Etching equipment

By using hydrogen-containing gas modification and fluorine-containing gas removal steps in plasma treatment, the selectivity and accumulation problems of silicon nitride etching on the silicon oxide region are solved, and an efficient etching process is achieved.

CN114156156BActive Publication Date: 2024-11-15TOKYO ELECTRON LTD
View PDF 9 Cites 0 Cited by

Patent Information

Application Number
CN202111453386.8
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Priority Date
2017-04-25
Filing Date
2017-12-13
Publication Date
2024-11-15
Estimated Expiration
2037-12-13

AI Technical Summary

Technical Problem

When selectively etching the first region formed of silicon nitride relative to the second region formed by silicon oxide, it is difficult to achieve a high selection ratio using plasma etching using hydrofluorocarbon gas in the prior art, and the accumulation is prone to clogging the etching. Opening, resulting in discontinuity of etching.

Method used

The first gas containing hydrogen-containing gas is used to perform the modification step, and the first region of hydrogen-active species is modified is generated, and the second gas containing fluorine-containing gas is used to perform the removal step, and the fluorine-active species is used to selectively etch the fluorine-active species to avoid accumulation. Generate, improve the selection ratio.

Benefits of technology

Etching with high selection ratio is achieved, reducing accumulation generation and ensuring continuity and efficiency of etching.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN114156156B_ABST
    Figure CN114156156B_ABST
Patent Text Reader

Abstract

The present invention provides an etching device, which includes: a chamber with a gas inlet and an exhaust port; a substrate support portion arranged in the chamber, the substrate support portion including an electrode to which high-frequency bias power can be supplied; a plasma generating portion; and a control portion that performs the following a control to c control, wherein a control is to place a substrate including a first region formed by silicon nitride and a second region formed by silicon oxide on the substrate support portion, b control is to supply the high-frequency bias power and generate a first plasma from a first hydrogen-containing gas to modify the first region, and c control is to stop the supply of the high-frequency bias power and generate a second plasma from a second fluorine-containing gas to remove the modified first region.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] Embodiments of the present invention relate to methods of selectively etching a first region formed of silicon nitride relative to a second region formed of silicon oxide. Background Art

[0002] In the manufacture of electronic devices such as semiconductor devices, it is sometimes required to selectively etch one of two regions formed of different materials relative to the other region. For example, a method of selectively etching a first region formed of silicon nitride relative to a second region formed of silicon oxide is required.

[0003] In order to selectively etch the first region formed of silicon nitride relative to the second region formed of silicon oxide, plasma etching using hydrofluorocarbon gas is generally performed. In the plasma etching using hydrofluorocarbon gas, the second region is protected by the deposit of fluorocarbon compounds, while the first region is etched by active species in the plasma. Patent Document 1 describes such plasma etching.

[0004] Prior art literature

[0005] Patent Literature

[0006] Patent Document 1: Japanese Patent Application Publication No. 2003-229418 Summary of the invention

[0007] The technical problem that the invention is intended to solve

[0008] In the process of selectively etching the first region formed of silicon nitride with respect to the second region formed of silicon oxide, a higher selectivity than plasma etching using a hydrofluorocarbon gas is required.

[0009] In addition, when plasma etching using hydrofluorocarbon gas is performed, the second region is protected by the deposits as described above. Therefore, when etching of the first region is performed to form a narrow opening, the opening may be blocked by the deposits, and the etching of the first region may be stopped.

[0010] Therefore, in the process of selectively etching the first region formed of silicon nitride with respect to the second region formed of silicon oxide, a technology for suppressing the generation of deposits and obtaining a high selectivity is sought.

[0011] Technical solutions for solving technical problems

[0012] In one embodiment, a method for selectively etching a first region formed of silicon nitride relative to a second region formed of silicon oxide is provided. The method includes: (i) preparing a workpiece having a first region and a second region in a chamber provided by a chamber body of a plasma processing device; (ii) generating a plasma of a first gas containing a hydrogen-containing gas in the chamber so that a portion of the first region is modified by active species of hydrogen to form a modified region (hereinafter referred to as a "modification step"); and (iii) generating a plasma of a second gas containing a fluorine-containing gas in the chamber so that the modified region is removed by active species of fluorine (hereinafter referred to as a "removal step").

[0013] In one embodiment, a portion of the first region is modified using active species of hydrogen generated in the modification step to form a modified region that can be easily removed using active species of fluorine. On the other hand, the second region formed by silicon oxide is stable and is therefore not modified by the active species of hydrogen. Therefore, in the removal step, the modified region can be selectively removed relative to the second region. Therefore, according to this method, the first region can be selectively etched relative to the second region. In addition, the active species in the plasma generated in the modification step and the removal step have a relatively low stacking property or virtually no stacking property compared to the active species in the plasma of the hydrofluorocarbon gas. Therefore, by this method, the generation of deposits can be suppressed.

[0014] In one embodiment, in the chamber, the workpiece is mounted on a table including an electrode, and a high frequency for guiding ions to the workpiece, i.e., a high frequency for biasing, can be supplied to the electrode. In one embodiment, a high frequency for biasing is supplied to the electrode. With this embodiment, the modification of the first region can be performed more efficiently. In one embodiment, in the step of generating the plasma of the second gas, a high frequency for biasing is not supplied to the electrode. That is, in this embodiment, instead of sputtering etching of ions, the modified region is removed by a chemical reaction between the modified region and an active species of fluorine.

