Wheel anti-gravity casting equipment with crucible insulation furnace

By using multi-lift pipes and specific gate design in wheel casting, the problems of long filling distance and slow cooling speed in traditional aluminum alloy wheel casting are solved, and fast sequential solidification and efficient production are achieved , improves the mechanical properties and pass rate of the product.

CN111804888BActive Publication Date: 2024-11-08BEIHANG UNIV

Patent Information

Application Number
CN202010842272.1
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2020-08-20
Publication Date
2024-11-08
Estimated Expiration
2040-08-20

AI Technical Summary

Technical Problem

In traditional aluminum alloy wheel casting technology, the filling of single-lift liquid pipes leads to long filling distances, difficult forming, low cooling speed, easy to form shrinkage holes and loosening defects, and difficult to control the cooling temperature field, affecting product performance and pass rate.

Method used

Using wheel differential die casting equipment with crucible insulation furnace, through multi-lift pipe and specific gate sleeve design, the gate is set directly under the wheel rim, combined with a two-stage pressurization process to achieve rapid sequential solidification of metal melt. , shorten the filling distance and solidification time.

Benefits of technology

It significantly improves the wheel cooling speed and cooling effect, achieves rapid sequential solidification, improves production efficiency and mechanical properties, reduces the occurrence of shrinkage defects, and improves the stability and qualification rate of the product.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN111804888B_ABST
    Figure CN111804888B_ABST
Patent Text Reader

Abstract

The invention discloses a wheel anti-gravity casting device with a crucible insulation furnace, comprising a mold and a crucible insulation furnace, wherein a crucible is arranged in the crucible insulation furnace, and a metal melt is contained in the crucible, and an electric heating device, a temperature measuring thermocouple, two-side riser pipes, and a high-pressure gas source are arranged on the furnace body; a pouring cup and a pouring sleeve are connected above the two-side riser pipes, and the pouring cup is connected to the two-side riser pipes below, and the pouring sleeve corresponds to the position directly below the wheel mold rim, and is connected to the cavity inlet for pouring into the mold cavity, and the rising metal melt is pressed and poured into the cavity. The invention is suitable for a multi-gate side injection method in which the gate is arranged directly below the wheel rim, and solves the problems of poor long-distance shrinkage compensation effect and difficulty in controlling the solidification temperature field after enhanced cooling in the traditional large-size wheel single riser pipe technology, thereby improving the performance and production stability of the wheel, shortening the production cycle, and improving the production efficiency and the qualified rate of the wheel.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of casting, in particular to a wheel anti-gravity casting device with a crucible insulation furnace. Background Art

[0002] Lightweighting is one of the most important ways to save energy and reduce emissions for fuel vehicles and to reduce consumption and increase range for new energy vehicles. Replacing traditional steel materials with lightweight materials such as aluminum alloys has become an inevitable choice for the renewal of automobile design. Aluminum alloys used in automobiles can be divided into cast aluminum alloys and deformed aluminum alloys. Cast aluminum alloys are mainly used to manufacture components such as engines, clutch housings, wheels, and chassis parts. With the demand for improved casting quality and the development of casting technology, more parts are produced by low-pressure casting, differential pressure casting, and pressure-regulated casting, all of which belong to anti-gravity casting methods. The basic principle of this type of casting is to use low-pressure gas to drive the molten metal in the crucible or holding furnace, so that it rises through the riser and enters the mold cavity. After the filling is completed, the molten metal in the mold completes solidification and shrinkage compensation under pressure.

