or less than 0.2 mass %. The acid contained in the light-absorbing composition may be a component or a part of a component contained in the compound that supplies the copper component.
[0017] When a curable resin is added to the light-absorbing composition itself or to a composition prepared by adding a specific solvent to the light-absorbing composition, a light-absorbing film can be formed. For example, a light-absorbing film can be formed on the surface of an optical film, an optical filter, or an optical functional element such as a lens or a diffraction grating (hereinafter collectively referred to as a "support") by solidifying a composition derived from the light-absorbing composition. This allows the function of absorbing and blocking light having a specific wavelength to be added.
[0018] The ratio r1 in the light-absorbing composition is closely related to the amount of light-absorbing compound required for the desired function. By setting the ratio r1 to 15% or more, it is possible to avoid the need for a relatively large amount of light-absorbing composition to exhibit the desired absorption characteristics. In addition, the amount of solvent evaporation required to form the light-absorbing film can be reduced, making it less likely that an increase in haze due to solvent evaporation or variation in absorption characteristics within the surface of the light-absorbing film will occur. By setting the ratio r1 to 55% or less, aggregation of the light-absorbing compound is more likely to be prevented in the light-absorbing composition or in a composition prepared using the light-absorbing composition. The ratio r1 is preferably 20% to 50%.
[0019] The light-absorbing compound is not limited to a specific substance as long as it can impart desired characteristics, such as a transmission spectrum, to a light-absorbing body such as a light-absorbing film produced using the light-absorbing composition. The light-absorbing compound may contain, for example, at least one selected from the group consisting of phosphonic acid and a phosphate ester, and a copper component. The light-absorbing compound may contain phosphonic acid, a phosphate ester, and a copper component.
[0020] The light absorbing compound may contain phosphoric acid and a copper component, may contain phosphinic acid and a copper component, may contain metaphosphoric acid and a copper component, or may contain pyrophosphoric acid and a copper component.
[0021] The light-absorbing compound may be formed as a complex of a phosphorus- and oxygen-containing atomic group with a copper component. Examples of the phosphorus- and oxygen-containing atomic group include phosphonic acid, phosphate ester, phosphinic acid, phosphoric acid, metaphosphoric acid, and pyrophosphoric acid. The light-absorbing compound may be, for example, M 1 / n Cu m P.O. 4-z In this composition, M is a metal other than Cu, n and m are natural numbers, and z is a positive integer less than 4.
[0022] As the light-absorbing compound, these compounds may be used alone, or a plurality of compounds may be used in combination. Atomic groups containing phosphorus and oxygen, such as phosphonic acid, phosphinic acid, phosphate ester, and phosphoric acid, may coexist. For example, the light-absorbing compound may exist as a compound containing phosphonic acid, phosphate ester, and a copper component. When the light-absorbing compound is a complex containing phosphonic acid and a copper component, the light-absorbing composition may contain a phosphate ester as a dispersant. In this case, a compound containing phosphonic acid, phosphate ester, and a copper component may also coexist.
[0023] The light-absorbing composition may contain, in addition to the light-absorbing compounds described above, a compound containing a sulfonic acid and a copper component, a compound containing tungsten oxide, a metal oxide such as indium tin oxide (ITO) or antimony tin oxide (ATO), or an organic dye-based compound. Examples of the organic dye-based compound include diimmonium-based compounds, cyanine-based compounds, squarylium-based compounds, phthalocyanine-based compounds, and pyrrolopyrrole-based compounds.
[0024] The copper component in the light-absorbing compound is a concept that includes copper ions, copper complexes, and compounds containing copper atoms, etc. The copper component can have desired absorption characteristics for a portion of light in the near-infrared region. Specifically, due to the transition of electrons in the d orbital of the divalent copper ion, light of a wavelength in the near-infrared region corresponding to this energy is selectively absorbed, thereby exhibiting desired near-infrared absorption characteristics. The copper component may have, for example, a hexacoordinated structure with one or more types of ligands. In this case, it is expected that the ability to absorb light in the infrared region will be enhanced.
[0025] The phosphonic acid that can be contained in the light-absorbing compound is not limited to a specific phosphonic acid, as long as the light absorber produced using the light-absorbing composition has a desired transmission spectrum. The phosphonic acid is, for example, represented by the following formula (a1) or (a2):
[0026]
[0027] In formula (a1), R is an alkyl group or a halogenated alkyl group in which at least one hydrogen atom in the alkyl group is substituted with a halogen atom. In this case, the transmission band of the light absorber produced using the light-absorbing composition is likely to extend to a wavelength of around 700 nm, and the light absorber is likely to have the desired transmittance characteristics. Phosphonic acids having these groups are collectively referred to as alkylphosphonic acids. Examples of alkylphosphonic acids include methylphosphonic acid, ethylphosphonic acid, normal (n-)propylphosphonic acid, isopropylphosphonic acid, normal (n-)butylphosphonic acid, isobutylphosphonic acid, sec-butylphosphonic acid, tert-butylphosphonic acid, and bromomethylphosphonic acid.
[0028] In formula (a2), R2 is, for example, an aryl group, a halogenated aryl group in which at least one hydrogen atom in the aryl group is substituted with a halogen atom, or a group in which at least one hydrogen atom in the aryl group is substituted with a nitro group or a hydroxy group. The aryl group is, for example, a phenyl group. The halogenated aryl group is, for example, a halogenated phenyl group. In this case, the light absorber produced using the light-absorbing composition is more likely to have the desired transmittance characteristics. Phosphonic acids having these groups are collectively referred to as arylphosphonic acids. Examples of arylphosphonic acids include phenylphosphonic acid, bromophenylphosphonic acid, benzylphosphonic acid, fluorophenylphosphonic acid, iodophenylphosphonic acid, nitrophenylphosphonic acid, hydroxyphenylphosphonic acid, tolylphosphonic acid, xylylphosphonic acid, and naphthylphosphonic acid.
[0029] The phosphonic acid may include one or more phosphonic acids selected from the above phosphonic acids, as long as the light absorber produced using the light-absorbing composition has a desired transmission spectrum. Furthermore, the phosphonic acid may include an alkylphosphonic acid and an arylphosphonic acid, or may include one or more types of alkylphosphonic acid and one or more types of arylphosphonic acid. Furthermore, each of the alkylphosphonic acid and the arylphosphonic acid may be bound to a copper component to form a light-absorbing compound.
[0030] The light-absorbing composition may contain, for example, a phosphate ester so as to form a part of the light-absorbing compound, or may contain a phosphate ester to suppress aggregation of the light-absorbing compound in a solvent. The function of the phosphate ester facilitates proper dispersion of the light-absorbing compound in the light-absorbing composition and in a light absorber prepared using the light-absorbing composition. The phosphate ester may function as a dispersant for the light-absorbing compound, and a portion of the phosphate ester may react with a metal component such as a copper component to form a compound. For example, the phosphate ester may be coordinated to the light-absorbing compound, or may react with the light-absorbing compound, or may partially form a complex with the copper component. As long as the light absorber prepared using the light-absorbing composition has a desired transmission spectrum, the compound containing the phosphate ester and the copper component may also absorb light of some wavelengths.
[0031] The phosphate ester is not limited to a specific phosphate ester. The phosphate ester has, for example, a polyoxyalkyl group. The phosphate ester may be, for example, a phosphate diester represented by the following formula (b1) or a phosphate monoester represented by the following formula (b2). The phosphate ester may also be a phosphate ester in which a phosphate diester and a phosphate monoester are mixed in any ratio. In the following formulas (b1) and (b2), R 21 , R 22 , and R3 are each —(CH2CH2O) n R is a monovalent functional group represented by R, n is an integer of 1 to 25, R represents an alkyl group having 6 to 25 carbon atoms, and R 21 , R 22 and R3 are the same or different functional groups.
[0032]
[0033] Examples of such phosphate esters are PLYSURF A208N: polyoxyethylene alkyl (C12, C13) ether phosphate ester, PLYSURF A208F: polyoxyethylene alkyl (C8) ether phosphate ester, PLYSURF A208B: polyoxyethylene lauryl ether phosphate ester, PLYSURF A219B: polyoxyethylene lauryl ether phosphate ester, PLYSURF AL: polyoxyethylene styrenated phenyl ether phosphate ester, PLYSURF A212C: polyoxyethylene tridecyl ether phosphate ester, and PLYSURF A215C: polyoxyethylene tridecyl ether phosphate ester. All of these are products manufactured by Dai-ichi Kogyo Seiyaku Co., Ltd. Other examples of phosphate esters are NIKKOL DDP-2: polyoxyethylene alkyl ether phosphate ester, NIKKOL DDP-4: polyoxyethylene alkyl ether phosphate ester, and NIKKOL DDP-6: polyoxyethylene alkyl ether phosphate ester. All of these are products manufactured by Nikko Chemicals Co., Ltd. These phosphate ester compounds may be used alone or in combination. Plysurf and NIKKOL are registered trademarks of Daiichi Kogyo Seiyaku Co., Ltd. and Nikko Chemicals Co., Ltd., respectively.
[0034] The light-absorbing composition may contain an ultraviolet absorber that absorbs a portion of ultraviolet light. The inclusion of an ultraviolet absorbing compound in the light-absorbing composition and the light absorber prepared using the light-absorbing composition can reduce the possibility of deterioration of the resin and light-absorbing compound that may be contained in the light absorber, or of undesirable effects on electronic devices and the like equipped with the light absorber. The ultraviolet absorbing compound is not limited to a specific compound as long as the light absorber prepared using the light-absorbing composition has a desired transmission spectrum. The ultraviolet absorbing compound is preferably selected from the viewpoints of absorbing light in a desired wavelength range, being compatible with specific solvents, dispersing well in the light-absorbing composition, and having excellent environmental resistance. Examples of ultraviolet absorbing compounds include benzophenone-based compounds, benzotriazole-based compounds, salicylic acid-based compounds, and triazine-based compounds. Examples of ultraviolet absorbers are Tinuvin PS, Tinuvin 99-2, Tinuvin 234, Tinuvin 326, Tinuvin 329, Tinuvin 900, Tinuvin 928, Tinuvin 405, and Tinuvin 460. These are ultraviolet absorbing compounds manufactured by BASF, and Tinuvin is a registered trademark.
[0035] The solvent contained in the light-absorbing composition is not limited to a specific solvent. The solvent may be one that causes a reaction between the phosphorus- and oxygen-containing compound and the copper component. When it is planned to extract the reaction product formed by the reaction between the phosphorus- and oxygen-containing compound and the copper component as a solid by solid separation, a solvent that functions as a poor solvent may be used. An example of solid separation may be filtration. This reaction product may include the above-mentioned light-absorbing compound. When the process of preparing the light-absorbing composition includes a process of separating the first solvent and extracting the solid content of the light-absorbing compound, a portion of the first solvent may remain in the solid content, and the first solvent may ultimately be contained in the light-absorbing composition. The first solvent is not limited to a specific solvent as long as it has such roles and functions.
[0036] Examples of the first solvent include methanol, ethanol, n-propanol, i-propanol, n-butanol, i-butanol, 2-butanol, t-butanol, n-pentanol, i-pentanol, 2-methylbutanol, 2-pentanol, t-pentanol, 3-methoxybutanol, n-hexanol, 2-methylpentanol, 1-hexanol, 2-hexanol, 2-ethylbutanol, 1-heptanol, 2-heptanol, 3-heptanol, n-octanol, 2-ethylhexanol, 2-octanol, n-nonyl alcohol, 2,6-dimethyl- Examples of the first solvent include alcohols such as 4-heptanol, n-decanol, cyclohexanol, methylcyclohexanol, 3,3,5-trimethylcyclohexanol, benzyl alcohol, and diacetone alcohol, heterocyclic compounds such as xylenes, dichlorobenzene, heptanone, cyclopentanone, cyclohexanone, cyclohexane, dimethylformamide, dimethylacetamide, toluene, tetrahydrofuran (THF), and oxetane, and chlorinated solvents such as methylene chloride (dichloromethane), chloroform, dichloroethane, and tetrachloroethane. One or more of these solvents may be selected and mixed for use as the first solvent.
