Methods and systems for substrate passivation using direct atomic layer deposition

The microreactor-based DALP system addresses the challenge of defect-free passivation in semiconductor devices by enabling direct, mask-free formation of passivation layers, improving device reliability and efficiency through precise thickness control and uniform deposition.

WO2026236299A1PCT designated stage Publication Date: 2026-11-12ATLANT 3D APS +1
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
PCT/US2026/026803
Authority / Receiving Office
WO · WO
Patent Type
Applications
Current Assignee / Owner
Priority Date
2025-05-06
Filing Date
2026-05-06
Publication Date
2026-11-12

AI Technical Summary

Technical Problem

Existing substrate passivation technologies face challenges in achieving defect-free passivation at scale without introducing new failure mechanisms, particularly in semiconductor devices, solar cells, MEMS devices, and III-V optoelectronic devices, due to issues with edge metallization compatibility, doping methods, stress-engineered films, and thermally stable passivation layers.

Method used

The use of a microreactor-based direct atomic layer deposition (DALP) system that allows for direct formation of passivation layers on predetermined substrate areas without the need for lithography masks, utilizing a nozzle to dispense precursors and reactants, and a housing to form a discrete reaction environment, enabling conformal coating and precise thickness control.

Benefits of technology

The DALP system achieves high-resolution, uniform passivation with reduced defect densities and improved mechanical/optical performance, enhancing device reliability and efficiency by suppressing recombination and stress-related issues in semiconductor devices.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure US2026026803_12112026_PF_FP_ABST
    Figure US2026026803_12112026_PF_FP_ABST
Patent Text Reader

Abstract

The disclosure relates to methods and systems for substrate passivation using microreactor, direct atomic layer deposition (DALP). Specifically, the disclosure relates to methods for substrate passivation implemented in a system obviating forming lithography masks over the whole substrate, allowing for directly forming a passivation layer.
Need to check novelty before this filing date? Find Prior Art

Description

METHODS AND SYSTEMS FOR SUBSTRATE PASSIVATION USING DIRECT ATOMIC LAYER DEPOSITIONBACKGROUND

[0001] The disclosure is directed to methods and systems for substrate passivation using direct atomic layer deposition (DALP). Specifically, the disclosure is directed to methods for substrate passivation implemented in a system obviating forming lithography masks over the whole substrate, allowing for directly forming a passivation layer.

[0002] Edge passivation techniques are typically used to enhance the performance and reliability of various semiconductor devices, whereby different substrate technologies requiring tailored approaches. For example, in silicon solar cells, edge passivation addresses recombination losses at cut edges introduced during shingling or cell separation. Chemical etching methods, such as those employing optimized procedures to passivate edge shunts, have demonstrated efficiency improvements of 10%-30% in degraded cells, with some cases showing over 100% recovery. For shingled modules, passivated edge technology (PET) using dielectric layers like AI2O3 deposited postmetallization improves pseudo-fill factor (pFF) by -0.5% while maintaining interconnection integrity. However, preventing parasitic deposition of passivation layers over metallization areas remains challenging, which compromises module reliability during thermal cycling.

[0003] Likewise, in high-power systems in chip (SiC) devices, edge termination structures like junction termination extensions (ITE) and field guard rings are essential to manage high electric fields. Low dopant diffusion coefficients in SiC further complicates the formation of deep junctions (>1 pm), necessitating precise ion implantation and annealing. Dielectric layers must withstand critical fields exceeding 3 MV / cm, but material limitations often lead to premature breakdown or reliability issues under prolonged voltage cycling stress. Moreover, and for GaAs / AlGaAs-based edge-emitting laser diodes, oxidation-induced defects leading to catastrophic optical mirror damage (COMD), can be reduced with facet passivation using, for example, crystalline oxide layers.

[0004] Microelectromechanical systems (MEMS)-based pressure sensors and resonators are exposed to edge-related stresses from packaging processes. Crossbeam film designs and composite diaphragm structures help concentrate stress for sensitivity improvements, but mismatches in coefficient of thermal expansion (CTE) between die materials and substrates, can and does induce warping or resonant frequency shifts. Furthermore, outgassing from epoxy -based die attach materialsfurther degrades passivation layers, necessitating low-modulus adhesives or hermetic packaging to prevent contamination. Resonant pressure sensors utilizing anodic bonding for vacuum encapsulation achieve quality factors >20,000, yet long-term stability under mechanical fatigue remains a concern.

[0005] In III-V optoelectronic devices, such as GalnP -based photoelectrochemical cells, reliance on wide-bandgap passivation layers like GaN to minimize interfacial recombination is exercised. XPS studies showed valence band offsets of -1.90 eV between GalnP and GaN, facilitating electron transport while suppressing oxidative corrosion. However, Fermi-level pinning at III-V surfaces due to native oxides (e.g., AS2O3 on GaAs) has been shown to create upward band bending of 0.38 eV, requiring sub-nm interfacial control during atomic-layer deposition. For edge-emitting lasers (EELs), non-uniform oxidation across high-aluminum-content facets (e.g., >40% Al) limits the effectiveness of conventional passivation, driving the need for in-situ surface tailoring prior to coating.

[0006] To reiterate, there is a gap across all domains involving achieving defect-free passivation at scale without introducing new failure mechanisms. Solar cell PET processes struggle with edge metallization compatibility, while SiC edge terminations lack cost-effective doping methods beyond ion implantation. MEMS devices require novel stress-engineered films compatible with e.g., CMOS integration, as current polysilicon-based passivation anneals (Temp.>1000°C) destroy underlying circuitry. III-V systems need thermally stable passivation layers that maintain band alignment under operational biases, as GaN’s 0.44 eV conduction band offset with GalnP risks carrier blocking if interface traps form. Cross-cutting challenges include developing in-line metrology for edge defect quantification and unifying passivation processes across disparate manufacturing workflows, particularly for hybrid modules combining shingled cells with heterogeneous III-V tandems.

[0007] The disclosed technology aims to address some of the current shortcomings.SUMMARY

[0008] Disclosed, in various exemplary implementations, are methods and systems for substrate passivation using microreactor, direct atomic layer deposition (DALP). Specifically, disclosed are methods for substrate passivation implemented in a system obviating the need for forming lithography masks over the whole substrate, allowing for directly forming a passivation layer on predetermined areas of the substrate.

[0009] In an exemplary implementation provided herein is a method for passivating a substrate, implemented in a microreactor direct atomic layer deposition (DALP) system, the method comprising: using the DALP system, depositing a passivating material on the substrate over a predetermined area of the substrate, wherein the step of depositing comprises forming an area-conforming surface having a predetermined thickness, the predetermined thickness is adapted, sized and configured to passivate the predetermined area of the substrate.

[0010] In another exemplary implementation, the DALP system comprises: a substrate plate for holding the substrate; a nozzle defining a basal facet adapted, sized and configured to selectably dispense onto the substrate at least one precursor and at least one reactant; a first inlet supply conduit in fluid communication with: the nozzle; and a precursor reservoir a second inlet supply conduit in fluid communication with: the nozzle; and a reactant reservoir a third inlet supply conduit in fluid communication with: the nozzle; and an inert gas reservoir one or more exhaust conduit in fluid communication with the nozzle, adapted sized and configured to remove: non-deposited precursor; non-deposited reactant; and residual inert; and a housing, having a housing portion extending basally from basal facet of the nozzle defining a peripheral wall having a predetermined perimeter cross section extending basally beyond the basal facet of the nozzle, wherein the housing portion is adapted, sized and configured to form a discrete reaction environment between the at least one precursor and the reactant.

