A sintered NdFeB magnetic material and a preparation method thereof

By adding Cu, Al and other elements to the sintered NdFeB magnetic material and adopting a fast-condensing thin tape process, combining hydrogen crushing and airflow grinding to powder, the corrosion problem of magnetic material in high temperature environment is solved, and corrosion resistance is improved. Coercive force, and the reasonable use of rare earth elements and cerium reduces costs, achieving high-performance and low-cost magnetic material preparation.

CN112992459BActive Publication Date: 2024-11-29NINGBO SHENGYU MAGNETOELECTRIC TECH CO LTD
View PDF 2 Cites 0 Cited by

Patent Information

Application Number
CN202110264257.8
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2021-03-11
Publication Date
2024-11-29
Estimated Expiration
2041-03-11

Smart Images

  • Figure DEST_PATH_IMAGE002
    Figure DEST_PATH_IMAGE002
Patent Text Reader

Abstract

The present application relates to the field of magnetic materials, and specifically discloses a sintered NdFeB magnetic material and a preparation method thereof. A sintered NdFeB magnetic material includes PrNd30‑40wt%, B1.5‑1.8wt%, Ce15‑17wt%, Ga2.5‑3.5wt%, Zr0.1‑0.3wt%, La0.1‑0.3wt%, Cu0.1‑0.3wt%, Al0.1‑0.3wt%, Co0.9‑1.2wt%, and the rest is Fe and irremovable impurities; its preparation method is: each raw material is weighed in proportion and placed in a vacuum melting furnace for high-temperature smelting, and alloy flakes are quickly cast using cooling rollers, crushed to powder by hydrogen crushing and air flow grinding, and pressed under vacuum to obtain a pressed blank, and then subjected to high-temperature sintering and tempering treatment, and finally air-cooled. The sintered NdFeB magnetic material of the present application can be used for machines that are susceptible to corrosion in the wilderness, such as wind turbines, and has high corrosion resistance.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present application relates to the field of magnetic materials, and more specifically, to a sintered NdFeB magnetic material and a preparation method thereof. Background Art

[0002] NdFeB is composed of neodymium, iron, and boron (Nd2Fe 14 B) The tetragonal crystals formed, NdFeB can be divided into two types: sintered NdFeB and bonded NdFeB.

[0003] Sintered NdFeB permanent magnets have the advantages of high magnetic energy product, small size and light weight, and have been widely used in defense aviation, communications, electronics, medical and machinery. In recent years, due to the rapid development of my country's energy-saving and environmental protection industry, the output of rare earth permanent magnet motors used in wind power generation, new energy vehicles and variable frequency air conditioners has also increased rapidly, and the comprehensive performance requirements for sintered NdFeB are getting higher and higher. People not only have requirements for the magnetic properties of magnets, but also have higher requirements for the temperature stability and corrosion resistance of magnets.

[0004] Take wind turbines as an example. Since they work in the wilderness and are subjected to high temperature, severe cold, humidity and even salt spray, once corroded, the corrosion products produced on the surface of the magnets will not only reduce the magnetic properties of the magnets, but also affect the performance and safety of the wind turbines. Therefore, the magnets used in wind turbines are required to have not only magnetic properties that meet the requirements, but also have high corrosion resistance. Summary of the invention

[0005] In order to improve the corrosion resistance of sintered NdFeB magnetic materials, the present application provides a sintered NdFeB magnetic material and a preparation method thereof.

[0006] In the first aspect, the present application provides a sintered NdFeB magnetic material, which adopts the following technical solution:

[0007] A sintered NdFeB magnetic material, comprising 30-40wt% PrNd, 1.5-1.8wt% B, 15-17wt% Ce, 2.5-3.5wt% Ga, 0.1-0.3wt% Zr, 0.1-0.3wt% La, 0.1-0.3wt% Cu, 0.1-0.3wt% Al, 0.1-0.3wt% Co, and the remainder being Fe and impurities that cannot be removed.

[0008] By adopting the above technical solution, elements such as Cu and Al are added to form intermetallic compounds at the grain boundaries, forming Nd-Fe-Cu intergranular phases and Nd-Fe-Al intergranular phases, which replace the original boron-rich phases, prevent the growth of tetragonal phase grains, thereby refining the grains and improving the microstructure of the magnet, and increasing the coercive force. In addition, the formed intergranular phase will partially replace the neodymium-rich phase, reducing the potential difference between the phases of the magnet.