[0037] The light-absorbing composition may contain a second solvent in addition to the first solvent. A light-absorbing compound or an ultraviolet-absorbing compound capable of absorbing light of a specific wavelength may be dissolved in the light-absorbing composition, or may be contained in the light-absorbing composition in the form of fine particles. By including the second solvent in the light-absorbing composition, such a compound can be contained in the light-absorbing composition in a desired amount.
[0038] Examples of the second solvent include, but are not limited to, methanol, ethanol, n-propanol, i-propanol, n-butanol, i-butanol, 2-butanol, t-butanol, n-pentanol, i-pentanol, 2-methylbutanol, 2-pentanol, t-pentanol, 3-methoxybutanol, n-hexanol, 2-methylpentanol, 1-hexanol, 2-hexanol, 2-ethylbutanol, 1-heptanol, 2-heptanol, 3-heptanol, n-octanol, 2-ethylhexanol, 2-octanol, n-nonyl alcohol, Examples of the second solvent include alcohols such as 2,6-dimethyl-4-heptanol, n-decanol, cyclohexanol, methylcyclohexanol, 3,3,5-trimethylcyclohexanol, benzyl alcohol, and diacetone alcohol, heterocyclic compounds such as xylenes, dichlorobenzene, heptanone, cyclopentanone, cyclohexanone, cyclohexane, dimethylformamide, dimethylacetamide, toluene, tetrahydrofuran (THF), and oxetane, and chlorinated solvents such as methylene chloride (dichloromethane), chloroform, dichloroethane, and tetrachloroethane. One or more of these solvents may be selected and mixed for use as the second solvent.
[0039] The second solvent may be determined in consideration of the properties of the resin component contained in the light absorber produced using the light absorbing composition, the stability of the composition for a light absorbing film, the stability of the process for producing the light absorber, the properties required for the light absorber, etc. When the light absorber is produced by a solution casting method, a solvent with a low boiling point (for example, a chlorine-based solvent) is desirably used.
[0040] The light-absorbing composition may have a predetermined transmission spectrum. The light-absorbing composition exhibits, for example, a transmission spectrum having the following characteristics (i) to (iv). The transmission spectrum of the light-absorbing composition is measured, for example, by placing the composition in a transparent quartz cell in which the physical optical path length of light passing through the composition is 1±0.25 mm. The physical optical path length is the optical path length (actual length) without taking into account the refractive index of the medium. The transmission spectrum of the light-absorbing composition is measured at an ambient temperature of 25±5°C using a measurement sample prepared by adjusting the amount of solvent added or by adding a solvent so that the transmittance at a wavelength of 800 nm is 10±1%. (i) The average transmittance within the wavelength range of 800 nm to 1100 nm is 20% or less. (ii) The average transmittance within the wavelength range of 460 nm to 580 nm is 80% or more. (iii) Within the wavelength range of 300 nm to 400 nm, the cutoff wavelength at which the transmittance is 50% is within the wavelength range of 320 nm to 380 nm. (iv) Within the wavelength range of 600 nm to 800 nm, the cutoff wavelength at which the transmittance is 50% is within the wavelength range of 680 nm to 780 nm.
[0041] Due to the above (i), a light absorber produced using the light-absorbing composition can exhibit desired infrared-shielding properties. This can improve the match between the light reaching the imaging element and the visual sensitivity of humans, who generally do not perceive light in the infrared region. The average transmittance in the wavelength range of 800 nm to 1100 nm is preferably 15% or less, more preferably 10% or less, even more preferably 8% or less, and particularly preferably 6% or less.
[0042] According to the above (ii), the luminous flux of light in the visible light region that has passed through the light absorber increases, making it easier to obtain a brighter image. The average transmittance in the wavelength range of 460 nm to 580 nm is preferably 85% or more, and more preferably 90% or more.
[0043] The above (iii) allows for improved blocking of light in the ultraviolet range. By improving the blocking of light in the ultraviolet range, it is possible to improve the match between the light reaching the imaging element and the visual sensitivity of humans, who generally do not perceive light in the ultraviolet range. Furthermore, it is possible to reduce the effect of color fringing, such as purple fringing, that occurs when light with short wavelengths is included in the light reaching the imaging element. Within the wavelength range of 300 nm to 400 nm, the cutoff wavelength at which the transmittance is 50% is preferably in the range of 340 nm to 365 nm, and more preferably in the range of 345 nm to 360 nm.
[0044] The above (iv) allows for improved blocking of light in the infrared range. By improving the blocking of light in the infrared range, it is possible to improve the match between the light reaching the imaging element and the visual sensitivity of humans, who generally do not perceive light in the infrared range. Within the wavelength range of 600 nm to 800 nm, the cutoff wavelength at which the transmittance is 50% is preferably in the range of 700 nm to 760 nm, and more preferably in the range of 720 nm to 740 nm.
[0045] The above-mentioned transmission spectrum of the light-absorbing composition may further have the following (v): (v) the wavelength range corresponding to the band in which the transmittance is 50% or more within the wavelength range of 300 nm to 1200 nm is 350 nm to 420 nm.
[0046] The above (v) specifies the width of the so-called transmission band, and by the above (v), it is possible to prevent the band in the visible light region from becoming narrow and blocking a portion of the visible light. In addition, it is possible to sufficiently block light outside the visible light region. The wavelength range corresponding to the band in which the transmittance is 50% or more in the wavelength range of 300 nm to 1200 nm is preferably 350 nm to 410 nm, and more preferably 360 nm to 390 nm.
[0047] The above transmission spectrum of the light-absorbing composition may further have the following (vi): (vi) the average value of the transmittance in the wavelength range of 1100 nm to 1200 nm is 10% or less.
[0048] Light-absorbing compositions containing a light-absorbing compound containing phosphorus, oxygen, and copper tend to have high transmittance in the wavelength range of 1100 nm or more, and even if the transmittance in the wavelength range of 800 nm to 1100 nm is sufficiently low, the transmittance at 1100 nm or more may not be low. The average transmittance in the wavelength range of 1100 nm to 1200 nm is desirably 8% or less.
[0049] The above transmission spectrum of the light-absorbing composition may further have the following (vii): (vii) The standard deviation of the transmittance in the wavelength range of 900 nm to 1100 nm is 0.5% or less.
[0050] When adjusting the concentration or amount of the light-absorbing compound in a light-absorbing composition to enhance light absorption in the wavelength range of 800 nm to 1200 nm, it is advantageous that the transmittance in the wavelength range of 900 nm to 1100 nm varies little and the transmission spectrum visually observed in this wavelength range has a flat pattern. By using (vii) above, for example, it is easy to avoid a situation where the transmittance in a wavelength range of 800 nm to 1100 nm is adjusted to a sufficiently low level while the transmittance in some wavelength ranges is not sufficiently reduced. The standard deviation in (vii) above is desirably 0.3% or less.
[0051] The method for producing the light-absorbing composition includes, for example, the following steps (a), (b), and (c): (a) mixing a phosphorus-containing compound and a copper salt in a first solvent; (b) separating and removing the first solvent to obtain a solid containing phosphorus and copper; and (c) adding the solid to a second solvent and adjusting by distillation the ratio of the dry mass of the light-absorbing composition to the mass of the light-absorbing composition to 15% to 55%.
[0052] In the above (c), the distillation may be carried out at 100°C or less. This makes it difficult for thermal damage to occur to the solid material, and the light absorber obtained using the light-absorbing composition is likely to have a desired transmission spectrum. The distillation may be carried out at a temperature of preferably 95°C or less, more preferably 90°C or less, even more preferably 85°C or less, particularly preferably 75°C or less, and especially preferably 65°C or less.
[0053] In the above (c), the distillation may be performed at a pressure lower than atmospheric pressure. This allows the second solvent to be removed by distillation at a predetermined temperature lower than the boiling point, even if the second solvent has a high boiling point. For example, the distillation may be performed at a pressure of 500 hectopascals (hPa) or less.
[0054] In (a), the copper salt is not limited to a specific copper salt. The copper salt may be an anhydrous or hydrated copper salt of an organic acid, such as copper acetate, copper benzoate, copper pyrophosphate, or copper stearate, or a mixture thereof. These copper salts may be used alone, or multiple copper salts or a mixture thereof may be used.
[0055] An example of a method for producing the light-absorbing composition will now be described. The method for producing the light-absorbing composition is not limited to the following method.
[0056] A copper salt, which serves as a source of copper components, is added to a first solvent and stirred for several minutes to several hours to prepare a copper salt solution. A phosphate ester is added to this copper salt solution and stirred for several minutes to several hours to prepare a phosphate ester-copper salt solution. Next, a phosphonic acid is added to a separately prepared first solvent and stirred for several minutes to several hours to prepare a phosphonic acid solution. Next, the phosphate ester-copper salt solution and the phosphonic acid solution are mixed and stirred at room temperature for several minutes to several hours. In these processes, a so-called poor solvent that significantly precipitates a reaction product that also contains a light-absorbing compound can be selected as the first solvent. A poor solvent essentially refers to a solvent that has low solubility for the solute. However, here, the poor solvent may have the role or function of significantly precipitating the resulting fine particles, etc., or agglomerating the fine particles, etc. The first solvent may be a poor solvent for the reaction product containing the light-absorbing compound. In this case, the solid content of the reaction product can be easily separated from the solvent and extracted. Furthermore, the material of the container for producing the above solution or reaction product may be glass, including borosilicate glass such as Pyrex (registered trademark), or stainless steel, particularly high-grade stainless steel such as SUS316.
[0057] In this way, a reaction product containing phosphorus and copper is separated out and precipitated in the first solvent. It is very difficult to clarify the details of the reaction process between the phosphorus- and oxygen-containing compound, such as phosphonic acid and phosphate ester, and the copper component, and to precisely identify the reaction product. For this reason, the reaction product containing phosphorus and copper may be, for example, a compound containing phosphonic acid and a copper component (e.g., a phosphonic acid copper compound), a compound containing a phosphate ester and a copper component (e.g., a phosphate ester copper compound), a compound containing phosphonic acid, a phosphate ester, and a copper component (e.g., a phosphonic acid-phosphate ester copper compound), or a mixture thereof. The reaction product may also contain compounds other than these. For example, water (HO) and acetate ions (CHCOO - ) and the like can also coordinate to copper ions, and the reaction product may also contain these compounds and ions.
[0058] Next, the solid reaction product in the solvent is separated from the solvent by a solid-liquid separation technique. Examples of solid-liquid separation techniques include filtration and centrifugation. Filtration can be performed using coarse filtration (10 μm or larger mesh size, the same applies below), microfiltration (50 nm to 10 μm), ultrafiltration (1 to 50 nm), or any of these. Filtration can be performed by gravity filtration, using its own weight as a driving force, or by suction filtration, which reduces pressure to shorten the time. Examples of filter media include filter paper and filter cloth, and either can be used. If a cake layer is formed during the filtration process and serves as the filter media, a specific filter media does not need to be used. The retention particle size of the filter paper is, for example, 1 μm to 100 μm.
[0059] Next, the solid reaction product separated by filtration is added to the first solvent and stirred for several minutes to several hours. As before, the reaction product precipitates in the first solvent, forming a precipitate. The precipitated solid reaction product in the solvent is separated from the solvent by filtration. This process, which includes reprecipitation of the reaction product in the first solvent and separation of the solid reaction product by filtration, may be repeated once or twice or more times. This is expected to wash the reaction product, remove unwanted compounds and impurities, and promote the purification of the desired compound. The above-mentioned precipitation of the reaction product and separation of the reaction product by filtration are repeated a predetermined number of times, resulting in the final reaction product being obtained as a light-absorbing compound.
