A silicon-on-insulator structure and method thereof
The two-step etching method solves the problem of poor thickness uniformity of the top silicon in SOI materials, achieves efficient planarization of the top silicon in the SOI process, and improves the performance of integrated circuits.
Patent Information
- Application Number
- CN202011445232.X
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2020-12-08
- Publication Date
- 2024-10-29
- Estimated Expiration
- 2040-12-08
AI Technical Summary
In the process of silicon-on-insulator (SOI) materials, the thickness uniformity of the top layer of silicon is difficult to meet the increased requirements. The existing chemical mechanical polishing (CMP) process cannot effectively solve this problem, resulting in poor thickness uniformity of the top layer of silicon.
A two-step etching method is adopted: first, hydrogen is used for the first etching and thinning at a lower temperature (900℃~1000℃), and then hydrogen is used for the second etching at a higher temperature (above 1050℃). , by adjusting the etching temperature and gas flow to planarize the top silicon to ensure thickness uniformity.
Through this method, the thickness uniformity of the top silicon can be significantly improved to meet the technical requirements of deep sub-micron low-voltage, low-power integrated circuits.
Smart Images

Figure CN112599470B_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to the field of semiconductor manufacturing, and in particular to a silicon-on-insulator structure and a method thereof. Background Art
[0002] Silicon-On-Insulator (SOI) is a technology that introduces at least one buried oxide layer between the top silicon and the back substrate. It mainly means that the silicon transistor structure is on top of the insulator. The principle is that by adding an insulator material between the silicon transistors, the parasitic capacitance between the two can be reduced by half. Advantages of SOI materials: It can achieve dielectric isolation of components in integrated circuits and completely eliminate the parasitic latch effect in bulk silicon CMOS circuits; integrated circuits made of this material also have the advantages of small parasitic capacitance, high integration density, fast speed, simple process, small short channel effect and are particularly suitable for low-voltage and low-power circuits. Therefore, it can be said that SOI will likely become the mainstream technology for deep submicron low-voltage and low-power integrated circuits. In addition, SOI materials are also used to manufacture MEMS optical switches, such as using bulk micromachining technology.
[0003] For SOI materials, the uniformity of the top silicon thickness is a key parameter that has a significant impact on device performance. In the SOI process, the top silicon is usually flattened using the Chemical Mechanical Polishing (CMP) process. However, as the requirements for the uniformity of the top silicon increase, the polishing effect of the CMP process can no longer meet the process requirements.
[0004] In order to solve the above problems, etching gas HCl is usually used to react with silicon wafers under high temperature conditions to flatten the top silicon surface. However, in this process, there is a certain difference between the etching rate of the etching gas HCl at the edge position and the etching rate at the center position of the silicon wafer. As the etching proceeds, the thickness uniformity of the top silicon is poor. Summary of the invention
[0005] The invention provides a silicon-on-insulator structure and a method thereof, which can improve the thickness uniformity of the top silicon layer when the top silicon layer is planarized.
[0006] In order to solve the above technical problems, the present invention provides a method for a silicon-on-insulator structure, comprising the following steps:
[0007] Step S1: providing a bonding structure, wherein the bonding structure comprises a first substrate, a second substrate and an insulating buried layer, wherein the insulating buried layer is located between the first substrate and the second substrate;
[0008] Step S2: peeling off and removing a portion of the thickness of the first substrate from the bonding structure to obtain a first film;
[0009] Step S3: etching the first film for the first time at a first temperature to remove the first film having a first thickness;
[0010] Step S4: etching the first film for a second time at a second temperature to planarize the first film and remove a second thickness of the first film, wherein the first temperature is lower than the second temperature, the first thickness is higher than the second thickness, and the first thickness and the second thickness are the total etching thickness of the first film.
[0011] Optionally, step S3 includes:
[0012] In a rapid thermal annealing device or an epitaxial device, hydrogen is used as a first carrier gas and a first etching gas is used to perform a first etching on the first film to remove the first film having a first thickness.
