A shingled battery structure and preparation method
By using a dotted main gate structure of fine secondary gates and low-temperature silver paste in the stacked tiling assembly, combined with colloidal adhesion, the high linear loss and high cost problems in the battery cell connection are solved, and the electrical connection quality and reliability of the components are improved , reducing the amount and cost of silver.
Patent Information
- Application Number
- CN202111408679.4
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2021-11-24
- Publication Date
- 2024-11-22
- Estimated Expiration
- 2041-11-24
AI Technical Summary
The existing stacked tiles have problems of high wire loss and high cost in battery cell connections, and it is difficult to control the amount of conductive adhesive, which can easily lead to insufficient adhesion or risk of glue spills, affecting the reliability and authenticity of the components.
A fine sub-grid is printed on the cell and cut into a battery cell. Low-temperature silver paste is used instead of conductive glue, and ohmic contact is formed through the dotted main gate and colloid to achieve electrical connection, and adhesion is enhanced through two overlapping printing.
The electrical connection quality of the stacked tiles is improved, the amount and cost of silver is reduced, the authenticity and reliability of the components are enhanced, and the risks of heat spots and poor adhesions are reduced.
Smart Images

Figure CN114122164B_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of solar photovoltaics, and in particular relates to a shingled cell structure and a preparation method thereof. Background Art
[0002] At present, with the continuous development of the photovoltaic industry, the battery conversion efficiency and the power of the module are constantly improving. In response to the development of the market, the shingled module version came into being, and its higher power density is welcomed by the market. The shingled module is a module formed by cutting the battery sheet (mother sheet) into battery cells of preset size according to a certain method, and then rearranging the battery cells in series and parallel. The shingled module does not use welding ribbons to stack the battery cells in the limited space of the module, which not only reduces the line loss of the module but also increases the power of the module.
[0003] With the development of shingled modules, on the one hand, the pursuit of higher module power is pursued, and on the other hand, the cost of modules is reduced.
[0004] Reference Figure 1 and Figure 2 After cutting, each battery cell has a thicker main grid and several thin sub-grids on the front (N side) and back (P side). The sub-grids are used to collect the current generated by the battery under the photovoltaic effect and converge it to the main grid. In the production process of shingled modules, the main grids at the edges of two battery cells, the front (N side) of a battery cell and the back (P side) of a battery cell overlap each other and are bonded with conductive glue. The area from the main grid to the edge of the battery cell will be overlapped and covered and will no longer play a role. Generally, the width of the main grid itself is 0.5mm, and the minimum distance from the edge of the main grid to the edge of the battery cell is 0.5mm. In this way, the overlap is minimum 1.5mm in total (one main grid + two main grid edges to the edge of the battery).
[0005] Currently, conductive glue is used to bond two battery cells. Conductive glue uses organic matter in the glue to bond the metal main grids on the two battery cells, and uses the metal (usually silver) in the conductive glue to reduce the resistance of the organic matter and improve the conductivity. Finally, the two battery cells form an electrical connection. This bonding method still has high line loss, which becomes an obstacle to the increase of component power. In order to ensure the quality of the bonding of the two battery cells and achieve good adhesion, the conductive glue is printed, and the bonding surface width generally exceeds the main grid width, that is, more than 0.5mm, so the cost of the conductive glue will be at a higher cost ratio.
[0006] In the existing manufacturing process, in order to improve the utilization rate of batteries, the overlap of two overlapping battery cells is gradually decreasing, and the difficulty of controlling the amount of conductive glue used to connect the two battery cells is also increasing. If the amount of conductive glue used is too small, there will be areas between the batteries where there is no conductive glue to adhere to each other, and the adhesion between the battery cells will decrease, resulting in poor reliability of the assembly; if the amount of conductive glue used is too large, not only will the cost increase significantly, but there will also be a risk of glue overflow during the bonding process. The conductive glue overflows from the edge of the battery cell and contacts the other side of the battery cell, forming the battery cell itself conductive, causing leakage, and the shingled assembly will also have the risk of hot spots, thereby reducing the reliability and authenticity of the shingled assembly. Summary of the invention
[0007] The present invention provides a shingled battery structure and a preparation method, which improves the electrical connection of components while reducing the amount of silver used and the cost.