[0060] The light-absorbing compound thus obtained is added to an appropriate amount of the second solvent and stirred for several minutes to several hours. It is confirmed that the light-absorbing compound is uniformly dispersed. At this time, it is presumed that the phosphorus-containing compound used as the raw material plays a role in suppressing aggregation of the light-absorbing compound while improving its dispersibility. In this case, a second solvent having good solvent properties may be selected for the first solvent, which is a poor solvent.
[0061] In order to adjust the amount of the light-absorbing compound in the second solvent, a predetermined amount of the second solvent is removed by distillation. Distillation is preferably performed at or near the boiling point of the solvent to be removed, or at a temperature equal to or higher than the boiling point. On the other hand, distillation at a temperature exceeding 100°C, for example, may have a thermal effect on the light-absorbing compound. Therefore, in order to adjust the amount of the light-absorbing compound in the solvent, it is preferable to perform distillation to remove the solvent at a temperature of 100°C or lower. On the other hand, if the boiling point of the selected second solvent is, for example, above 100°C, distillation accompanied by reduced pressure (vacuum distillation) may be performed. For example, when toluene is used as the second solvent, the boiling point of toluene under atmospheric pressure is 111°C. However, by setting the pressure inside the distiller tank to, for example, 500 hPa or less (approximately 0.5 atmospheres or less), distillation at 100°C or less is possible. Since rapid solvent evaporation rapidly increases the concentration of the light-absorbing compound and makes it more likely for the light-absorbing compound to aggregate, caution is required when rapidly evaporating the solvent. In adjusting the dry mass of the light-absorbing composition, when distillation is performed under reduced pressure, the pressure may be preferably 350 hPa or less, more preferably 250 hPa or less. Conditions that suppress a sudden rise in temperature and bumping are important, and even if the pressure during vacuum distillation is lowered to lower the maximum temperature, a sudden change in conditions must be avoided. It is important to suppress a sudden change in state to a compound containing a phosphorus component and a copper component during purification. The heating temperature for obtaining the light-absorbing composition by vacuum distillation, when considered as the temperature of the bath (oil bath) used to heat it, is preferably 85 ° C or less, more preferably 65 ° C or less, and even more preferably 45 ° C or less.
[0062] In this way, a light-absorbing composition is obtained in which the ratio r1 is adjusted to 15% to 55%. The ratio r1 can be determined, for example, as follows: A liquid sample of the obtained light-absorbing composition is obtained and its mass M1 is measured. Next, the light-absorbing composition sample is heated in a heating oven to leave only the solid content. The mass m1 of the remaining solid content is measured. The value m1 / M1 is calculated to identify the ratio r1 in the light-absorbing composition.
[0063] Furthermore, the acid concentration in the light-absorbing composition prepared in this manner is less than 0.2% by mass. The acid that can be contained in the light-absorbing composition is acetic acid if the copper salt in (a) contains copper acetate, or benzoic acid if the copper salt is copper benzoate, and is a component contained in the copper component supply compound. If the acid concentration in the light-absorbing composition is 0.2% by mass or higher, aggregation and discoloration due to aggregation and redispersion occur, making it impossible to increase the amount of light-absorbing compound that can be contained in the optical film. This necessitates an increase in the film thickness to achieve a certain level of absorption, which hinders low profile when incorporated into an imaging device or the like. The acid concentration in the light-absorbing composition is preferably 0.18% by mass or less, more preferably 0.15% by mass or less. The acid concentration in the light-absorbing composition can be measured, for example, by capillary electrophoresis.
[0064] In addition to additives capable of exerting other functions, resins may be added to the light-absorbing composition as appropriate during its preparation. As described below, the light-absorbing composition is used as a raw material for a composition for a light-absorbing film, and therefore may contain a predetermined amount of resin components intended to be contained in the composition for a light-absorbing film. Additives include, but are not limited to, the aforementioned ultraviolet-absorbing compounds, plasticizers, fine particles, leveling agents, and release promoters. The addition of a release promoter is effective, for example, when a film-shaped light absorber is prepared using the light-absorbing composition by a solution casting method. Note that these additives may be added in the subsequent process of preparing the composition for a light-absorbing film.
[0065] When a resin component is added to the light-absorbing composition, if the resin component is a solid such as granules, powder, or pellets, the resin component is desirably dissolved in the second solvent. A solvent capable of dissolving the resin component may be selected as the second solvent. The resin component may be added before adding the light-absorbing compound or a liquid containing the light-absorbing compound to the second solvent.
[0066] The composition for a light-absorbing film according to the present invention contains a light-absorbing compound, a solvent, and a resin. The light-absorbing compound can absorb light of a specific wavelength. The solvent disperses or dissolves the light-absorbing compound in the light-absorbing composition. The light-absorbing compound contains phosphorus and copper. The ratio r2 of the dry mass of the composition for a light-absorbing film to the mass of the composition for a light-absorbing film is 10% to 55%. The dry mass of the composition for a light-absorbing film is the mass of the residue remaining after removing liquid components such as the solvent from the composition for a light-absorbing film by evaporation, for example, by heating. The mass of the composition for a light-absorbing film is the mass of the composition for a light-absorbing film provided as a product before the solvent is removed.
[0067] The light-absorbing film composition is, for example, applied to the surface of a support or the like. The light-absorbing film composition is a precursor to a light-absorbing film formed into a film by a known method. The light-absorbing film has the ability to absorb light of a specific wavelength, is self-supporting, and is a tradeable and circulative product such as a film having a small thickness relative to its main surface, or is formed on the surface of some other product with a small thickness relative to its main surface. The light-absorbing film may be a layer or coating formed on the surface of a support such as an electronic component, optical component, or substrate, or it may be self-supporting without a support or the like. The support has the function and role of supporting the light-absorbing film. The light-absorbing film composition is, for example, a liquid composition containing the above-mentioned light-absorbing composition or the above-mentioned light-absorbing composition subjected to a predetermined treatment (hereinafter simply referred to as the light-absorbing composition), a resin, and a solvent, and serves as a precursor for forming the light-absorbing film. Furthermore, the light-absorbing film may be referred to as a film when it has a thickness of less than 250 μm, or as a sheet when it has a thickness of 250 μm or more.
[0068] In the composition for a light-absorbing film, the resin is, for example, for encapsulating the light-absorbing compound contained in the light-absorbing composition. The solvent is, for example, for dissolving or dispersing the resin in the composition for a light-absorbing film. The description of the light-absorbing compound in the light-absorbing composition also applies to the light-absorbing compound contained in the composition for a light-absorbing film.
[0069] In coating a composition for a light-absorbing film and processing it into a film (hereinafter referred to as coating, etc.), the lower the viscosity of the composition for a light-absorbing film, the easier it is to spread the coating film. On the other hand, it is difficult to form a coating film with a predetermined thickness or more. Conversely, if the viscosity of the composition for a light-absorbing film is high, it is relatively easy to increase the film thickness, but problems may arise in the coating workability. In the composition for a light-absorbing film, since the ratio r2 is 10% to 55%, the composition for a light-absorbing film is likely to have the desired handling and flowability, and the coating workability is likely to be improved. The composition for a light-absorbing film may be referred to as a coating liquid based on its handling and the working manner for forming a light-absorbing film.
[0070] The composition for a light-absorbing film may contain an ultraviolet absorbing compound, a light stabilizer, a plasticizer, fine particles, a leveling agent, a silane coupling agent, or the like. The composition for a light-absorbing film may be used to prepare a light-absorbing film by a solution casting method. In this case, a substance having a function for improving peelability from the surface to be used for casting may be added to the composition for a light-absorbing film.
[0071] The resin contained in the light-absorbing film composition may contain a light-absorbing compound. This resin is not limited to a specific resin. The resin may be a thermosetting resin or a thermoplastic resin. Examples of thermosetting resins include epoxy resins (EP) and silicone resins. Examples of thermoplastic resins include acrylic resins (PMMA), polyamide resins (PA), polycarbonate resins (PC), polyethylene terephthalate resins (PET), cyclic polyolefin resins (cycloolefin resins) (COP), polyvinyl butyral resins (PVB), polyethersulfone resins (PES), and polyester resins. One or more of these resins may be mixed and used. An example of an epoxy resin is Epicron (registered trademark) manufactured by DIC Corporation. Examples of silicone resins include DOWSIL (registered trademark) manufactured by Nagase & Co., Ltd. and various silicone resins manufactured by Shin-Etsu Chemical Co., Ltd. Examples of acrylic resins are ACRYPET (registered trademark) manufactured by Mitsubishi Chemical Corporation and OZ-1000 and OZ-1100 manufactured by Resonac Corporation. Examples of cyclic olefin resins are ARTON (registered trademark) manufactured by JSR Corporation, ZEONOR (registered trademark) manufactured by Nippon Zeon Co., Ltd., and APEL (registered trademark) manufactured by Mitsui Chemicals, Inc. An example of PVB is MOBITAL (registered trademark) manufactured by Kuraray Co., Ltd. An example of polyester resins is the OKP series manufactured by Osaka Gas Chemicals Co., Ltd.
[0072] The content of the resin in the composition for a light-absorbing film is not limited to a specific value, and is, for example, 5% by mass to 60% by mass, and preferably 15% by mass to 50% by mass.
[0073] In the composition for a light-absorbing film, the solvent is, for example, a solvent suitable for dissolving a resin. In this case, for example, a granular, powdered, or pellet-shaped resin may be used in preparing the composition for a light-absorbing film. For example, when forming a light-absorbing film from the composition for a light-absorbing film by a solution casting method, drying is performed to remove the solvent after casting. For this reason, a solvent with a relatively low boiling point may be selected, for example, a solvent with a boiling point of 70°C or less may be selected. In this case, it is also important that the solvent has properties suitable for dissolving the resin. On the other hand, the solvent has a boiling point, for example, above 30°C. This makes it easy to avoid an increase in viscosity due to evaporation of the solvent during formulation or mixing, or a significant shortening of the pot life.
[0074] The amount of solvent in the composition for a light-absorbing film is not limited to a specific value, as long as the ratio r2 is 10% to 55%. In the composition for a light-absorbing film, the ratio of the solvent content to the resin content, on a mass basis, is, for example, 0.1 to 50, and preferably 0.3 to 20. Examples of low-boiling point solvents contained in the composition for a light-absorbing film include acetone (boiling point 56°C), chloroform (boiling point 61°C), dichloromethane (methylene chloride) (boiling point 40°C), diethyl ether (boiling point 35°C), ethyl formate (boiling point 52°C), hexane (boiling point 69°C), methanol (boiling point 65°C), methyl acetate (boiling point 57°C), pentane (boiling point 36°C), and tetrahydrofuran (boiling point 66°C). One or more of these solvents may be mixed and used.
[0075] The composition for a light-absorbing film may contain an ultraviolet-absorbing compound for absorbing a portion of ultraviolet light. By including the ultraviolet-absorbing compound in the composition for a light-absorbing film and further in the light-absorbing film, ultraviolet light that may deteriorate the resin and the light-absorbing compound or have undesirable effects on electronic devices, etc. The ultraviolet-absorbing compound is not limited to a specific compound as long as the light-absorbing film has a desired transmission spectrum.
