A composite turbulence controller for tundish in continuous slab casting

By designing a composite slab continuous cast tundra turbulence controller, using a special structure of a round table-shaped core and isostatic forming base plate, the problems of poor performance and high cost of the tundra turbulence controller in the existing technology are solved, and the Improved liquid molten steel flow and extended service life.

CN111113635BActive Publication Date: 2024-11-15LAIWU STEEL YINSHAN SECTION CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202010065262.1
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2020-01-20
Publication Date
2024-11-15
Estimated Expiration
2040-01-20

AI Technical Summary

Technical Problem

The existing tundra turbulence controller cannot meet the performance requirements of metallurgical functionalization, longevity and low cost at the same time, and the overall performance is poor, making it prone to brick removal and lack of quality stability.

Method used

Designed with composite slab continuous casting tundra turbulence controller, including composite structure of shell, sleeve and bottom plate. The sleeve is a round table-shaped magnesium prefabricated piece, and is made of disposable foam inner mold and magnesium casting, and the bottom plate is etc. The entire magnesium carbon brick formed by static pressure has a special cavity shape designed to improve the flow state of the steel, extend the residence time and reduce turbulence energy.

Benefits of technology

It improves the average residence time and service life of the steel, reduces the preparation cost, simplifies the process flow, enhances the overall performance, and solves the problems of poor performance and high cost in the existing technology.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN111113635B_ABST
    Figure CN111113635B_ABST
Patent Text Reader

Abstract

The invention relates to the technical field of continuous casting refractory material process, and specifically to a composite slab continuous casting tundish turbulence controller and a preparation method thereof. The tundish turbulence controller comprises an outer shell, a sleeve core and a bottom plate. The bottom plate is arranged on the bottom surface of an inner cavity of the outer shell, the sleeve core is arranged in the inner cavity of the outer shell, and the longitudinal center line of the sleeve core coincides with the longitudinal center line of the inner cavity of the outer shell. A joint seam is arranged between the outer shell and the sleeve core. The outer portion of the sleeve core is a truncated cone-shaped magnesium preform, the inner portion of the sleeve core is a parabolic inner cavity, the bottom plate is a whole piece of magnesium-carbon brick, the sleeve core is sleeved in the outer shell of the turbulence controller, and the joint seam between the outer shell and the sleeve core is filled with sintered magnesia sand, which can prolong the response time and average residence time of molten steel, increase the piston flow volume, reduce the dead zone volume, effectively reduce the turbulent energy of ladle injection, and better improve the flow field of molten steel in the tundish, and effectively solve the problem of injection slag roll in the impact zone.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of continuous casting refractory materials, in particular to a composite slab continuous casting tundish turbulence controller. Background Art

[0002] Setting a turbulence controller in the tundish of a continuous casting machine can change the route of molten steel in the tundish, prolong the residence time, and promote the floating and removal of inclusions, which plays an important role in improving the quality of the ingot. At the same time, it can slow down the scouring of the impact zone of the tundish working lining by the ladle injection and increase the continuous casting time of the tundish. In recent years, the production technology of turbulence controllers has developed towards metallurgical functionalization, longevity, and low cost, but the tundish turbulence controllers produced by existing technologies cannot meet the performance requirements of metallurgical functionalization, longevity, and low cost at the same time.

[0003] CN103658577B discloses a method for preparing a composite turbulence controller for a continuous casting tundish, wherein the composite turbulence controller comprises an outer shell, a bottom plate, a sleeve core, an expansion joint, and an anti-oxidation coating. The outer shell is cast and formed by magnesium casting material, the bottom plate is built by machine-pressed magnesium carbon bricks, the sleeve core is built by machine-pressed "fan-shaped" magnesium carbon bricks, expansion joints are set between the outer shell and the bottom plate, and between the outer shell and the sleeve core, and an anti-oxidation coating is applied on the outer surface of the sleeve core. However, the inner cavity shape of the invention is "cylindrical", which has a poor effect on suppressing the turbulent kinetic energy of the ladle injection turbulence, and is not conducive to improving the flow characteristics of the molten steel in the tundish. At the same time, the sleeve core is built by "fan-shaped" magnesium carbon bricks, which has poor overall performance, is prone to brick removal, and lacks quality stability.

[0004] CN109591158A discloses a tundish flow stabilizer, which is composed of an outer shell and a hollow inner cavity integrally inlaid, wherein the shape and size of the outer shell are designed to be adapted to the impact zone of the tundish, the center of the outer shell is concave, so that the outer shell is in the shape of a "concave", and the outer shell is formed by a steel fiber aluminum-magnesium castable preform, wherein the steel fiber aluminum-magnesium castable preform is integrally cast; and the hollow inner cavity is cylindrical and suitable for being embedded in the center of the outer shell, the hollow inner cavity is flush with the top of the outer shell, and the hollow inner cavity is masonry-made of a magnesium-carbon preform, wherein the carbon preform is isostatically pressed integrally; and a method for manufacturing a tundish flow stabilizer is also disclosed, by improving the inner cavity of the flow stabilizer from the traditional masonry molding method of multiple magnesium-carbon bricks to an integrally pressed molding method, thereby eliminating the easily corroded inner cavity brick seams in the traditional flow stabilizer, and completely solving the problem of steel seepage and steel penetration in the brick seams of the inner cavity of the traditional flow stabilizer, and greatly extending the life of the tundish flow stabilizer. However, the preparation cost is high and the promotion and application are limited.

[0005] The disposable foam inner mold is made of existing polystyrene foam and is suitable for various inner cavity shapes and specifications. It is disposable and does not require demolding. It is simple and convenient, saving time and labor. It does not deform or absorb water during use and has good compression resistance, elasticity and rigidity.