[0013] Furthermore, the process parameters of the first etching are: etching temperature is 900° C. to 1000° C., flow rate of the first carrier gas is 40 slm to 120 slm, and volume fraction of the first etching gas is less than 1%.
[0014] Optionally, the proportion of the first thickness to the total etched thickness does not exceed 70%.
[0015] Optionally, step S4 includes:
[0016] In a rapid thermal annealing device or an epitaxial device, hydrogen is used as a second carrier gas and a second etching gas is used to etch the first film for a second time to planarize the first film and remove a second thickness of the first film.
[0017] Furthermore, it is characterized in that the process parameters of the second etching are: the etching temperature is higher than 1050°C, the flow rate of the second carrier gas is 40slm~120slm, the volume fraction of the second etching gas is lower than 0.5%, and the volume fraction of the second etching gas is lower than the volume fraction of the first etching gas.
[0018] Furthermore, the first etching gas and the second etching gas both include HCl gas.
[0019] Optionally, the method for forming the bonding structure includes:
[0020] providing a first substrate and a second substrate;
[0021] growing a first oxide layer on the front side of the first substrate;
[0022] Performing an ion implantation process from the front side of the first substrate into the first substrate to obtain a damaged layer;
[0023] The front side of the first substrate and the front side of the second substrate are bonded to form a bonding structure.
[0024] Furthermore, when the thickness of the insulating buried layer is When the thickness of the insulating buried layer is greater than When the buried insulating layer includes a first oxide layer and a second oxide layer;
[0025] and while growing a first oxide layer on the front side of the first substrate,
[0026] A second oxide layer is formed on the front surface of the second substrate.
[0027] Furthermore, the thickness of the first oxide layer is The thickness of the second oxide layer is
[0028] Further, step S2 includes:
[0029] Performing a first annealing treatment on the bonding structure, the bonding structure is peeled off along the damaged layer, and a first thin film located on the insulating buried layer is obtained, and the second substrate, the insulating buried layer and the first thin film constitute a silicon-on-insulator structure;
[0030] performing a second annealing process on the silicon-on-insulator structure;
[0031] The surface of the first film is cleaned.
[0032] Furthermore, the second annealing treatment is performed in an oxygen-containing atmosphere, and a silicon oxide film layer is grown on the surface of the first film; and the cleaning treatment is used to remove the silicon oxide film layer.
[0033] The present invention also provides a silicon-on-insulator structure, which is prepared by the above method.
[0034] Compared with the prior art, the present invention has the following beneficial effects:
[0035] The present invention provides a silicon-on-insulator structure and a method thereof, the method comprising the following steps: step S1: providing a bonding structure, the bonding structure comprising a first substrate, a second substrate and an insulating buried layer, the insulating buried layer being located between the first substrate and the second substrate; step S2: stripping and removing a portion of the thickness of the first substrate from the bonding structure to obtain a first film; step S3: etching the first film for the first time at a first temperature to remove the first film of a first thickness; step S4: etching the first film for the second time at a second temperature to flatten the first film and remove the first film of a second thickness, the first temperature being lower than the second temperature, the first thickness being higher than the second thickness, the first thickness and the second thickness being the total etching thickness of the first film. The present invention thins the first film by etching at the first temperature in step S3, and then flattens the first film at the second temperature in step S4, and simultaneously reaches the target thickness of the first film, so that the uniformity of the thickness of the top silicon can be improved while flattening the top silicon. BRIEF DESCRIPTION OF THE DRAWINGS
[0036] Figure 1 It is a schematic flow chart of a method for a silicon-on-insulator structure according to an embodiment of the present invention;
[0037] Figure 2a-2i It is a structural schematic diagram of each step of a method for a silicon-on-insulator structure according to an embodiment of the present invention;
[0038] Figure 3 It is a temperature-time curve diagram of a cleaning process, a first etching and a second etching in one embodiment of the present invention.