[0011] These and other features of the methods and systems for substrate passivation using microreactor, direct atomic layer deposition (DALP), will become apparent from the following detailed description when read in conjunction with the figures and examples, which are exemplary, not limiting.BRIEF DESCRIPTION OF THE FIGURES

[0012] For a better understanding of the methods and systems for substrate passivation using microreactor, direct atomic layer deposition (DALP), with regard to the exemplary implementations thereof, reference is made to the accompanying examples and figures, in which:

[0013] FIG.s 1, and 2 are schematics illustrating the use of the DALP system for passivation of substrate edges;

[0014] FIG. 3, illustrates current edge passivation techniques;

[0015] FIG. 4, illustrates actual PV panel edge passivated using the methods disclosed;

[0016] FIG. 5, depicts lifetime in ps of panels passivated using an exemplary implementation of the methods disclosed; and

[0017] FIG. 6A, is a schematic illustrating a bottom perspective of an exemplary implementation of the DALP system’s head, with FIG. 6B, illustrating a top perspective thereof, while FIG. 6C, illustrates an exemplary implementation of the microreactor optionally coupled to the head.DETAILED DESCRIPTION

[0018] Provided herein are exemplary implementations of methods and systems for substrate passivation using microreactor, direct atomic layer deposition (DALP). Specifically, provided herein are exemplary implementations of methods for substrate passivation implemented in systems obviating the need for forming lithography masks over the whole substrate, allowing for directly forming a passivation layer.

[0019] The disclosure is directed to an apparatus and method for edge-side passivation of semiconductor wafers using a microreactor direct atomic layer deposition (hereinafter, DALP) system. The nozzle of the system allows for high-resolution deposition of thin films (e.g., SisN^ AI2O3, Pt) directly onto the vertical and top edge surfaces of a rotating wafer (see e.g., FIG.s 1, 2). It is capable of:• Conformal coating through ALD-like localized processes. Selective edge etching (e.g., O3, CL) and surface treatment (e.g., plasma, UV, ion implantation);• Multi-nozzle high-throughput configuration for scalable manufacturing

[0020] Furthermore, the systems disclosed enable controlled vertical deposition, in mechanically integrated systems, ensuring high-speed precise alignment and uniformity on rotating wafers, with edge-only passivation capability, eliminating global film deposition and etching steps.

[0021] As illustrated in FIG. 3, and going from top to bottom, current methods involve depositing 10 a passivation layer 400 all around the substrate 200, following by deposition 11 of a (photoresist)mask 410 all around the passivation layer 400, followed by double sided patterning 12 using e.g., lithography, partially removing the (photo)resist mask, followed by selective etching 13, leaving the passivating layer 400, on the vertical side walls of substrate 200.

[0022] Accordingly and in an exemplary implementation, provided herein is a method for passivating a substrate, implemented in a microreactor direct atomic layer deposition (DALP) system(see e.g., FIG. 6), the method comprising: using the DALP system 1000 having nozzle 100 (see e.g., FIG. 3), depositing a passivating material 210, 220 on the substrate over a predetermined area of the substrate 200, wherein the step of depositing comprises forming an area-conforming surface having a predetermined thickness, the predetermined thickness is adapted, sized and configured to passivate the predetermined area of the substrate.

[0023] As indicated, the methods provided utilizes a microreactor direct atomic layer deposition (DALP) system to deposit a passivating material on a substrate’s predetermined area. The deposited material forms an area-conforming surface with a predetermined thickness (0.5-200 nm, ±5% uniformity) tailored to passivate the target region. Thickness optimization is configured to balance defect suppression (e.g., recombination velocity <10 cm / s for solar cells) and mechanical / optical performance. Parameters controlled during the deposition can be substrate temperature (25-400'Cj and velocity as well as other parameters associated with the precursors and reactants. Measurement instruments used to validate the integrity of the deposited passivation layer, can be, for example, spectroscopic ellipsometry (thickness), X-ray photoelectron spectroscopy (XPS) (composition), and transmission electron microscopy (TEM) (interface quality).

[0024] As indicated, and illustrated schematically, in FIG. 6, the DALP system comprises: a substrate plate for holding the substrate (not shown); a nozzle 101 defining a basal facet 105 adapted, sized and configured to selectably dispense onto the substrate 200 at least one precursor and at least one reactant; a first inlet supply conduit 122 in fluid communication with: the nozzle 101; and a precursor reservoir (not shown) a second inlet supply conduit 124 in fluid communication with: the nozzle 101 ; and a reactant reservoir (not shown) a third inlet supply 128 conduit in fluid communication with: the nozzle 101; and an inert gas reservoir (not shown), as well as one or more exhaust conduit 121 in fluid communication with the nozzle 101, adapted sized and configured to remove: non-deposited precursor; non-deposited reactant; and residual inert gas; and a housing, having a housing portion 107 extending basally from basal facet 105 of the nozzle 101 defining a peripheral wall 1071 having a predetermined perimeter cross section extending basally beyond the basal facet 105 of the nozzle 101, wherein the housing portion 107 is adapted, sized and configured to form a discrete reaction environment chamber 1070 between the at least one precursor and the reactant. For example, the system can incorporate a thermally conductive substrate plate (e.g., aluminum nitride, having a heat transfer coefficient between about 180 W / m-K and about 220 W / m-K) with, for example electrostatic clamping (500-2,000 V), or mechanical clamps to securelyhold substrates during processing. A precision nozzle featuring a basal facet dispense precursors and reactants in controlled pulses (0.1-10 pL / pulse). Precursors can be delivered via temperature-regulated reservoirs (20-150°C) at partial pressures of between about 0.1 Torr and about 1 Torr, while reactants like H2O or O3 flow through mass-controlled conduits (between about 10 seem and about 500 seem, ±1% stability). Inert purge gases (N2, Ar) typically cycle at 1-10 SLM to maintain contamination levels below 0.1%. Residual byproducts are evacuated through e.g., vacuum pumps operating at between about 106Torr and about 103Torr, with optional in-line gas analyzers ensuring chamber purity. The substantially hermetically sealed reaction chamber can have a peripheral wall extending between about 5 mm and about 20 mm beyond the nozzle, its cross-sectional geometry (circular / rectangular, hexagonal and the like) tailored to match substrate features such as laser facets or MEMS trenches. In addition, the nozzle can be a part of a nozzle array, allowing large area scalability.

[0025] In another exemplary implementation, the substrate is a component of: an edge emitting laser (EEL), a photovoltaic (PV) device, a semiconductor wafer, a high-power electronic device, a microelectromechanical system (MEMS) device, or a IILV optoelectronic device. Edgeemitting lasers (EELs) refer to semiconductor devices that emit coherent light from cleaved facets, widely used in fiber-optic communications for high-speed data transmission and LiDAR systems for autonomous vehicles. Photovoltaic (PV) devices, such as PERC and heterojunction solar cells, convert sunlight into electricity, enabling grid-scale renewable energy generation and residential solar installations. Semiconductor wafers, primarily silicon-based, serve as substrates for manufacturing integrated circuits in electronics like processors and memory chips, while advanced materials like silicon carbide (SiC) and gallium nitride (GaN) support high-power applications. High-power electronic devices, including IGBTs (insulated-gate bipolar transistors) and SiC MOSFETs (Silicon Carbide Metal-Oxide-Semiconductor Field-Effect Transistors), manage energy conversion in electric vehicle drivetrains, industrial motor drives, and smart grids. MEMS devices integrate mechanical and electrical components at microscale, with applications ranging from accelerometers in automotive airbag systems to microphones in smartphones and pressure sensors in medical diagnostics. IILV optoelectronic devices, fabricated from compounds like GaAs and InP, enable high-efficiency LEDs for displays, laser diodes for optical networking, and photodetectors for 5G and quantum communication systems. These technologies collectively drive advancements intelecommunications, clean energy, computing, and loT, balancing performance, scalability, and reliability across industries.