[0006] Isostatic pressing is a molding method that subjects the clay to equal liquid static pressure in all directions. Liquid is used as the pressure transmission medium. The clay is loaded into an elastic mold and pressed into shape in a high-pressure cylinder. The isostatic press consists of a high-pressure container and a high-pressure oil pump. The high-pressure container is made of high-grade alloy steel and has a certain thickness to withstand huge pressure. The size of the container is selected according to the size of the molded product. The liquid medium in the high-pressure container can be oil, water or glycerin, etc. Brake oil or anhydrous glycerin is generally used. The compressibility of these two liquids is very small, and almost all the pressure can be transmitted to the elastic mold. Summary of the invention

[0007] The purpose of the present invention is to overcome the shortcomings of the prior art and provide a composite slab continuous casting tundish turbulence controller and a preparation method thereof. The composite structure of the main body shell, sleeve core and bottom plate is designed. The sleeve core is a truncated cone-shaped magnesium preform with a special inner cavity shape designed based on water model experimental research. It is cast using a disposable foam inner mold and magnesium castable. The bottom plate is a whole piece of magnesium-carbon brick formed by isostatic pressing, which meets the technical performance requirements of metallurgical functionalization and longevity.

[0008] To achieve the above-mentioned purpose, the present invention provides the following technical solutions: a composite slab continuous casting tundish turbulence controller, comprising a shell, a sleeve core and a bottom plate, wherein the bottom plate is arranged on the bottom surface of the inner cavity of the shell, the sleeve core is arranged in the inner cavity of the shell, and the longitudinal center line of the sleeve core coincides with the longitudinal center line of the inner cavity of the shell, and a joint seam is arranged between the shell and the sleeve core, characterized in that: the outer portion of the sleeve core is a truncated cone-shaped magnesium preform, so that the side wall thickness of the upper part of the sleeve core is greater than the side wall thickness of the lower part, which adapts to the side wall scouring and erosion rate of the upper part of the sleeve core being greater than the side wall of the lower part, and realizes the synchronization of the service life of various parts of the side wall of the sleeve core, and the inner and outer walls of the sleeve core are designed as a rotating surface as a whole , eliminating the crack problem caused by thermal stress concentration on the side wall of the core sleeve. The interior of the core sleeve is a parabolic cavity, and the bottom plate is a whole piece of magnesia-carbon brick. The cavity is divided into an upper part of the core sleeve cavity and a lower part of the core sleeve cavity. The upper part of the core sleeve cavity is a rotating surface with a circular arc cross-section, and the lower part of the core sleeve cavity is a concave rotating parabola. The bottom of the core sleeve cavity is open. The use of this shape of cavity has a direct impact on the flow state of the molten steel in the middle, prolonging the response time and average residence time of the molten steel, increasing the piston flow volume, and reducing the dead zone volume. It can effectively reduce the turbulent energy of the ladle injection and better improve the flow field of the molten steel in the tundish, and effectively solve the problem of slag rolling in the impact zone.

[0009] Preferably, a concave cavity is provided at the bottom of the inner cavity of the shell, the bottom plate matches the concave cavity, the bottom plate and the bottom of the inner cavity are in the same plane, and when pouring the bottom of the inner cavity of the shell, the concave cavity for accommodating the bottom plate is reserved by burying the mold.

[0010] Preferably, the core sleeve is a truncated cone-shaped magnesium prefabricated part cast by using a disposable foam inner mold and a magnesium castable, and the base plate is a whole piece of magnesium-carbon brick formed by isostatic pressing.

[0011] Furthermore, the diameter D1 of the upper bottom surface of the truncated cone core is 720-750 mm, and the diameter D2 of the lower bottom surface of the truncated cone is 635-665 mm; the upper part of the core cavity of the core of the turbulence controller is in a bell-mouth shape, the outer diameter ¢ is 480-500 mm, the arc radius R is 75-80 mm, and the height a of the upper part of the core cavity is 80-100 mm. The shape design of the upper part of the core cavity of the above-mentioned shape is conducive to effectively reducing the turbulent energy of the ladle injection and better improving the flow field of the molten steel in the tundish, which can reduce the scouring of the inner cavity wall by the steel flow, maintain the shape of the inner cavity wall, and improve the service life;

[0012] Furthermore, the lower part of the core cavity has a small upper opening and a large lower opening. The upper opening diameter d1 of the core is 420-440 mm, the lower opening diameter d2 is 460-480 mm, and the height h of the lower part of the core cavity is 320-350 mm. The design of the special shape of the lower part of the core cavity changes the running trajectory of the steel flow, extends the flow route, and extends the average residence time of the molten steel in the tundish.

[0013] Preferably, the bottom surface of the bottom plate is square, the side length c is 40-60 mm larger than d2, and the thickness b is 90-110 mm, so that the bottom of the sleeve core presses the bottom plate to prevent the bottom plate from floating and ensure that the steel flow does not impact the outer shell outside the bottom plate.

[0014] Preferably, the width of the joint is larger at the top and smaller at the bottom, with the upper width m being 10-15 mm and the lower width n being 5-10 mm, which can naturally increase the density of the filling material at the bottom of the joint and effectively prevent the problem of steel seepage from the top to the bottom of the joint.

[0015] By using the tundish turbulence controller with the above dimensions, the average residence time of the molten steel in the tundish can be increased by more than 6.7% year-on-year, the dead zone ratio can be reduced by more than 5.2% year-on-year, and the inclusion removal rate can be increased by more than 10% year-on-year.

[0016] The method for preparing the tundish turbulence controller with the above inner cavity shape comprises the following steps:

[0017] 1. Casting the shell with magnesium spinel castable;

[0018] 2. Casting the core sleeve with a disposable foam inner mold and magnesium casting material;

[0019] 3. preparing the base plate into a whole magnesia carbon brick by isostatic pressing;

[0020] 4. Apply a layer of magnesium coating with a thickness of 25-35mm on the outer surface of sintered magnesia;

[0021] 5. Install the core sleeve into the shell of the turbulence controller, ensure that the longitudinal center line of the core sleeve coincides with the longitudinal center line of the inner cavity of the shell, and fill the joint between the shell and the core sleeve with sintered magnesia sand with a particle size of ≤1mm, and naturally cure for 1 to 2 days.