[0039] Description of reference numerals:
[0040] I-first time period; II-second time period; III-third time period;
[0041] 10-bonding structure; 10'-silicon-on-insulator structure; 100-first substrate; 100a-front side of the first substrate; 100b-back side of the first substrate; 110-first film layer; 111-ion implantation layer; 112-silicon oxide film layer; 200-insulating buried layer; 210-first oxide layer; 220-second oxide layer; 300-second substrate; 300a-front side of the second substrate; 300b-back side of the second substrate. DETAILED DESCRIPTION
[0042] A silicon-on-insulator structure and method of the present invention will be described in further detail below. The present invention will be described in more detail below with reference to the accompanying drawings, in which preferred embodiments of the present invention are shown, and it should be understood that those skilled in the art can modify the present invention described herein and still achieve the beneficial effects of the present invention. Therefore, the following description should be understood as being widely known to those skilled in the art and not as a limitation of the present invention.
[0043] For the sake of clarity, not all features of the actual embodiments are described. In the following description, well-known functions and structures are not described in detail because they would clutter the invention with unnecessary detail. It should be recognized that in the development of any actual embodiment, a large number of implementation details must be made to achieve the developer's specific goals, such as changing from one embodiment to another according to the limitations of the relevant system or the relevant business. In addition, it should be recognized that such development work may be complex and time-consuming, but it is just a routine task for those skilled in the art.
[0044] In order to make the purpose and features of the present invention more obvious and easy to understand, the specific implementation methods of the present invention are further described below in conjunction with the accompanying drawings. It should be noted that the accompanying drawings are all in a very simplified form and use inaccurate ratios, which are only used to conveniently and clearly assist in explaining the purpose of the embodiments of the present invention.
[0045] Figure 1 FIG. 2 is a flow chart of a method for a silicon-on-insulator structure according to the present embodiment. Figure 1 As shown, a method for a silicon-on-insulator structure provided in this embodiment includes the following steps:
[0046] Step S1: providing a bonding structure, wherein the bonding structure comprises a first substrate, a second substrate and an insulating buried layer, wherein the insulating buried layer is located between the first substrate and the second substrate;
[0047] Step S2: peeling off and removing a portion of the thickness of the first substrate from the bonding structure to obtain a first film;
[0048] Step S3: etching the first film for the first time at a first temperature to remove the first film having a first thickness;
[0049] Step S4: etching the first film for a second time at a second temperature to planarize the first film and remove a second thickness of the first film, wherein the first temperature is lower than the second temperature, the first thickness is greater than the second thickness, and the first thickness and the second thickness are the total etching thickness of the first film.
[0050] Combine the following Figure 1 as well as Figure 2a~2iA method for a silicon-on-insulator structure disclosed in this embodiment is introduced in more detail.
[0051] Figure 2a It is a schematic diagram of the cross-sectional structure of the first substrate provided in this embodiment. Figure 2b It is a schematic diagram of the cross-sectional structure of the second substrate provided in this embodiment. Figure 2c It is a schematic diagram of the cross-sectional structure of the first substrate after the ion implantation process in this embodiment. Figure 2d Schematic diagram of the cross-sectional structure of the bonding structure of this embodiment.
[0052] like Figure 2a to 2d As shown, step S1 is first performed to provide a bonding structure 10, wherein the bonding structure 10 includes a first substrate 100, a second substrate 300 and an insulating buried layer 200, wherein the insulating buried layer 200 and the first substrate 100 are stacked on the second substrate 300 in sequence, that is, the insulating buried layer 200 is located between the first substrate 100 and the second substrate 300.
