A soft-bottomed carpet made from recycled yarn and a method for manufacturing the same

The soft-bottom carpet structure prepared by recycling yarn, combined with adhesive and latex layer, solves the problems of carpet substrate stability and energy consumption, achieves soft, comfortable, stable and environmentally friendly effects, and reduces resource waste and the environment pollute.

CN111319313BActive Publication Date: 2024-11-26SUZHOU TUNTEX FIBER & CARPET CO LTD
View PDF 8 Cites 0 Cited by

Patent Information

Application Number
CN202010199802.5
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2020-03-20
Publication Date
2024-11-26
Estimated Expiration
2040-03-20

AI Technical Summary

Technical Problem

Existing carpet substrate materials such as PVC and nonwovens have problems such as insufficient stability and high energy consumption, and defective fibers are difficult to recycle, resulting in waste of resources and environmental pollution.

Method used

The soft-bottom carpet structure prepared using recycled yarns, including the carpet fiber layer and the recycled fiber layer, is formed by combining the adhesive and latex layer, using PO-cadyl carbonate adhesive and SBR latex layer, combined with the non-woven layer, to form a Three-dimensional fiber structure, reducing energy consumption and secondary pollution.

Benefits of technology

It realizes a carpet with soft material, high comfort, good elasticity, stable physical properties and good temperature insulation effect, while reducing energy consumption and resource waste, improving the overall stability and environmental protection of the carpet.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN111319313B_ABST
    Figure CN111319313B_ABST
Patent Text Reader

Abstract

The invention discloses a soft-bottomed carpet made from recycled yarn, belonging to the technical field of carpet manufacturing. The carpet comprises, from top to bottom, a carpet fiber layer and a recycled fiber layer, the carpet fiber layer comprises carpet fibers and a first long-fiber non-woven fabric, the carpet fibers are tufted on the first long-fiber non-woven fabric, the recycled fiber layer comprises recycled fibers and a second long-fiber non-woven fabric, the recycled fibers are tufted on the second long-fiber non-woven fabric; the carpet fiber layer and the recycled fiber layer are fixedly bonded. The invention has the advantages of soft material, high comfort, good elasticity, stable physical properties, good thermal insulation effect, etc.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of carpet manufacturing, and in particular relates to a soft-bottomed carpet prepared by utilizing recycled yarn and a manufacturing method thereof. Background Art

[0002] At present, most domestic carpets use PVC or asphalt as the base material of the carpet after the carpet surface is tufted. A glass fiber layer can be added in the middle to improve the dimensional stability of the carpet, or a non-woven fabric base material can be attached after the carpet surface is tufted. However, PVC base material used in carpets is usually hard and not comfortable. Major manufacturers have been trying to find a new material to replace PVC as the carpet base material; and non-woven fabric base materials, although relatively soft compared to PVC materials, have quality defects that continue to emerge during use due to their dimensional instability and easy warping properties. Therefore, we have been committed to creating a base material that combines the stability of PVC / asphalt and the comfort of a soft base, and incorporates the scientific concept of green recycling and environmental protection.

[0003] We found that during the production and processing of fibers, some defective products will be produced due to color deviation, physical property abnormalities, and color transition. These defective products cannot be used in the production of normal carpets, so the conventional practice is to discard them or cut and recycle them. Cutting recycling means that the fibers are cut and then melted at high temperature and granulated, and then melted at high temperature to make other corresponding products as needed. However, this recycling method requires the use of cutting, melting, granulation, molding and other equipment. These high-power equipment consumes a lot of energy, and high-frequency operations also consume a lot of manpower. In the process of cutting fibers, a large amount of dandruff and dust will be generated, which will further cause physical damage to the operators. The secondary pollution and large consumption of energy will have an irreversible impact on the environment. Summary of the invention

[0004] Purpose of the invention: The technical problem to be solved by the present invention is to provide a carpet made of recycled yarn to reduce energy consumption and secondary pollution in the yarn recycling process, while having the advantages of soft material, high comfort, good elasticity, stable physical properties, and good thermal insulation effect;

[0005] Another technical problem to be solved by the present invention is to provide a method for preparing the carpet prepared by using the recycled yarn.