[0009] At the same time, its texture is relatively smooth and can surround the main phase, so that a large amount of stable intermetallic compounds can greatly improve the corrosion resistance and high temperature resistance of sintered NdFeB magnetic materials.

[0010] Cobalt forms an intermediate phase of Nd3Co in the neodymium-rich grain boundary phase. These grain boundary phases partially replace the grain boundary neodymium-rich phase, thereby reducing the activity of the grain boundary neodymium-rich phase and improving the corrosion resistance of the sintered NdFeB magnet.

[0011] In addition, Co will replace the position of Fe in the main phase, which can greatly inhibit the oxidation corrosion behavior of NdFeB magnetic materials above 200°C.

[0012] The content of rare earth elements in the raw materials accounts for a relatively high proportion. The increase of rare earth elements can increase the bending strength of NdFeB magnets and improve their mechanical properties.

[0013] In addition, the microstructure of NdFeB magnets is mainly composed of NdFeB phase, Nd-rich phase, B-rich phase, NdO, α-Fe phase and foreign dopants. Among them, NdFeB phase is polygonal, Nd-rich phase is distributed along grain boundaries or at grain boundary corners, and B-rich phase exists in isolated blocks or particles.

[0014] There are three distribution states of neodymium-rich phase, namely, blocky neodymium-rich phase, thin-layered neodymium-rich phase and dispersed neodymium-rich phase that can only be observed in individual grains. Blocky neodymium-rich phase is embedded on the grain boundary of NdFeB; thin-layered neodymium-rich phase is continuously distributed on the grain boundary and grain corners with different thicknesses; the number of dispersed neodymium-rich phase is very small and distributed inside the NdFeB grains.

[0015] The neodymium-rich phase can promote the sintering of the neodymium iron boron magnet and play a role in assisting sintering. The neodymium-rich phase begins to melt at about 650°C, laying a good foundation for the densification of the neodymium iron boron magnet and can promote the densification of the neodymium iron boron magnet. At the same time, the thin layer of neodymium-rich phase continuously distributed along the grain boundary can play the role of exchange coupling, which is beneficial to improve the coercive force of the neodymium iron boron magnet, and will not occupy the volume fraction of the neodymium iron boron phase, and has almost no effect on the magnetic energy product.

[0016] The boron-rich phase mostly exists in the form of polygonal particles at the corners of the grain boundaries or on the NdFeB grain boundaries, and fine granular boron-rich phase is precipitated inside individual NdFeB grains.

[0017] Sintered NdFeB magnets are prone to oxidation, i.e. chemical corrosion. The oxidation abilities of NdFeB phase, Nd-rich phase and Boron-rich phase are different. Boron-rich phase and Nd-rich phase have stronger oxidation abilities, and Nd-rich phase and Boron-rich phase are generally distributed at grain boundaries. Therefore, the oxidation of NdFeB magnets generally starts from grain boundaries, forming grain boundary corrosion.

[0018] When the microstructure of the NdFeB magnet has fine and uniform NdFeB phase grains, and the Nd-rich phase is less distributed on the main phase grain boundaries and is mainly concentrated at the triangular grain boundaries, it can effectively inhibit the intergranular corrosion of the Nd-rich phase of the magnet and improve the corrosion resistance of the magnet.

[0019] As the rare earth content increases, the corrosion rate of sintered NdFeB magnets increases. Therefore, the chemical properties, distribution state and content of the Nd-rich phase are key factors affecting the corrosion resistance of NdFeB. When the Nd-rich phase of the magnet is distributed in a network-like manner on the grain boundaries of the main phase, the sintered NdFeB magnet is prone to selective intergranular corrosion, thereby reducing the corrosion resistance of the sintered NdFeB magnet.

[0020] Preferably, the amount of cerium used is 16 wt %.

[0021] By adopting the above technical solution, the added cerium can replace part of the praseodymium-neodymium, and because the price of cerium is significantly lower than that of neodymium, while ensuring the high performance of the magnet, the use of cerium to replace part of the neodymium is beneficial to promote the comprehensive utilization of rare earth resources, thereby reducing the production cost of sintered NdFeB magnets.