[0076] The ultraviolet absorbing compound is preferably selected from the viewpoints of absorbing light in a desired wavelength range, being compatible with a specific solvent, dispersing well in the composition for a light-absorbing film, and having excellent environmental resistance. Examples of ultraviolet absorbing compounds include benzophenone-based compounds, benzotriazole-based compounds, salicylic acid-based compounds, and triazine-based compounds, and one or more compounds may be mixed and contained in the composition for a light-absorbing film. Examples of ultraviolet absorbers include Tinuvin PS, Tinuvin 99-2, Tinuvin 234, Tinuvin 326, Tinuvin 329, Tinuvin 900, Tinuvin 928, Tinuvin 405, and Tinuvin 460. These are ultraviolet absorbing compounds manufactured by BASF, and Tinuvin is a registered trademark.
[0077] The content of the ultraviolet absorber in the composition for a light-absorbing film is not limited to a specific value. The ratio of the content of the ultraviolet absorber to the content of the resin in the composition for a light-absorbing film is, for example, 0.00001 to 0.2, and preferably 0.0001 to 0.05, on a mass basis.
[0078] The composition for a light-absorbing film may contain, for example, a light stabilizer. In this case, deterioration of the resin or light-absorbing compound due to the action of light, including ultraviolet light, when forming the light-absorbing film can be suppressed. The above-mentioned ultraviolet-absorbing compound may also function as a light stabilizer. An example of a light stabilizer is a hindered amine light stabilizer (HALS). The ratio of the content of the light stabilizer to the content of the resin in the composition for a light-absorbing film is, for example, 0.00001 to 0.2, and preferably 0.0001 to 0.05, on a mass basis. As the hindered amine light stabilizer, for example, the Adeka STAB series manufactured by Adeka Corporation may be selected, or multiple types of light stabilizers may be mixed and used.
[0079] The composition for a light-absorbing film may contain a silane coupling agent. Silane coupling agents are generally included in various compositions to strengthen the bond between organic materials and inorganic materials. For example, when a light-absorbing film is formed on an inorganic support such as glass after casting the composition for a light-absorbing film, the silane coupling agent can strengthen the bond between the organic resin component contained in the light-absorbing film and the support, thereby improving peel resistance. In addition, the silane coupling agent can strengthen the bond between the inorganic light-absorbing compound contained in the composition for a light-absorbing film and the resin component, thereby improving weather resistance, etc.
[0080] Examples of the silane coupling agent include alkoxysilane monomers or hydrolyzates thereof. Examples of the silane coupling agent include tetramethoxysilane, tetraethoxysilane, methyltrimethoxysilane, methyltriethoxysilane, dimethyldiethoxysilane, dimethyldimethoxysilane, phenyltrimethoxysilane, phenyltriethoxysilane, 3-glycidoxypropyltrimethoxysilane, 3-glycidoxypropyltriethoxysilane, and 3-glycidoxypropylmethyldiethoxysilane. The silane coupling agent may be an aminosilane-based compound. Examples of the aminosilane-based compound include 3-aminopropyltriethoxysilane, N-2-(aminoethyl)-3-aminopropyltrimethoxysilane, N-2-(aminoethyl)-N'-2-(aminoethyl)-3-aminopropyltriethoxysilane, and 3-anilinopropyltrimethoxysilane. The silane coupling agent may be a vinylsilane-based compound. Examples of vinylsilane compounds are vinyltrimethoxysilane and N-2-(N-vinylbenzylaminoethyl)-3-aminopropyltrimethoxysilane. The silane coupling agent may be other silane compounds. Examples of other silane compounds are 3-methacryloxypropyltrimethoxysilane, 3-chloropropyltrimethoxysilane, and 3-mercaptopropyltrimethoxysilane. The light-absorbing film composition may contain one or more silane coupling agents selected from these, depending on the type of resin contained therein.
[0081] The ratio of the content of the silane coupling agent to the content of the resin in the composition for a light-absorbing film is, for example, 0.01 to 0.2, and preferably 0.02 to 0.1, on a mass basis.
[0082] The composition for a light-absorbing film can be used to provide, for example, a light-absorbing film 10. As shown in Fig. 1A, the light-absorbing film 10 may be, for example, a self-supporting film. In this case, an optical filter 1a including only the light-absorbing film 10 can be provided.
[0083] The light-absorbing film 10 contains a light-absorbing compound having phosphorus and copper, and a resin. The above description of the light-absorbing compound in the light-absorbing composition or the composition for a light-absorbing film also applies to the light-absorbing compound contained in the light-absorbing film 10. The description of the resin in the composition for a light-absorbing film also applies to the resin contained in the light-absorbing film 10.
[0084] The light-absorbing film 10 has a thickness of 300 μm or less. In addition, when light having a wavelength of 300 nm to 1200 nm is incident on the light-absorbing film 10 at an incident angle of 0°, the light-absorbing film 10 exhibits a transmission spectrum having the following characteristics (I) to (IV): (I) The average transmittance within the wavelength range of 800 nm to 1100 nm is 20% or less. (II) The average transmittance within the wavelength range of 460 nm to 580 nm is 80% or more. (III) The first cutoff wavelength at which the transmittance is 50% within the wavelength range of 300 nm to 400 nm is in the wavelength range of 320 nm to 400 nm. (IV) The second cutoff wavelength at which the transmittance is 50% within the wavelength range of 600 nm to 800 nm is in the wavelength range of 650 nm to 750 nm.
[0085] For example, when the light-absorbing film 10 is mounted inside an imaging device, it is advantageous for the light-absorbing film 10 to have a thickness of 300 μm or less in terms of reducing the height of the imaging device or its camera module. The thickness of the light-absorbing film 10 is preferably 70 μm to 280 μm, and more preferably 80 μm to 250 μm. In this case, it is possible to avoid a significant decrease in the rigidity and mechanical strength of the light-absorbing film 10, and the light-absorbing film 10 is easy to handle.
[0086] From the above (I), the light-absorbing film 10 can exhibit sufficient infrared shielding properties. This can improve the match between the light reaching the imaging element and the visual sensitivity of humans, who generally do not perceive light in the infrared region. In the light-absorbing film 10, the average transmittance within the wavelength range of 800 nm to 1100 nm is preferably 15% or less, more preferably 10% or less. When attempting to further reduce the transmittance within the wavelength range of 800 nm to 1100 nm, for example, the light-absorbing film may contain other light-absorbing compounds in addition to the light-absorbing compound containing a phosphonic acid, a phosphate ester, and a copper component. Examples of other light-absorbing compounds include organic dyes, pigments, M 1 / n Cu m P.O. 4-z compounds having the composition: metal oxides such as ITO and ATO, and compounds containing tungsten oxide. 1 / n Cu m P.O. 4-z In the composition, M is a metal element other than Cu, n and m are natural numbers, and z is a positive integer less than 4. One or more light-absorbing compounds from these may be contained in the light-absorbing film 10. Alternatively, two or more light-absorbing compounds containing a phosphonic acid, a phosphate ester, and a copper component may be contained in the same light-absorbing film 10. The light-absorbing compound may be contained in advance in the light-absorbing composition or a composition for a light-absorbing film. As another means for attempting to further reduce the transmittance in the wavelength range of 800 nm to 1100 nm, a laminate may be formed including a light-absorbing film 10 containing a phosphonic acid, a phosphate ester, and a copper component and another light-absorbing film containing the other light-absorbing compound.
[0087] From the above (II), the luminous flux of light belonging to the visible light range that passes through the light absorbing film 10 and reaches the imaging element becomes large, which is advantageous from the viewpoint of forming a brighter image.
[0088] From the above (III), the light-absorbing film 10 can improve the blocking ability of light in the ultraviolet range. This can improve the match between the light reaching the imaging element and the visual sensitivity of humans, who generally do not perceive light in the ultraviolet range. This can reduce the possibility of color bleeding such as purple fringing occurring due to the inclusion of light with short wavelengths in the light reaching the imaging element.
[0089] From the above (IV), the ability to block light in the infrared region can be improved by using the light-absorbing film 10. This makes it possible to improve the match between the light reaching the imaging element and the visual sensitivity of humans, who generally do not perceive light in the infrared region.
[0090] In the above transmission spectrum of the light-absorbing film 10, the transmittance at a wavelength of 430 nm may be 80% or more, which is more advantageous from the viewpoint of forming a brighter image.
[0091] The transmission spectrum of the light-absorbing film 10 may have at least one characteristic selected from the group consisting of the following (V) to (IX): (V) The transmittance at a wavelength of 800 nm is 3% or less. (VI) The transmittance at a wavelength of 900 nm is 1.5% or less. (VII) The transmittance at a wavelength of 950 nm is 0.5% or less. (VIII) The transmittance at a wavelength of 1000 nm is 0.5% or less. (IX) The transmittance at a wavelength of 1100 nm is 0.5% or less.
[0092] As shown in Fig. 1B, an optical filter 1b including a light-absorbing film 10 may be provided. The optical filter 1b includes a support 20 in addition to the light-absorbing film 10. The support 20 supports the light-absorbing film 10. For example, the light-absorbing film 10 is obtained by applying the above-mentioned composition for a light-absorbing film to the support 20. The support 20 is not limited to a specific support as long as the optical filter 1b has the desired performance. Furthermore, the shape of the support 20 is not limited to a specific shape.
[0093] From the viewpoint of facilitating application of the light-absorbing film composition and ensuring the versatility of the optical filter, the support 20 may be in the form of a parallel plate, as shown in FIG. 1B . The support 20 may include a curved surface or a convex or concave surface. The support 20 does not have to be plate-shaped. The support 20 may have an optical function. Examples of supports having an optical function include optical elements such as lenses, polarizers, prisms, reflective elements, and diffraction gratings. These optical elements may include surfaces having both curved and flat surfaces. Further examples of the support 20 may include photoelectric conversion elements such as photodiodes and phototransistors. The support 20 may also be an image sensor in which a large number of photoelectric conversion elements, such as CCDs and CMOSs, are arranged, or an image sensor equivalent to such an image sensor. In some cases, the light-absorbing film 10 may be formed directly on the light-receiving surface or window glass of such an image sensor. Another example of the support 20 is a display device such as a display of a portable terminal or the like.
[0094] The support 20 may be transparent. When the support 20 is transparent, the transmission spectrum of the light-absorbing film is likely to be reflected in the transmission spectrum of the optical filter 1b. When the support 20 is transparent, in the transmission spectrum of a parallel plate made of the same material as the material constituting the support 20 and having a thickness of 3 mm, the transmittance may be 90% or more in the wavelength range of 360 nm to 900 nm, and 85% or more in the wavelength range of 350 nm to 1200 nm.
[0095] An example of such a transparent support 20 is a glass support. In this case, examples of glass include transparent glass made of silicate glass such as soda-lime glass and borosilicate glass, and phosphate glass and fluorophosphate glass containing coloring components such as Cu and Co. Phosphate glass and fluorophosphate glass containing coloring components are, for example, infrared-absorbing glass, and are themselves light-absorbing. When a light-absorbing film is used together with an infrared-absorbing glass support, the light absorption and transmission spectra of both can be adjusted to produce an optical filter with desired optical characteristics, allowing for a high degree of freedom in designing the optical filter.
[0096] The support 20 may be made of a resin. In this case, examples of the resin include cyclic olefin resins, acrylic resins, polyimide resins, polyetherimide resins, polysulfone resins, polyethersulfone resins, polycarbonate resins, and silicone resins. Resins are significantly more processable and moldable than glass. Therefore, supports of various shapes for optical elements and the like can be easily produced from resin.
[0097] The support 20 may be a light-absorbing support. The light-absorbing support itself has the function of absorbing part of light of a specific wavelength, and supports the light-absorbing film 10. The light-absorbing support may be a support made of the above-mentioned colored glass containing a coloring component such as Cu or Co, or may be a support made of a resin containing a dye, pigment, or coloring material.