[0006] Technical solution:

[0007] A soft-bottomed carpet made from recycled yarn, the carpet comprising, from top to bottom, a carpet fiber layer and a recycled fiber layer, the carpet fiber layer comprising carpet fibers and a first long-fiber non-woven fabric, the carpet fibers being tufted on the first long-fiber non-woven fabric, the recycled fiber layer comprising recycled fibers and a second long-fiber non-woven fabric, the recycled fibers being tufted on the second long-fiber non-woven fabric; the carpet fiber layer and the recycled fiber layer, the pile surfaces after tufting comprising various loop piles, cut piles and a mixture of loop and cut piles.

[0008] The carpet fiber layer and the recycled fiber layer are fixedly bonded.

[0009] Wherein, the material of the carpet fiber is PP, PET, PTT, nylon, PO or wool, preferably nylon or PP.

[0010] Wherein, the first long fiber nonwoven fabric and the second long fiber nonwoven fabric are 70-150g / m 2 , preferably 90-100g / m 2 .

[0011] Wherein, the carpet fiber layer and the recycled fiber layer are bonded by an adhesive.

[0012] Wherein, the material of the adhesive is PVC, asphalt, PO, PU, ​​PE or EVA, preferably PO.

[0013] Wherein, a latex layer is provided between the carpet fiber layer and the recycled fiber layer.

[0014] Wherein, the material of the latex layer is EVA, water-based PU, acrylic or SBR, preferably SBR.

[0015] Wherein, a non-woven fabric layer is provided under the recycled fiber layer.

[0016] Wherein, the recycled fiber layer and the non-woven fabric layer are connected by an adhesive.

[0017] Wherein, the non-woven fabric layer has a gram weight of 50 to 1200 g / m 2 , preferably 50 to 300 g / m 2 .

[0018] Wherein, the heat shrinkage rate of the non-woven fabric layer is less than 2%.

[0019] The pile of the recycled fiber layer is not less than 100,000 tufts / m 2 .

[0020] The method for manufacturing the soft-bottomed carpet using the recycled yarn comprises the following steps:

[0021] (1) Carpet fiber tufting: tufting carpet fibers on a first long-fiber non-woven fabric to obtain a carpet fiber layer, wherein the carpet fibers are made of PP, PET, PTT, nylon, PO or wool;

[0022] (2) Latex pre-coating and drying: water-based latex SBR, antibacterial agent, calcium carbonate, and foaming agent are mixed uniformly in a mass ratio of 62-100:0-1:0-35:0-2, preferably 65-70:0-1:28-35:0-1, and air foamed by a foaming machine with a foaming ratio of 1.2-10 times, preferably 1.5-3 times, and evenly coated on the back of the carpet fiber layer with a coating amount of 50-800 g / m 2 , preferably 80 to 350 g / m 2 The amount of dry glue is dried to obtain a latex layer;

[0023] (3) Recycled fiber tufting: The recycled fibers are classified and twisted into 850D-4000D coarse recycled fibers, and the coarse recycled fibers are tufted onto the second long-fiber nonwoven fabric to obtain a recycled fiber layer. The pile density of the pile surface on the recycled fiber layer is specifically 100,000 fibers / m 2 ~450000 / m 2 , the pile height is specifically 2.5 mm to 12 mm, preferably 3.5 mm to 6.5 mm, to obtain a recycled fiber layer;

[0024] (4) Recycled fiber tufted soft backing: PO and calcium carbonate are added in a mass ratio of 20-45:55-80, heated and melted, and stirred evenly. The mass ratio of PO and calcium carbonate is preferably 20-30:70-80. The mixture is cooled and granulated to obtain PO-calcium carbonate adhesive particles. The PO-calcium carbonate adhesive particles are added to a carpet tile bonding machine, heated and melted at 130-220° C., and then evenly coated on the pile surface of the recycled fiber layer with an extruder, and scraped with a scraper to a height of 0.5 mm-1.0 mm, preferably 0.5 mm-0.8 mm. The amount of PO and calcium carbonate adhesive is 150-2000 g / m2. 2 , preferably 500~800g / m 2 , combining the recycled fiber tufted layer with the non-woven fabric layer, pressing them by rollers, and cooling them at 5-30°C to form a recycled fiber tufted soft bottom layer;