[0003] Traditional aluminum alloy low-pressure, differential pressure and pressure-regulated wheel casting technology usually adopts a single-gate single-riser tube filling technology. Taking aluminum alloy wheels as an example, a riser tube is set at the center of the wheel, that is, the wheel center position of the wheel, so that the metal melt enters the mold cavity and completes the filling and solidification. This method is simple in design and easy to implement, but the disadvantages are that the filling distance is long and the molding is difficult. In order to avoid cold shut, the temperature of the wheel metal mold is generally as high as 400°C or above, resulting in a low cooling rate of the wheel, coarse structure, and easy formation of shrinkage cavities and shrinkage in the hot joints. Casting defects such as shrinkage cavities and shrinkage are easy to form. In order to refine the structure and eliminate casting defects such as shrinkage cavities and shrinkage, water cooling, water mist cooling and other methods are generally used in the prior art to strengthen the cooling of the wheel mold. However, strengthening the cooling greatly shortens the solidification time of the wheel. For example, the solidification time of a large-size wheel after strengthening cooling can be shortened to less than 100s, but at the same time, it causes the problem of difficulty in controlling the temperature field of the wheel cooling and solidification process during the production process, resulting in difficulty in achieving sequential solidification, unstable product performance, and low pass rate.

[0004] There have been attempts at other filling methods in the prior art of wheels. Patent CN201010107026.8 discloses a low-pressure casting double-sided pouring process and device for aluminum alloy wheels. Gates are set on both sides of the wheel to allow molten aluminum to enter from the rim. By controlling the cooling, the molten aluminum crystallizes from the wheel center to the rim at the rapidly cooled mold temperature, shortening the distance the molten aluminum flows. Combined with cooling, shrinkage defects at the R angle or rim area are reduced. Patents CN201310557627.2, CN201410825962.0 and other documents disclose the use of a combination of a central gate and a gate on both sides in the hope of reducing the weight of the hub and improving the mechanical strength. CN201610390494.8 uses a one-machine dual-mold hub mold, and the gate is also set at the rim position to achieve one-time casting of two hubs.

[0005] However, the above-mentioned device and method also have obvious defects. For the method in which the aluminum liquid enters only from the rim, the inlet is set in the middle of the rim, which will cause diversion after entering, that is, filling the wheel center and the wheel rim at the same time, resulting in uncontrollable filling time at each location, and then uncontrollable solidification sequence, which is easy to form shrinkage defects. For the method of combining the central gate and the gate on both sides, since the aluminum liquid enters from two inlets, it will form a convergence in the middle position, which is easy to cause cold shut due to reasons such as poor gas discharge.

[0006] The applicant has designed a rapid sequential solidification wheel forming device and method based on multiple riser tubes, in which the gate of the mold is set just below the wheel rim or outside the R angle above the lower rim. By filling the mold with liquid in multiple riser tubes, the problem of long-distance shrinkage compensation after filling is solved. However, due to the change in the position and shape of the gate, the traditional circular casting assembly can no longer be used for filling. Therefore, how to use reasonable insulation furnace heating and matching casting devices to achieve stable filling in this way has become a problem to be solved. Summary of the invention

[0007] In order to solve the above technical problems, the present invention provides a wheel differential pressure casting equipment with a crucible insulation furnace.

[0008] The complete technical solution of the present invention includes:

[0009] A wheel anti-gravity casting device with a crucible insulation furnace, characterized in that it at least includes a crucible insulation furnace and a mold;

[0010] The crucible insulation furnace comprises a furnace body, an insulation layer formed by refractory material is provided on the inner wall of the furnace body, a crucible is provided in the furnace body, molten metal is contained in the crucible, an electric heating device is provided in the furnace body, a furnace cover is provided on the upper part of the furnace body, a temperature measuring thermocouple is provided on the furnace cover, the furnace cover is connected to the liquid riser pipes on both sides, and the furnace cover is connected to the high-pressure gas source; the thermocouple measures the temperature of the molten metal in the crucible insulation furnace and controls the electric heating device to keep it at the filling temperature, and the high-pressure gas source is used to make the molten metal rise to the mold cavity.

[0011] A pouring assembly is connected above the riser tubes on both sides, and the pouring assembly includes a pouring cup and a pouring sleeve. The pouring cup is connected to the riser tubes on both sides below. A pouring sleeve is provided above the pouring cup. The pouring sleeve corresponds to the position directly below the rim of the wheel mold, is connected to the cavity inlet for pouring into the mold cavity, and pours the rising molten metal into the cavity. The mold cavity inlet corresponding to each pouring sleeve is set on the annular surface directly below the rim of the wheel.