[0022] However, the amount of cerium added should not be too much. When the amount of cerium is 16wt% of the total amount of NdFeB magnets, the magnet coercive force and magnetic energy product of NdFeB magnets are not significantly reduced. When the amount of cerium added exceeds 17wt%, excessive cerium will increase the proportion of cerium phase in the rare earth-rich phase, and cerium will be oxidized to form cerium oxide during the firing process. During the firing process, the rare earth-rich phase and part of the cerium oxide fall off, which will cause a large number of irregular holes to appear in the sintered NdFeB magnets, resulting in a decrease in the density of the sintered NdFeB magnets.

[0023] When NdFeB magnets are placed in a warm and humid environment, the Nd-rich phase on the surface of the magnets first reacts with water molecules to generate hydrogen. After the reaction, the hydrogen atoms generated by the decomposition of water penetrate into the grain boundaries of the magnets and further react with the Nd-rich phase to generate NdH3, which causes intergranular corrosion of the magnets. The generation of NdH3 causes the volume of the grain boundaries to expand, generates stress at the grain boundaries, and destroys the grain boundaries. If the damage is severe, the grain boundaries will rupture, causing the magnets to pulverize, resulting in reduced magnetic properties.

[0024] In a second aspect, the present application provides a method for preparing a sintered NdFeB magnetic material, using the following technical solution:

[0025] A method for preparing a sintered NdFeB magnetic material comprises the following steps:

[0026] S1. Weigh the raw materials according to the components of the final product, put them into a vacuum melting furnace for high-temperature melting, and use cooling rollers to quickly cast them into alloy sheets;

[0027] S2, hydrogen crushing the alloy flakes in S1 into coarse particles;

[0028] S3, using a jet mill to grind the coarse particles in S2 into powder to obtain NdFeB alloy powder;

[0029] S4, under vacuum conditions, pressing the NdFeB alloy powder into a compact to obtain a green compact;

[0030] S5, sintering the compact obtained in S4 at high temperature;

[0031] S6. Temper the product sintered at high temperature in S5, and air cool it to obtain sintered NdFeB magnetic material.

[0032] By adopting the above technical solution, the sintered NdFeB magnetic material prepared by the rapid solidification thin strip process can improve the coercive force and corrosion resistance compared with the traditional ingot casting process.

[0033] When magnets are prepared by the traditional ingot casting process, the main phase grains of the prepared magnets are coarse, and the distribution of the neodymium-rich phase is relatively concentrated, not evenly distributed around the main phase, and is accompanied by segregation of the α-Fe phase, and its composition and organizational structure are uneven.

[0034] The rapid solidification thin strip process can improve the defects of the traditional ingot casting process, so that the columnar crystals of the main phase of the prepared magnet grow well and are small in size, the neodymium-rich phase is very thin and evenly distributed around the main phase columnar crystals, and there is no segregation of the α-Fe phase, making the grain structure of the magnet fine and uniform.

[0035] Hydrogen crushing is a very effective process for producing coarse crushed powder from rare earth permanent magnet materials. This process uses the characteristics of rare earth permanent magnet alloys that absorb and release hydrogen, and in this process, the alloy itself undergoes grain boundary fracture and transgranular fracture to pulverize, thereby obtaining alloy powder of a certain particle size.

[0036] Since the oxidation in the powder making process is relatively serious, in order to reduce the degree of oxidation of the magnetic powder, the alloy powder obtained by hydrogen crushing is generally further crushed by air flow milling to crush the hydride.

[0037] The method of hydrogen crushing and air flow grinding can solve the problem of mechanical crushing of alloys, especially when α-Fe exists in the alloy ingot.

[0038] When the compacts that have been crushed by hydrogen and ground by air flow are sintered in a vacuum furnace, the hydrogen in the furnace reduces the oxidation of the charge. The compacts that have been crushed by hydrogen and ground by air flow can reduce the sintering temperature and avoid grain growth.

[0039] Preferably, in S2, the size of the coarse particles is 0.25-0.3 mm.

[0040] By adopting the above technical solution, coarse particles below 0.325 mm can directly enter the air flow mill, which simplifies the process and greatly reduces the cost of mechanical coarse crushing.

[0041] Preferably, in S3, the particle size of the NdFeB alloy powder is 3-4 μm.