[0022] The shape and size of the shell are designed according to the shape and size of the impact zone of the continuous casting tundish working lining, and are cast by using magnesium spinel castable produced by existing technology, and are prepared after natural curing and baking in a heating furnace.

[0023] The magnesium spinel castable is produced by existing technology, with MgO content ≥71wt%, volume density ≥3.03g / cm3, and flexural strength (1500°C) ≥9Mpa.

[0024] Preferably, the magnesium carbonaceous coating material refers to a coating material prepared by the prior art using recycled granular materials of waste magnesium carbon bricks with a particle size of 1mm≦<3mm and a particle size of 0.074mm<1mm and sintered magnesia sand fine powder, soft clay, silicon micropowder, sodium tripolyphosphate, etc. in a certain ratio, wherein the weight percentage of the recycled magnesium carbonaceous particles is 60-70%.

[0025] According to a preferred embodiment of the present invention, a preparation method for casting a core sleeve using a disposable foam inner mold and a magnesium castable comprises the following steps: adding the magnesium castable for the core sleeve into a mixer and dry mixing for 2 to 3 minutes, adding 4.0 to 5.0% water of the total weight of the material, wet mixing for 4 to 6 minutes, and after mixing, placing the castable into a core sleeve casting outer mold with a disposable foam inner mold, vibrating with a vibrating rod, and when no large bubbles emerge, the casting of the core sleeve is completed, removing the core sleeve casting outer mold after solidification for 12 to 24 hours, and naturally curing for 12 to 24 hours. Then bake in a heating furnace: ① heat up from room temperature to 120-150℃ at a heating rate of 10℃ / h; ② keep warm at 120-150℃ for 11-13h; ③ heat up to 220-250℃ at a heating rate of 10℃ / h; ④ keep warm at 220-250℃ for 7-9h; ⑤ heat up to 360-390℃ at a heating rate of 15℃ / h; ⑥ keep warm at 360-390℃ for 7-9h; ⑦ stop firing and cool naturally. After cooling to room temperature, clean up the residue of the disposable foam inner mold, and the core sleeve preparation is completed.

[0026] Preferably, according to the present invention, the bottom plate is prepared by isostatic pressing and is made of the following raw materials in percentage by weight:

[0027] Main material: sintered magnesia 76-84wt%

[0028] Auxiliary materials: flake graphite 11.5~16wt%

[0029] Antioxidant: 2-5wt% of one or a mixture of aluminum powder, silicon powder, silicon carbide powder

[0030] Binder: 3.5-4.0wt% phenolic resin.

[0031] The sintered magnesia is made of light-burned magnesia with a MgO content of 95wt% as raw material, produced by processes such as ball pressing and high-temperature vertical kiln calcination, with a MgO content of 94-95wt%, and is mixed with 1mm≦particle size≤3mm, 0.074mm<particle size<1mm, and particle size≦0.074mm.

[0032] The flake graphite has a purity C content of ≥98wt% and a particle size of 100 meshes.

[0033] The aluminum powder has a purity AI content of ≥99wt% and a particle size of 100 meshes.

[0034] The silicon powder has a purity Si content of ≥97wt% and a particle size of 100 meshes.

[0035] The silicon carbide has a purity SiC content of ≥94wt% and a particle size of 100 meshes.

[0036] The phenolic resin has a solid content of ≥72wt%, a residual carbon content of ≥42wt%, and a moisture content of ≤5wt%.

[0037] According to the present invention, the base plate is prepared by isostatic pressing, which comprises the following steps:

[0038] 1) Ingredients: weigh the above raw materials according to the above ratio;

[0039] 2) Mixing: preheat the mixer to 40-50°C, add sintered magnesia with a particle size of 1mm≦≤3mm and 0.074mm<particle size<1mm at low speed → add phenolic resin after dry mixing for 1-2 minutes → add flake graphite after wet mixing for 2-3 minutes → add sintered magnesia with a particle size of ≦0.074mm and antioxidant after wet mixing for 2-3 minutes → wet mixing for 2-3 minutes → high-speed mixing for 10-15 minutes → discharge, and the temperature of the mud during mixing is less than 70°C;

[0040] 3) Green body molding: fill the clay into the mold, then remove the air in the mold, press it under 200-250MPa with isostatic pressure and then take it out of the mold, and the green body molding is completed;

[0041] 4) Natural drying and baking: After the green body is naturally dried for 8 to 16 hours, it is put into the kiln for baking: ① Continuously heat from room temperature to 140-160℃ at a heating rate of 10℃ / h, and keep warm for 4 to 8 hours; ② Continuously heat from 140-160℃ to 200-220℃ at a heating rate of 10℃ / h, and keep warm for 16 to 24 hours; ③ Stop the fire and cool naturally to room temperature. The preparation of the base plate is completed, and its compressive strength is ≥40MPa.

[0042] Compared with the prior art, the present invention has the following beneficial effects:

[0043] (1) The composite structure design of the main body shell, sleeve core and bottom plate simplifies the preparation process and reduces the preparation cost.

[0044] (2) The core sleeve of the turbulence controller for the slab continuous casting tundish of the present invention is a truncated cone-shaped preform with a special inner cavity shape designed based on water model experimental research and application test verification. The results of the water model experimental research show that the tundish turbulence controller designed by the present invention is better than the composite turbulence controller for the continuous casting tundish described in CN103658577B: the average residence time of the molten steel in the tundish is increased by more than 6.7% year-on-year, and the dead zone ratio is reduced by more than 5.2% year-on-year. The present invention is used for a single-stream slab continuous casting tundish, and the total oxygen content in the molten steel in the crystallizer is reduced by more than 12% year-on-year.