[0012] The sprue sleeve and the cavity inlet can be arranged at positions on the annular surface corresponding to the outer side of the window area, or at positions on the annular surface corresponding to the connection between the rim and the spoke.

[0013] There is also an insulation layer under the furnace cover, and a charging port is opened on one side of the furnace cover for adding molten aluminum.

[0014] A roller is provided at the bottom of the furnace body, and the roller is located on a track and can move along the track.

[0015] The cross-sectional shape of the gate sleeve connected to the cavity entrance is: including a first arc segment and a second arc segment, the first arc segment and the second arc segment are concentric, and the radius and size of the first arc segment are smaller than the second arc segment, and the first arc segment and the second arc segment are connected on both sides by a connecting segment.

[0016] The sprue sleeve and the sprue cup are positioned and installed through the step portion. A certain installation margin is left between the outer wall of the sprue sleeve and the inner wall of the sprue cup. The lower opening of the sprue sleeve is connected with the upper opening of the sprue cup. The upper opening of the sprue sleeve is a special-shaped opening and is connected with the inlet of the mold cavity. A net placing groove is provided at the upper opening of the sprue sleeve for placing a filter net. The lower opening of the sprue cup is connected with the liquid riser.

[0017] The cross-sectional shape of the filter screen is the same as that of the liquid inlet channel.

[0018] The advantages of the present invention over the prior art are:

[0019] The applicant proposed a rapid sequential solidification wheel forming device and method based on a multi-riser tube, in which the gate of the mold is set just below the rim of the wheel. By filling the mold with liquid in multiple riser tubes, the filling distance of the molten metal is shortened by more than half compared with the existing single riser tube mode, and the temperature of the metal mold can be reduced from the existing 420°C to below 320°C, which naturally accelerates the cooling speed and cooling effect of the wheel and realizes rapid sequential solidification. Since the position and shape of the gate have changed, the traditional circular casting assembly can no longer be used for filling. The anti-gravity casting device of the crucible insulation furnace designed by the present invention is suitable for the multi-gate side injection method in which the gate is set just below the rim of the wheel, and realizes a stable casting and filling method at the edge of the wheel. When used in conjunction with the multi-riser tube side injection method, the filling distance of the molten metal can be shortened by more than half compared with the existing stage, breaking the problem of the difficulty of long-distance shrinkage compensation of existing large-size wheels. At the same time, the solidification time is further shortened, and the production efficiency and the mechanical properties of the wheel are significantly improved. Through the optimized two-stage filling and pressurizing process design, the metal melt flows smoothly in the initial filling and then quickly fills the cavity, giving full play to the advantage of rapid filling of multi-liter liquid tubes and improving production efficiency. BRIEF DESCRIPTION OF THE DRAWINGS

[0020] Figure 1 It is a schematic structural diagram of the wheel anti-gravity casting equipment with a crucible insulation furnace according to the present invention.

[0021] Figure 2 for Figure 1 sectional view of .

[0022] Figure 3 It is a schematic diagram of the distribution of the annular surface of the gate sleeve of the present invention just below the rim.

[0023] Figure 4 This is a schematic diagram of the structure of the pouring cup and the pouring sleeve of the present invention.

[0024] Figure 5 It is a schematic diagram of the structure with local pressurization and refinement device.

[0025] Figure 6 Schematic diagram of wheel structure in the prior art.

[0026] Figure 7 a is Figure 1 The parts of the device that are prone to air entrainment during the filling process.

[0027] Figure 7 b is Figure 7 A partial enlarged view of a.

[0028] Figure 7 c is Figure 7 a Schematic diagram of the filling sequence during slow filling. DETAILED DESCRIPTION

[0029] The present invention will be further described below in conjunction with the accompanying drawings and specific embodiments.