[0025] (5) Bonding the carpet fiber layer to the recycled fiber layer: heating and melting PO and calcium carbonate in a mass ratio of 25-50:50-75, preferably 25-35:65-75, cooling, and granulating to obtain PO-calcium carbonate adhesive particles;

[0026] Feed the PO-calcium carbonate adhesive particles into the square carpet bonding machine, heat and melt them at 130-220℃, and then use an extruder to evenly apply them on the tufted back of the recycled fiber tufted soft bottom layer, scrape off the excess part with a scraper, and bond them with the latex surface of the carpet fiber tufted layer. The amount of PO-calcium carbonate adhesive is controlled at 500g / m2 2 ~2500g / m 2 , thickness is 0.8mm~1.5mm; after bonding, it is pressed by rollers and put into a cooling box at 5~30℃ for cooling.

[0027] In step (2), the drying conditions are as follows: drying temperature 140-200° C., and drying time 2-8 minutes.

[0028] The recycled yarn needs to be classified, recycled and produced according to the material of the yarn fiber. Recycled fibers of the same material need to be classified according to the fiber thickness (Denny number). Fibers with the same or similar Denny numbers can be grouped together, and fibers with different Denny numbers or large differences in Denny numbers need to be managed separately. According to the fiber thickness requirements during tufting, the thinner fibers can be plyed to reach or approach the thickness of the tufted fibers, and tufted on the second long-fiber non-woven fabric. The heat shrinkage rate of the fibers used in the same roll of recycled fiber layer must be consistent, and the heat shrinkage rate must be ensured to be within ±3%.

[0029] In the production process of yarn fibers, defective products may be produced due to color deviation, physical property deviation, color change transition and other situations of the products. The recycled fibers described in the present invention are fibers that cannot be used due to such color deviation, physical property deviation, and color change transition. The prior art adopts direct discarding or cutting and recycling. If directly discarded, it will cause waste of raw materials and increase production costs. The present invention classifies the recycled fibers according to the different materials of the recycled fibers, and divides them into categories such as PP, nylon, PET, PTT, PO, wool, etc., and then classifies them according to the fiber thickness and heat shrinkage rate of the defective products. Recycled fibers of the same material also need to be classified according to the fiber thickness (Daniel number D). Fibers with the same or similar Danny numbers can be grouped together, and fibers with different Danny numbers or large differences in Danny numbers need to be managed separately. According to the thickness requirements of the fibers during tufting, the thinner fibers can be plyed to reach or approach the thickness of the tufted fibers, and the tufting is on the second long-fiber non-woven fabric. For example, when using nylon recycled fiber, 1100D yarn is twisted into 2200D in two strands, and 680D yarn is twisted into 2040D in three strands, and used separately. The heat shrinkage rate of the fibers used in the same roll of recycled fiber layer must be consistent and ensure that the heat shrinkage rate is within ±3%.

[0030] The purpose of this classification is to ensure that the raw materials, thickness, height and density of the fibers are uniform throughout the production process. In order to ensure the flatness of the recycled fiber layer during use, the height of the pile heads needs to be strictly controlled during the weaving process to be consistent, with the height requirement within plus or minus 2mm, to ensure that the comfort and softness of the entire batch of products are consistent.

[0031] Beneficial effects:

[0032] The present invention is based on the concept of green environmental protection. On the basis of the traditional carpet production process, the use of PVC and asphalt is reduced as much as possible, and these raw materials may not even be used, thereby creating a greener, safer and more comfortable carpet.

[0033] In addition to the advantages of soft material, high comfort, good elasticity, stable physical properties, and good thermal insulation effect, the present invention can not only eliminate the output and waste of defective fibers, but also absorb defective products produced by other manufacturers, and use them directly in carpets using existing equipment in the industry without adding other equipment, truly achieving maximum energy conservation and emission reduction;

[0034] The present invention tufts recycled fibers onto long-fiber non-woven fabrics and adopts a three-dimensional fiber structure, thereby reducing the horizontal or vertical weaving in the existing non-woven fabric substrate production technology. The three-dimensional structure has good stability as a carpet substrate for the drastic impact of thermal expansion and contraction, improves softness and resilience, and further improves the overall stability of the carpet. BRIEF DESCRIPTION OF THE DRAWINGS

[0035] Figure 1 Schematic diagram of the structure of the present invention.