[0008] To achieve the above object, a method for preparing a shingled battery according to the present invention comprises the following steps:
[0009] Step 1: Printing and sintering multiple groups of front and back auxiliary grids of battery cells on the front and back of the battery cell, respectively. The auxiliary grid of each battery cell includes two mutually parallel longitudinal auxiliary grids and multiple mutually parallel transverse auxiliary grids, and the two ends of the transverse auxiliary grid are respectively connected to the two longitudinal auxiliary grids;
[0010] Step 2: Cut the battery cell into multiple battery units along a cutting line parallel to the longitudinal auxiliary grid;
[0011] Step 3, printing a main grid arranged in dotted lines on the secondary grid at the main grid position on the battery unit, wherein the width of the main grid is less than 0.5 mm;
[0012] Step 4: Print colloid on both sides of the main grid;
[0013] Step 5: Overlap multiple battery cells and then cure them on a curing table. During this process, the low-temperature silver paste used to print the main grid passes through the front passivation layer and the base silicon to form an ohmic contact to achieve electrical connection; the colloid bonds adjacent battery cells together.
[0014] Furthermore, in step 1, the width of the secondary gate is 30 μm-50 μm.
[0015] Furthermore, in step 1, the front sub-grid is printed with high-temperature silver paste, and the back sub-grid is printed with aluminum paste.
[0016] Furthermore, in step 3, the main grid is printed using low-temperature silver paste.
[0017] Furthermore, in step 3, the virtual-to-real ratio of the main grid is 1:2.
[0018] Furthermore, in step 4, the screen used for printing the colloid does not contact the lower main grid.
[0019] Further, in step 4, the colloid is printed using a screen and a scraper;
[0020] The screen is provided with a plurality of hollow areas for accommodating the low-temperature silver glue in the main grid area, a bracket is arranged outside the hollow area, and an ink-permeable strip is arranged on both sides of the hollow area for ink-permeable printing of the glue;
[0021] The scraper includes a mounting plate and a plurality of blades, which are fixed on the mounting plate in sequence and at intervals. When the scraper is working, the blades are inserted between two adjacent hollow area frames to squeeze the colloid on the screen into the ink-permeable strips so that it is printed on the battery cell.
[0022] A shingled battery structure comprises a plurality of overlapping battery cells, wherein the battery cells comprise a back passivation layer, a P-type substrate, an N-type diffusion layer and a front passivation layer arranged in sequence from bottom to top, wherein two longitudinal sub-grids and a plurality of mutually parallel transverse sub-grids are printed on the front passivation layer, and two longitudinal sub-grids are connected to two ends of the transverse sub-grids respectively; a back sub-grid is printed on the back passivation layer; the back sub-grid of the first battery cell is butted against the front sub-grid at the main grid position of the second battery cell, the back sub-grid of the second battery cell is butted against the front sub-grid at the main grid position of the third battery cell, and so on, and the contact points of two adjacent battery cells are fixedly connected by colloid.
[0023] Compared with the prior art, the present invention has at least the following beneficial technical effects:
[0024] The method described in the present invention is that the main grids on both sides of the battery cell are no longer printed during the battery manufacturing stage, and only the secondary grids are printed to form current collection, and the battery cells are cut into battery cells. When the battery cells of the shingled assembly are pasted, low-temperature silver paste is used to replace the conductive glue, and the virtual and real low-temperature silver pastes are printed at the original battery cell main grid position, that is, the position where the secondary grid is printed. After the two battery cells overlap and solidify, the low-temperature silver paste passes through the passivation layer such as silicon nitride on the surface of the battery cell, and forms an ohmic contact with another battery substrate, and at the same time, a good electrical connection is formed between the two battery cells. Through this method, the authenticity rate of the shingled assembly is improved, the risk of hot spots and weak adhesion is reduced, and the electrical connection of the assembly can be improved, the amount of silver used can be reduced, and the cost can be reduced.