[0030] like Figure 1-2 As shown, taking low-pressure casting as an example, a wheel anti-gravity casting device with a crucible insulation furnace of the present invention comprises a crucible insulation furnace 1 and a mold 2;

[0031] The crucible insulation furnace 1 comprises a furnace body, the inner wall of the furnace body is provided with an insulation layer 3 formed of refractory material, a base is provided below the furnace body, a crucible 4 is provided on the base, a metal melt 5 is contained in the crucible 4, an electric heating device 6 is provided in the furnace body, a furnace cover is provided on the upper part of the furnace body, an insulation layer is also provided below the furnace cover, a charging port is provided on one side of the furnace cover, and a temperature measuring thermocouple is provided, the furnace cover is connected to the liquid riser 7 on both sides, and the furnace cover is connected to a high-pressure gas source; wherein the charging port, high-pressure gas source, and temperature measuring thermocouple provided on the furnace cover are prior art, and are not shown in the figure for the sake of simplifying the view. The thermocouple measures the temperature of the metal melt in the crucible insulation furnace, and controls the electric heating device to keep it at the filling temperature, the charging port is used to add aluminum liquid, and the high-pressure gas source is used to make the metal melt rise to the mold cavity.

[0032] A pouring assembly is connected above the riser tubes on both sides, and the pouring assembly includes a pouring cup 8 and a pouring sleeve 9. The pouring cup 9 is connected to the riser tubes on both sides below. A pouring sleeve is provided above the pouring cup, and the pouring sleeve corresponds to the position directly below the rim of the wheel mold, is connected to the cavity inlet for pouring into the mold cavity, and pours the rising metal melt into the cavity by pressing the edge.

[0033] The furnace body bottom is provided with rollers, which are located on tracks and can be moved along the tracks. This is prior art and is not shown in the figure for the sake of simplifying the view.

[0034] The mold cavity inlet corresponding to each sprue bushing is arranged on the annular surface 10 directly below the wheel rim. It is particularly noted that the "annular surface directly below the wheel rim" in the present invention refers to the annular surface formed on the side of the rim opposite to the wheel flange, surrounding the center axis of the wheel. The outer circle of the annular surface is the circle formed by the outermost contour line of the wheel on the surface, and the inner circle is the circle formed by the outer contour line of the window area of ​​the wheel around the center axis of the wheel. Figure 3-4 Correspondingly, the position where the sprue sleeve is connected to the mold is also arranged at this location.

[0035] It is particularly preferred that the sprue sleeve and the cavity inlet can be arranged at positions on the annular surface corresponding to the outer side of the window area, or can be arranged at positions on the annular surface corresponding to the connection between the rim and the spoke.

[0036] In particular, the cross-section of the sprue sleeve in communication with the cavity inlet generally follows the shape of the cavity inlet at the filling point of the casting.

[0037] Specifically, Figure 3 As shown, the cross-sectional shape of the gate sleeve 9 connected to the cavity entrance is: including a first arc segment 11 and a second arc segment 12, the first arc segment and the second arc segment are concentric, and the radius and size of the first arc segment are smaller than the second arc segment, and the first arc segment and the second arc segment are connected on both sides by a connecting segment 13.

[0038] The length of the first arc segment is 72-76 mm, the length of the second arc segment is 76-80 mm, and the length of the connecting segments on both sides is 8-12 mm.

[0039] The specific connection relationship between the pouring cup 8 and the pouring sleeve 9 of the present invention is described below. Figure 4 As shown, the sprue sleeve and sprue cup of the present invention are positioned and installed through the step portion 14, and a certain installation margin is left between the outer wall 15 of the sprue sleeve and the inner wall of the sprue cup. The lower opening of the sprue sleeve is connected with the upper opening of the sprue cup. The upper opening 16 of the sprue sleeve is a special-shaped opening and is connected with the inlet of the mold cavity. A net placing groove 17 is opened at the upper opening of the sprue sleeve for placing a filter net 18, and the lower opening 19 of the sprue cup is connected with the liquid riser.