[0026] In an exemplary implementation, the substrate sought to be passivated using the systems disclosed, is a component in of the edge emitting laser (EEL), and the method comprises providing an EEL device having a front cleaved facet surface, a rear cleaved facet surface and an outer surface; and using the DALP system, depositing a passivation layer having a thickness of between about 2 nanometer (nm) and about 10 nm of hafnium oxide (HfCL), or an amorphous silicon (Sia), on each of the front cleaved facet surface, and the rear cleaved facet surface. As indicated, the cleaved facets can be passivated with hafnium oxide (HfCL) or amorphous silicon layers deposited at thicknesses ranging from 2-10 nm under temperatures between 150-300°C. These layers are deposited at a thickness configured to suppress catastrophic optical mirror damage (COMD) by reducing facet temperature rise under high optical flux conditions. Use of EEL examples can be, for example; LiDAR lasers operating at wavelengths of 905 nm with HI'CL-passivated facets enabling operation at temperatures exceeding 100°C, and / or, in another example, vertical-cavity surface-emitting laser (VCSEL) arrays passivated with amorphous silicon for integration into smartphone-based 3D sensing modules.

[0027] Additionally, or alternatively, depositing the passivation layer further comprises: using the DALP system, annealing the HI'CL or Sialayer at 300-500°C under an inert atmosphere, whereby the annealing step is configured to reduce interfacial defect density to <10ncm2as measured by cross-sectional TEM. In other words, annealing of HI'CL or amorphous silicon (Sia) layers can be carried out at temperatures of between 450-500°C for 1-5 minutes under an inert nitrogen atmosphere which can reduce interfacial defect densities to less than 1011cm2by enabling structural relaxation and oxygen redistribution while simultaneously suppressing crystallization-induced defects. For HI'CL, for example, rapid thermal annealing (RTA) at 500°C for 3 minute intervals improves Si interface passivation, as oxygen diffusion from HI'CL to the Si substrate can form a crystalline SiCL interfacial layer of between 1-2 nm, mitigating dangling bonds. Since, annealing at lower temperatures (T<400°C) would leave HfCL amorphous, but retain mixed HfCL / SiCL interfacial disorder, exceeding 550°C would induces polycrystalline HfCL (orthorhombic phase) and thicker crystalline SiCL, increasing the probability for defects.

[0028] Likewise, for Sia, annealing at 300— 4()0°C for 5-10 minutes in argon can facilitate hydrogen effusion from Sia:H layers, thereby reducing interfacial traps. Cross-sectional TEM can beused to confirm defect densities correlated with interfacial SiCh crystallinity and HI'C)2phase stability, with optimal results seemingly at 5 (KFC due to balanced oxygen stoichiometry and minimal grain boundary formation (referring to boundaries among various centers of nucleation of the same or different crystalline polymorphs).

[0029] Furthermore, the step of depositing the HfO2passivation layer can further involve creating a gradient; transitioning from a deposition of a HfO2-rich composition wherein the HfO2-rich composition comprises no less than 95% (w / w) of HfO2, on each of the front cleaved facet surface, and the rear cleaved facet surface, to a HfSiOx-rich composition at the outer surface, with total thickness variance <±0.2 nm across each of the front cleaved facet surface, and the rear cleaved facet surface, to the outer surface, while maintaining the ratio between Hf:Si at about 3:1. The transitioning from a Hl'Ch-rich (>95% w / w) inner layer to an outer HfSiOx(Hf:Si ~ 3:1) layer on EEL facets is done in certain exemplary implementations, to improves passivation using the DALP systems disclosed, by leveraging Hl'CE’s high dielectric constant (K ~ 20) to suppress surface recombination at the interface while mitigating mechanical stress and interfacial trap states. The HfCE-rich base ensures minimal oxygen vacancies (p< 1017cm3) and strong band offset alignment (AE_v ~ 1.9 eV) with GaAs / AlGaAs facets, reducing non-radiative recombination velocities to v<20 cm / s. Gradual silicon incorporation forming the gradient, stabilizes the HfSiOxouter layer by passivating dangling bonds via Si-0 network formation, lowering interfacial defect density (p< 1011cm2) and enhancing adhesion to subsequent coatings (e.g., SiO2encapsulation). The Hf:Si ratio of 3:1 optimizes stoichiometry to balance HfO2’s high-k benefits with Si’s stress-relief properties, reducing thermal CTE mismatch-induced cracking and crack propagation during high-power operation (>100 mW) and cycling. The <±0.2 nm thickness variance ensures uniform electric field distribution across facets, preventing localized Joule heating that triggers COMD. This structured gradient also improves moisture resistance by replacing hygroscopic HI'O2surface sites with Si-0 bonds, which is beneficial for long-term reliability in humid environments (e.g., 85°C / 85% RH).

[0030] In yet another exemplary implementation, the DALP system further comprises a plasma generator in fluid communication with the nozzle, the plasma generator being coupled to a hydrogen source, whereby the method further comprises, prior to the step of depositing, using the DALP system, pre-treating the front panel surface with a hydrogen plasma, wherein the plasma exposure time is configured to yield a predetermined final SiNxhydrogen content as quantified byFTIR absorption at 3350 cm-1. As indicated, Photovoltaic (PV) panels can employ passivation layers composed of silicon nitride (SiNx) or aluminum oxide (AI2O3). SiNxlayers ranging from 70-110 nm in thickness are operable as anti-reflective coatings and surface passivation layers for PERC cells, while AI2O3 layers, at a thickness between about 10 nm and about 30 nm can provide rearsurface field-effect passivation in heterojunction (HJT) cells. Use examples include rooftop solar modules achieving efficiencies exceeding 22% and radiation-hardened HJT cells designed for space applications. Similarly, the ultra-thin SiCE ensures minimal resistive losses, while the doped poly-Si enables precise control over carrier transport. Tunnel oxide passivated contact (TOPCon) photovoltaic devices employ a tunnel oxide passivation layer primarily composed of ultra-thin silicon dioxide (SiCE) with typical thicknesses ranging from 1 to 2 nanometers, forming an insulating barrier that enables quantum tunneling of charge carriers while minimizing surface recombination. Its functionality lies in allowing majority carriers (electrons or holes) to pass through via tunneling effects while blocking minority carriers, thereby reducing electron-hole recombination losses at the silicon surface. The thickness of between about l.lnm and about 1.5 nm can be used to balance carrier transport efficiency and passivation quality. The ultra-thin SiO2affects minimal resistive losses, while the doped poly-Si enables precise control over carrier transport.

[0031] Further, additional hydrogen-containing layers, such as aluminum oxide (AI2O3) or silicon nitride (SiNx), can be deposited using the methods disclosed, to further improve passivation. These layers are adapted to release hydrogen atoms during annealing processes, which diffuse into the silicon bulk and passivate dangling bonds at the SiO2 / Si interface. In certain exemplary implementation, A12O3is used due to its negative fixed charges, which can repel electrons and reduce surface recombination for p-type silicon. SiNxlayers also be deposited, providing anti-reflective properties while contributing hydrogen for defect passivation.