[0045] (3) The core sleeve of the turbulence controller of the slab continuous casting tundish of the present invention is cast by a disposable foam inner mold and a magnesium castable, and the bottom plate is a whole piece of magnesium carbon brick formed by isostatic pressing, which improves the casting quality and the overall performance. It effectively solves the problems of poor overall performance, easy brick falling, and lack of quality stability of the composite turbulence controller of the continuous casting tundish described in CN103658577B. It is used for a single-stream slab continuous casting tundish and has a service life of more than 17-21 hours.

[0046] (4) The core sleeve of the turbulence controller of the slab continuous casting tundish of the present invention is cast by a disposable foam inner mold, which meets the design requirements of the inner mold with a special inner cavity shape. It does not require demolding, simplifies the preparation process, and shortens the preparation period. The preparation period is shortened by 8 to 24 hours year-on-year, realizing synchronous mass production and solving the problem that mass production is restricted by the number of steel films. BRIEF DESCRIPTION OF THE DRAWINGS

[0047] In order to more clearly illustrate the embodiments of the present invention or the technical solutions in the prior art, the drawings required for use in the embodiments or the description of the prior art will be briefly introduced below. Obviously, the drawings described below are only some embodiments of the present invention. For ordinary technicians in this field, other drawings can be obtained based on these drawings without paying creative work.

[0048] Figure 1 This is a front view of the structure of the composite slab continuous casting tundish turbulence controller of the present invention;

[0049] Figure 2 It is a top view of the structure of the composite slab continuous casting tundish turbulence controller of the present invention;

[0050] Figure 3 The present invention is a schematic diagram of the sleeve core of the composite slab continuous casting tundish turbulence controller being cast using a disposable foam inner mold.

[0051] In the figure, 1. outer shell; 2. core sleeve; 3. joint seam; 4. upper part of the inner cavity of the core sleeve; 5. lower part of the inner cavity of the core sleeve; 6. bottom plate; 7. disposable foam inner mold; 8. outer mold for casting the core sleeve. DETAILED DESCRIPTION

[0052] The technical scheme in the embodiments of the present invention will be clearly and completely described below in conjunction with the drawings in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, rather than all of the embodiments. The magnesium castables and magnesium coatings used in the embodiments are all produced using existing technologies.

[0053] See also Figure 1-3 ,

[0054] Embodiment 1:

[0055] like Figure 1 , Figure 2 , Figure 3 As shown, a composite slab continuous casting tundish turbulence controller comprises a shell 1, a core 2 and a bottom plate 6, wherein the bottom plate 6 is arranged on the bottom surface of the inner cavity of the shell 1, the core 2 is arranged in the inner cavity of the shell 1, and the longitudinal center line of the core 2 coincides with the longitudinal center line of the inner cavity of the shell 1, and a joint seam 3 is arranged between the shell 1 and the core 2, characterized in that: the outer portion of the core 2 is a truncated cone-shaped magnesium preform, the inner portion of the core 2 is a parabolic inner cavity, the bottom plate 6 is a whole piece of magnesium-carbon brick, and the inner cavity is divided into The core-sleeve cavity comprises an upper portion 4 and a lower portion 5 of the core-sleeve cavity. The upper portion 4 of the core-sleeve cavity is a rotating surface with a circular arc cross section, the lower portion 5 of the core-sleeve cavity is a concave rotating parabola, and the bottom of the core-sleeve cavity is open. The use of the inner cavity of this shape has a direct impact on the flow state of the molten steel in the middle, prolongs the response time and the average residence time of the molten steel, increases the piston flow volume, reduces the dead zone volume, can effectively reduce the turbulent energy of the ladle injection flow and better improve the flow field of the molten steel in the tundish, and effectively solves the problem of slag entanglement in the impact zone.

[0056] Preferably, the bottom of the inner cavity of the shell 1 is provided with an inner concave cavity, the bottom plate 6 matches the inner concave cavity, the bottom plate 6 and the bottom of the inner cavity are in the same plane, and when pouring the bottom of the inner cavity of the shell 1, the inner concave cavity for accommodating the bottom plate 6 is reserved by burying the tire mold.

[0057] Preferably, the core sleeve 2 is a truncated cone-shaped magnesium prefabricated part cast by using a disposable foam inner mold 7 and a magnesium castable, and the bottom plate 6 is a whole piece of magnesium-carbon brick formed by isostatic pressing.

[0058] The core sleeve 2 of the turbulence controller has a truncated cone shape with a large upper bottom surface and a small lower bottom surface. Preferably, the diameter D1 of the upper bottom surface of the truncated cone is 720 mm, and the diameter D2 of the lower bottom surface of the truncated cone is 635 mm; the hollow inner cavity upper part 4 of the core sleeve 2 of the turbulence controller is in a trumpet shape, with an outer diameter ¢ of 480 mm, an arc radius R of 75 mm, and a height a of the upper part 4 of the core sleeve inner cavity of 80 mm; the lower part 5 of the core sleeve inner cavity is in a "drum" shape with a small upper opening and a large lower opening, with an upper opening diameter d1 of 420 mm, a lower opening diameter d2 of 460 mm, and a height h of the lower part 5 of the core sleeve inner cavity of 320 mm.

[0059] The bottom surface of the bottom plate 6 is square, with a side length c of 500 mm and a thickness b of 90 mm.

[0060] The width of the joint seam 3 is larger at the top and smaller at the bottom, with the upper width m being 10 mm and the lower width n being 5 mm.

[0061] The shape and size of the shell 1 are designed according to the shape and size of the impact zone of the continuous casting tundish working lining, and are cast by using magnesium castables produced by existing technology, and are prepared after natural curing and baking in a heating furnace.