[0053] This step specifically includes the following steps:
[0054] like Figure 2a and Figure 2b As shown, first, a first substrate 100 and a second substrate 300 are provided. The first substrate 100 and the second substrate 300 are, for example, both bare chips. Specifically, the first substrate 100 and the second substrate 300 are, for example, both bare silicon substrates. Preferably, the shape of the first substrate 100 is the same as that of the second substrate 300, and the size of the first substrate 100 is the same as that of the second substrate 300. The first substrate 100 includes a front side 100a and a back side 100b that are oppositely arranged; the second substrate 300 includes a front side 300a and a back side 300b that are oppositely arranged.
[0055] Next, when the thickness of the insulating buried layer 200 is In the following case, the buried insulating layer 200 only includes the first oxide layer 210. At this time, the first oxide layer 210 is grown on the front surface 100a of the first substrate. The thickness of the first oxide layer 210 is, for example, The thickness of the buried insulating layer 200 is equal to the thickness of the first oxide layer 210 .
[0056] When the thickness of the insulating buried layer 200 is greater than When the buried insulating layer 200 includes a first oxide layer 210 and a second oxide layer 220, the first oxide layer 210 is grown on the front surface of the first substrate 100, and the thickness of the first oxide layer 210 is, for example, At the same time, a second oxide layer 210 is formed on the front surface 300a of the second substrate. The thickness of the second oxide layer 210 is, for example, The thickness of the buried insulating layer 200 is the sum of the thickness of the first oxide layer 210 and the thickness of the second oxide layer 210. In this embodiment, the thickness of the buried insulating layer 200 is greater than Therefore, the buried insulating layer 200 includes a first oxide layer 210 and a second oxide layer 220 .
[0057] like Figure 2c As shown, next, an ion implantation process is performed into the first substrate 100 from the front side 100 a of the first substrate to obtain an ion implantation layer 111 of the first substrate 100 .
[0058] In this step, since ion implantation is one of the important means in the semiconductor production process, semiconductor doping can be easily achieved by ion implantation, especially the introduction of impurities at a specified position and depth, which is very critical in the preparation process of semiconductor devices; moreover, ion implantation can also accurately control impurities and has high repeatability, which is not met by conventional doping methods. In this embodiment, an ion implantation process is performed from the surface of the first oxide layer 210 into the first substrate 100 to form an implantation damage layer at a preset depth inside the first substrate 100, that is, an ion implantation layer 111, and then the first film can be stripped and transferred in the ion implantation layer 111. The implantation energy of the ion implantation determines the depth of the implanted ion aggregation, that is, the thickness of the transferred first film. Therefore, the preset depth depends on the thickness of the transferred first film. The energy of the ion implantation must be sufficient to enable the implanted ions to reach the preset depth in the first substrate 100. The ion implantation energy in the ion implantation process of this embodiment is 10KeV~200KeV, and the dose is 5.5*10 16 / cm 2 ~7.5*10 16 / cm 2 .
[0059] Among them, the ion implantation process adopts any one or more ions of hydrogen ions, helium ions, neon ions, argon ions, krypton ions, xenon ions, radon ions or hydrogen ions for co-injection, such as hydrogen and helium ion co-injection. When the ion implantation is performed by hydrogen and helium ion co-injection, the implantation sequence of hydrogen ions and helium ions can also be appropriately adjusted according to actual needs. In the present embodiment, the implantation sequence of hydrogen ions and helium ions is, for example, to first implant hydrogen ions and then implant helium ions, and the implantation depth of helium ions is deeper than the implantation depth of hydrogen ions.
[0060] Due to the appendages generated when the first oxide layer 210 and the second oxide layer 220 are formed and the particle contamination generated during the ion implantation process, cleaning is required to obtain a clean surface for the subsequent bonding process. Therefore, the first substrate 100 and the second substrate 300 are then cleaned to clean the surface of the first oxide layer 210 and the surface of the second oxide layer 220.
[0061] like Figure 2d As shown, next, the first oxide layer 210 and the second oxide layer 220 are bonded to bond the front side 100 a of the first substrate and the front side 300 a of the second substrate, thereby forming a bonding structure 10 .