[0036] Figure 2 Schematic diagram of the preparation process of the present invention.

[0037] Figure 3 Schematic diagram of the preparation process of the present invention. DETAILED DESCRIPTION

[0038] The technical solution of the present invention is further described below in conjunction with the accompanying drawings.

[0039] Figure 1 In the figure, 1 is carpet fiber, 2 is the first long fiber nonwoven fabric, 3 is the first resin bonding layer, 4 is the second long fiber nonwoven fabric, 5 is recycled fiber, 6 is the second resin bonding layer, 7 is the latex layer, and 8 is the nonwoven fabric.

[0040] A soft-bottomed carpet made from recycled yarn, the carpet comprising a carpet fiber layer and a recycled fiber layer arranged in sequence from top to bottom, the carpet fiber layer comprising carpet fibers and a first long-fiber non-woven fabric, the carpet fibers being tufted on the first long-fiber non-woven fabric, the recycled fiber layer comprising recycled fibers and a second long-fiber non-woven fabric, the recycled fibers being tufted on the second long-fiber non-woven fabric; the carpet fiber layer and the recycled fiber layer, the pile surfaces after tufting comprising various loop piles, cut piles, and a mixture of loop and cut piles, etc.

[0041] The carpet fiber layer and the recycled fiber layer are fixedly bonded.

[0042] Wherein, the material of the carpet fiber is PP, PET, PTT, nylon, PO or wool.

[0043] The first long-fiber nonwoven fabric and the second long-fiber nonwoven fabric have a gram weight of 70 to 150 g / m 2 , thickness less than 1.2mm, strength more than 10kgf, heat shrinkage rate less than 0.9%, long fiber non-woven fabric is a high-quality non-woven fabric material, which is characterized by strong strength and can ensure that the lateral size always remains stable; the first long fiber non-woven fabric and the second long fiber non-woven fabric are made of polyester.

[0044] Wherein, the carpet fiber layer and the recycled fiber layer are bonded by an adhesive.

[0045] The material of the adhesive is PVC, asphalt, PO, PU, ​​PE or EVA. The adhesive is used to bond the carpet fiber layer and the recycled fiber layer, and the adhesive can also be used to bond the recycled fiber layer to the non-woven fabric layer. The preferred material of the adhesive is PO, and PO and calcium carbonate are mixed in a mass ratio of 25-50:50-75.

[0046] The ratio can be modified or other additives can be added as needed; first, PO and calcium carbonate are added in a ratio of 25-50:50-75, and then heated and melted. After the PO is melted, it is evenly stirred with the calcium carbonate to ensure good dispersion of the calcium carbonate, and then cooled and granulated. Then the material is fed into the square carpet bonding machine. After the raw materials are heated and melted at 130-220°C, they are fed into the feeding port of the square carpet bonding machine for extrusion coating, and then a scraper is used to evenly coat the back of the tufts of the soft bottom layer of the recycled fiber tufts, and the excess part is removed to bond it to the latex surface of the carpet fiber layer. According to the actual needs of production, the dosage is controlled at 500-2500g / m 2 The thickness is controlled at 0.8mm to 1.5mm according to the actual needs of production. After coating, it is put into a cooling box at 5 to 30°C for steady cooling. During the cooling process, the product is ensured to be flat. After cooling, the finished product is cut and produced.

[0047] Preferably, a latex layer is provided between the carpet fiber layer and the recycled fiber layer, and the material of the latex layer is EVA, water-based PU, acrylic or SBR, preferably SBR. Adding a latex layer can make the carpet more elastic and softer. EVA water-based PU, acrylic or SBR coating amount Dry 50g / m 2 ~800g / m 2 , coating method: foaming glue.

[0048] The latex layer preferably adopts the following formula: the mass ratio of SBR, antibacterial agent, calcium carbonate and foaming agent is 62-100:0-1:0-35:0-2, and the antibacterial agent, calcium carbonate and foaming agent are optional components.