[0040] The liquid inlet channel formed by the inner surface of the gate sleeve is roughly in the shape of the cavity gate of the casting mold at this filling point, and its shape is described as the cross-sectional shape of the front gate sleeve 9.

[0041] In a preferred embodiment, the cross-sectional shape of the filter screen is the same as that of the liquid inlet channel.

[0042] The number of the sprue bushings is two, which are symmetrically arranged on both sides relative to the wheel axis. The number of the sprue bushings can also be greater than two, which are arranged around the wheel axis.

[0043] Particularly preferably, a local pressure device is provided below the wheel center position corresponding to the wheel on the mold to promote shrinkage compensation at the wheel center position, such as Figure 5 As shown, the local pressurizing device includes a pressure driving mechanism 20, a pressure transmitting mechanism 22 and a pressure applying mechanism 23. The pressure applying mechanism 23 is in contact with the metal melt and applies pressure to the metal melt after the filling is completed.

[0044] In particular, the pressure driving mechanism may be a hydraulic cylinder, the pressure transmission mechanism may be a hydraulic rod, and the pressure applying mechanism may be a pressure block. The specific pressurization process is to apply a mechanical pressure of 1000KPa to 12000KPa after the filling is completed. The aluminum liquid here is solidified under extremely high pressure to prevent shrinkage cavities and shrinkage defects from forming here due to insufficient edge shrinkage pressure.

[0045] A refinement device may be provided above the wheel mold corresponding to the position of the wheel center, i.e., corresponding to the diverter cone of the conventional center bottom injection molding method. The refinement mechanism may be an ultrasonic refinement mechanism or a vibration refinement mechanism. For example, the refinement device may include a vibration generator 24 and a vibration rod 21. The vibration rod 21 is inserted into the aluminum liquid to vibrate the aluminum liquid during the solidification process, so that the dendrites formed by the aluminum liquid crystallization are broken, the nucleation is enhanced, the grains are refined, and the mechanical properties of the wheel are improved.

[0046] The anti-gravity wheel forming process used in conjunction with the present invention is described below.

[0047] Figure 6 This is a typical wheel structure diagram, in which in the prior art, the center of the wheel is usually called the wheel center, the part on the outside of the wheel that is assembled with the tire and supports the tire is called the rim, the wheel part that is installed and connected to the axle wheel center and supports the rim is called the spoke, and there is a window in the middle of the multiple spokes. The rim part that maintains and supports the direction of the tire is called the flange.

[0048] In the existing production of low-pressure or differential-pressure cast aluminum alloy wheels, almost all of them use a riser pipe set at the central wheel center position of the wheel, and allow the melt to pass through the insulation cup and pouring assembly connected to the riser pipe, enter the mold cavity from the gate at the wheel center, and be diverted under the action of the diverter cone, and fill the mold in the order of wheel center-spoke-rim-rim, and solidify after filling the mold cavity. This is because in actual production, it is easiest to set the gate and riser pipe here, and the cross-sectional shape of the gate is a regular circle, which is simple to process. At the same time, the area of ​​the gate is large, which can make the filling speed fast. However, some problems caused by the above-mentioned pouring and filling method have never been well solved, such as the long gate distance, the long filling distance, and it is very difficult to compensate for shrinkage at the hot joints such as the connection between the rim and the spoke, which is easy to form shrinkage cavities and shrinkage, becoming a major problem that plagues the production of the wheel industry. Although water cooling, water mist cooling and other methods are used to enhance cooling in order to achieve sequential solidification, the short filling and solidification time of the wheel makes it difficult to accurately control the temperature field, and a considerable proportion of scrap is still inevitable.

[0049] In the prior art, bilateral pouring is performed at the middle of the rim side. However, the filling and solidification sequence is uncontrollable due to the filling diversion, which also easily leads to shrinkage defects.

[0050] The present invention also discloses a counter-gravity casting process suitable for the filling mode. Since the pouring and filling method of the present invention has undergone tremendous changes compared with the prior art, the original filling method and solidification process cannot be applied to the present invention. Based on this, the present invention also designs a process suitable for the filling position.