[0098] As shown in FIG. 1C , an optical filter 1c may be provided, including a light-absorbing film 10 and an anti-reflection film 30. The anti-reflection film 30 is provided on the surface of the light-absorbing film 10 and prevents or reduces Fresnel reflection at the interface between the light-absorbing film 10 and air. The anti-reflection film 30 may be a single-layer or multi-layer dielectric film. In this case, the dielectric is not limited to a specific dielectric. Examples of dielectrics include metal compounds such as MgF, SiO , TiO , and Ta O . The anti-reflection film 30 may be formed by stacking one or more dielectrics selected from these. Examples of methods for manufacturing the anti-reflection film 30 include vapor deposition and sputtering. Another example of a method for manufacturing the anti-reflection film 30 is the sol-gel method. According to the sol-gel method, a metal oxide (organic-inorganic compound) film containing organic groups is formed by hydrolysis and condensation polymerization of a metal alkoxide. For example, a liquid alkoxide containing Si is hydrolyzed in the presence of water on the surface of the target article or light-absorbing film, followed by condensation polymerization and solidification. This allows the preparation of a film that can be anti-reflection or reflection-reducing while adjusting the film thickness.Si-containing alkoxides are inexpensive, and the hydrolysis and polycondensation reactions are easily controlled, making it easy to obtain a film with a relatively low refractive index.Furthermore, when the film obtained by the sol-gel method is required to have further anti-reflection or reflection-reducing performance, it is advantageous to include hollow particles such as hollow silica in the alkoxide, which can further reduce the refractive index of the film.
[0099] As shown in FIG. 1D, an optical filter 1d may be provided that includes a light-absorbing film 10, a support 20, and an anti-reflection film 30.
[0100] As shown in FIG. 1E, an optical filter 1e may be provided that includes a light-absorbing film 10 (first light-absorbing film) and a second light-absorbing film 12. The second light-absorbing film 12 may be disposed for the purpose of improving light absorption, for example, adjusting the blocked wavelength band and reducing transmittance. The second light-absorbing film 12 includes, for example, a second light-absorbing compound and a resin component. The second light-absorbing compound is a compound that can absorb light in a wavelength range different from the wavelength range of light absorbed by the light-absorbing compound contained in the light-absorbing film 10. For example, the absorption maximum wavelength of the second light-absorbing compound is different from the absorption maximum wavelength of the light-absorbing compound contained in the light-absorbing film 10. The second light-absorbing compound may be a light-absorbing compound that includes a phosphorus- and oxygen-containing compound of a type different from the phosphorus- and oxygen-containing compound of the light-absorbing compound contained in the light-absorbing film 10, and a copper component. The second light-absorbing compound may include, for example, a phosphonic acid containing an aryl group, a copper component, a polyoxyalkyl ether phosphate ester, or a reaction product thereof. In this case, the second cutoff wavelength can be easily shortened, and depending on the application of the optical filter, desired transmission characteristics can be imparted to the optical filter.
[0101] The second light-absorbing compound is M 1 / n Cu m P.O. 4-z compounds containing sulfonic acid and a copper component; compounds containing tungsten oxide; and metal oxides such as ITO and ATO.
[0102] 1F , an optical filter 1f may be provided, which includes a light-absorbing film 10, a second light-absorbing film 12, and an intermediate layer 40. The intermediate layer 40 is a layer for physically separating the light-absorbing film 10 from the second light-absorbing film 12, and may be provided particularly for preventing interaction between the light-absorbing film 10 and the second light-absorbing film 12. The intermediate layer 40 may contain, for example, a dielectric such as a metal compound listed as a material for the anti-reflection film 30 above, or may contain a metal oxide (organic-inorganic compound) containing an organic group formed by a sol-gel method.
[0103] The light-absorbing film 10 is formed using, for example, the above-mentioned composition for a light-absorbing film. The method for producing the light-absorbing film 10 is not limited to a specific method as long as it is possible to form a film that can block a portion of light in a specific wavelength range. When producing the light-absorbing film 10 on a support 20, examples of methods for attaching (applying) the composition for a light-absorbing film to the support 20 include a dipping method, a casting method, a spray method, a spin coating method, an inkjet method, and a slit die coating method. The method for producing the light-absorbing film 10 may be appropriately determined taking into consideration the specifications, performance, mass productivity, yield, etc. of the light-absorbing film 10.
[0104] The spin coating method involves dropping a composition for a light-absorbing film onto the support 20 while rotating the support 20 with a spindle or the like, and spreading and adhering the composition for a light-absorbing film in a direction from the center of the spindle outward. The spin coating method allows precise control of film thickness by adjusting the spin coating conditions. This method is also suitable when a component or the like of a limited size is used as the support 20, or when a light-absorbing film 10 is formed on an uneven surface such as a convex or concave surface.
[0105] The casting method is a method in which a liquid composition for a light-absorbing film is dropped or extruded onto a support 20 to spread the composition for a light-absorbing film and form a coating film having a desired thickness, and is also called a solution casting method. Dropping of the composition for a light-absorbing film onto the support 20 may be performed using, but is not limited to, a dispenser or a slot die. The support 20 to which the casting method can be applied is a support having a smooth surface. The casting method can be applied to small-sized supports that are prepared on a desk and relatively large-sized supports.
[0106] When an optical filter consisting only of the light-absorbing film 10 is produced, examples of methods for producing the light-absorbing film 10 include a casting method, an extrusion molding method, and a calendaring method. Among these, a casting method may be used from the viewpoints of smoothness, low haze, and mass productivity required for optical components, as well as the thermal properties of the light-absorbing compound contained in the light-absorbing film composition. According to the casting method, for example, a light-absorbing film composition is thinly cast onto the main surface of a smooth glass plate, metal belt, or metal plate by dropping or extruding it using a dispenser or die, and the cast product is dried or reacted to obtain a solidified product. The solidified product is then peeled off from the glass plate, metal belt, or metal plate to obtain a self-supporting light-absorbing film 10.
[0107] The casting method is similar to the desktop production of the light-absorbing film 10 and can be used to produce small-sized light-absorbing films 10 for research, experiments, and prototyping, as well as relatively large-sized films requiring high mass productivity. In a production method suitable for small-scale production, for example, a glass plate with a smooth main surface is used as a temporary support, and a composition for a light-absorbing film is cast onto the glass plate to a predetermined thickness. Thereafter, a portion of the solvent contained in the composition for a light-absorbing film is evaporated, and the curable resin is reacted to dry the cast composition for a light-absorbing film, thereby obtaining a solidified product. The solidified product is then peeled off to obtain a self-supporting light-absorbing film 10. The peeled solidified product may be subjected to a post-cure treatment. It is also possible to apply an agent, such as a surface treatment agent containing a fluorine compound, that promotes peeling of the solidified product to the main surface of the glass plate that serves as the temporary support, to facilitate peeling of the solidified product. Furthermore, when preparing a light-absorbing film 10 of a predetermined thickness, for example, a frame of any shape may be placed on the surface of a temporary support, and a predetermined amount of a composition for a light-absorbing film may be dropped and cast inside the frame to adjust the thickness of the coating film.
[0108] A method suitable for mass production is a method for continuously producing a large-area light-absorbing film 10. For example, a light-absorbing film composition is applied and cast using a slit die or the like onto a smooth, endless metal belt that is continuously moved by multiple rollers. A portion of the solvent contained in the light-absorbing film composition is evaporated on the belt, causing the curable resin to react, thereby drying the cast light-absorbing film composition and obtaining a solidified product. The dried solidified product is then peeled from the belt, and passed through, for example, an oven to nearly completely evaporate the solvent or promote the reaction, thereby performing post-cure. The film-like solidified product is then continuously transported, and if necessary, stretched using multiple rollers. The light-absorbing film 10 may then be wound up using a winding roller to obtain a roll of the light-absorbing film 10.
[0109] When the light-absorbing film 10 is produced by the casting method, the resin content in the composition for a light-absorbing film is, for example, 10% by mass to 35% by mass. In this case, even when a thin light-absorbing film 10 is required, the viscosity of the composition for a light-absorbing film supplied from the slot die can be easily adjusted to the desired range, and the casting state is likely to be good. In addition, a decrease in the castability of the composition for a light-absorbing film can be avoided, and the variation in the thickness of the light-absorbing film 10 is likely to be small. The resin content in the composition for a light-absorbing film is desirably 15% by mass to 30% by mass.
[0110] The present invention will be described in more detail below using examples, but the present invention is not limited to the following examples.
[0111] Example 1: 4.88 g of copper acetate monohydrate (Kanto Chemical Co., Ltd.) and 195.12 g of ethanol (Kanto Chemical Co., Ltd., EL grade for electronics industry) were mixed and stirred for 3 hours to obtain a copper acetate solution. Next, 2.572 g of a phosphate ester compound (Dai-ichi Kogyo Seiyaku Co., Ltd., product name: Plysurf A208N) was added to the resulting copper acetate solution and stirred for 30 minutes to obtain a copper acetate-phosphate ester solution, Solution A1. Next, 2.886 g of n-butylphosphonic acid and 40 g of ethanol were added and stirred for 10 minutes to obtain a phosphonic acid solution, Solution B1. Furthermore, while stirring Solution A1, Solution B1 was added to Solution A1, and the mixture was stirred at room temperature for 15 minutes to allow the reaction to proceed, obtaining Solution C1, a phosphate ester-phosphonic acid-copper solution. A solid precipitate, believed to have formed as a result of the reaction, was visually observed in Solution C1. The reaction product is believed to be a compound containing phosphonic acid, phosphate ester, and some or all of the copper component.
[0112] The C1 solution was subjected to suction filtration to obtain a solid reaction product. The solid reaction product was added to 200 g of ethanol and stirred at room temperature for 10 minutes. Suction filtration was then performed again to obtain a solid reaction product that had been purified once. This solid reaction product was then added to 80 g of toluene and stirred at room temperature for 10 minutes to obtain the D1 solution. In the D1 solution, the solid reaction product was not visible, and the reaction product was dispersed. Therefore, the solid reaction product also contained a certain amount of phosphate ester, which has a dispersing effect, and it is believed that the phosphate ester contributes to the dispersion of the reaction product in toluene.
[0113] Solution D1 was placed in a flask and heated in an oil bath (manufactured by Tokyo Rikakikai Co., Ltd., model: OSB-2100) set to 85°C, while a solvent removal treatment was carried out using a rotary evaporator (manufactured by Tokyo Rikakikai Co., Ltd., model: N-1110SF). During this treatment, the interior of the flask was depressurized using a vacuum pump, and the pressure was reduced stepwise from atmospheric pressure to a predetermined pressure, taking care to prevent bumping. After confirming that the solvent had been reduced to a certain amount, the process was terminated, and solution E1 was obtained. Ultimately, 39.71 g of light-absorbing composition E1 was obtained. In light-absorbing composition E1, a reaction product containing phosphonic acid, phosphate ester, and some or all of the copper component was dispersed, and it was confirmed that the appearance of light-absorbing composition E1 was transparent green. In the appearance color column of Table 2, "A" indicates that the appearance was transparent green, and "X" indicates that the appearance was not transparent green.
[0114] In the preparation of light-absorbing composition E1, the use of copper acetate monohydrate as a copper component source is thought to have produced acetic acid as a by-product along with the production of reaction products (particularly copper phosphonate compounds). However, the characteristic odor of acetic acid was not detected from light-absorbing composition E1, suggesting that acetic acid had been sufficiently removed. This is thought to be the result of the effective functioning of the precipitation of the reaction product by the action of a poor solvent such as ethanol, the purification or washing process by filtration, and the solvent removal process by distillation. In the preparation of light-absorbing composition E1, ethanol was the first solvent and toluene was the second solvent.