[0049] Preparation method of latex layer: put SBR, antibacterial agent, calcium carbonate and foaming agent into the mixing tank according to the proportion, stir evenly, use foaming machine to foam, evenly apply on the back of carpet fiber layer, scrape off the excess. The coating amount is 50g / m 2 ~800g / m 2 , in order to play the role of fiber reinforcement, to avoid shedding and causing appearance defects; after coating, put it into a 140-200℃ oven at a speed of 5m / min for 2-8 minutes of drying, and roll up the blanket for use after the latex is completely dry.

[0050] Wherein, a non-woven fabric layer is provided under the recycled fiber layer, and the heat shrinkage rate of the non-woven fabric is less than 2%; the gram weight range is: 50~1200g / m 2 The non-woven fabric layer is not a necessary structure. It can be added for aesthetics or to further improve the stability of the carpet. The material of the non-woven fabric layer can be polyester or nylon, with a heat shrinkage rate of less than 2%, ensuring that it is not easy to pilling and delamination, and the gram weight is 50-1200g / m 2 between.

[0051] Embodiment 1: The method for manufacturing the soft-bottomed carpet using the recycled yarn comprises the following steps:

[0052] (1) Carpet fiber tufting

[0053] The nylon fibers are tufted on the first long-fiber non-woven fabric using a tufting carpet loom to form a carpet fiber layer, which is rolled up for later use. The pile side of the carpet fiber layer is the carpet pile surface, and the other side is the tuft back side, which is to be pre-coated with latex.

[0054] (2) Latex pre-coating and drying

[0055] Use water-based environmentally friendly latex SBR, the ratio is SBR: antibacterial agent: calcium carbonate: foaming agent = 62-100: 0-1: 0-35: 0-2, preferably 65-70: 0-1: 28-35: 0-1, wherein the content of antibacterial agent and foaming agent can be 0, put the above raw materials into a stirring tank according to the ratio, stir evenly, use a foaming machine for air foaming, the foaming ratio is 1.2-10 times, preferably 1.5-3.0 times, evenly apply it on the tufted back of the carpet fiber layer, and scrape off the excess latex with a scraper. Control the coating amount to 50-800g / m 2 , preferably 80 to 350 g / m 2 The amount of dry glue is to be dried in an oven at 140-200℃ for 2-8 minutes at a speed of 5m / min after coating. After the latex is dried, it is rolled for use;

[0056] (3) Recycled fiber tufting

[0057] The recycled fiber is made of nylon coarse fiber of about 850D to 4000D after plying. The fibers with similar thickness are directly tufted on the second long-fiber non-woven fabric through the tufting carpet weaving machine to make a recycled fiber layer, which is rolled for standby use. The pile density of the suede is specifically 100,000 strands / m 2 ~450000 / m 2 The pile height is specifically 2.5mm to 12mm.

[0058] Special note: The direction of the bonding surface of the recycled fiber layer can be switched according to the needs. That is, the back side of the recycled fiber layer can be bonded to the non-woven fabric layer, and the velvet side of the recycled fiber layer can be bonded to the latex side of the carpet fiber layer.

[0059] (4) PO bonding layer (the second resin bonding layer is an optional structure)

[0060] PO and calcium carbonate are added in a ratio of 20-45:55-80 (preferably 20-30:70-80), and then heated and melted (temperature 130-220°C). After PO is melted, it is stirred evenly with calcium carbonate to ensure good dispersibility of calcium carbonate, and then cooled (temperature 5-30°C) and granulated (particle size is less than 4-40 meshes) to ensure uniform melting. After the raw materials are heated and melted at 130-220°C, they are fed into the feeding port 11 of the square carpet bonding machine for extrusion coating, and then the scraper 10 is used to evenly coat the velvet surface of the recycled fiber layer, scraping out a suitable height of 0.5mm-1.0mm (preferably 0.5mm-0.8mm), and the dosage is controlled at 150-2000g / m per square meter. 2 (Preferably 500 to 800 g / m 2), combine the recycled fiber layer with the non-woven fabric layer. Press it with rollers and cool it steadily at 5-30℃. During the cooling process, ensure that the product is flat, form a soft bottom layer of recycled fiber tufts, and roll it for use.