[0051] The specific steps include:

[0052] (1) Liquor lifting: The aluminum liquid in the holding furnace is pressurized by a high-pressure gas source, so that the aluminum liquid rises to the pouring gate position along the liquid riser under pressure. The pressure raising speed in this stage is 2.8-4.0 KPa / s, and the pressure is increased to 20 KPa;

[0053] (2) Filling: Continue to increase the pressure to allow the aluminum liquid to enter the mold cavity through the gate. This filling stage is a two-stage pressurization. The pressure increase rate in the first stage is 0.1-0.2 KPa / s for 2-4 seconds. Then enter the second stage to increase the pressure rapidly until the mold cavity is filled. At this time, the pressure reaches 35 KPa.

[0054] The pressure increase speed P' of the second stage is determined as follows:

[0055]

[0056] Where:

[0057] P′ is the pressure increase rate, in kPa / s; H is the total height of the cavity, in mm; ρ is the density of the metal melt, in g / cm 3 ; K is the resistance coefficient, and its value range is 1 to 1.5; t is the preset filling time, in seconds, preferably 10 seconds; 102 is the unit conversion coefficient; N is the number of liquid riser tubes, and its value range is 2 to 6, which can be selected according to the number of windows of different types of wheels, preferably 2 to 4; x is its liquid rise index, and its value range is 0.2 to 0.8. In the wheel type scheme adopted in this embodiment, the value is 0.5.

[0058] (3) Crystallization pressurization and pressure holding: After filling is completed, the pressure is rapidly increased to 150 KPa at a pressure increase rate of 8 to 10 KPa / , and the pressure is maintained for 60 to 150 seconds. At this time, the wheel solidification is completed.

[0059] (4) Depressurization and venting: After the aluminum alloy wheel has solidified, the gas pressure in the holding furnace is released, allowing the unsolidified aluminum liquid in the riser and pouring nozzle to flow back into the holding furnace.

[0060] As for the selection of the pressure increasing speed in the liquid raising stage and the mold filling stage, since the inner diameter of the liquid raising pipe is fixed during the liquid raising, turbulence will basically not be generated, so a fast pressure increasing speed is adopted so that the metal melt can be quickly raised to the gate position and the liquid raising time is shortened. In the mold filling stage, the complex shapes of the mold cavity and the gate must be taken into consideration. In the traditional mold filling method, since the method of pouring from the wheel center position is adopted, the cross-sectional area of ​​the liquid raising pipe and the gate is not much different, and the cross-sectional area of ​​the mold cavity at the wheel center is large, and turbulence is not easy to be generated. Therefore, the filling pressure increasing speed can be obtained by experience or experiment. For the mold filling method of the present invention, the mold filling is carried out on the annular surface of the rim, which is an irregular conformal gate. The shape area of ​​the liquid raising pipe and the gate is very different. At the same time, the space at the rim is small. If the filling pressure is unreasonable, turbulent air is easily generated, resulting in pore defects. The filling pressure design in the prior art adopts the calculation method under the ideal state, combined with the resistance coefficient, etc. for correction. The flow state change caused by the change of the cross-sectional area of ​​the liquid raising pipe and the gate is not considered. Therefore, it is impossible to obtain the ideal filling and pressurizing speed by using the empirical formula in the prior art.