[0042] By adopting the above technical solution, NdFeB alloy powder with a size of 3-4 μm can be directly used to manufacture sintered NdFeB magnetic materials, which simplifies the process and reduces the production cost.

[0043] Preferably, in S4, the NdFeB alloy powder is vertically oriented and pressed in a nitrogen atmosphere at a magnetic field of 3-5T, a pressure of 40-60Mpa, and then secondary pressed by cold isostatic pressing in a magnetic field of 180-220MPa.

[0044] By adopting the above technical solution, the vertical orientation method is conducive to obtaining a higher orientation factor. At the same time, the above pressing method has the advantages of low power consumption, high efficiency, convenient operation and reliability.

[0045] Preferably, in S3, an antioxidant TH-412S is added to the NdFeB alloy powder.

[0046] By adopting the above technical solution, in the preparation process of NdFeB magnets, a small amount of oxygen will enter the sintered NdFeB in each process, and the oxygen will react with rare earth elements and more active metals to generate corresponding oxides, thereby reducing the magnetic properties of the sintered NdFeB magnets. The addition of antioxidants can reduce the oxygen content in the NdFeB alloy powder.

[0047] Preferably, in S5, the sintering temperature of the high temperature sintering is 1000-1050° C., and the sintering time is 2-3 hours.

[0048] By adopting the above technical solution, the sintering temperature of 1000-1050°C can fully remove the organic matter in the compact, the gas adsorbed on the surface of the particles and the gas retained in the pores.

[0049] Too high sintering temperature will reduce the magnetic properties of sintered NdFeB magnets. As the sintering temperature increases, the liquid phase increases, more small particles dissolve and precipitate in the liquid phase, and more particles precipitate on the surface of large particles, resulting in abnormal grain growth. When the temperature is too high, the driving force for grain growth is large.

[0050] Too long sintering time will reduce the magnetic properties of sintered NdFeB magnets. As the sintering time increases, the duration of solid phase sintering increases, the diffusion between grains increases, and the interface between grains gradually disappears, resulting in the phenomenon that several grains grow into one grain.

[0051] Preferably, in S6, the tempering treatment includes firstly performing primary tempering at 880-920° C. and maintaining for 2-4 hours, and then performing secondary tempering at 520-560° C. and maintaining for 2-4 hours.

[0052] By adopting the above technical solution, the secondary annealing method can make the grain boundaries become obvious and clear, better separate the main phase grains, and greatly improve the intrinsic coercive force.

[0053] Because the neodymium-rich phase has serious agglomeration phenomenon before tempering, after the secondary tempering, the neodymium-rich phase is evenly distributed around the grain boundaries of the main phase, and a thin layer of grain boundary phase is precipitated, which reduces its agglomeration phenomenon on the grain boundaries and at the intersection of grain boundaries.

[0054] Therefore, the secondary tempering can better isolate the main phase grains and remove the exchange coupling between the grains, which is beneficial to the improvement of coercivity. Moreover, after the secondary tempering treatment, the grain boundaries of the main phase are very regular, making it difficult for the antimagnetic domain to form.

[0055] Preferably, the sintered NdFeB magnetic material after air cooling in S6 is subjected to phosphating treatment.

[0056] By adopting the above technical scheme, the method of adding rare earth elements into the raw materials can essentially improve the corrosion resistance of sintered NdFeB magnets. On this basis, coating the surface of the sintered NdFeB magnets for protection can further improve the corrosion resistance of the sintered NdFeB magnets.

[0057] Phosphating sintered NdFeB magnets is a way to form a protective layer on the surface of the magnet to prevent air, moisture or other corrosive substances from entering the magnet surface, thereby improving the magnet's corrosion resistance.

[0058] The phosphating process is simple and does not require equipment investment. The phosphating production process consumes little, mainly acid, alkali and phosphating solution, and has low production costs. As a process corrosion protection, it will not significantly increase the production cost of the magnet, and can avoid the loss of magnets during storage, with a high rate of return.

[0059] After phosphating, the product has uniform color and clean surface, and can be vacuum packaged to greatly extend the storage time. The storage method is better than the previous oil immersion and oil coating storage methods. The complete phosphating film can resist oxidation corrosion in the normal atmospheric environment.