[0032] In certain exemplary implementations, the SiCE layer deposited by the DALP systems disclosed using the methods provided, is paired with a doped polycrystalline silicon (poly-Si) layer deposited atop it, with a thickness of about 20 nanometers. This poly-Si layer can be doped with, for example, phosphorus (for n-type TOPCon) or boron (for p-type TOPCon) to create a conductive pathway for majority carriers. The doping process enhances carrier selectivity by aligning energy bands at the interface, ensuring efficient extraction of one carrier type (electrons or holes) while reflecting the other. The combination of SiO2 and doped poly-Si forms a passivating contact thatsimultaneously minimizes recombination and maintains low contact resistance, a key advantage over conventional solar cell designs

[0033] It is noted, that controlling final hydrogen content in SiNxlayers for photovoltaic cells can be beneficial to the long-term reliability and longevity of the panel, because hydrogen passivates dangling bonds at the silicon surface, reducing carrier recombination and enhancing minority carrier lifetimes. Predetermined hydrogen concentrations e.g., between about 15% and about 25 atomic %, can be used to reduce defect passivation while simultaneously avoiding instability from excess hydrogen effusion during subsequent high-temperature processing and cycling. Pre-treating the front panel with hydrogen plasma introduces reactive hydrogen species that bond to subsurface defects, creating nucleation sites for subsequent SiNxdeposition and ensuring uniform hydrogen distribution. The DALP systems disclosed, a coupled hydrogen plasma source is operable to generate a low-power (e.g., 10-50 W) plasma at 0.1-1 Torr, with exposure time of between about 5 sec. and about 30 seconds, which is calibrated to substrate temperature of between about 200 and about 400°C and plasma density p of between about IO10e-cm’3and about 1011ccm3). The substantially hermetically sealed microreactor confines the plasma to the target area via the nozzle’s peripheral wall, while mass flow controllers included with the system regulate H2gas inflow and turbomolecular vacuum pumps evacuate byproducts (e.g., atomic hydrogen clusters) to prevent contamination. FTIR spectroscopy integrated into the DALP system can be used to monitor Si-H and N-H bond formation in real time, adjusting plasma parameters (e.g., hydrogen inflow and exposure times) to achieve the target hydrogen content quantified by absorption peaks at 3350 cm1(N-H) and 2160 cm1(Si-H). This in-situ plasma pretreatment can be used to ensure stoichiometric control and interfacial compatibility with subsequent DALP-deposited SiNx, improving cell efficiency by 0.5-1.2% absolute compared to ex-situ methods.

[0034] In an exemplary implementation, the substrate is a semiconductor wafer, the method comprising: providing the semiconductor wafer having a front panel and a rear panel, wherein the substrate of the semiconductor wafer is a silicon-based substrate, or a germanium-based substrate; and using the DALP system, depositing a passivation layer over the substrate having a thickness of between about 4 nanometer (nm) and about 110 nm of silicon nitride (SiNx), or aluminum oxide (AI2O3) on the front panel surface, and optionally on the rear panel surface. Semiconductor wafers utilize silicon nitride or aluminum oxide passivation depending on substrate type. Silicon wafers are typically passivated with SiNxlayers having thickness between 70-100 nm to achieve fixed chargedensities QfiXaround IxlO12Gem2, while germanium wafers typically use AI2O3 layers ranging from 4-10 nm to suppress interface trap densities below 5xlO10eV 'em2. Use examples include logic chips with leakage currents below 1 pA / pm and short-wave infrared (SWIR) image sensors achieving quantum efficiencies exceeding 80% at wavelengths near 1550 nm.

[0035] Additionally, or alternatively the step of depositing aluminum oxide (AI2O3), when used, on the front panel surface, and optionally on the rear panel surface, at a thickness of between about 4 nm and about 35 nm, further comprises: using the DALP system, creating a stacked lattice by depositing a plurality of alternating sub layers of AI2O3, and TiCh, each the AI2O3 sub-layer having a thickness of between about 0.5 nm and about 2 nm, and each layer of the TiCh layer having a thickness of between about 0.3 nm and about 1.0 nm. Here too, alternating sub-layers of AI2O3 (0.5-2 nm) and Ti()2(0.3-1 nm) in a superlattice structure can enhance passivation by synergizing AFOs’s high negative fixed charge density QfiXof about 1013Coulomb-cm2, with TiCUs lower propensity for interfacial defects. The AI2O3 sub-layers provide strong field-effect passivation, repelling minority carriers from the silicon surface (referring to the type of charge carriers; electrons, or holes, which are present in a smaller concentration compared to the majority carriers), while ultrathin Ti()2interlayers mitigate fixed charge accumulation at the AbCWSi interface, thereby reducing upward band bending and recombination-active defect density by 40-60%. This nanolaminate design can be used in yet another exemplary implementation, to suppresses oxygen vacancy diffusion through TiCUs high chemical stability, preventing Fermi-level pinning caused by A DOG s intrinsic oxygen vacancies. The periodicity (2-10 repeating units) can create a graded band structure that minimizes interfacial strain, improving adhesion and thermal stability during metallization (350— 450°C).

[0036] Additionally, TiCb’s higher refractive index (2.4-2.7) compared to AI2O3 (1.7-1.8) enhances anti-reflective properties when deposited on PERC cells (see e.g., FIG. 5), reducing frontsurface reflection losses by 1.2-1.8% absolute. The superlattice’s defect-trapping interfaces lower bulk trap density to p<5x 1010cm3-cV, which can be measured by deep-level transient spectroscopy (DLTS), while simultaneously maintaining surface recombination velocities v<5 cm / s.

[0037] As illustrated in FIG. 4, which depicts an optical image of solar cell corner edge passivated using the methods disclosed, with a passivating layer of TiO2. A TiO21ine was deposited along the edge of a 25x50 mm2solar cell substrate. Deposition time was 1.5h. Conventional fabrication would require 2 complete AED + lithography + etching process cycles (front and back ofthe cell). The effects of the passivation are depicted in FIG. 5, showing from left to right, the major carrier lifetime improvement after edge passivation with TiCF. As illustrated in FIG. 5, using the grayscale, before passivation (left-most image) carrier lifetime, referring to the average time a minority carrier (e.g., electron in p-type material or hole in n-type material) can exist before recombining) is between about 280 ps and about 420 ps, where after passivation (second image from left) , carrier lifetime improves to between about 350 ps and about 580 ps, while after annealing at T1 (second image from right), carrier lifetime improves to between about 380 ps and about 600 ps, whereas, annealing at T2 was not as effective, resulting in carrier lifetimes of between about 380 ps and about 590 ps.

[0038] In an exemplary implementation, the substrate is a component of the MEMS device, the method comprising: providing the MEMS device, wherein the MEMS device comprises: at least one movable component, a side wall of a deep etched feature, a sacrificial layer interface, or a combination thereof; and using the DALP system, depositing a passivation layer having a thickness of between about 1 nanometer (nm) and about 200 nm of silicon nitride (SiNx), or a self-assembling carboxylate layer on the at least one movable component, the side wall of a deep etched feature, the sacrificial layer interface, or their combination. It is noted, that MEMS devices benefit from passivation using silicon nitride or self-assembled monolayers (SAMs). S0N4 layers deposited at thicknesses between 100-200 nm are used in certain implementations, as wear resistance by reducing friction coefficients between moving parts to below 0.1, while SAMs formed from zirconium-carboxylate complexes can be used additionally, or alternatively, to create hydrophobic surfaces with contact angles exceeding 110°. Use examples include MEMS accelerometers designed for ±50g ranges in industrial vibration sensors and microphone diaphragms resistant to humidity-induced sensitivity drifts.