[0061] Therefore, the present invention has studied the above problems, combined with the riser, the gate, the shape and cross-sectional area of ​​the cavity above the gate, and the flow characteristics of the metal melt. It is found that for the wheel rim position, if Figure 7 In the circle indicated by the arrow in a, there are two parts where the area changes significantly in the initial stage of filling, such as Figure 7 At the circular frame indicated by the arrow in b, if turbulence occurs, air entrainment is very likely to form at this position. After design and calculation, the present invention adopts a two-stage pressurization. The first stage significantly reduces the pressurization speed so that the metal melt can flow smoothly in the initial stage of filling and fill the above area to avoid air entrainment. Figure 7 c (the arrow here indicates the direction of melt filling), and then enters the second stage of rapid pressure increase to shorten the filling time. In the second stage of the filling process of the present invention, it is found that the filling stability is significantly related to the number of riser tubes, because the traditional method of pouring from the wheel center position has only one riser tube and gate, so the law can be obtained through experiments and quantitative processing can be performed. In the filling method of the present invention, the number of riser tubes and gates can be 2 or more. Under the same boosting conditions, the flow rate at the gate and the flow rate in the cavity above the gate will change significantly, resulting in uncontrollable filling flow mode. Therefore, the present invention obtains the boosting method of the second stage through research. It can be seen from formula (1) that within the same preset filling time, as the number of riser tubes increases, the boosting speed that can be adopted can be gradually increased, and will not cause turbulent air entrainment and other problems. The value of the resistance coefficient is related to the viscosity of the molten metal, the complexity of the casting cavity, etc. When the resistance is small, the lower limit is taken, and when the resistance is large, the upper limit is taken.

[0062] Embodiment 1:

[0063] Two riser tubes and pouring gates are used, and the mass percentage composition of the metal melt used is as follows: Si: 7-9%, Mg: 0.6-0.9%, Zr: 0.01-0.02%, B: 0.005-0.007%, RE: 0.002-0.005%, Nd: 0.002-0.005%, Fe: 0-0.15%, Mn: 0.05-0.1%, Ti: 0.12-0.14%, and the rest is Al and unavoidable impurities.

[0064] (1) Liquor lifting: The aluminum liquid in the holding furnace is pressurized by a high-pressure gas source, so that the aluminum liquid rises to the pouring gate position along the liquid riser under pressure. The pressure raising speed in this stage is 3.5 KPa / s, and the pressure is increased to 20 KPa;

[0065] (2) Filling: Continue to increase the pressure to allow the aluminum liquid to enter the mold cavity through the gate. The pressure increase rate in the first stage is 0.2 KPa / s and the time is 1.8 s, so that the metal melt is filled steadily. Figure 7 b The area indicated by the arrow enters the second stage and then quickly fills the mold at a pressure increase rate of 0.66 KPa / s until the cavity is filled.

[0066] (3) Crystallization pressurization and pressure holding: After the filling is completed, the pressure is quickly increased to 150KPa at a pressure increase rate of 8KPa / s, and the pressure is maintained. The hydraulic cylinder drives the hydraulic rod to drive the pressure block to apply 2000KPa mechanical pressure to the wheel center position, and the vibration generator drives the vibration rod to vibrate and refine the aluminum liquid until the wheel solidifies. During the pressure holding process, the high pressure shrinkage of the rim hot section is maintained at the gate. Under the high-pressure aluminum liquid shrinkage, the possibility of shrinkage cavities and shrinkage at this location is completely eliminated. At the same time, the pressure block locally pressurizes the metal liquid at the wheel center, eliminating the possibility of shrinkage cavities and shrinkage at this location.

[0067] (4) Depressurization and venting: After the aluminum alloy wheel has solidified, the gas pressure in the holding furnace is released, allowing the unsolidified aluminum liquid in the riser and pouring nozzle to flow back into the holding furnace.

[0068] The above description is only a preferred embodiment of the present invention and does not limit the present invention in any way. Any simple modification, change and equivalent structural change made to the above embodiment based on the technical essence of the present invention still falls within the protection scope of the technical solution of the present invention.