[0060] In summary, this application has the following beneficial effects:

[0061] 1. Since the present application adopts the method of adding elements such as Cu and Al to the raw materials, intermetallic chemicals are formed at the grain boundaries, thereby improving the corrosion resistance of the sintered NdFeB magnetic material.

[0062] 2. In this application, the preferred amount of cerium is 16wt%, which is beneficial to promote the comprehensive utilization of rare earth resources while ensuring the high performance of the magnet, thereby reducing the production cost of sintered NdFeB magnets.

[0063] 3. The method of the present application improves the defects of the traditional ingot casting process by adopting the rapid solidification thin strip process, so that the grain structure of the sintered NdFeB magnet is fine and uniform.

[0064] 4. The method of the present application solves the problem of difficulty in mechanically crushing alloys by adopting hydrogen crushing and air flow grinding to make powder. DETAILED DESCRIPTION

[0065] The present application is further described in detail below in conjunction with embodiments.

[0066] The alkaline degreasing agent in this application is selected from Jinan Beiyate Chemical Technology Co., Ltd.

[0067] Example 1

[0068] A method for preparing a sintered NdFeB magnetic material comprises the following steps:

[0069] S1, weighing each raw material in proportion, putting them into a vacuum melting furnace for high-temperature melting, and using a cooling roller to quickly cast them into alloy flakes to obtain alloy flakes;

[0070] S2, hydrogen crushing the alloy flakes in S1 into coarse particles of 0.25 mm;

[0071] S3, using a jet mill to grind the coarse particles in S2 into powder to obtain 3 μm NdFeB alloy powder;

[0072] S4, vertically orienting the NdFeB alloy powder prepared in S3 in a magnetic field of 4T, a pressure of 50 MPa, and a nitrogen atmosphere, and then performing secondary pressing by cold isostatic pressing in a magnetic field of 220 MPa to obtain a compact;

[0073] S5, sintering the compact obtained in S4 at a high temperature, wherein the sintering temperature is 1020° C. and the sintering time is 2 h;

[0074] S6. The product after high temperature sintering in S5 is subjected to secondary tempering, including primary tempering at 900°C and maintaining for 3 hours, secondary tempering at 540°C and maintaining for 3 hours, and then air cooling to obtain sintered NdFeB magnetic material, and finally phosphating.

[0075] Here, in the sintered NdFeB magnetic material, the components are calculated by mass percentage as follows: PrNd 35wt%, B 1.7wt%, Ce 16wt%, Ga 3.0wt%, Zr 0.1wt%, La 0.2wt%, Cu 0.3wt%, Al 0.2wt%, Co 1.1wt%, and the rest are Fe and unremovable impurities.

[0076] Phosphating treatment includes the following steps:

[0077] A1. Degrease the sintered NdFeB magnets using an alkaline degreasing agent at 60°C for 4 minutes.

[0078] A2. Wash the degreased sintered NdFeB magnetic material with water;

[0079] A3. Put the washed sintered NdFeB magnet into the phosphating solution and let it stand for 4 minutes;

[0080] A4. Wash again and finally dry.

[0081] Basic formula and process parameters of phosphating solution: 50g / L sodium dihydrogen phosphate, 12ml / L phosphoric acid, 0.6g / L sodium molybdate, room temperature, time 4min.

[0082] Embodiment 2-5

[0083] The preparation method of sintered NdFeB magnetic material in Example 2-5 is the same as that in Example 1, except that as shown in Table 1-2:

[0084] Table 1 Raw material composition and dosage of sintered NdFeB magnetic materials in Examples 1-5

[0085] Weight percentage / wt% Example 1 Example 2 Example 3 Example 4 Example 5 PcqI 35 30 40 35 38 B 1.7 1.8 1.5 1.6 1.7 Ce 16 17 16 15 16 Ga 3 2.5 3.0 3.5 3.0 Zr 0.1 0.3 0.2 0.1 0.3 La 0.2 0.2 0.1 0.3 0.2 Cu 0.3 0.3 0.1 0.2 0.2 Al 0.2 0.1 0.2 0.3 0.2 Co 1.1 0.9 1.1 1.2 1.0 Fe and irremovable impurities 42.4 46.9 37.8 42.8 39.4

[0086] Table 2 Parameters of sintered NdFeB magnetic materials in Examples 1-5

[0087]

[0088] Example 6

[0089] The preparation method of the sintered NdFeB magnetic material of Example 6 is the same as that of Example 1, except that the vertical orientation molding in S4 is replaced by horizontal orientation molding.