[0061] (5) PO adhesive layer

[0062] PO and calcium carbonate are added in a ratio of 25-50:50-75, and then heated and melted (temperature 130-220°C). After the PO is melted, it is stirred evenly with calcium carbonate to ensure good dispersion of calcium carbonate, and then cooled (temperature 5-30°C) to granulate the particles with a particle size of less than 4-40 mesh. After heating and melting the raw materials at 130-220°C, feed them into the feeding port 11 of the square carpet bonding machine for extrusion coating, and then use a scraper 10 to evenly coat it on the tufted back of the soft bottom layer of the recycled fiber tufts, and remove the excess part to make it bonded to the latex surface of the carpet fiber layer. The dosage is controlled at 500g / m per square meter. 2 ~2500g / m 2 (Preferably 600 to 1200 g / m 2 ), the thickness is controlled at 0.8mm to 1.5mm. After bonding, it is pressed by rollers and put into a cooling box at 5 to 30°C for steady cooling. The product is ensured to be flat during the cooling process. According to actual needs, the finished soft-bottomed carpet is cut into a certain size.

[0063] The test data of the above-mentioned method for manufacturing soft-bottomed carpets using recycled yarns are as follows:

[0064] Example 2: Resilience Ratio of Wheelchair Experiment

[0065] Take the finished square carpet with a size of 500mm*500mm, use a thickness gauge to measure the full thickness of the sample, and record the valid data. Place the measured carpet on the bottom plate of the castor chair tester and fix it, place the simulated wheelchair foot with a load of 90kg on the carpet surface, set the rotation number to 2000, and start the instrument. After the rotation is completed, take out the sample carpet and let it stand horizontally for 24 hours. After completing the above steps, use the thickness gauge to measure the full thickness of the sample again to obtain valid data. Calculate the rebound ratio after comparing the valid data.

[0066] A soft-bottomed carpet made of recycled yarn and a soft-bottomed carpet made of recycled yarn without unnecessary structure were manufactured according to the method of Example 1.

[0067] Conclusion: The higher the percentage, the higher the resilience and the better the elasticity.

[0068] Table 1 Rebound ratio of wheelchair test of the present invention and competitor's products

[0069]

[0070] Table 2 Resilience ratio of the wheelchair test of the present invention and the carpet without unnecessary structure

[0071]

[0072] 2 Six-legged drum test rebound ratio---Supplementary data for good elasticity

[0073] Take the finished square carpet, use the thickness gauge to measure the full thickness of the sample, and record the valid number. After cutting to size, fit it on the inner wall of the drum, put it into the six-legged roller test instrument, set it to 12,000 revolutions, and start the instrument. After the rotation is completed, take out the sample carpet and let it stand horizontally for 24 hours. After completing the above steps, use the thickness gauge to measure the full thickness of the sample again to obtain valid data. Calculate the rebound resilience ratio after comparing the valid data.

[0074] Conclusion: The higher the percentage, the higher the resilience and the better the elasticity.

[0075] Table 3 The experimental resilience ratio of the six-legged roller of the present invention and the competitive carpet

[0076]

[0077] Table 4 Resilience ratio of the six-legged roller of the present invention and the carpet without unnecessary structure

[0078]

[0079] 3. Softness and hardness test---supplementary data for soft materials and high comfort

[0080] The size of the finished square carpet is 500mm*500mm, and 25 sampling points are planned on average. The data of each sampling point is measured and recorded using a hardness tester in a fixed order. Finally, the effective test data is obtained with the average value of the 25 sampling points.

[0081] Conclusion: The lower the value, the higher the softness and the better the softness.

[0082] Table 5 Softness and hardness test of the carpet of the present invention and competing products

[0083]

[0084] Table 6 Hardness test of the present invention and carpet without unnecessary structure

[0085]

[0086] 4 Carpet insulation effect - Supplementary data for good insulation effect

[0087] Take the finished square carpet and cut it to the same size as the iron plate, and cover the equipment iron plate. Set the equipment temperature to 80℃ and maintain this temperature until the end of the test. After the finished square carpet is placed on the 80℃ equipment iron plate, immediately measure the initial temperature at the center of the carpet surface and record the valid data, then start timing, perform a carpet surface thermal conductivity temperature test every 6 minutes, and record the valid data.