[0062] Figure 2e FIG. 4 is a schematic cross-sectional structural diagram of a silicon-on-insulator structure formed in this embodiment. Figure 2f FIG. 4 is a schematic cross-sectional structural diagram of the silicon-on-insulator structure after the second annealing treatment of this embodiment.
[0063] Then, step S2 is performed to peel off and remove a portion of the thickness of the first substrate 100 from the bonding structure 10 to obtain a first film 110 .
[0064] This step specifically includes:
[0065] like Figure 2e As shown, first, the bonding structure 10 is subjected to a first annealing treatment, and the bonding structure 10 is peeled off along the ion implantation layer 111 (damaged layer) to obtain a first film 110 located on the insulating buried layer 200 and a first substrate 100 after peeling. Among them, the first film 110 is the first substrate 100 of partial thickness, and the first substrate 100 after peeling off the first film 110 can be recycled to serve as the first substrate for forming the bonding structure 10 next time. The second substrate 300, the insulating buried layer 200 and the first film 110 together constitute a silicon-on-insulator structure 10'. In this embodiment, the annealing temperature of the first annealing process can be 400°C to 600°C, and the annealing time does not exceed 30 minutes.
[0066] like Figure 2f As shown, the silicon-on-insulator structure 10' is then subjected to a second annealing treatment, which is performed in an oxygen-containing atmosphere. Physical and chemical reactions occur at the bonding interface, which can significantly increase the bonding strength. The annealing temperature of the second annealing treatment is lower than 1250° C. During the second annealing treatment, since the first film 110 is exposed to an oxygen-containing atmosphere, the silicon in the first film 110 reacts with oxygen, and a silicon oxide film layer 112 grows on the surface of the first film 110.
[0067] like Figure 2g As shown, the silicon oxide film layer 112 is then removed by a cleaning process. Hydrogen fluoride (HF) is introduced into the cleaning process to clean and remove the silicon oxide film layer 112.
[0068] After step S2, the surface of the first film 110 is then cleaned. Specifically, in a rapid thermal annealing device or an epitaxial device, a temperature environment of more than 1100° C. is adopted, and a reducing gas such as hydrogen is introduced, and the flow rate of the reducing gas is 20slm to 100slm. The cleaning treatment time is 30s to 60s, so as to clean and remove the natural oxide layer on the surface of the first film 110. This step can ensure the uniformity of the subsequent etching of silicon by HCl.
[0069] Figure 2h is a schematic diagram of the cross-sectional structure of the present embodiment after the first thickness is removed. Figure 2h As shown, step S3 is then performed to etch the first film 110 for the first time at a first temperature to remove the first film 110 having a first thickness.
[0070] Specifically, Figure 2h As shown, the temperature in the rapid thermal annealing equipment or the epitaxial equipment is lowered to 900°C to 1000°C, for example 900°C, 910°C, 920°C, 930°C, 940°C, 950°C, 960°C, 970°C, 980°C, 990°C, 1000°C, etc., and hydrogen is used as the first carrier gas, and a first etching gas (such as HCl gas) reacts with the first film 110, and the flow rate of the first carrier gas is 40slm to 120slm. Preferably, the flow rate of the first carrier gas is 60slm to 120slm, and the volume fraction of the first etching gas is less than 1%. Since the etching rate at the edge of the first film 110 is relatively small compared to the etching rate at the center during etching at the first temperature after the temperature is reduced, and the volume fraction of the first etching gas of the etching process is relatively large, that is, a relatively fast etching is performed using a first etching gas with a large flow rate to obtain the first film 110 close to the target thickness, the etching process of this step performs etching at a relatively large flow rate at a relatively low first temperature to obtain a top layer of silicon (first film 110) with good thickness uniformity. Wherein, the first thickness, for example, accounts for no more than 70% of the total etching thickness.