Claims

1. A wheel anti-gravity casting device with a crucible insulation furnace, comprising at least a crucible insulation furnace and a mold; The crucible insulation furnace comprises a furnace body, the inner wall of the furnace body is provided with an insulation layer formed by refractory materials, a crucible is provided in the furnace body, a metal melt is contained in the crucible, an electric heating device is provided in the furnace body, a furnace cover is provided on the upper part of the furnace body, a temperature measuring thermocouple is provided on the furnace cover, the furnace cover is connected to the liquid riser pipes on both sides, and the furnace cover is connected to the high-pressure gas source; the thermocouple measures the temperature of the metal melt in the crucible insulation furnace, and controls the electric heating device to keep it at the filling temperature, and the high-pressure gas source is used to make the metal melt rise to the mold cavity; A pouring assembly is connected above the riser pipes on both sides. The pouring assembly includes a pouring cup and a pouring sleeve. The pouring cup is connected to the riser pipes on both sides below. A pouring sleeve is provided above the pouring cup. The pouring sleeve corresponds to the position directly below the rim of the wheel mold, is connected to the cavity inlet for pouring into the mold cavity, and pours the rising metal melt into the cavity by pressing the edge. It is characterized in that The sprue sleeve and the sprue cup are positioned and installed through the step portion, and a certain installation margin is left between the outer wall of the sprue sleeve and the inner wall of the sprue cup. The lower opening of the sprue sleeve is connected with the upper opening of the sprue cup. The upper opening of the sprue sleeve is a special-shaped opening and is connected with the mold cavity entrance. A net placing groove is provided at the upper opening of the sprue sleeve for placing a filter net, and the lower opening of the sprue cup is connected with the riser pipe; the mold cavity entrance corresponding to each sprue sleeve is arranged on the annular surface just below the rim of the wheel; the annular surface just below the rim refers to the annular surface formed around the center axis of the wheel on the side of the rim opposite to the wheel flange; the outer circle constituting the annular ring is the circle formed by the outermost contour line of the wheel on the surface, and the inner circle is the circle formed by the outer contour line of the window area of ​​the wheel around the center axis of the wheel; The cross-sectional shape of the gate sleeve communicating with the cavity inlet is: comprising a first arc segment and a second arc segment, the first arc segment and the second arc segment are concentric, the radius and size of the first arc segment are smaller than those of the second arc segment, and the first arc segment and the second arc segment are connected at both sides by a connecting segment; The filling process of the wheel anti-gravity casting equipment with a crucible insulation furnace is a two-stage pressurization process, in which the pressure increase rate in the first stage is 0.1-0.2 kPa / s for 2-4 seconds, and then the second stage is rapidly pressurized until the cavity is filled, at which time the pressure reaches 35 kPa; The boost speed of the second stage Determined by: (1) Where: is the pressure increase rate, in kPa / s; H is the total height of the cavity, in mm; is the density of the metal melt, in g / cm 3 ; is the resistance coefficient, and its value range is 1~1.5; is the preset filling time, in seconds; 102 is the unit conversion factor; N is the number of riser tubes, and its value range is 2~6; Its liquid rise index ranges from 0.2 to 0.

8.

2. The wheel anti-gravity casting equipment with a crucible insulation furnace according to claim 1, characterized in that: The sprue sleeve and the cavity inlet are arranged at positions on the annular surface corresponding to the outer side of the window area, or at positions on the annular surface corresponding to the connection between the rim and the spoke.

3. The wheel anti-gravity casting equipment with a crucible insulation furnace according to claim 1, characterized in that: There is also an insulation layer under the furnace cover, and a charging port is opened on one side of the furnace cover for adding molten aluminum.

4. The wheel counter-gravity casting equipment with a crucible insulation furnace according to claim 1, characterized in that: A roller is provided at the bottom of the furnace body, and the roller is located on a track and can move along the track.

5. The wheel anti-gravity casting equipment with a crucible insulation furnace according to claim 1, characterized in that: The cross-sectional shape of the filter screen is the same as that of the liquid inlet channel.

Citation Information

Patent Citations

  • Low-pressure casting process and device for aluminum alloy wheel by bilateral pouring

    CN101837443A

  • Low-pressure casting die for wheel hub and pouring method of low-pressure casting die

    CN103551545A

  • Combined pouring and purifying system for automobile aluminium alloy wheel with big diameter being more than 26 inches

    CN104550843A

  • One unit-dual simulator hub mold

    CN105855514A

  • Casting pouring gate structure of hub

    CN103658540A

Cited By

  • Casting process method, equipment and medium

    CN120885671A