[0039] Additionally, or alternatively, the self-assembling carboxylate layer comprises zirconium-carboxylate coordination complexes, whereby the step of depositing comprises: using the DALP system, exposing the substrate to a ZrCL precursor, and reacting the deposited precursor with an adipic acid reactant, forming a monolayer of Zr-carboxylate, following exposure to inert gas and removal of unreacted precursor and reactant.

[0040] IILV optoelectronic devices typically employ silicon nitride deposited via low-frequency PECVD or epitaxial indium phosphide cladding layers depending on application requirements. Epitaxial growth of indium phosphide (InP) refers to the crystalline deposition of InPlayers on a substrate where the atomic arrangement of the deposited material aligns with the substrate’s crystal lattice. Epitaxial growth can occur via homoepitaxy, where InP is grown on an InP substrate, or heteroepitaxy, where InP is grown on a dissimilar substrate, such as silicon.Homoepitaxy is used for lattice-matched structures, while heteroepitaxy requires careful management of lattice mismatch (-8% for InP / Si), which can be controlled using the systems and methods disclosed herein.

[0041] SiNxpassivation layers with thickness of about 80 nm deposited using the methods provided, are configured to suppress surface recombination velocities to below -IxlO4cm / s in nanopillar sidewalls or laser diode facets, while epitaxial InP cladding layers grown as heteroepitaxy at thicknesses between 2-3 nm enable room-temperature operation in nanowire-based III-V photodetectors. Use examples can be SWIR photodiodes achieving dark current densities below -1 nA / cm2and / or GaN-based VCSELs demonstrating wall-plug efficiencies exceeding -50%.

[0042] Accordingly and in another exemplary implementation, the substrate is a component of the III-V optoelectronic device, the method comprising: providing the III-V optoelectronic device, wherein the III-V optoelectronic device comprises a plurality of nanopillar sidewalls, a plurality of laser diode facets, a nanowire surface or a combination thereof; and using the DALP system, depositing a passivation layer having a thickness of between about 2 nanometer (nm) and about 90 nm of silicon nitride (SiNx), and / or indium phosphide (InP), on the plurality of nanopillar sidewalls, the plurality of laser diode facets, the nanowire surface or their combination.

[0043] Additionally, or alternatively, prior to the step of depositing silicon nitride (SiNx), and / or indium phosphide (InP), the method further comprises: pretreating the nanopillar sidewalls comprised with the III-V device, with a (NH^S solution, thereby chemically removing native oxides, such as gallium oxide (GazCh) and arsenic oxide (AS2O3), from the surface. These native oxides can introduce surface states that act as non-radiative recombination centers, significantly reducing the internal quantum efficiency (IQE, referring to percentage of incident photons that are converted into usable signals) of the device. The sulfur atoms from the (NH^hS solution chemically bond to the exposed GaAs surface, forming a stable Ga-S layer that passivates dangling bonds and prevents reoxidation under ambient conditions.

[0044] This pretreatment, when used, can create a clean and chemically inert interface, enhancing subsequent deposition of dielectric passivation layers, such as silicon nitride (SiNx), by improving adhesion and reducing interfacial defect density.

[0045] Furthermore, the InP passivation layer is formed using tertiarybutylphosphine (TBP) precursor and trimethylindium (TMIn) reactant having, V / III ratio configured to effect 2D layer-by-layer growth. It is noted that using tertiarybutylphosphine (TBP) and trimethylindium (TMIn) at a V / III ratio of about 100 enables two dimensional (2D) layer-by-layer growth of InP passivation layers by maintaining stoichiometric phosphorus (group V element) availability while suppressing indium (group III element) adatom migration. The relatively high V / III ratio ensures an excess of phosphorus radicals (P-related species) saturate surface sites growth, forcing sequential In-P bond formation and minimizing 3D island nucleation. This results in atomically smooth InP (mono)layers, as confirmed by Reflection high-energy electron diffraction (RHEED) oscillations and cross-sectional TEM. Having a layer-by-layer growth eliminates in certain implementations of the methods disclosed, interfacial defects (e.g., antiphase boundaries) by ensuring complete monolayer coverage before subsequent deposition, which is beneficial for passivating III-V nanopillars or laser facets. The 2D growth mode can also enable sub-nm thickness control (±0.1 nm) across high- aspectratio nanostructures, reducing surface recombination velocities to <103cm / s by eliminating trap states from incomplete bonding.

[0046] Additionally, the conformal coverage achieved via 2D growth seals oxygen-sensitive III-V surfaces (e.g., GaAs) more effectively than 3D modes, preventing As / Ga oxide formation and maintaining valence band offsets >1.9 eV. This is particularly advantageous for optoelectronic devices, where uniform passivation improves internal quantum efficiency by >30% in InP-clad nanowire LEDs and reduces threshold currents in laser diodes by minimizing facet oxidation-induced losses.

[0047] An exemplary implementation of a portion of the DALP system’s head, is illustrated in FIG.s 6A, 6B. As illustrated the DALP system comprises: a substrate plate (not shown) for holding the substrate; a print head 60 with a nozzle 605 defining a basal facet 610 adapted, sized and configured to selectably dispense onto a substrate (engaged by the substrate plate) at least one precursor and at least one reactant; a first inlet 623 (see e.g., FIG. 6B) supply conduit in fluid communication with: the nozzle (see e.eg, FIG. 6A outlet 613) and a precursor reservoir (not shown), as well as a second inlet supply 624 conduit in fluid communication with: the nozzle (see e.g., FIG. 6A outlet 614); and a reactant reservoir (not shown) a third inlet supply conduit in fluid communication with: the nozzle (see e.eg, FIG. 6A outlet 615); and an inert gas reservoir (not shown) one or more exhaust conduit(s) 611, 612 in fluid communication with the nozzle, adaptedsized and configured to remove: non-deposited precursor and / or non-deposited reactant, as well as residual inert gas; and a housing 600 having an apical surface 601, and a basal surface 602, with a plurality of recesses 606i configured to receive a plurality of anchoring members (e.g., screws, detents, and the like), the housing adapted sized and configured to accommodate at least a portion of the nozzle 605.

[0048] In yet another exemplary implementation, housing 600 can further comprise a housing portion 61 illustrated in FIG. 6C, extending basally from basal facet 602 of housing 600, coupled to the nozzle 605, defining a peripheral wall 654 having a predetermined perimeter cross section which can be any polygon or a circle, extending basally beyond the basal facet 610 of the nozzle, wherein the housing portion 61 is adapted, sized and configured to form a discrete reaction environment 660 formed as a reaction chamber (interchangeable wit “microreactor”) between the at least one precursor and the reactant while defining a discrete reaction area on the substrate. Housing portion 61 can be reversibly coupled to the basal facet 602 of housing 600, and can further define an upper flange 640 having upper surface 651 and a basal surface 652, with side wall 653. Upper surface 651, may further define an annular channel 655, adapted sized and configured to accommodate a sealant, for example, an O-ring (not shown).