[0071] Figure 2i is a schematic diagram of the cross-sectional structure of the present embodiment after the second thickness is removed. Figure 2iAs shown, step S4 is then performed to etch the first film 110 for the second time at a second temperature to planarize the first film 110 and remove the first film 110 of a second thickness, wherein the first temperature is lower than the second temperature, the first thickness is greater than the second thickness, and the first thickness and the second thickness are the total etching thickness of the first film 110.
[0072] Specifically, the temperature in the rapid thermal annealing equipment or the epitaxial equipment is increased to a temperature higher than 1050°C, such as 1060°C, 1070°C, 1080°C, 1090°C, 1100°C, 1110°C, 1120°C, 1130°C, 1150°C, 1200°C, 1300°C, etc., and the heating rate is 3°C / s to 4°C / s (degrees Celsius per second), and hydrogen is used as the second carrier gas, and a second etching gas (such as HCl gas) reacts with the first film 110, and the flow rate of the second carrier gas is 40slm to 120slm. Preferably, the flow rate of the second carrier gas is 60slm to 120slm, and the volume fraction of the second etching gas is less than 0.5%, and the volume fraction of the second etching gas is lower than the volume fraction of the first etching gas. Since a small amount of etching with a smaller flow rate is performed at the second temperature after the temperature is raised, the etching rate is almost unaffected by the temperature. Since the etching amount at the second temperature is smaller (the second thickness is smaller), the surface roughness of the first film decreases with increasing temperature, that is, etching at high temperature is more conducive to planarization.
[0073] Figure 3 2 is a temperature-time curve diagram of the cleaning process, the first etching and the second etching of this embodiment. Figure 3 As shown, after the rapid thermal annealing equipment or epitaxial equipment, there are three time periods, which are the first time period I, the second time period II, and the third time period III. In the first time period I, the silicon-on-insulator structure enters the equipment and is rapidly heated to 1100°C, and is kept at 1100°C for several seconds, and the silicon oxide film layer is removed by hydrogen etching to clean the surface of the first film layer; in the second time period II, the temperature is reduced to 900°C, and the first film layer with most of the thickness (first etching thickness) is removed by etching with a large flow of the first etching gas, so as to thin the first film layer at the edge and the center at a low temperature and obtain a uniform thickness; in the third time period III, the temperature is rapidly increased to 1150°C, and the first film layer with a small thickness (second etching thickness) is removed by etching with a small flow of the second etching gas, so as to achieve the thinning and flattening of the top silicon. In this process, the flattening effect and the uniformity of the thickness of the top silicon are adjusted to a certain extent by changing the etching thickness ratio at the first temperature and the second temperature.
[0074] This embodiment also provides a silicon-on-insulator structure, which is prepared by the above preparation method.
[0075] In summary, the present invention provides a silicon-on-insulator structure and a method thereof, the method comprising the following steps: step S1: providing a bonding structure, the bonding structure comprising a first substrate, a second substrate and an insulating buried layer, the insulating buried layer being located between the first substrate and the second substrate; step S2: peeling and removing a portion of the thickness of the first substrate from the bonding structure to obtain a first film; step S3: etching the first film for the first time at a first temperature to remove the first film of the first thickness; step S4: etching the first film for the second time at a second temperature to flatten the first film and remove the first film of the second thickness, the first temperature is lower than the second temperature, the first thickness is greater than the second thickness, and the first thickness and the second thickness are the total etching thickness of the first film. The present invention thins the first film by etching at the first temperature in step S3, and then flattens the first film at the second temperature in step S4, and simultaneously reaches the target thickness of the first film, so that the uniformity of the thickness of the top silicon can be improved while flattening the top silicon.
[0076] In addition, it should be noted that, unless otherwise specified or indicated, the terms "first" and "second" in the specification are only used to distinguish the various components, elements, steps, etc. in the specification, and are not used to indicate the logical relationship or sequential relationship between the various components, elements, steps, etc.