[0025] Furthermore, the original overlapping printing of the shingled component is changed to two overlapping printings. The main grid of the overlapping shingled battery is a dotted line for the first time, and the ratio of dot to real is 1:2, which saves silver paste. The second printing is to print the colloid again on both sides of the low-temperature silver paste to enhance the adhesion of the battery cell. The two overlapping battery cells form ohmic contact and good electrical connection.
[0026] Furthermore, a colloid with strong adhesion is printed on both sides of the low-temperature silver paste. After the colloid with strong adhesion is cured, the adhesion of the colloid after curing is greater than the adhesion requirement between the batteries, and the adhesion between the two battery cells is greater, thereby enhancing the adhesion of the two battery cells.
[0027] The shingled battery structure described in the present invention replaces the original solid main grid with a combination of a dotted main grid and a thin auxiliary grid, and the battery cells of the shingled module are well electrically connected through low-temperature silver paste. This not only improves the quality rate of the shingled module, reduces the risk of hot spots and weak adhesion, but also improves the electrical connection of the module and reduces the amount of silver used, thereby reducing costs. BRIEF DESCRIPTION OF THE DRAWINGS
[0028] Figure 1 Schematic diagram of a battery cell;
[0029] Figure 2 is a schematic diagram of a battery unit;
[0030] Figure 3 A schematic diagram of the overlap width of battery cells in the existing process;
[0031] Figure 4 This is a schematic diagram of printing the secondary grid of the battery cell;
[0032] Figure 5 The cross-sectional structure diagram of the secondary grid printed at the main grid position on the front of the battery;
[0033] Figure 6 The battery cell after dicing and cutting of the present invention;
[0034] Figure 7 The battery cell after printing the main grid;
[0035] Figure 8 It is a top view schematic diagram of the printing screen of five battery units;
[0036] Fig. 9 A schematic diagram of the front side of the five-cell printing screen with the front hollowed-out border hidden;
[0037] Fig.10 This is a schematic diagram of the front side of the five-cell printing screen;
[0038] Fig.11 This is a schematic diagram of the front of the scraper;
[0039] Fig.12 It is a schematic diagram of the combination of the scraper and the screen;
[0040] Fig.13 Schematic diagram of battery cell adhesion.
[0041] In the attached figure: 1. battery cell, 2. battery unit, 3. main grid, 4. front sub-grid, 5. back passivation layer, 6. substrate, 7. N-type diffusion layer, 8. front passivation layer, 9. back sub-grid, 10. back sub-grid, 11. mesh area, 12. screen frame, 14. hollow area, 15. ink holes, 16. hollow area frame, 17. scraper, 18. low-temperature silver paste, 19. colloid, 20. mounting plate, 21. blade. DETAILED DESCRIPTION
[0042] In order to make the purpose and technical solution of the present invention clearer and easier to understand, the present invention is further described in detail below in conjunction with the accompanying drawings and embodiments. The specific embodiments described herein are only used to explain the present invention and are not used to limit the present invention.
[0043] In the description of the present invention, it should be understood that the terms "center", "longitudinal", "lateral", "up", "down", "front", "back", "left", "right", "vertical", "horizontal", "top", "bottom", "inside", "outside" and the like indicate positions or positional relationships based on the positions or positional relationships shown in the accompanying drawings, and are only for the convenience of describing the present invention and simplifying the description, rather than indicating or implying that the device or element referred to must have a specific orientation, be constructed and operated in a specific orientation, and therefore cannot be understood as limiting the present invention. In addition, the terms "first" and "second" are used only for descriptive purposes, and cannot be understood as indicating or implying relative importance or implicitly indicating the number of technical features indicated. Thus, the features defined as "first" and "second" may explicitly or implicitly include one or more of the features. In the description of the present invention, unless otherwise specified, "multiple" means two or more. In the description of the present invention, it should be noted that, unless otherwise clearly specified and limited, the terms "installed", "connected", and "connected" should be understood in a broad sense, for example, it can be a fixed connection, a detachable connection, or an integral connection; it can be a mechanical connection or an electrical connection; it can be a direct connection, or it can be indirectly connected through an intermediate medium, or it can be the internal communication of two components. For ordinary technicians in this field, the specific meanings of the above terms in the present invention can be understood according to specific circumstances.