[0115] (Calculation of dry mass ratio) 10 g (= M1) of the light-absorbing composition E1 liquid was accurately measured and placed in an aluminum petri dish, and the petri dish was then placed on a hot plate with a surface temperature set to 180°C. The dish was left standing for approximately 10 minutes, and it was confirmed that the liquid components in the petri dish had almost completely evaporated. The mass of the petri dish containing the dried light-absorbing composition was measured, and the dry mass m1 of the light-absorbing composition was calculated by subtracting the mass of the petri dish from the measured value. m1 / M1 was calculated as the dry mass ratio. The dry mass ratio of the light-absorbing composition E1 according to Example 1 was 15.1 mass%.
[0116] (Evaluation of redispersibility) In order to confirm whether the reaction product contained in the light-absorbing composition E1 has redispersibility, the amount of solvent was adjusted so that the light-absorbing composition E1 was 10 mass% dry mass ratio with the same solvent as the solvent used for distillation, and the redispersion of the reaction product was attempted.As a result, the reaction product was redispersed, and the light-absorbing composition had a green, highly transparent appearance, and was in a good state without opaque turbidity, that is, it was confirmed that the redispersibility was good.In the redispersibility section of Table 2, "A" indicates that the redispersibility was good, and "X" indicates that the redispersibility was not good.
[0117] (Measurement of Residual Acetic Acid Concentration in Light-Absorbing Composition) A small amount of sample was obtained from the light-absorbing composition E1 according to Example 1, and an appropriate amount of toluene was added so that the dry mass ratio was 10% by mass to prepare a sample for measuring the residual acetic acid concentration. Next, an appropriate amount of pure water was added to the sample for measuring the residual acetic acid concentration to perform solution extraction, and the aqueous layer was collected to prepare a measurement sample for capillary electrophoresis (CE). Using a CE device (manufactured by Agilent Technologies, product name: Agilent1600), capillary electrophoresis was performed on the measurement sample for CE by indirect absorption. Here, a 2,6-pyridinedicarboxylic acid-based electrophoresis solution (pH = 12) was used as the electrophoresis solution, and a capillary made of fused silica was used. From this measurement, the content of acetic acid remaining in the light-absorbing composition E1 according to Example 1 was determined to be 0.08% by mass.
[0118] (Measurement of Transmission Spectrum of Light-Absorbing Composition) The light-absorbing composition E1 according to Example 1 was placed in a quartz cell (manufactured by Starna Scientific, model number: 20 / C / Q1, optical path length: 1 mm, optical path width: 10 mm, external dimensions: length 3.5 mm, width 12.5 mm, height 45 mm, capacity: 0.31 ml), and the transmittance for each wavelength in the wavelength range of 300 nm to 1200 nm at an incident angle of 0° was measured using an ultraviolet-visible-near-infrared spectrophotometer (manufactured by JASCO Corporation, model number: V770). Note that the sample for measuring the transmission spectrum was prepared by several trial-and-error experiments, by adding an appropriate amount of toluene as a solvent to adjust the concentration of the light-absorbing composition so that the transmittance at a wavelength of 800 nm was 10%±1%. The transmission spectrum of the light-absorbing composition according to Example 1 is shown in FIG. 2. Furthermore, parameters at specific wavelengths or wavelength ranges that can be observed from the transmission spectrum are shown in Table 3.
[0119] Example 2 Using the following compounds as raw materials, 36.67 g of light-absorbing composition E2 according to Example 2, with a dry mass ratio of 17.0 mass%, was prepared under the same conditions and by the same method as in Example 1. The appearance and redispersibility of light-absorbing composition E2 according to Example 2, evaluated under the same conditions and by the same method as in Example 1, were both good. [Raw materials] First solvent: methanol Copper acetate monohydrate 4.88 g Phosphonic acid: butylphosphonic acid 2.835 g Phosphate ester: Plysurf A208N 2.829 g Second solvent: toluene 80 g [Purification (reduced pressure distillation) conditions] Oil bath temperature 85°C / pressure 600 hPa or less
[0120] Example 3 Using the following compounds as raw materials, 21.50 g of light-absorbing composition E3 according to Example 3, with a dry mass ratio of 29.2 mass%, was prepared under the same conditions and by the same method as in Example 1. The appearance and redispersibility of light-absorbing composition E3 according to Example 3, evaluated under the same conditions and by the same method as in Example 1, were both good. The acetic acid concentration of light-absorbing composition E3 according to Example 3, measured under the same conditions and by the same method as in Example 1, was 0.11 mass%. [Raw materials] First solvent: methanol Copper acetate monohydrate 4.88 g Phosphonic acid: butylphosphonic acid 2.780 g Phosphate ester: Plysurf A208F 3.086 g Second solvent: toluene 60 g [Purification (reduced pressure distillation) conditions] Oil bath temperature 85°C / pressure 600 hPa or less
[0121] Example 4 Using the following compounds as raw materials, 23.31 g of light-absorbing composition E4 according to Example 4, with a dry mass ratio of 28.9 mass%, was prepared under the same conditions and by the same method as in Example 1. The appearance and redispersibility of light-absorbing composition E4 according to Example 4, evaluated under the same conditions and by the same method as in Example 1, were both good. [Raw materials] First solvent: ethanol Copper acetate monohydrate 4.88 g Phosphonic acid: butylphosphonic acid 3.284 g Phosphate ester: NIKKOL DDP2 manufactured by Nikko Chemicals 3.088 g Second solvent: toluene 60 g [Purification (reduced pressure distillation) conditions] Oil bath temperature 85°C / pressure 600 hPa or less
[0122] The transmission spectrum of light-absorbing composition E4 according to Example 4 was measured under the same conditions and by the same method as in Example 1. The transmission spectrum of light-absorbing composition E4 according to Example 4 is shown in Figure 3. Specific parameters that can be seen from the transmission spectrum are shown in Table 3.
[0123] Example 5 Using the following compounds as raw materials, 22.56 g of light-absorbing composition E5 according to Example 5, with a dry mass ratio of 29.5 mass%, was prepared under the same conditions and by the same method as in Example 1. Furthermore, the appearance and redispersibility of light-absorbing composition E5 according to Example 5, evaluated under the same conditions and by the same method as in Example 1, were both good. [Raw materials] First solvent: methanol Copper acetate monohydrate 4.88 g Phosphonic acid: butylphosphonic acid 3.334 g Phosphate ester: NIKKOL DDP2 2.984 g Second solvent: toluene 60 g [Purification (reduced pressure distillation) conditions] Oil bath temperature 85°C / pressure 600 hPa or less
[0124] Example 6 Using the following compounds as raw materials, 18.86 g of light-absorbing composition E6 according to Example 6, with a dry mass ratio of 27.9 mass%, was prepared under the same conditions and by the same method as in Example 1. The appearance and redispersibility of light-absorbing composition E6 according to Example 6, evaluated under the same conditions and by the same method as in Example 1, were both good. [Raw materials] First solvent: ethanol Copper acetate monohydrate 4.88 g Phosphonic acid: methylphosphonic acid 2.019 g Phosphate ester: Plysurf A208N 2.572 g Second solvent: toluene 60 g [Purification (reduced pressure distillation) conditions] Oil bath temperature 85°C / pressure 600 hPa or less
[0125] Example 7 Using the following compounds as raw materials, 19.23 g of light-absorbing composition E7 according to Example 7, with a dry mass ratio of 29.4 mass%, was prepared under the same conditions and by the same method as in Example 1. The appearance and redispersibility of light-absorbing composition E7 according to Example 7, evaluated under the same conditions and by the same method as in Example 1, were both good. [Raw materials] First solvent: ethanol Copper acetate monohydrate 4.88 g Phosphonic acid: ethylphosphonic acid 2.259 g Phosphate ester: Plysurf A208N 2.829 g Second solvent: toluene 60 g [Purification (reduced pressure distillation) conditions] Oil bath temperature 85°C / pressure 600 hPa or less
[0126] Example 8 Using the following compounds as raw materials, 13.78 g of light-absorbing composition E8 according to Example 8, with a dry mass ratio of 45.3 mass%, was prepared under the same conditions and method as in Example 1. The appearance and redispersibility of light-absorbing composition E8 according to Example 8, evaluated under the same conditions and method as in Example 1, were both good. The acetic acid concentration of light-absorbing composition E8 according to Example 8, measured under the same conditions and method as in Example 1, was 0.10 mass%. [Raw materials] First solvent: ethanol Copper acetate monohydrate 4.88 g Phosphonic acid: butylphosphonic acid 2.977 g Phosphate ester: Plysurf A208N 2.829 g Second solvent: toluene 60 g [Purification (reduced pressure distillation) conditions] Oil bath temperature 85°C / pressure 350 hPa or less
[0127] Example 9 Using the following compounds as raw materials, 11.94 g of light-absorbing composition E9 according to Example 9, with a dry mass ratio of 50.3 mass%, was prepared under the same conditions and method as in Example 1. Furthermore, under the same conditions and method as in Example 1, the appearance and redispersibility of light-absorbing composition E9 according to Example 9 were both good. [Raw materials] First solvent: ethanol Copper acetate monohydrate 4.88 g Phosphonic acid: butylphosphonic acid 2.886 g Phosphate ester: Plysurf A208N 2.572 g Second solvent: toluene 60 g [Purification (reduced pressure distillation) conditions] Oil bath temperature 60°C / pressure 250 hPa or less
[0128] The transmission spectrum of light-absorbing composition E9 according to Example 9 was measured under the same conditions and by the same method as in Example 1. The transmission spectrum of light-absorbing composition E9 according to Example 9 is shown in Figure 4. In addition, specific parameters that can be seen from the transmission spectrum are shown in Table 3.
[0129] Example 10 Using the following compounds as raw materials, 13.45 g of light-absorbing composition E10 according to Example 10, with a dry mass ratio of 49.4 mass%, was prepared under the same conditions and method as in Example 1. Furthermore, under the same conditions and method as in Example 1, the appearance and redispersibility of light-absorbing composition E10 according to Example 10 were both good. [Raw materials] First solvent: methanol Copper acetate monohydrate 4.88 g Phosphonic acid: butylphosphonic acid 3.214 g Phosphate ester: NIKKOL DDP2 3.008 g Second solvent: toluene 60 g [Purification (reduced pressure distillation) conditions] Oil bath temperature 60°C / pressure 250 hPa or less
[0130] Example 11: 4.88 g of copper acetate monohydrate (Kanto Chemical Co., Ltd.) and 195.12 g of ethanol (Kanto Chemical Co., Ltd., EL grade for electronics industry) were mixed and stirred for 3 hours to obtain a copper acetate solution. Next, 2.829 g of a phosphate ester compound (Dai-ichi Kogyo Seiyaku Co., Ltd., product name: Plysurf A208N) was added to the obtained copper acetate solution and stirred for 30 minutes to obtain a copper acetate-phosphate ester solution, Solution A11. Next, 2.977 g of n-butylphosphonic acid and 40 g of ethanol were added and stirred for 10 minutes to obtain a phosphonic acid solution, Solution B11. Furthermore, while stirring Solution A11, Solution B11 was added to Solution A11, and the mixture was allowed to react at room temperature for 15 minutes to obtain a phosphate ester-phosphonic acid-copper solution, Solution C11. In Solution C11, a solid precipitate believed to have formed as a result of the reaction was visually observed. The reaction product is believed to be a compound containing phosphonic acid, phosphate ester, and some or all of the copper component.
[0131] The C11 solution was subjected to suction filtration to obtain a solid reaction product. The solid reaction product was added to 200 g of ethanol and stirred at room temperature for 10 minutes. Suction filtration was then performed again to obtain a solid reaction product that had been purified once. This solid reaction product was then added to 140 g of methylene chloride and stirred at room temperature for 10 minutes to obtain the D11 solution. In the D11 solution, the solid reaction product was not visible, and the reaction product was dispersed. Therefore, the solid reaction product also contained a certain amount of phosphate ester, which has a dispersing effect, and it is believed that the phosphate ester contributes to the dispersion of the reaction product in the methylene chloride.