[0090] Comparative Example 1

[0091] The preparation methods of the sintered NdFeB magnetic materials in Comparative Example 1 are consistent with those in Example 1, except that no antioxidant is added to S3.

[0092] Comparative Example 2

[0093] The preparation method of the sintered NdFeB magnetic material in Comparative Example 2 is consistent with that in Example 1, except that the sintered NdFeB magnetic material after air cooling in S6 is not subjected to phosphating treatment.

[0094] Comparative Example 3

[0095] The preparation method of the sintered NdFeB magnetic material in Comparative Example 3 is consistent with that in Example 1, except that the amount of cerium in the raw material is 4 wt %.

[0096] Comparative Example 4

[0097] The preparation method of the sintered NdFeB magnetic material in Comparative Example 4 is consistent with that in Example 1, except that the amount of cerium in the raw material is 8 wt %.

[0098] Comparative Example 5

[0099] The preparation method of the sintered NdFeB magnetic material in Comparative Example 5 is consistent with that in Example 1, except that Al and Cu are not added to the raw materials.

[0100] Comparative Example 6

[0101] The preparation method of the sintered NdFeB magnetic material in Comparative Example 6 is consistent with that in Example 1, except that the sintering temperature in S5 is 1100° C. and the sintering time is 4 h.

[0102] Performance testing

[0103] Neutral salt spray test (NSS) was used to conduct corrosion test on sintered NdFeB magnets.

[0104] Detection method / test method

[0105] Coercivity: The coercivity of sintered NdFeB magnets is tested using the high-precision MicroSense from the United States.

[0106] Oxygen content: Use IRO-Ⅱ infrared oxygen analyzer to quantitatively analyze the oxygen content in the magnet.

[0107] Table 3 Test results of Examples 1-6

[0108] Test items Example 1 Example 2 Example 3 Example 4 Example 5 Example 6 Coercivity (KOe) 15.46 15.59 15.17 15.53 15.32 14.91 Oxygen content (ppm) 513.2 523.1 532.4 519.3 532.8 536.3 Weight loss rate after 48h corrosion time (wt%) 0.036 0.031 0.032 0.034 0.035 0.034 Weight loss rate after 96h corrosion time (wt%) 0.421 0.351 0.395 0.432 0.389 0.341 Weight loss rate after 144h corrosion time (wt%) 0.865 0.735 0.894 0.866 0.781 0.746

[0109] Table 4 Test results of comparative examples 1-6

[0110] Test items Comparative Example 1 Comparative Example 2 Comparative Example 3 Comparative Example 4 Comparative Example 5 Comparative Example 6 Coercivity (KOe) 14.52 14.26 14.77 13.36 13.16 12.83 Oxygen content (ppm) 1213.5 1325.6 635.6 511.6 1438.5 892.3 Weight loss rate after 48h corrosion time (wt%) 0.057 0.068 0.052 0.063 0.079 0.075 Weight loss rate after 96h corrosion time (wt%) 0.412 0.685 0.431 0.721 0.762 0.689 Weight loss rate after 144h corrosion time (wt%) 0.762 1.356 0.721 1.627 1.657 1.539

[0111] Combining Examples 1-5 and Comparative Examples 3-4 and Table 3-4, it can be seen that as the cerium content increases, the oxygen content of the sintered NdFeB magnetic material can be reduced, thereby improving the corrosion resistance of the sintered NdFeB magnetic material. When the cerium content is 16wt%, the corrosion resistance of the sintered NdFeB magnetic material is the best. When the cerium content exceeds 17wt%, the corrosion resistance decreases.

[0112] It can be seen from Example 1 and Example 6 and Table 3 that the magnetic properties of the sintered NdFeB magnets produced by vertical orientation molding are better than those of the sintered NdFeB magnets produced by horizontal orientation molding.

[0113] Combining Example 1 and Comparative Example 1 with Tables 3-4, it can be seen that adding an antioxidant can reduce the oxygen content of the sintered NdFeB magnetic material, thereby improving the corrosion resistance of the sintered NdFeB magnetic material. The lower the oxygen content, the better the corrosion resistance of the sintered NdFeB magnetic material.