[0044] Reference Figure 3In the manufacturing process of existing battery cells (mother cells), a P-type silicon wafer is used as a substrate, and an N-type diffusion layer 7 with a thickness of 200 to 400 nm is formed on the substrate by diffusing phosphorus to form a PN junction. In addition, a front passivation layer 8 with a thickness of 60 to 100 nm, such as silicon nitride or silicon oxide, is plated on the substrate forming the PN junction. Finally, a high-temperature silver paste is printed on the front (N-side) passivation layer 8 by screen printing. At a high temperature of 500°C to 800°C, the high-temperature silver paste passes through the front passivation layer 8 and forms an ohmic contact with the N-type diffusion layer 7.
[0045] Under the existing process, the minimum distance between the main grid 3 at the edge of the battery cell and the edge is 0.5 mm, the width of the main grid 3 is generally 0.5 mm, and the minimum width of the battery cell covered after overlapping is 1.5 mm.
[0046] Example 1
[0047] The invention provides a method for preparing a shingled battery, comprising the following steps:
[0048] Step 1: Print the secondary grid 4 on the cell 1. The cell 1 no longer prints the 0.5 mm main grid 3 according to the existing process plan, but prints the 30 μm wide secondary grid. In the existing secondary grid printing process, directly follow Figure 4 The pattern is printed and sintered, and two parallel longitudinal sub-grids and multiple parallel transverse sub-grids are printed on each battery cell 2. The two ends of the transverse sub-grids are respectively connected to two longitudinal sub-grids, so that the battery cell 2 after cutting and dicing can also form current collection. The sub-grid 4 on the front side of the battery cell 1 (N side) is formed by printing high-temperature silver paste, and the sub-grid 9 on the back side (P side) is formed by printing aluminum paste. The sintering temperature of the high-temperature silver paste is 500-800℃.
[0049] The schematic diagram of the cross section of the battery after printing the auxiliary grid is as follows Figure 5 As shown, the main grid area is left with a width of 0.5 mm, a secondary grid of about 30 μm is printed, and the distance D between the edge of the main grid area and the edge of the battery is 0.5 mm.
[0050] Step 2: Reference Figure 6 , cutting the battery sheet 1 into a plurality of battery cells 2 along a cutting line parallel to the longitudinal auxiliary grid; the cutting line does not pass through any transverse auxiliary grid;
[0051] Step 3, print low-temperature silver paste at the main grid position on the battery cell 2 to obtain the main grid. The general working temperature of low-temperature silver paste is 120-200°C. For example, Shanren AS9100, the battery cell 2 can be printed simultaneously as a group of multiple battery units. In this embodiment, a group of 5 pieces is taken as an example. After 5 battery cells 2 are transferred to the printing table, the printing of low-temperature silver paste begins. Since the battery cell already has a complete and fine secondary grid line, the main grid printed now is mainly for battery conduction collection, so a complete solid line is no longer required. Instead, a main grid arranged in dotted lines is printed, and the virtual-to-real ratio is 1:2, that is, the void is 1, and the length of the solid line is twice the length of the void, so as to achieve the effect of saving low-temperature silver paste. The virtual-to-real ratio can continue to be optimized and improved according to the continuous production effect in the later stage. The virtual-to-real ratio of 1:2 in the present invention can fully meet the needs of current transmission. The battery cell graphics after printing the main grid are as follows Figure 7 It should be noted that the width of the main grid after printing is not 0.5mm, but generally less than 0.5mm, which is determined by specific factors such as the viscosity of the low-temperature silver paste and the ink permeability of the printing screen. And after the two battery cells overlap, the width of the grid line should not exceed 0.5mm as much as possible.