[0062] The preparation method of the sleeve core 2 using a disposable foam inner mold and a magnesium castable for casting, comprising the following steps: adding the magnesium castable for the sleeve core 2 into a mixer and dry mixing for 2 minutes, adding 4.0% of the total weight of the material of water, wet mixing for 6 minutes, and after mixing, putting it into a sleeve core casting outer mold 8 with a disposable foam inner mold 7, vibrating it with a vibrating rod, and when no large bubbles emerge, the casting of the green body of the sleeve core 2 is completed, and after solidification for 12 hours, the sleeve core casting outer mold 8 is removed, and the sleeve core casting outer mold 8 is automatically Then cure for 12 hours, and then bake in a heating furnace: ① heat up from room temperature to 120℃ at a heating rate of 10℃ / h; ② keep warm at 120℃ for 11h; ③ heat up from 10℃ / h to 220℃; ④ keep warm at 220℃ for 7h; ⑤ heat up to 360℃ at a heating rate of 15℃ / h; ⑥ keep warm at 360℃ for 7h; ⑦ stop firing and cool naturally. After cooling to room temperature, clean up the remaining disposable foam inner mold 7, and the core sleeve 2 is prepared.

[0063] The bottom plate 6 is prepared by isostatic pressing and is made of the following raw materials in percentage by weight:

[0064] Main material: sintered magnesia 84wt%

[0065] Auxiliary materials: flake graphite 10.5wt%

[0066] Antioxidant: Aluminum powder 2.0wt%

[0067] Binder: 3.5wt% phenolic resin.

[0068] The bottom plate 6 is prepared by isostatic pressing, which includes the following steps:

[0069] 1) Ingredients: weigh the above raw materials according to the above ratio;

[0070] 2) Mixing: preheat the mixer to 40°C, add sintered magnesia with a particle size of 1mm≦≤3mm and 0.074mm<particle size<1mm at low speed → add phenolic resin after dry mixing for 1 minute → add flake graphite after wet mixing for 3 minutes → add sintered magnesia with a particle size of ≦0.074mm and antioxidant after wet mixing for 2 minutes → wet mixing for 3 minutes → high-speed mixing for 10 minutes → discharge, and the temperature of the mud during mixing is less than 70°C;

[0071] 3) Green body molding: fill the clay into the mold, then remove the air in the mold, press it under 200MPa with isostatic pressure and then take it out of the mold, and the green body molding is completed;

[0072] 4) Natural drying and baking: After the green body is naturally dried for 8 hours, it is put into the kiln for baking: ① Continuously heat from room temperature to 140℃ at a heating rate of 10℃ / h, and keep warm for 8 hours; ② Continuously heat from 140℃ to 200℃ at a heating rate of 10℃ / h, and keep warm for 24 hours; ③ Stop the fire and cool naturally to room temperature. The preparation of the base plate is completed, and its compressive strength is ≥40MPa.

[0073] A preparation method for a composite continuous casting tundish turbulence controller: a core sleeve 2 is installed in an outer shell 1 of the turbulence controller to ensure that the longitudinal center line of the core sleeve 2 coincides with the longitudinal center line of the inner cavity of the outer shell 1, and the joint seam 3 between the outer shell 1 and the core sleeve 2 is filled with sintered magnesia sand with a particle size of ≤1mm, and a layer of recycled magnesia carbonaceous coating with a thickness of 25mm is applied on its outer surface, and naturally cured for 1 day, and the preparation of the composite slab continuous casting tundish turbulence controller is completed.

[0074] The magnesium-carbon coating material refers to a coating material prepared by treating and processing waste magnesium-carbon bricks with a particle size of 1mm≦≤3mm and a particle size of 0.074mm<<1mm, and sintered magnesia sand fine powder with a particle size of ≤0.074mm, soft clay, silicon micropowder, sodium tripolyphosphate, etc. in a certain ratio, wherein the weight percentage of the recycled magnesium-carbon particle material is 60-70%, the MgO content is ≥65wt%, and the volume density is ≥1.87g / cm3.

[0075] Example 2

[0076] As described in Example 1, except that:

[0077] The core sleeve 2 of the turbulence controller has a diameter D1 of the upper bottom surface of the truncated cone of 750 mm, and a diameter D2 of the lower bottom surface of the truncated cone of 665 mm; the hollow inner cavity upper part 4 of the core sleeve 2 of the turbulence controller is in a trumpet shape, with an outer diameter ¢ of 500 mm, an arc radius R of 80 mm, and a height a of the upper part 4 of the core sleeve inner cavity of 100 mm; the upper diameter d1 of the lower part 5 of the core sleeve inner cavity is 440 mm, the lower diameter d2 is 480 mm, and the height h of the lower part 5 of the core sleeve inner cavity is 350 mm.

[0078] The bottom surface of the bottom plate 6 is square, with a side length c of 520 mm and a thickness b of 110 mm.

[0079] The width of the joint seam 3 is larger at the top and smaller at the bottom, with the upper width m being 15 mm and the lower width n being 10 mm.

[0080] The preparation method of the sleeve core 2 using a disposable foam inner mold and a magnesium castable for casting, comprising the following steps: adding the magnesium castable for the sleeve core 2 into a mixer and dry mixing for 3 minutes, adding 5.0% of the total weight of the material of water, wet mixing for 6 minutes, and after mixing, putting it into a sleeve core casting outer mold 8 with a disposable foam inner mold 7, vibrating it with a vibrating rod, and when no large bubbles emerge, the casting of the green body of the sleeve core 2 is completed, and after solidification for 24 hours, the sleeve core casting outer mold 8 is removed, and the natural Curing for 24 hours, and then baking in a heating furnace: ① heating from room temperature to 150℃ at a heating rate of 10℃ / h; ② keeping warm at 150℃ for 13h; ③ heating from 10℃ / h to 250℃; ④ keeping warm at 250℃ for 9h; ⑤ heating at a heating rate of 15℃ / h to 390℃; ⑥ keeping warm at 390℃ for 9h; ⑦ stopping the fire and cooling naturally, after cooling to room temperature, clean up the residue of the disposable foam inner mold 7, and the sleeve core 2 is prepared.