[0077] It is to be understood that, although the present invention has been disclosed as a preferred embodiment, the above embodiment is not intended to limit the present invention. For any person skilled in the art, without departing from the scope of the technical solution of the present invention, the technical content disclosed above can be used to make many possible changes and modifications to the technical solution of the present invention, or modified into equivalent embodiments of equivalent changes. Therefore, any simple modification, equivalent change and modification made to the above embodiments according to the technical essence of the present invention without departing from the content of the technical solution of the present invention still falls within the scope of protection of the technical solution of the present invention.
Claims
1. A method for a silicon-on-insulator structure, characterized in that: The following steps are involved: Step S1: providing a bonding structure, wherein the bonding structure comprises a first substrate, a second substrate and an insulating buried layer, wherein the insulating buried layer is located between the first substrate and the second substrate; Step S2: peeling off and removing a portion of the thickness of the first substrate from the bonding structure to obtain a first film; Step S3: etching the first film for the first time at a first temperature to remove the first film of the first thickness, wherein the process parameters of the first etching are: etching temperature of 900° C. to 1000° C., flow rate of the first carrier gas of 40 slm to 120 slm, and volume fraction of the first etching gas of less than 1%; Step S4: Etching the first film for a second time at a second temperature to planarize the first film and remove a second thickness of the first film, wherein the first thickness is greater than the second thickness, the first thickness and the second thickness are the total etching thickness of the first film, and the process parameters of the second etching are: the etching temperature is higher than 1050°C, the flow rate of the second carrier gas is 40slm~120slm, the volume fraction of the second etching gas is lower than 0.5%, and the volume fraction of the etching gas of the second etching is lower than the volume fraction of the etching gas of the first etching.
2. The method according to claim 1, characterized in that Step S3 includes: In a rapid thermal annealing device or an epitaxial device, hydrogen is used as a first carrier gas and a first etching gas is used to perform a first etching on the first film to remove the first film having a first thickness.
3. The method according to claim 1, characterized in that The first thickness accounts for no more than 70% of the total etched thickness.
4. The method according to claim 1, characterized in that Step S4 includes: In a rapid thermal annealing device or an epitaxial device, hydrogen is used as a second carrier gas and a second etching gas is used to etch the first film for a second time to planarize the first film and remove a second thickness of the first film.
5. The method according to claim 2 or 4, characterized in that The first etching gas and the second etching gas both include HCl gas.
6. The method according to any one of claims 1 to 4, characterized in that The method for forming the bonding structure comprises: providing a first substrate and a second substrate; growing a first oxide layer on the front side of the first substrate; Performing an ion implantation process from the front side of the first substrate into the first substrate to obtain a damaged layer; The front side of the first substrate and the front side of the second substrate are bonded to form a bonding structure.
7. The method according to claim 6, characterized in that When the thickness of the insulating buried layer is In the following case, the buried insulating layer includes a first oxide layer.
8. The method according to claim 6, characterized in that When the thickness of the insulating buried layer is greater than When the buried insulating layer includes a first oxide layer and a second oxide layer; and while growing a first oxide layer on the front side of the first substrate, A second oxide layer is formed on the front surface of the second substrate.
9. The method according to claim 8, characterized in that The thickness of the first oxide layer is The thickness of the second oxide layer is 10. The method according to claim 6, characterized in that Step S2 includes: Performing a first annealing treatment on the bonding structure, the bonding structure is peeled off along the damaged layer, and a first thin film located on the insulating buried layer is obtained, and the second substrate, the insulating buried layer and the first thin film constitute a silicon-on-insulator structure; performing a second annealing process on the silicon-on-insulator structure; The surface of the first film is cleaned.
11. The method according to claim 10, characterized in that The second annealing treatment is performed in an oxygen-containing atmosphere, and a silicon oxide film layer is grown on the surface of the first film; the cleaning is used to remove the silicon oxide film layer.
12. A silicon-on-insulator structure, characterized in that: Prepared by the method according to any one of claims 1 to 11.