[0132] The D11 solution was placed in a flask and heated in an oil bath (manufactured by Tokyo Rikakikai Co., Ltd., model: OSB-2100) set at 45 ° C., and a solvent removal treatment was carried out using a rotary evaporator (manufactured by Tokyo Rikakikai Co., Ltd., model: N-1110SF). At that time, the inside of the flask was reduced to 600 hPa or less using a vacuum pump, and the pressure was reduced stepwise from atmospheric pressure to a predetermined pressure, taking care to prevent bumping. Thereafter, the operation was terminated after confirming that the solvent had decreased to a certain amount, and 38.18 g of light-absorbing composition E11 according to Example 11 was obtained. In the preparation of light-absorbing composition E11, ethanol was the first solvent, and methylene chloride was the second solvent.
[0133] The dry mass ratio of the light-absorbing composition E11 according to Example 11, calculated under the same conditions and method as in Example 1, was 16.3%. The appearance and redispersibility of the light-absorbing composition E11 according to Example 11, evaluated under the same conditions and method as in Example 1, were both good. Table 1 also shows the raw materials of the light-absorbing composition E11 according to Example 11 and the evaluation results of the appearance and redispersibility. It was confirmed that a reaction product containing phosphonic acid, a phosphate ester, and some or all of the copper component was dispersed in the light-absorbing composition E11 according to Example 11, and that the appearance of the light-absorbing composition E11 was a transparent green. The acetic acid concentration of the light-absorbing composition E11 according to Example 11, measured in the same manner as in Example 1, was 0.09% by mass.
[0134] The transmission spectrum of light-absorbing composition E11 according to Example 11 was measured under the same conditions and by the same method as in Example 1. The transmission spectrum of light-absorbing composition E11 according to Example 11 is shown in Figure 5. In addition, specific parameters that can be seen from this transmission spectrum are shown in Table 3.
[0135] Example 12 Using the following compounds as raw materials, 37.54 g of light-absorbing composition E12 according to Example 12, with a dry mass ratio of 17.8 mass%, was prepared under the same conditions and by the same method as in Example 11. The appearance and redispersibility of the light-absorbing composition according to Example 12, evaluated under the same conditions and by the same method as in Example 1, were both good. [Raw materials] First solvent: methanol Copper acetate monohydrate 4.88 g Phosphonic acid: butylphosphonic acid 3.334 g Phosphate ester: NIKKOL DDP2 2.984 g Second solvent: methylene chloride 140 g [Purification (reduced pressure distillation) conditions] Oil bath temperature 45°C / pressure 600 hPa or less
[0136] Example 13 Using the following compounds as raw materials, 23.71 g of light-absorbing composition E13 according to Example 13, with a dry mass ratio of 24.5 mass%, was prepared under the same conditions and method as in Example 11. Furthermore, the appearance and redispersibility of light-absorbing composition E13 according to Example 13, evaluated under the same conditions and method as in Example 1, were both good. The acetic acid concentration of light-absorbing composition E13 according to Example 13, measured under the same conditions and method as in Example 1, was 0.10 mass%. [Raw materials] First solvent: ethanol Copper acetate monohydrate 4.88 g Phosphonic acid: butylphosphonic acid 2.943 g Phosphate ester: Plysurf A208N 2.315 g Second solvent: methylene chloride 100 g [Purification (reduced pressure distillation) conditions] Oil bath temperature 45°C / pressure 600 hPa or less
[0137] The transmission spectrum of the light-absorbing composition E13 according to Example 13 was measured under the same conditions and by the same method as in Example 1. Table 3 shows specific parameters that can be seen from this transmission spectrum.
[0138] Example 14 Using the following compounds as raw materials, 15.68 g of light-absorbing composition E14 according to Example 14, with a dry mass ratio of 37.9 mass%, was prepared under the same conditions and by the same method as in Example 11. The appearance and redispersibility of light-absorbing composition E14 according to Example 14, evaluated under the same conditions and by the same method as in Example 1, were both good. Table 1 also shows the raw materials of light-absorbing composition E14 according to Example 14 and the evaluation results of appearance and redispersibility. [Raw materials] First solvent: ethanol Copper acetate monohydrate 4.88 g Phosphonic acid: butylphosphonic acid 2.886 g Phosphate ester: Plysurf A208N 2.572 g Second solvent: methylene chloride 100 g [Purification (reduced pressure distillation) conditions] Oil bath temperature 45°C / pressure 600 hPa or less
[0139] The transmission spectrum of the light-absorbing composition E14 according to Example 14 was measured under the same conditions and by the same method as in Example 1. Table 3 shows specific parameters that can be seen from this transmission spectrum.
[0140] Example 15 Using the following compounds as raw materials, 11.88 g of light-absorbing composition E15 according to Example 15, with a dry mass ratio of 51.7 mass%, was prepared under the same conditions and method as in Example 11. The appearance and redispersibility of light-absorbing composition E15 according to Example 15, evaluated under the same conditions and method as in Example 1, were both good. The acetic acid concentration of light-absorbing composition E15 according to Example 15, measured under the same conditions and method as in Example 1, was 0.15 mass%. [Raw materials] First solvent: ethanol Copper acetate monohydrate 4.88 g Phosphonic acid: butylphosphonic acid 2.835 g Phosphate ester: Plysurf A208N 2.829 g Second solvent: methylene chloride 100 g [Purification (reduced pressure distillation) conditions] Oil bath temperature 45°C / pressure 350 hPa or less
[0141] The transmission spectrum of light-absorbing composition E15 according to Example 15 was measured under the same conditions and by the same method as in Example 1. The transmission spectrum of light-absorbing composition E15 according to Example 15 is shown in Figure 6. Specific parameters that can be seen from this transmission spectrum are shown in Table 3.
[0142] Comparative Example 1 Using the following compounds as raw materials, 10.31 g of a light-absorbing composition according to Comparative Example 1, with a dry mass ratio of 57.7% by mass, was prepared under the same conditions and method as in Example 1. During this process, excessive evaporation and removal of the solvent was promoted during the final vacuum distillation. According to an evaluation performed under the same conditions and method as in Example 1, the color of the appearance of the light-absorbing composition according to Comparative Example 1 was good, but redispersion caused the liquid to become cloudy. While the initial dispersibility was acceptable, it is suggested that redispersion reduced the dispersibility and caused partial aggregation. Table 1 also shows the raw materials of the light-absorbing composition according to Comparative Example 1, as well as the evaluation results of appearance and redispersibility. [Raw Materials] First Solvent: Ethanol Copper Acetate Monohydrate 4.88 g Phosphonic Acid: Butylphosphonic Acid 2.886 g Phosphate Ester: Plysurf A208N 2.572 g Second Solvent: Toluene 60 g [Purification (Vacuum Distillation) Conditions] Oil bath temperature 60°C / pressure 250 hPa or less
[0143] Comparative Example 2 Using the following compounds as raw materials, 8.91 g of a light-absorbing composition according to Comparative Example 2, with a dry mass ratio of 67.0 mass%, was prepared under the same conditions and by the same method as in Example 1. During the final vacuum distillation, evaporation and removal of the solvent was promoted to an even greater extent than in Comparative Example 1. According to evaluations performed under the same conditions and by the same method as in Example 1, the light-absorbing composition according to Comparative Example 2 exhibited a milky yellow appearance, and was not in a green, highly transparent liquid state as observed in the other Examples and Comparative Example 1. This suggests that the light-absorbing composition according to Comparative Example 2 does not contribute to solving the problems of the present invention. Table 1 also shows the raw materials of the light-absorbing composition according to Comparative Example 2 and the evaluation results of its appearance and redispersibility. [Raw materials] First solvent: ethanol, copper acetate monohydrate 4.88 g, phosphonic acid: butylphosphonic acid 2.886 g, phosphate ester: Plysurf A208N 2.572 g, second solvent: toluene 60 g [Purification (vacuum distillation) conditions] Oil bath temperature 60°C / pressure 250 hPa or less
[0144] Comparative Example 3: Using the following compounds as raw materials, 10.21 g of a light-absorbing composition according to Comparative Example 3, with a dry mass ratio of 58.4 mass%, was prepared under the same conditions and method as in Example 11. During this process, excessive evaporation and removal of the solvent was promoted during the final reduced-pressure distillation. According to evaluations performed under the same conditions and method as in Example 1, the light-absorbing composition according to Comparative Example 3 had a good color appearance, but redispersion caused the liquid to become cloudy. This suggests that the initial dispersibility was acceptable, but redispersion reduced dispersibility and caused partial aggregation. Table 1 also shows the raw materials for the light-absorbing composition according to Comparative Example 3, as well as the evaluation results for appearance and redispersibility. [Raw materials] First solvent: ethanol, copper acetate monohydrate 4.88 g, phosphonic acid: butylphosphonic acid 2.886 g, phosphate ester: Plysurf A208N 2.572 g, second solvent: methylene chloride 100 g [Purification (vacuum distillation) conditions] Oil bath temperature 45°C / pressure 350 hPa or less
[0145] Comparative Example 4 Using the following compounds as raw materials, 8.56 g of a light-absorbing composition according to Comparative Example 4, with a dry mass ratio of 69.5% by mass, was prepared under the same conditions and by the same method as in Example 11. In this case, the final reduced-pressure distillation promoted evaporation and removal of the solvent to an even greater extent than in Comparative Example 1. According to evaluations performed under the same conditions and by the same method as in Example 1, the light-absorbing composition according to Comparative Example 4 exhibited a milky yellow appearance, and was not in a highly transparent green liquid state as observed in the other Examples and Comparative Examples 1 and 3. This suggests that the light-absorbing composition according to Comparative Example 4 does not contribute to solving the problems of the present invention. Table 1 also shows the raw materials of the light-absorbing composition according to Comparative Example 4 and the evaluation results of its appearance and redispersibility. [Raw materials] First solvent: ethanol, copper acetate monohydrate 4.88 g, phosphonic acid: butylphosphonic acid 2.886 g, phosphate ester: Plysurf A208N 2.572 g, second solvent: methylene chloride 100 g [Purification (vacuum distillation) conditions] Oil bath temperature 45°C / pressure 350 hPa or less
[0146] Comparative Example 5 Using the following compounds as raw materials, 93.18 g of a light-absorbing composition according to Comparative Example 5 with a dry mass ratio of 6.4 mass% was prepared under the same conditions and method as in Example 1. In this case, the final distillation was performed without reducing the pressure, and the amount of solvent removed by evaporation was reduced. According to an evaluation performed under the same conditions and method as in Example 1, the color of the appearance of the light-absorbing composition according to Comparative Example 5 was good, but the liquid became cloudy after redispersion. This suggests that the initial dispersibility was acceptable, but that redispersion reduced the dispersibility and caused partial aggregation. Table 1 also shows the raw materials of the light-absorbing composition according to Comparative Example 5 and the evaluation results of the appearance and redispersibility. [Raw Materials] First Solvent: Ethanol Copper Acetate Monohydrate 4.88 g Phosphonic Acid: Butylphosphonic Acid 2.886 g Phosphate Ester: Plysurf A208N 2.572 g Second Solvent: Toluene 140 g [Purification (Vacuum Distillation) Conditions] Oil bath temperature 105°C / No vacuum
[0147] (Preparation of composition for light-absorbing film) Example 16 To the light-absorbing composition E1 according to Example 1, a toluene solvent and a silicone resin (KR-300 manufactured by Shin-Etsu Chemical Co., Ltd.) were added so that the dry mass ratio was 50 mass%, and the mixture was stirred at room temperature for 30 minutes to prepare a composition for light-absorbing film according to Example 16. The composition for light-absorbing film was prepared by adding the light-absorbing composition to a solvent to which a resin had been previously dissolved. The dry mass ratio in the composition for light-absorbing film is the ratio of the sum of the dry mass of the light-absorbing composition contained and the solid mass of the added resin component to the mass of the entire composition for light-absorbing film (the same applies to Examples 17 to 21).