[0049] In certain exemplary implementations, housing portion may be further adapted to accommodate a portion of the substrate, like an edge of a wafer. This can be done by, for example creating a window having a length sized and configured to accommodate a certain section of the wafer. It is further noted, that in the methods and systems disclosed, the substrate plate may be operable to move in X, Y, and Z axes relative to the (optionally static) nozzle while, in other exemplary implementation, the nozzle and the DALP system may be operable to move in X, Y, and Z axes relative to the substrate, which may be static.Definitions:

[0050] In the context of the disclosure, the term "operable" means the system and / or the device and / or the program, or a certain element or step is fully functional, sized, adapted, and calibrated, comprises elements for, and meets applicable operability requirements to perform a recited function when activated, coupled, implemented, actuated, effected, realized, or when an executable program is executed by at least one processor associated with the system and / or the device. In relation to systems and circuits, the term "operable" means the system and / or the circuit is fully functional and calibrated,comprises logic for, having the hardware and firmware necessary, as well as the circuitry for, and meets applicable operability requirements to perform a recited function when executed by at least one processor.

[0051] In the context of the disclosure, the term “passivation layer”, refers to a layer of material that functions as a shielding and / or coating layer on a substrate and is formed from a chemical reaction of the substrate with a reactant.

[0052] The term “fluid communication” refers to any area, a structure, or communication that allows for fluid communication between at least two fluid retaining regions, for example, a tube, duct, conduit or the like connecting two regions. One or more fluid communication can be configured or adapted to provide for example, vacuum driven flow, electrokinetic driven flow, control the rate and timing of fluid flow by varying the dimensions of the fluid communication passageway, rate of circulation or a combination comprising one or more of the foregoing. Alternatively, and in another exemplary implementation, the term “in communication” can also refer to gaseous and / or vapor communication, i.e. that gas and / or vapor may be transferred from one volume to another volume since these volumes are in communication. This term does not exclude the presence of a gas shutter or valve between the volumes that may be used to interrupt the gas communication between the volumes.

[0053] The terms “first,” “second,” and the like, when used herein do not denote any order, quantity, or importance, but rather are used to denote one element from another. The terms “a”, “an” and “the” herein do not denote a limitation of quantity and are to be construed to cover both the singular and the plural, unless otherwise indicated herein or clearly contradicted by context. The suffix “(s)” as used herein is intended to include both the singular and the plural of the term that it modifies, thereby including one or more of that term (e.g., the duct(s) includes one or more ducts). Reference throughout the specification to “one exemplary implementation”, “another exemplary implementation”, “an exemplary implementation”, and so forth, means that a particular element (e.g., feature, structure, and / or characteristic) described in connection with the exemplary implementation is included in at least one exemplary implementation described herein, and may or may not be present in other exemplary implementations. In addition, it is to be understood that the described elements may be combined in any suitable manner in the various exemplary implementations.

[0054] In addition, for the purposes of the present disclosure, directional or positional terms such as "top", “apical”, “basal”, “proximal”, “distal”, "bottom", "upper," "lower," "side," "front,""frontal," "forward," "rear," "rearward," "back," "trailing," "above," "below," "left," "right," "radial ," "vertical," "upward," "downward," "outer," "inner," "exterior," "interior," "intermediate," etc., are merely used for convenience in describing the various exemplary implementations of the present disclosure.

[0055] The term “coupled”, including its various forms such as “operably coupled”, "coupling" or "couplable", refers to and comprises any direct or indirect, structural coupling, connection or attachment, or adaptation or capability for such a direct or indirect structural or operational coupling, connection or attachment, including integrally formed components and components which are coupled via or through another component or by the forming process (e.g. an electromagnetic field). Indirect coupling may involve coupling through an intermediary member or adhesive, or abutting and otherwise resting against, whether frictionally (e.g., against a wall) or by separate means without any physical connection.

[0056] The term "comprising" and its derivatives, as used herein, are intended to be open ended terms that specify the presence of the stated features, elements, components, groups, integers, and / or steps, but do not exclude the presence of other unstated features, elements, components, groups, integers and / or steps. The foregoing also applies to words having similar meanings such as the terms, "including", "having" and their derivatives.

[0057] All ranges disclosed herein are inclusive of the endpoints, and the endpoints are independently combinable with each other. Furthermore, the terms “first,” “second,” and the like, herein do not denote any order, quantity, or importance, but rather are used to denote one element from another.

[0058] Likewise, the term "about" means that amounts, ranges, sizes, formulations, parameters, and other quantities and characteristics are not and do not need be exact, but may be approximate and / or larger or smaller, as desired, reflecting tolerances, conversion factors, rounding off, measurement error and the like, and other factors known to those of skill in the art. In general, an amount, ranges, size, formulation, parameter or other quantity or characteristic is "about" or "approximate" whether or not expressly stated to be such and is intended to include the degree of error associated with measurement of the particular quantity based upon the equipment available at the time of filing the application. For example, “about” can include a range of + / — 15% or 10%, or 5% of a given value.

[0059] In an exemplary implementation, the first surface modifier, or reactant can be, for example, at least one of: Trimethylaluminum (TMA), Tetrakis(dimethylamino)titanium (TDMAT), Bis(cyclopentadienyl)zirconium(IV) dichloride (Cp2ZrC12), Tetrakis(ethylmethylamino)hafnium (TEMAH), and Bis(ethylcyclopentadienyl)ruthenium(II) (Ru(EtCp)2), Titanium tetrachloride (TiCU), Tungsten hexafluoride (WFe), Hafnium tetrachloride (HfCU), Ruthenium trichloride (RuCh), and Molybdenum hexacarbonyl (Mo(CO)e), Diethyl zinc (DEZ), Dimethylamino magnesium (DMAMg), Bis(cyclopentadienyl)iron(II) (Cp2Fe), Triisobutylaluminum (TIBA), Tetrakis(trimethylsilyl)hafnium (TTHf), Aluminum isopropoxide (Al(O-iPr)3), Titanium isopropoxide (Ti(O-iPr)4), Zirconium n-propoxide (Zr(O-nPr)4), Hafnium ethoxide (Hf(OEt)4), Tantalum ethoxide (Ta(OEt)s), Bis(t-butylamino)silane (BTBAS), Bis(t-butylamino)zinc (BTBAS2), Bis(t-butylamino)titanium (BTBAT), Bis(t-butylamino)zirconium (BTBZ), Bis(t-butylamino)hafnium (BTBAH), Dimethylcyclopentadienyl platinum (MeCpPtMes), Bis(methylcyclopentadienyl)nickel (Ni(MeCp)2), Cyclopentadienyltungsten tricarbonyl (CpW(CO)s), Dimethylcyclopentadienyl manganese tricarbonyl (MeCpMn(CO)3), Iron pentacarbonyl (Fe(CO)s), A1(CH3)3 , A1C1(CH3)2, Sn(acac)2, BCI3, Hhfac , HCOOH, PMe3, dHF, Ga(CH3)3, SiCb, TiCl4and HC1.

[0060] In another exemplary implementation, the inert gas can be at least one of: Nitrogen, Argon, Helium, and Neon. It is noted that the choice of inert gas depends on factors such as process requirements, film properties, equipment capabilities, and cost considerations. Additionally, specific applications or variations may call for the use of other inert gases or gas mixtures.