[0088] Conclusion: Low surface temperature means poor thermal conductivity and good insulation effect

[0089] Table 7 Thermal insulation effect test of the present invention and competing carpets

[0090]

[0091] Table 8 Temperature effect test of the present invention and the carpet without non-essential structure

[0092]

Claims

1. A method for manufacturing a soft-bottomed carpet using recycled yarn, characterized in that: The steps include: (1) Carpet fiber tufting: tufting the carpet fibers onto the first long-fiber non-woven fabric to obtain a carpet fiber layer; (2) Latex pre-coating and drying: Mix water-based latex SBR, antibacterial agent, calcium carbonate and foaming agent in a mass ratio of (62-100): (0-1): (28-35): (0-2) and use a foaming machine to perform air foaming with a foaming ratio of 1.2-10 times. Apply it evenly on the back of the carpet fiber layer with a coating amount of 50-800g / m 2 The amount of dry glue is dried to obtain a latex layer; (3) Recycled fiber tufting: The recycled fibers are classified and ply into 850D~4000D coarse recycled fibers, and the coarse recycled fibers are tufted onto the second long fiber non-woven fabric to obtain a recycled fiber layer; (4) Recycled fiber tufted soft backing: PO and calcium carbonate are added in a mass ratio of (20-45): (55-80), heated to melt, stirred evenly, cooled, and granulated to obtain PO-calcium carbonate adhesive particles; the PO-calcium carbonate adhesive particles are added to a carpet tile bonding machine and heated to melt at 130-220°C, and then evenly coated on the tuft surface of the recycled fiber layer with an extruder, and then scraped with a scraper to a height of 0.5 mm-1.0 mm. The amount of PO and calcium carbonate adhesive is 150-2000 g / m2. 2 , combining the recycled fiber tufted layer with the non-woven fabric layer, pressing it with a roller, and cooling it at 5-30°C to form a recycled fiber tufted soft bottom layer; (5) Bonding the carpet fiber layer to the recycled fiber layer: PO and calcium carbonate are mixed in a mass ratio of 25-50:50-75, heated to melt, cooled, and granulated to obtain PO-calcium carbonate adhesive particles; Feed the PO-calcium carbonate adhesive particles into the square carpet bonding machine, heat and melt them at 130~220℃, and then use an extruder to evenly apply them on the tufted back of the soft bottom layer of the recycled fiber tufts. Use a scraper to scrape off the excess part and bond it with the latex side of the carpet fiber layer. The amount of PO-calcium carbonate adhesive is controlled at 500 g / m2 per square meter. 2 ~2500 g / m 2 , thickness is 0.8mm~1.5mm; after bonding, it is pressed by rollers and put into a cooling box at 5~30℃ for cooling; In step (2), the drying conditions are as follows: drying temperature 140-200° C., drying time 2-8 minutes.

2. The method for manufacturing a soft-bottomed carpet using recycled yarn according to claim 1, characterized in that: In step (1), the carpet fiber is made of PP, PET, PTT, nylon, PO or wool.

3. The method for manufacturing a soft-bottomed carpet using recycled yarn according to claim 1, characterized in that: The non-woven fabric layer has a gram weight of 50-1200 g / m 2 , the heat shrinkage rate of the non-woven fabric layer is less than 2%.

4. The method for manufacturing a soft-bottomed carpet using recycled yarn according to claim 1, characterized in that: The pile of the recycled fiber layer is not less than 100,000 pieces / m 2 The pile height is higher than 2.5mm and lower than 12mm.

Citation Information

Patent Citations

  • Soft-base carpet and its production process

    CN1440871A

  • Use of waste carpet as backing filler for floor coverings

    CN1753783A

  • Soft-bottom carpet prepared from recycled yarns

    CN212499212U

  • Carpet underlay

    EP0333396A2

  • Slip prevention working method for carpet

    JP1995308255A