[0081] The bottom plate 6 is prepared by isostatic pressing and is made of the following raw materials in percentage by weight:

[0082] Main material: sintered magnesia 76wt%

[0083] Auxiliary materials: flake graphite 16wt%

[0084] Antioxidant: Silicon powder 2wt%, Silicon carbide powder 2wt%

[0085] Binder: 4.0wt% phenolic resin.

[0086] The bottom plate 6 is prepared by isostatic pressing, which includes the following steps:

[0087] 1) Ingredients: weigh the above raw materials according to the above ratio;

[0088] 2) Mixing: preheat the mixer to 50°C, add sintered magnesia with a particle size of 1mm≦≤3mm and 0.074mm<particle size<1mm at low speed → add phenolic resin after dry mixing for 2 minutes → add flake graphite after wet mixing for 2 minutes → add sintered magnesia with a particle size of ≦0.074mm and antioxidant after wet mixing for 3 minutes → wet mixing for 2 minutes → high-speed mixing for 15 minutes → discharge, and the temperature of the mud during mixing is less than 70°C;

[0089] 3) Green body molding: fill the clay into the mold, then remove the air in the mold, press it under 250MPa with isostatic pressure and then take it out of the mold, and the green body molding is completed;

[0090] 4) Natural drying and baking: After the green body is naturally dried for 16 hours, it is put into the kiln for baking: ① continuously heat the temperature from room temperature to 160°C at a heating rate of 10°C / h, and keep it warm for 4 hours; ② continuously heat the temperature from 160°C to 220°C at a heating rate of 10°C / h, and keep it warm for 16 hours; ③ stop the fire, cool naturally to room temperature, and the preparation of the bottom plate 6 is completed, and its compressive strength is ≥40MPa.

[0091] A preparation method for a composite slab continuous casting tundish turbulence controller: a core sleeve 2 is inserted into an outer shell 1 of the turbulence controller to ensure that the longitudinal center line of the core sleeve 2 coincides with the longitudinal center line of the inner cavity of the outer shell 1, and a joint seam 3 between the outer shell 1 and the core sleeve 2 is filled with a sintered magnesia slab with a particle size of ≤1 mm, and a layer of magnesium coating with a thickness of 35 mm is applied on its outer surface, and naturally cured for 2 days, and the preparation of the composite continuous casting tundish turbulence controller is completed.

[0092] Example 3

[0093] As described in Example 1, except that:

[0094] The core sleeve 2 of the turbulence controller has a diameter D1 of 730 mm on the upper bottom surface of the truncated cone, and a diameter D2 of 650 mm on the lower bottom surface of the truncated cone; the hollow inner cavity upper part 4 of the core sleeve 2 of the turbulence controller is in a trumpet shape, with an outer diameter ¢ of 490 mm, an arc radius R of 77 mm, and a height a of 90 mm on the upper part 4 of the core sleeve inner cavity; the upper diameter d1 of the lower part 5 of the core sleeve inner cavity is 430 mm, the lower diameter d2 is 470 mm, and the height h of the lower part 5 of the core sleeve inner cavity is 330 mm.

[0095] The bottom surface of the bottom plate 6 is square, with a side length c of 510 mm and a thickness b of 100 mm.

[0096] The width of the joint seam 3 is larger at the top and smaller at the bottom, with the top width m being 12 mm and the bottom width n being 7 mm.

[0097] The preparation method of the sleeve core 2 using a disposable foam inner mold and a magnesium castable for casting, comprises the following steps: adding the magnesium castable for the sleeve core 2 into a mixer and dry mixing for 2 minutes, adding 4.5% of the total weight of the material of water, wet mixing for 5 minutes, and after mixing, putting it into a sleeve core casting outer mold 8 with a disposable foam inner mold 7, vibrating it with a vibrating rod, and when no large bubbles emerge, the casting of the green body of the sleeve core 2 is completed, and after solidification for 16 hours, removing the sleeve core casting outer mold 8, Natural curing for 16 hours, then baking in a heating furnace: ① heating from room temperature to 135℃ at a rate of 10℃ / h; ② keeping warm at 135℃ for 12h; ③ heating from 10℃ / h to 235℃; ④ keeping warm at 235℃ for 8h; ⑤ heating to 375℃ at a rate of 15℃ / h; ⑥ keeping warm at 375℃ for 8h; ⑦ stopping the fire and cooling naturally, after cooling to room temperature, clean up the residue of the disposable foam inner mold 7, and the core sleeve 2 is prepared.

[0098] The bottom plate 6 is prepared by isostatic pressing and is made of the following raw materials in percentage by weight:

[0099] Main material: sintered magnesia 79wt%

[0100] Auxiliary materials: flake graphite 14wt%

[0101] Antioxidant: Silica powder 3.3wt%

[0102] Binder: 3.7wt% phenolic resin.

[0103] The bottom plate 6 is prepared by isostatic pressing, which includes the following steps:

[0104] 1) Ingredients: weigh the above raw materials according to the above ratio;

[0105] 2) Mixing: preheat the mixer to 45°C, add sintered magnesia with a particle size of 1mm≦≤3mm and 0.075mm<particle size<1mm at low speed → add phenolic resin after dry mixing for 1 minute → add flake graphite after wet mixing for 3 minutes → add sintered magnesia with a particle size of ≦0.075mm and antioxidant after wet mixing for 3 minutes → wet mixing for 2 minutes → high-speed mixing for 10 minutes → discharge, and the temperature of the mud during mixing is less than 70°C;

[0106] 3) Green body molding: fill the clay into the mold, then remove the air in the mold, press it under 220MPa with isostatic pressure and then take it out of the mold, and the green body molding is completed;

[0107] 4) Natural drying and baking: After the green body is naturally dried for 12 hours, it is put into the kiln for baking: ① continuously heat the temperature from room temperature to 150°C at a heating rate of 10°C / h, and keep it warm for 6 hours; ② continuously heat the temperature from 150°C to 210°C at a heating rate of 10°C / h, and keep it warm for 20 hours; ③ stop the fire, cool naturally to room temperature, and the preparation of the bottom plate 6 is completed, and its compressive strength is ≥40MPa.