[0061] In addition, another exemplary implementation, the reactant, coreactant or coreagent in gas or plasma phase can be one or a mixture of: HF, CHF3, CF4., H2, NF3 , XeF2 , BCI3 / Q2 , C4H3F7O, C3H3F3, HBr, O2, CF4 / O2 F2 / He, C4F8, CH3F, A1(CH3)3, C4F8plasma, WF6, BCI3 , SF4, SO2CI2 , and Hacac. It is noted that the choice of reactant depends on factors such as process requirements, film properties, equipment capabilities, and cost considerations. Additionally, specific applications or variations may call for the use of other reagents or reagent gas mixtures.

[0062] Surface treatment of the substrate used in the methods described herein can be at least one of: solvent (e.g., acetone, isopropyl alcohol (IPA), or ultrasonic cleaning to remove organic contaminants and particles) or acid (e.g., sulfuric acid (H2SO4) or hydrochloric acid (HC1)), cleaning; plasma (e.g., using reactive gases like oxygen (O2), hydrogen (H2), or fluorine-based gases (CF4, SFe), is done to remove native oxide layers or to pattern the substrate surface), and / or wet (e.g., to remove unwanted layers or roughen the surface for improved film adhesionfor example, for sequentialinfiltration synthesis etching; and surface functionalization (e.g., silane coupling agents, such as APTES (aminopropyltriethoxysilane) or HMDS (hexamethyldisilazane), by introducing specific chemical groups that enhance film bonding or modify surface energy).

[0063] Accordingly, provided herein is a method for passivating a substrate, implemented in a direct atomic layer deposition (DALP) system, the method comprising: using the DALP system, depositing a passivating material on the substrate over a predetermined area of the substrate, wherein the step of depositing comprises forming an area-conforming surface having a predetermined thickness, the predetermined thickness is adapted, sized and configured to passivate the predetermined area of the substrate, wherein (i) the DALP system comprises: a substrate plate for holding the substrate, a nozzle defining a basal facet adapted, sized and configured to selectably dispense onto the substrate at least one precursor and at least one reactant, a first inlet supply conduit in fluid communication with: the nozzle, and a precursor reservoir a second inlet supply conduit in fluid communication with: the nozzle, and a reactant reservoir a third inlet supply conduit in fluid communication with: the nozzle, and an inert gas reservoir one or more exhaust conduit in fluid communication with the nozzle, adapted sized and configured to remove: non-deposited precursor, non-deposited reactant, and residual inert gas, and a housing, adapted sized and configured to accommodate at least a portion of the nozzle, wherein (ii) the substrate is a component of: an edge emitting laser (EEL), a photovoltaic (PV) device, a semiconductor wafer, a high-power electronic device, a microelectromechanical system (MEMS) device, or a IILV optoelectronic device, (iii) and / or a component of the EEL, the method comprising: providing an EEL device having a front cleaved facet surface, a rear cleaved facet surface and an outer surface, and using the DALP system, depositing a passivation layer having a thickness of between about 2 nanometer (nm) and about 10 nm of hafnium oxide (HfCL), or an amorphous silicon (Sia), on each of the front cleaved facet surface, and the rear cleaved facet surface, (iv) or wherein the substrate is a panel of the PV device, the method comprising: providing the panel of the PV device, wherein the panel is a Passivated Emitter and Rear Cell (PERC), TopCon cell, heterojunction cell (HJT) and the like, each having a front panel facet and a rear panel facet, and using the DALP system, depositing a passivation layer having a thickness of between about 2 nanometer (nm) and about 110 nm of silicon nitride (SiNx), aluminum oxide (A12O3), Titanium Oxide (TiO2) or hafnium oxide (HfO2), on the front panel surface, and optionally on the rear panel surface and / or panel sides, (v) or wherein the substrate is a semiconductor wafer, the method comprising: providing the semiconductor wafer, wherein thesubstrate of the semiconductor wafer is a silicon-based substrate, or a germanium-based substrate, and using the DALP system, depositing a passivation layer over the silicon-based substrate, or the germanium-based substrate, the passivation layer having a thickness of between about 4 nanometer (nm) and about 110 nm of silicon nitride (SiNx), or aluminum oxide (A12O3) on the front panel surface, and optionally on the rear panel surface, or (vi) wherein the substrate is a component of the MEMS device, the method comprising: providing the MEMS device, wherein the MEMS device comprises: at least one movable component, a side wall of a deep etched feature, a sacrificial layer interface, or a combination thereof, and using the DALP system, depositing a passivation layer having a thickness of between about 1 nanometer (nm) and about 200 nm of silicon nitride (SiNx), or a self-assembling carboxylate layer on the at least one movable component, the side wall of a deep etched feature, the sacrificial layer interface, or their combination, or (vii) wherein the substrate is a component of the III-V optoelectronic device, the method comprising: providing the III-V optoelectronic device, wherein the III-V optoelectronic device comprises a plurality of nanopillar sidewalls, a plurality of laser diode facets, a nanowire surface or a combination thereof, and using the DALP system, depositing a passivation layer having a thickness of between about 2 nanometer (nm) and about 90 nm of silicon nitride (SiNx), and / or indium phosphide (InP), on the plurality of nanopillar sidewalls, the plurality of laser diode facets, the nanowire surface or their combination, wherein (viii) depositing the passivation layer further comprises: using the DALP system, annealing the HI'CL or Sialayer at 300-450°C under an inert atmosphere, the annealing configured to reduce interfacial defect density to <10ncm2as measured by cross-sectional TEM, (ix) the step of depositing the HI'CL passivation layer further comprises transitioning from a deposition of a HfCL-rich composition on each of the front cleaved facet surface, and the rear cleaved facet surface, to a HfSiOxcomposition at the outer surface, with total thickness variance <±0.2 nm across each of the front cleaved facet surface, and the rear cleaved facet surface, wherein the HfO2-rich composition comprises no less than 95% (w / w) of HfCL, and wherein the ratio between Hf:Si is about 3:1, wherein (x) the DALP system further comprises a plasma generator in fluid communication with the nozzle, the plasma generator being coupled to a hydrogen source, the method further comprising: prior to the step of depositing, using the DALP system, pre-treating the front panel surface with a hydrogen plasma , wherein the plasma exposure time is configured to yield a predetermined final SiNxhydrogen content as quantified by FTIR absorption at 3350cm wherein (xi) the step of depositing aluminum oxide (AI2O3) on the front panel surface, and optionally on the rear panel surface, at a thickness of between about 4 nm andabout 35 nm, further comprises: using the DALP system, depositing a plurality of sub layers of AI2O3, and TiCh, the AI2O3 sub-layer having a thickness of between about 0.5 nm and about 2 nm, and the TiCh layer having a thickness of between about 0.3 nm and about 1.0 nm, (xii) the method further comprising doping the SiNxlayer in situ with terbium (Tb3+) ions via alternating Tb3+pulses of the precursor used in the DALP system, wherein the Tb-doped SiNxis configured to have a fractional weight concentration (w / w) configured to yield 20% higher breakdown field compared to undoped layers, wherein (xiii) the self-assembling carboxylate layer comprises zirconium-carboxylate coordination complexes, and wherein the step of depositing comprises: using the DALP system, exposing the substrate to a ZrCL precursor reacting the deposited precursor with an adipic acid reactant, forming a monolayer, wherein (xiv), prior to the step of depositing the method further comprises: pretreating the nanopillar sidewalls with a (NLL^S solution, (xiv), wherein the InP passivation layer is formed using tertiarybutylphosphine (TBP) precursor and trimethylindium (TMIn) reactant having, V / III ratio configured to effect 2D layer-by-layer growth, and wherein (xv) the housing further comprises a housing portion extending basally from basal facet of the nozzle, defining a peripheral wall having a predetermined perimeter cross section extending basally beyond the basal facet of the nozzle, wherein the housing portion is adapted, sized and configured to form a discrete reaction environment between the at least one precursor and the reactant

[0064] While in the foregoing specification the devices, systems and methods, have been described in relation to certain preferred exemplary implementations, and many details are set forth for purpose of illustration, it will be apparent to those skilled in the art that the disclosure is susceptible to additional exemplary implementations and that certain of the details described in this specification and as are more fully delineated in the following claims can be varied considerably without departing from the basic principles of this disclosure.