[0052] Step 4, after the low-temperature silver paste 18 is printed, print the colloid 19 on both sides of the low-temperature silver paste 18. The main function of the colloid 19 is to form good adhesion after the two battery cells 2 overlap. Colloid 19 is an insulator, and a silicone-based or acrylic colloid is used. The adhesion of this type of colloid after curing is much greater than the adhesion requirement between batteries, such as the E240E / E224H model colloid of Dongshu New Materials, which has good adhesion and practical operability. It should be noted that after printing the low-temperature silver paste and when printing the colloid, the screen does not contact the low-temperature silver paste to avoid destroying the silver paste distribution and silver paste characteristics. Therefore, it is necessary to use a special screen and scraper, which can be designed according to the number of sheets printed simultaneously during actual production. The present invention uses a design of 5 pcs per group.
[0053] The screen is hollowed out at the low-temperature silver paste grid line, and a hard bracket is provided at the hollow edge to isolate the silver paste area and prevent the colloid 19 from flowing out of the screen. After the screen covers the battery cell, the scraper moves up and down on the screen to squeeze the colloid so that the colloid 19 is printed on the battery cell 2. Figure 8 This is a schematic diagram of a top view of a screen, in which there are five groups of hollow areas 14 in the form of dotted lines, which respectively cover the low-temperature silver paste areas of five battery cells. Hard brackets are erected around the hollow areas to prevent the colloid 19 from flowing out. There is an ink-penetrating strip on each side of the hollow area for ink-penetrating printing of the colloid 19. When the scraper is printing, it moves along the hollow direction to squeeze the colloid 19 and print it on the battery cell. Fig. 9 This is a schematic diagram of the front side of the screen. The front hollow area border is hidden in this figure. If it is not hidden, it will be Fig.10 .
[0054] After the screen is designed, a matching scraper is also required. The scraper body is the same as the existing scraper, but it needs to match the border of the hollow area. Fig.11 and Fig.12 The scraper 17 includes a mounting plate 20 and a plurality of blades 21. The plurality of blades 21 are fixed on the mounting plate 20 in sequence. The spacing between two adjacent blades 21 is slightly larger than the spacing between the corresponding hollow area frames. When the scraper 17 is working, the blade 21 is inserted between two adjacent hollow area frames 16, and the hollow area frame 16 is inserted between two adjacent blades 21. The lower end surface of the blade 21 contacts the screen, and the colloid 19 on the screen is squeezed into the ink-permeable strip 15 to be printed on the battery cell 2.
[0055] Step 5: After printing, the battery cells overlap each other and are then cured on a curing table at about 200°C. At this temperature, the low-temperature silver paste 18 can penetrate the passivation layer such as silicon nitride on the surface of the battery cell and form an ohmic contact with the N-type diffusion layer to achieve a good electrical connection. In addition, the colloid 19 will make the two battery cells 2 form a good adhesion. The final adhesion diagram is shown in FIG. Fig.13 The back side grid 10 of the first battery cell 2 is docked with the main grid position of the second battery cell, and is connected through low-temperature silver paste 18 and colloid 19. The back side grid 10 of the second battery cell 2 is docked with the main grid position of the third battery cell, and is connected through low-temperature silver paste 18 and colloid 19, and so on.
[0056] A shingled battery structure includes a plurality of overlapping battery cells 2, wherein the battery cells 2 include a back passivation layer 5, a P-type substrate 6, an N-type diffusion layer 7, and a front passivation layer 8 arranged in sequence from bottom to top, and two longitudinal sub-grids and a plurality of mutually parallel transverse sub-grids are printed on the front passivation layer, and two longitudinal sub-grids are connected to the two ends of the transverse sub-grids. The back sub-grid 10 of the first battery cell 2 is butted against the front sub-grid 4 at the main grid position of the second battery cell 2, and the back sub-grid 10 of the second battery cell 2 is butted against the front sub-grid at the main grid position of the third battery cell, and so on. The contact points of two adjacent battery cells are bonded with a colloid 19.