[0108] A preparation method for a composite slab continuous casting tundish turbulence controller: a core sleeve 2 is inserted into an outer shell 1 of the turbulence controller to ensure that the longitudinal center line of the core sleeve 2 coincides with the longitudinal center line of the inner cavity of the outer shell 1, and the joint seam 3 between the outer shell 1 and the core sleeve 2 is filled with sintered magnesia sand with a particle size of ≤1mm, and a layer of magnesium coating with a thickness of 30mm is applied on the outer surface thereof, and naturally cured for 2 days, and the preparation of the composite continuous casting tundish turbulence controller is completed.

[0109] Comparative example: CN201244677B discloses a preparation method of a composite turbulence controller for a continuous casting tundish, comprising an outer shell, a bottom plate, a core sleeve, an expansion joint, and an anti-oxidation coating. The outer shell is cast by magnesium castable, the bottom plate is built by machine-pressed magnesium-carbon bricks, the core sleeve is built by machine-pressed "fan-shaped" magnesium-carbon bricks, expansion joints are arranged between the outer shell and the bottom plate, and between the outer shell and the core sleeve, and an anti-oxidation coating is applied to the outer surface of the core sleeve.

[0110] Examples 1-3 of the present invention and the comparative document CN201244677B disclose a method for preparing a composite turbulence controller for a continuous casting tundish) are both used to establish water models according to a similarity ratio of 1:2. The water model experimental results and comparative analysis are shown in Table 1 below:

[0111] Table 1

[0112]

[0113] Compared with the comparative example, the invention has a year-on-year increase of more than 6.7% and a year-on-year increase of more than 9.0%, a year-on-year decrease of more than 5.2%.

[0114] By comparing the data in Table 1 above, the tundish turbulence controller designed by the present invention is better than the composite turbulence controller for continuous casting tundish described in CN103658577B: the average residence time of molten steel in the tundish is increased by more than 6.7% year-on-year, and the dead zone ratio is reduced by more than 5.2% year-on-year. The structural materials, service life and total oxygen content of molten steel in the crystallizer (comparison test steel grade SPHC) of Examples 1-3 of the present invention and the comparative document CN201244677B, which discloses a method for preparing a composite turbulence controller for continuous casting tundish, are compared in the application of slab continuous casting tundish of Laiwu Iron and Steel Group Yinshan Steel Co., Ltd., as shown in Table 2 below:

[0115] Table 2

[0116]

[0117] Compared with the comparative example, the present invention simplifies the preparation process, shortens the preparation period, improves the casting quality, and improves the overall performance. The year-on-year improvement is more than 4 hours and the year-on-year reduction is 12.6%.

[0118] By comparing the data in Table 2 above, the service life of the new long-life continuous casting tundish turbulence controller prepared by the present invention is more than 4 hours longer than that of the composite turbulence controller produced by the existing patent technology CN103658577B, and the total oxygen content in the molten steel in the crystallizer is reduced by more than 12% year-on-year.

[0119] It will be apparent to those skilled in the art that the invention is not limited to the details of the exemplary embodiments described above and that the invention can be implemented in other specific forms without departing from the spirit or essential features of the invention. Therefore, the embodiments should be considered exemplary and non-limiting in all respects, and the scope of the invention is defined by the appended claims rather than the foregoing description, and it is intended that all variations falling within the meaning and scope of the equivalent elements of the claims be included in the invention. Any reference numeral in a claim should not be considered as limiting the claim to which it relates.

Claims

1. A composite slab continuous casting tundish turbulence controller, comprising a shell (1), a core (2) and a bottom plate (6), wherein the bottom plate (6) is arranged on the bottom surface of the inner cavity of the shell (1), the core (2) is arranged in the inner cavity of the shell (1), and the longitudinal center line of the core (2) coincides with the longitudinal center line of the inner cavity of the shell (1), and a joint seam (3) is provided between the shell (1) and the core (2), characterized in that: The core sleeve (2) is a truncated cone-shaped magnesium prefabricated part cast by using a disposable foam inner mold (7) and a magnesium castable. The bottom plate (6) is a whole piece of magnesium-carbon brick formed by isostatic pressing. The thickness of the side wall of the upper part of the core sleeve (2) is greater than the thickness of the side wall of the lower part. The core sleeve (2) has a parabolic inner cavity, which is divided into an upper part (4) and a lower part (5). The upper part (4) is a rotating surface with a circular arc cross section, and the lower part (5) is a concave rotating surface. The paraboloid is a rotating parabola, wherein the upper portion (4) of the sleeve core cavity of the sleeve core (2) is in a trumpet shape, the outer diameter ¢ is 480-500 mm, the arc radius R is 75-80 mm, the height a of the upper portion (4) of the sleeve core cavity is 80-100 mm, and the lower portion (5) of the sleeve core cavity is small at the upper end and large at the lower end. The upper diameter d1 of the lower portion (5) of the sleeve core cavity is 420-440 mm, the lower diameter d2 is 460-480 mm, and the height h of the lower portion (5) of the sleeve core cavity is 320-350 mm.

2. The composite slab continuous casting tundish turbulence controller according to claim 1, characterized in that: The bottom of the inner cavity of the shell (1) is provided with an inner concave cavity, the bottom plate (6) matches the inner concave cavity, and the bottom plate (6) and the bottom of the inner cavity are in the same plane.

3. The composite slab continuous casting tundish turbulence controller according to claim 2, characterized in that: The diameter D1 of the upper bottom surface of the truncated cone-shaped sleeve core (2) is 720-750 mm, and the diameter D2 of the lower bottom surface of the truncated cone is 635-665 mm.

4. The composite slab continuous casting tundish turbulence controller according to claim 3, characterized in that: The bottom surface of the bottom plate (6) is square, the side length c is 40 to 60 mm greater than d2, and the thickness b is 90 to 110 mm.