[0148] Example 17 To the light-absorbing composition E4 according to Example 4, a toluene solvent and a silicone resin (KR-300 manufactured by Shin-Etsu Chemical Co., Ltd.) were added so that the dry mass ratio was 30 mass %, and the mixture was stirred at room temperature for 30 minutes to prepare a composition for a light-absorbing film according to Example 17. This composition for a light-absorbing film was prepared in such a manner that the resin was dissolved in advance in a solvent to be added, and then the light-absorbing composition was added.
[0149] Example 18 To the light-absorbing composition of Example 9, toluene as a solvent and a silicone resin (KR-300 manufactured by Shin-Etsu Chemical Co., Ltd.) were added so that the dry mass ratio was 25 mass %, and the mixture was stirred at room temperature for 30 minutes to prepare a composition for a light-absorbing film of Example 18. The composition for a light-absorbing film was prepared in such a manner that the resin was dissolved in advance in a solvent to be added, and then the light-absorbing composition was added.
[0150] Example 19 Toluene as a solvent and a cyclic olefin resin (ZEONOR 1060R manufactured by ZEON Corporation) were added to the light-absorbing composition of Example 9 so that the dry mass ratio was 30 mass %, and the mixture was stirred at room temperature for 30 minutes to prepare a composition for a light-absorbing film of Example 19. The composition for a light-absorbing film was prepared in such a manner that the resin was dissolved in advance in a solvent to be added, and then the light-absorbing composition was added.
[0151] Example 20 Methylene chloride as a solvent and a silicone resin (KR-300 manufactured by Shin-Etsu Chemical Co., Ltd.) were added to the light-absorbing composition of Example 11 so that the dry mass ratio was 50 mass %, and the mixture was stirred at room temperature for 30 minutes to prepare a composition for a light-absorbing film of Example 20. The composition for a light-absorbing film was prepared in such a manner that the resin was dissolved in advance in a solvent to be added, and then the light-absorbing composition was added.
[0152] Example 21 Methylene chloride as a solvent and a silicone resin (KR-300, manufactured by Shin-Etsu Chemical Co., Ltd.) were added to the light-absorbing composition of Example 15 so that the dry mass ratio was 50 mass %, and the mixture was stirred at room temperature for 30 minutes to prepare a composition for a light-absorbing film of Example 21. The composition for a light-absorbing film was prepared in such a manner that the resin was dissolved in advance in a solvent to be added, and then the light-absorbing composition was added.
[0153] (Fabrication of Light-Absorbing Film) Example 22 A transparent, plate-shaped borosilicate glass (D263 T eco, manufactured by SCHOTT) measuring 76 mm x 76 mm x 0.21 mm was prepared as a support (support glass). The arithmetic mean roughness Ra of the glass's main surface was less than 1 nm, and the main surface was sufficiently smooth. The support glass was sequentially washed with acetone, ethanol, and pure water. A stainless steel frame (frame) measuring 70 mm x 70 mm in plan view and with an opening measuring 60 mm x 60 mm was placed on the main surface of the plate-shaped support glass so that the opening was located approximately in the center of the support glass. The height (thickness) of the frame was approximately 1 mm. An appropriate amount of the light-absorbing film composition according to Example 16 was dispensed into the opening of the frame on the support glass using a dispenser equipped with a filter-integrated tip with a particle size retention capacity of 5 μm. The composition was then left to stand for an appropriate period of time, allowing it to flow over the entire opening, resulting in a workpiece having a uniform coating (cast film) formed on the support glass. Next, this workpiece was placed in a heat circulation oven and heated at an actual furnace temperature of 85°C for 6 hours, and then the workpiece was removed from the oven. The cast film on the support glass was solidified and integrated with the support glass. In this way, the light-absorbing film of Example 22 was produced by cast on a support. The thickness of the light-absorbing film formed on the support glass was 115 μm. The thickness of the light-absorbing film was measured using a laser displacement meter LK-H008 manufactured by Keyence Corporation.
[0154] For the optical filter of Example 22, which includes a support and a light-absorbing film, the transmittance for each wavelength in the wavelength range of 300 nm to 1200 nm at an incident angle of 0° was measured using an ultraviolet-visible-near-infrared spectrophotometer (manufactured by JASCO Corporation, model number: V770), to obtain the transmission spectrum of the optical filter of Example 22. The transmission spectrum of the optical filter of Example 22 is shown in FIG. 7. Parameters related to wavelength or transmittance that can be observed from this transmission spectrum are also shown in Table 4. FIG. 8 shows the transmission spectrum of borosilicate glass (manufactured by SCHOTT: D263 T eco; thickness: 0.21 mm) used as the support when the incident angle is 0°. The glass used as the support exhibits a substantially constant transmittance in the wavelength range of 350 nm or more, and a decrease in transmittance due to Fresnel reflection at the interface between the glass and air can be confirmed.
[0155] Example 23 A light-absorbing film and optical filter according to Example 23 were produced in the same manner as in Example 22, except that the composition for a light-absorbing film according to Example 17 was used instead of the composition for a light-absorbing film according to Example 16. The thickness of the light-absorbing film formed on the support was 207 μm. The transmission spectrum of the optical filter according to Example 23 was measured in the same manner as in Example 22. FIG. 9 shows the transmission spectrum of the light-absorbing film according to Example 23. Parameters related to wavelength or transmittance that can be seen from this transmission spectrum are shown in Table 4.
[0156] Example 24 A light-absorbing film and an optical filter according to Example 24 were produced in the same manner as in Example 22, except that the composition for a light-absorbing film according to Example 18 was used instead of the composition for a light-absorbing film according to Example 16. The thickness of the light-absorbing film formed on the support was 192 μm. The transmission spectrum of the optical filter according to Example 24 was measured in the same manner as in Example 22. FIG. 10 shows the transmission spectrum of the light-absorbing film according to Example 24. Furthermore, parameters relating to wavelength or transmittance that can be seen from this transmission spectrum are shown in Table 4.
[0157] Example 25 A light-absorbing film and an optical filter according to Example 25 were produced in the same manner as in Example 22, except that the composition for a light-absorbing film according to Example 19 was used instead of the composition for a light-absorbing film according to Example 16. The thickness of the light-absorbing film formed on the support was 205 μm. The transmission spectrum of the optical filter according to Example 25 was measured in the same manner as in Example 22. FIG. 11 shows the transmission spectrum of the light-absorbing film according to Example 25. Parameters relating to wavelength or transmittance that can be seen from this transmission spectrum are shown in Table 4.
[0158] Example 26 A light-absorbing film and an optical filter according to Example 26 were produced in the same manner as in Example 22, except that the composition for a light-absorbing film according to Example 20 was used instead of the composition for a light-absorbing film according to Example 16. The thickness of the light-absorbing film formed on the support was 93 μm. The transmission spectrum of the optical filter according to Example 26 was measured in the same manner as in Example 22. FIG. 12 shows the transmission spectrum of the light-absorbing film according to Example 26. Furthermore, parameters relating to wavelength or transmittance that can be seen from this transmission spectrum are shown in Table 4.
[0159] Example 27 A light-absorbing film and optical filter according to Example 27 were produced in the same manner as in Example 22, except that the composition for a light-absorbing film according to Example 21 was used instead of the composition for a light-absorbing film according to Example 16. The thickness of the light-absorbing film formed on the support was 103 μm. The transmission spectrum of the optical filter according to Example 27 was measured in the same manner as in Example 22. FIG. 13 shows the transmission spectrum of the light-absorbing film according to Example 27. Parameters related to wavelength or transmittance that can be seen from this transmission spectrum are shown in Table 4.
[0160]
[0161]
[0162]
[0163]
Claims
1. A light absorbing composition comprising: a light absorbing compound having phosphorus and copper; and a solvent, wherein the ratio of the dry mass of the light absorbing composition to the mass of the light absorbing composition is 15% to 55%.
2. The light absorbing composition according to claim 1, wherein the light absorbing compound comprises at least one selected from the group consisting of phosphonic acid and phosphoric acid ester, and a copper component.
3. The light-absorbing composition according to claim 1 or 2, characterized in that the acid concentration is 0.2 mass % or less.
4. The light-absorbing composition according to any one of claims 1 to 3, having a transmission spectrum satisfying the following conditions (i) to (iv): (i) an average transmittance in the wavelength range of 800 nm to 1100 nm is 20% or less; (ii) an average transmittance in the wavelength range of 460 nm to 580 nm is 80% or more; (iii) within the wavelength range of 300 nm to 400 nm, the wavelength at which the transmittance is 50% is in the wavelength range of 320 nm to 380 nm; (iv) within the wavelength range of 600 nm to 800 nm, the wavelength at which the transmittance is 50% is in the wavelength range of 680 nm to 780 nm.
5. The light-absorbing composition according to claim 4, wherein the transmission spectrum satisfies the following condition (v): (v) the wavelength range in which the transmittance is 50% or more at wavelengths of 300 nm to 1200 nm is 350 nm to 420 nm.
6. The light-absorbing composition according to claim 4 or 5, wherein the transmission spectrum satisfies the following condition (vi): (vi) the average transmittance within a wavelength range of 1100 nm to 1200 nm is 10% or less.
7. The light-absorbing composition according to any one of claims 4 to 6, wherein the transmission spectrum satisfies the following condition (vii): (vii) the standard deviation of the transmittance within a wavelength range of 900 nm to 1100 nm is 0.5% or less.
8. A method for producing a light absorbing composition, comprising: mixing a phosphorus-containing compound and a copper salt in a first solvent; separating the first solvent to obtain a solid having phosphorus and copper; and adding the solid to a second solvent and adjusting by distillation the ratio of the dry mass of the light absorbing composition to the mass of the light absorbing composition to be 15% to 55%.
9. The method for producing a light-absorbing composition according to claim 8, wherein the acid concentration is less than 0.2% by mass.
10. The method for producing a light-absorbing composition according to claim 8 or 9, wherein the distillation is carried out at 100°C or lower.
11. The method for producing a light-absorbing composition according to any one of claims 8 to 10, wherein the distillation is carried out at a pressure lower than atmospheric pressure.
12. A composition for a light-absorbing film, comprising: a light-absorbing compound having phosphorus and copper; a solvent; and a silicone resin, wherein the ratio of the dry mass of the composition for a light-absorbing film to the mass of the composition for a light-absorbing film is 10% to 55%.
13. A light absorbing film comprising a light absorbing compound containing phosphorus and copper and a silicone resin, having a thickness of 300 μm or less, and exhibiting a transmission spectrum having the following (I) to (IV) when light having a wavelength of 300 nm to 1200 nm is incident at an incident angle of 0°. (I) The average transmittance in the wavelength range of 800 nm to 1100 nm is 20% or less. (II) The average transmittance in the wavelength range of 460 nm to 580 nm is 80% or more. (III) The first cutoff wavelength at which the transmittance is 50% in the wavelength range of 300 nm to 400 nm is in the wavelength range of 320 nm to 400 nm. (IV) The second cutoff wavelength at which the transmittance is 50% in the wavelength range of 600 nm to 800 nm is in the wavelength range of 650 nm to 750 nm.
14. The light absorbing film according to claim 13, wherein in the transmission spectrum, the transmittance at a wavelength of 430 nm is 80% or more.
Citation Information
Patent Citations
Near-infrared absorbing composition, near-infrared absorbing film, and image sensor for solid-state imaging element
JP2019081896A
Optical filter and light-absorbing composition
WO2020071461A1
Near-infrared-absorbing composition, near-infrared-absorbing film, and image sensor for solid-state imaging element
WO2020195701A1