[0057] The above contents are only for explaining the technical idea of the present invention and cannot be used to limit the protection scope of the present invention. Any changes made on the basis of the technical solution in accordance with the technical idea proposed by the present invention shall fall within the protection scope of the claims of the present invention.
Claims
1. A method for preparing a shingled battery, It is characterized in that The following steps are involved: Step 1: printing a plurality of groups of front sub-grids (4) and back sub-grids (10) of battery cells (2) on the front and back sides of a battery cell (1) respectively and sintering them, wherein the front sub-grid of each battery cell (2) comprises two mutually parallel longitudinal sub-grids and a plurality of mutually parallel transverse sub-grids, and two ends of the transverse sub-grids are respectively connected to the two longitudinal sub-grids; Step 2: cutting the battery sheet (1) into a plurality of battery cells (2) along a cutting line parallel to the longitudinal auxiliary grid; Step 3, printing a main grid (3) arranged in a dotted line on the secondary grid at the main grid position on the front side of the battery unit (2), wherein the width of the main grid (3) is less than 0.5 mm; Step 4: Printing colloid (19) on both sides of the main grid (3); Step 5: overlap the plurality of battery cells (2) and then cure them on a curing table. During this process, the low-temperature silver paste (18) for printing the main grid passes through the front passivation layer (8) and forms an ohmic contact with the base silicon to achieve electrical connection. The colloid (19) adheres the adjacent battery cells (2) together. The back subgrid (10) of the first battery cell is butted against the front subgrid (4) at the main grid position of the second battery cell. In the step 1, the front sub-grid (4) is printed with high-temperature silver paste, and the back sub-grid (10) is printed with aluminum paste; In the step 3, the main grid (3) is printed using low-temperature silver paste.
2. A method for preparing a shingled battery according to claim 1, It is characterized in that In the step 1, the width of the secondary gate is 30 μm-50 μm.
3. A method for preparing a shingled battery according to claim 1, It is characterized in that In step 3, the virtual-to-real ratio of the main grid (3) is 1:
2.
4. A method for preparing a shingled battery according to claim 1, It is characterized in that In the step 4, the screen used for printing the colloid (19) does not contact the main grid (3).
5. A method for preparing a shingled battery according to claim 4, It is characterized in that In the step 4, the colloid (19) is printed using a screen and a scraper (17); The screen is provided with a plurality of hollow areas (14) for accommodating low-temperature silver glue in the main grid area, a bracket is arranged outside the hollow areas, and both sides of the hollow areas (14) are provided with an ink-permeable strip for ink-permeable printing of the glue (19); The scraper (17) comprises a mounting plate (20) and a plurality of blades (21), wherein the plurality of blades (21) are fixed on the mounting plate (20) at intervals in sequence. When the scraper (17) is working, the blades (21) are inserted between two adjacent hollow area frames (16), and the colloid (19) on the screen is squeezed into the ink-permeable strip (15), so that the colloid is printed on the battery cell (2).
6. A shingled battery structure prepared by the method of claim 1, It is characterized in that The invention comprises a plurality of battery cells (2) arranged in an overlapping manner, wherein the battery cells (2) comprise a back passivation layer (5), a P-type substrate (6), an N-type diffusion layer (7) and a front passivation layer (8) arranged in sequence from bottom to top, wherein two longitudinal sub-grids and a plurality of mutually parallel transverse sub-grids are printed on the front passivation layer (8), and two ends of the transverse sub-grids are respectively connected to two longitudinal sub-grids; a back sub-grid (10) is printed on the back passivation layer (5); the back sub-grid (10) of the first battery cell is butted against the front sub-grid (4) at the main grid position of the second battery cell, the back sub-grid (10) of the second battery cell (2) is butted against the front sub-grid (4) at the main grid position of the third battery cell, and so on, the contact points of two adjacent battery cells are fixedly connected by a colloid (19), and the main grids (3) are arranged in dotted lines.