5. The composite slab continuous casting tundish turbulence controller according to claim 4, characterized in that: The width of the joint seam (3) is larger at the top and smaller at the bottom, with the top width m being 10 to 15 mm and the bottom width n being 5 to 10 mm.

6. A method for preparing a composite slab continuous casting tundish turbulence controller according to any one of claims 1 to 5, comprising the following steps:

1. The shell (1) is casted using a magnesium spinel castable, wherein the shape and size of the shell (1) are designed according to the shape and size of the impact zone of the working lining of the continuous casting tundish, and the shell (1) is casted using a magnesium spinel castable produced by prior art, and is prepared after natural curing and baking in a heating furnace; the magnesium spinel castable is produced by prior art, has a MgO content of ≥71 wt%, a bulk density of ≥3.03 g / cm3, and a flexural strength of ≥9 MPa at 1500°C; 2. The core sleeve (2) is casted using a disposable foam inner mold (7) and a magnesium castable. The method for preparing the core sleeve (2) by casting using a disposable foam inner mold (7) and a magnesium castable comprises the following steps: adding the magnesium castable for the core sleeve (2) into a mixer and dry mixing for 2 to 3 minutes, adding water accounting for 4.0 to 5.0% of the total weight of the material, wet mixing for 4 to 6 minutes, and after mixing, placing the mixture into a core sleeve casting outer mold (8) on which a disposable foam inner mold (7) is placed, and vibrating the mixture with a vibrating rod. When no large bubbles are emitted, the casting of the green body of the core sleeve (2) is completed. After solidification for 12 to 24 hours, the core sleeve is removed. The outer mold (8) is poured and naturally cured for 12 to 24 hours, and then baked in a heating furnace: ① heating from room temperature to 120 to 150°C at a heating rate of 10°C / h; ② keeping the temperature at 120 to 150°C for 11 to 13 hours; ③ heating to 220 to 250°C at a heating rate of 10°C / h; ④ keeping the temperature at 220 to 250°C for 7 to 9 hours; ⑤ heating to 360 to 390°C at a heating rate of 15°C / h; ⑥ keeping the temperature at 360 to 390°C for 7 to 9 hours; ⑦ stopping the fire and cooling naturally. After cooling to room temperature, the residue of the disposable foam inner mold (7) is cleaned, and the sleeve core (2) is prepared; 3. The bottom plate (6) is prepared into a whole magnesia carbon brick by isostatic pressing. The bottom plate (6) is prepared by isostatic pressing and is prepared from the following raw materials in percentage by weight: Main material: sintered magnesia 76-84wt%; Auxiliary materials: flake graphite 11.5~16wt%; Antioxidant: 2-5 wt % of one or a mixture of aluminum powder, silicon powder, silicon carbide powder; Binder: phenolic resin 3.5-4.0wt%; the sum of the weight percentages of all raw materials of the base plate (6) is 100%; The sintered magnesia is made of light-burned magnesia with a MgO content of 95 wt% as raw material, produced by ball pressing and high-temperature vertical kiln calcination process, with a MgO content of 94-95 wt%, and is mixed with 1mm≦particle size≤3mm, 0.074mm<particle size<1mm, and particle size≦0.074mm; The flake graphite has a purity C content of ≥98wt% and a particle size of 100 mesh; The aluminum powder has a purity Al content of ≥99wt% and a particle size of 100 mesh; The silicon powder has a purity Si content of ≥97wt% and a particle size of 100 mesh; The silicon carbide has a purity SiC content of ≥94wt% and a particle size of 100 mesh; The phenolic resin has a solid content of ≥72wt%, a residual carbon content of ≥42wt%, and a moisture content of ≤5wt%; The bottom plate (6) is prepared by isostatic pressing, which comprises the following steps: 1) Ingredients: weigh the above raw materials according to the ratio; 2) Mixing: preheat the mixer to 40-50℃, add sintered magnesia with a particle size of 1mm≦≤3mm and 0.074mm<particle size<1mm at low speed → add phenolic resin after dry mixing for 1-2 minutes → add flake graphite after wet mixing for 2-3 minutes → add sintered magnesia with a particle size of ≦0.074mm and antioxidant after wet mixing for 2-3 minutes → wet mixing for 2-3 minutes → high-speed mixing for 10-15 minutes → discharge, the mud temperature is less than 70℃ during the mixing process; 3) Green body molding: fill the clay into the mold, then remove the air in the mold, press it under 200~250MPa with isostatic pressure and then take it out of the mold, and the green body molding is completed; 4) Natural drying and baking: After the green body is naturally dried for 8 to 16 hours, it is put into a kiln for baking: ① continuously heating from room temperature to 140 to 160°C at a heating rate of 10°C / h, and keeping warm for 4 to 8 hours; ② continuously heating from 140 to 160°C to 200 to 220°C at a heating rate of 10°C / h, and keeping warm for 16 to 24 hours; ③ stopping the firing, cooling naturally to room temperature, and the preparation of the bottom plate (6) is completed, and its compressive strength is ≥40MPa; 4. Apply a layer of magnesium-carbon coating material with a thickness of 25-35mm on the outer surface of sintered magnesia. The magnesium-carbon coating material refers to the coating material prepared by using the recycled granular material of waste magnesia-carbon bricks with a particle size of 1mm≦<3mm and a particle size of 0.074mm<<1mm and sintered magnesia fine powder, soft clay, silicon powder, and sodium tripolyphosphate in a certain ratio, wherein the weight percentage of the recycled magnesium-carbon granular material is 60-70%; 5. The core sleeve (2) is placed inside the shell (1) of the turbulence controller, ensuring that the longitudinal center line of the core sleeve (2) coincides with the longitudinal center line of the inner cavity of the shell (1), and the joint seam (3) between the shell (1) and the core sleeve (2) is filled with sintered magnesia sand with a particle size of ≤1 mm. The core sleeve is naturally cured for 1 to 2 days, and the preparation of the composite continuous casting tundish turbulence controller is completed.