Claims

What is claimed is1. A method for passivating a substrate, implemented in a direct atomic layer deposition (DALP) system, the method comprising: using the DALP system, depositing a passivating material on the substrate over a predetermined area of the substrate, wherein the step of depositing comprises forming an area-conforming surface having a predetermined thickness, the predetermined thickness is adapted, sized and configured to passivate the predetermined area of the substrate.2 The method of claim 1, wherein the DALP system comprises:a) a substrate plate for holding the substrate;b) a nozzle defining a basal facet adapted, sized and configured to selectably dispense onto the substrate at least one precursor and at least one reactant;c) a first inlet supply conduit in fluid communication with:i. the nozzle; andii. a precursor reservoird) a second inlet supply conduit in fluid communication with:i. the nozzle; andii. a reactant reservoire) a third inlet supply conduit in fluid communication with:i. the nozzle; andii. an inert gas reservoirf) one or more exhaust conduit in fluid communication with the nozzle, adapted sized and configured to remove:i. non-deposited precursor;ii. non-deposited reactant; andiii. residual inert gas; andg) a housing, adapted sized and configured to accommodate at least a portion of the nozzle.

3. The method of claim 2, wherein the substrate is a component of: an edge emitting laser (EEL), a photovoltaic (PV) device, a semiconductor wafer, a high-power electronic device, a microelectromechanical system (MEMS) device, or a IILV optoelectronic device.4 The method of claim 3, wherein the substrate is a component of the EEL, the method comprising:a) providing an EEL device having a front cleaved facet surface, a rear cleaved facet surface and an outer surface; andb) using the DALP system, depositing a passivation layer having a thickness of between about 2 nanometer (nm) and about 10 nm of hafnium oxide (HfCL), or an amorphous silicon (Sia), on each of the front cleaved facet surface, and the rear cleaved facet surface.5 The method of claim 3, wherein the substrate is a panel of the PV device, the method comprising:a) providing the panel of the PV device, wherein the panel is a Passivated Emitter and Rear Cell (PERC), TopCon cell, heterojunction cell (HJT) and the like, each having a front panel facet and a rear panel facet; andb) using the DALP system, depositing a passivation layer having a thickness of between about 2 nanometer (nm) and about 110 nm of silicon nitride (SiNx), aluminum oxide (A12O3), Titanium Oxide (TiO2) or hafnium oxide (HfO2), on the front panel surface, and optionally on the rear panel surface and / or panel sides.6 The method of claim 3, wherein the substrate is a semiconductor wafer, the method comprising:a) providing the semiconductor wafer, wherein the substrate of the semiconductor wafer is a silicon-based substrate, or a germanium-based substrate; andb) using the DALP system, depositing a passivation layer over the silicon-based substrate, or the germanium-based substrate, the passivation layer having a thickness of betweenabout 4 nanometer (nm) and about 110 nm of silicon nitride (SiNx), or aluminum oxide (A12O3) on the front panel surface, and optionally on the rear panel surface.

7. The method of claim 3, wherein the substrate is a component of the MEMS device, the method comprising:a) providing the MEMS device, wherein the MEMS device comprises: at least one movable component, a side wall of a deep etched feature, a sacrificial layer interface, or a combination thereof; andb) using the DALP system, depositing a passivation layer having a thickness of between about 1 nanometer (nm) and about 200 nm of silicon nitride (SiNx), or a self-assembling carboxylate layer on the at least one movable component, the side wall of a deep etched feature, the sacrificial layer interface, or their combination.8 The method of claim 3, wherein the substrate is a component of the III-V optoelectronic device, the method comprising:a) providing the III-V optoelectronic device, wherein the III-V optoelectronic device comprises a plurality of nanopillar sidewalls, a plurality of laser diode facets, a nanowire surface or a combination thereof; andb) using the DALP system, depositing a passivation layer having a thickness of between about 2 nanometer (nm) and about 90 nm of silicon nitride (SiNx), and / or indium phosphide (InP), on the plurality of nanopillar sidewalls, the plurality of laser diode facets, the nanowire surface or their combination.9 The method of claim 4, wherein depositing the passivation layer further comprises:a) using the DALP system, annealing the HI'CL or Sialayer at 30( 50°C under an inert atmosphere, the annealing configured to reduce interfacial defect density to <1O11cm-2as measured by cross-sectional TEM.10 The method of claim 4, wherein the step of depositing the HfO2passivation layer further comprises transitioning from a deposition of a HfO2-rich composition on each of the front cleaved facet surface, and the rear cleaved facet surface, to a HfSiOxcomposition at the outer surface, withtotal thickness variance <±0.2 nm across each of the front cleaved facet surface, and the rear cleaved facet surface, wherein the HfO2-rich composition comprises no less than 95% (w / w) of HfO2, and wherein the ratio between Hf:Si is about 3:1.

11. The method of claim 5, wherein the DALP system further comprises a plasma generator in fluid communication with the nozzle, the plasma generator being coupled to a hydrogen source, the method further comprising: prior to the step of depositing, using the DALP system, pre-treating the front panel surface with a hydrogen plasma , wherein the plasma exposure time is configured to yield a predetermined final SiNxhydrogen content as quantified by FTIR absorption at 3350 cm-1.

12. The method of claim 5, wherein the step of depositing aluminum oxide (AI2O3) on the front panel surface, and optionally on the rear panel surface, at a thickness of between about 4 nm and about 35 nm, further comprises: using the DALP system, depositing a plurality of sub layers of AI2O3, and TiCL, the AI2O3 sub-layer having a thickness of between about 0.5 nm and about 2 nm, and the TiCL layer having a thickness of between about 0.3 nm and about 1.0 nm.

13. The method of claim 6, further comprising doping the SiNxlayer in situ with terbium (Tb3+) ions via alternating Tb3+pulses of the precursor used in the DALP system, wherein the Tb-doped SiNxis configured to have a fractional weight concentration (w / w) configured to yield 20% higher breakdown field compared to undoped layers.

14. The method of claim 7, wherein the self-assembling carboxylate layer comprises zirconiumcarboxylate coordination complexes, and wherein the step of depositing comprises:a) using the DALP system, exposing the substrate to a ZrCL precursorb) reacting the deposited precursor with an adipic acid reactant, forming a monolayer.

15. The method of claim 8, wherein, prior to the step of depositing the method further comprises: pretreating the nanopillar sidewalls with a (NH02S solution.

16. The method of claim 8, wherein the InP passivation layer is formed using tertiarybutylphosphine (TBP) precursor and trimethylindium (TMIn) reactant having, V / III ratio configured to effect 2D layer-by-layer growth.

17. The method of claim 1, wherein the housing further comprises a housing portion extending basally from basal facet of the nozzle, defining a peripheral wall having a predetermined perimeter cross section extending basally beyond the basal facet of the nozzle, wherein the housing portion is adapted, sized and configured to form a discrete reaction environment between the at least one precursor and the reactant.