[0114] If the oxygen content in the magnet is very high, the rare earth oxides formed during the sintering and aging process will exist in the grain boundaries in the form of solid particles, thereby reducing the wetting effect of the neodymium-rich phase on the main phase grains, making it easy for the neodymium-rich phase to be enriched in the corners of the grain boundaries, and increasing the oxygen content in the local area of ​​the sintered NdFeB magnet. This will cause the surface corrosion of the sintered NdFeB magnet to expand to the inside of the magnet, causing the main phase grains to fall off, increasing the weight loss rate, and reducing the corrosion resistance of the sintered NdFeB magnet.

[0115] It can be seen from Example 1 and Comparative Example 2 and Tables 3-4 that the corrosion resistance of the sintered NdFeB magnetic material that has been phosphated is better than that of the sintered NdFeB magnetic material that has not been phosphated.

[0116] Combining Example 1 and Comparative Example 5 with Tables 3-4, it can be seen that the magnetic properties of the sintered NdFeB magnetic material obtained without adding Al and Cu to the raw materials are significantly reduced. At the same time, the corrosion resistance of the sintered NdFeB magnetic material is also significantly reduced.

[0117] It can be seen from Example 1 and Comparative Example 6 and Tables 3-4 that if the sintering temperature is too high and the sintering time is too long, the magnetic properties of the sintered NdFeB magnetic material will be reduced and its corrosion resistance will be affected.

[0118] This specific embodiment is merely an explanation of the present application and is not a limitation of the present application. After reading this specification, those skilled in the art may make modifications to the present embodiment without any creative contribution as needed, but such modifications are protected by the patent law as long as they are within the scope of the claims of the present application.

Claims

1. A sintered NdFeB magnetic material, characterized in that: Calculated by mass percentage, it includes the following components: PrNd 35wt%, B 1.7wt%, Ce 16wt%, Ga 3.0wt%, Zr 0.1wt%, La 0.2wt%, Cu 0.3wt%, Al0.2wt%, Co 1.1wt%, the rest is Fe and unremovable impurities; The preparation method of the sintered NdFeB magnetic material comprises the following preparation steps: S1. Weigh the raw materials according to the components of the final product, put them into a vacuum melting furnace for high-temperature melting, and use cooling rollers to quickly cast them into alloy sheets; S2, hydrogen crushing the alloy flakes in S1 into coarse particles; S3, using a jet mill to grind the coarse particles in S2 into powder to obtain NdFeB alloy powder, and adding an antioxidant TH-412S to the NdFeB alloy powder; S4, under vacuum conditions, pressing the NdFeB alloy powder into a compact to obtain a green compact; S5, sintering the compact obtained in S4 at high temperature, wherein the sintering temperature is 1000-1050° C. and the sintering time is 2-3 hours; S6. Temper the product sintered at high temperature in S5, air cool it to obtain sintered NdFeB magnets, and phosphate the sintered NdFeB magnets after air cooling.

2. The method for preparing a sintered NdFeB magnetic material according to claim 1, characterized in that: In S2, the size of the coarse particles is 0.25-0.3 mm.

3. The method for preparing a sintered NdFeB magnetic material according to claim 1, characterized in that: In S3, the particle size of the NdFeB alloy powder is 3-4 μm.

4. The method for preparing a sintered NdFeB magnetic material according to claim 1, characterized in that: In S4, the NdFeB alloy powder is vertically oriented and pressed in a nitrogen atmosphere at a magnetic field of 3-5T, a pressure of 40-60Mpa, and then cold isostatically pressed in a magnetic field of 180-220MPa for a secondary pressing.

5. The method for preparing a sintered NdFeB magnetic material according to claim 1, characterized in that: In S6, the tempering treatment includes firstly performing a primary tempering at 880-920°C and maintaining it for 2-4 hours, and then performing a secondary tempering at 520-560°C and maintaining it for 2-4 hours.

Citation Information

Patent Citations

  • Lanthanide-compounded NdFeB magnetic material and preparation method thereof

    CN104347216A

  • Low-cost N35 NdFeB magnet with high cerium content and sintering method thereof

    CN107610858A