[0015] In one embodiment, the second gas may include NF 3 gas as the fluorine-containing gas.

[0016] In one embodiment, the second gas may further contain hydrogen. The ratio of the number of hydrogen atoms in the second gas to the number of fluorine atoms in the second gas is 8 / 9 or more. The plasma of the second gas can further improve the etching selectivity of the first region.

[0017] In one embodiment, the second gas may include NF 3 gas as the fluorine-containing gas and further include H 2 gas.

[0018] In one embodiment, the ratio of the flow rate of the H2 gas in the second gas to the flow rate of the NF3 gas in the second gas is 3 / 4 or more. The plasma of the second gas can further improve the etching selectivity of the first region.

[0019] In one embodiment, the first gas includes H 2 gas as the hydrogen-containing gas.

[0020] In one embodiment, a plurality of processes each comprising a modification step and a removal step may be performed sequentially.

[0021] In one embodiment, the workpiece further includes a third region formed of silicon. The first gas further includes an oxygen-containing gas. In the modification step of this embodiment, the surface of the third region is oxidized by the active species of oxygen in the first gas, and the etching of the third region can be suppressed in the etching performed by the removal step. Therefore, the first region is selectively etched relative to the second region and the third region. In one embodiment, the first region can be arranged to cover the second region and the third region.

[0022] In one embodiment, a plurality of processes each including a modification step and a removal step are performed in sequence. The workpiece further includes a third region formed of silicon. Before performing the plurality of processes, the first region is configured to cover the second region and the third region. The plurality of processes include one or more first processes and one or more second processes. The one or more first processes are one or more processes performed before the third region is about to be exposed or until the third region is exposed in the plurality of processes. The one or more second processes are one or more processes performed after the one or more first processes in the plurality of processes for oxidizing the surface of the third region. In at least one of the second processes, the first gas further includes an oxygen-containing gas. In the modification step of this embodiment, the surface of the third region is oxidized, and the etching of the third region can be suppressed in the etching performed by the removal step. Therefore, through this embodiment, the first region can be selectively etched relative to the second region and the third region.

[0023] In one or more first processes, the first gas may not contain oxygen-containing gas. The multiple processes may also contain one or more third processes. The one or more third processes are one or more processes performed after the one or more second processes in the multiple processes. The first gas may not contain oxygen-containing gas only in one or more third processes, or in addition to one or more first processes and in one or more third processes.

[0024] In one embodiment, the ratio of the flow rate of the oxygen-containing gas in the first gas to the flow rate of the hydrogen-containing gas in the first gas is 3 / 100 or more and 9 / 100 or less. According to this embodiment, the first region can be etched with a higher selectivity to the third region.

[0025] In one embodiment, the oxygen-containing gas may be O2 gas.

[0026] Effects of the Invention

[0027] As described above, in the process of selectively etching the first region formed of silicon nitride with respect to the second region formed of silicon oxide, it is possible to suppress the generation of deposits and obtain a high selectivity. BRIEF DESCRIPTION OF THE DRAWINGS

[0028] Figure 1 is a flow chart representing a method of one embodiment.

[0029] Figure 2 This is an enlarged cross-sectional view showing a part of an example of a workpiece obtained by applying a method according to one embodiment.

[0030] Figure 3 This is an enlarged cross-sectional view showing a part of an example of a workpiece obtained by applying a method according to one embodiment.

[0031] Figure 4 FIG. 1 is a diagram schematically showing a plasma processing apparatus that can be used in the methods of various embodiments.

[0032] Figure 5 (a) is a diagram for explaining step ST1 of a method of one embodiment, Figure 5 (b) is a diagram showing a state of the workpiece after execution of step ST1 of the method according to one embodiment.

[0033] Figure 6 (a) is a diagram for explaining step ST2 of a method of one embodiment, Figure 6 (b) is a diagram showing a state of a workpiece after execution of step ST2 of a method according to one embodiment of the present invention. Figure 6 (c) is a diagram showing a state of a workpiece when a method according to one embodiment is completed.

[0034] Figure 7 (a) is a diagram showing a state of a workpiece after execution of step ST1 of a method according to one embodiment, Figure 7 (b) is a diagram showing a state of a workpiece after execution of step ST2 of a method according to one embodiment of the present invention. Figure 7 (c) is a diagram showing a state of a workpiece when a method according to one embodiment is completed.

[0035] Figure 8 is a flow chart showing a method of another embodiment.

[0036] Fig. 9 (a) Fig. 9 (b) are used to illustrate Figure 8 FIG. 1 is a diagram showing step ST1 of the first process in the first example of the method shown, and step ST1 of the second process, Fig. 9 (c) is a diagram showing a state where the surface of the third region is oxidized by executing step ST1 in the second process.

[0037] Fig.10 (a) Fig.10 (b) are used to illustrate Figure 8 FIG. 1 is a diagram showing step ST1 of the first flow and step ST1 of the second flow in the second example of the method shown in FIG. Fig.10 (c) is a diagram showing a state after the surface of the third region is oxidized by executing step ST1 in the second process.

[0038] Fig.11 is a flowchart showing a method according to yet another embodiment.

[0039] Fig.12 (a) Fig.12 (b) Fig.12 (c) are used to illustrate Fig.11 FIG. 1 is a diagram of step ST1 in the first flow, step ST1 in the second flow, and step ST1 in the third flow of the method shown.

[0040] Fig.13 (a) Fig.13 (b) and Fig.13 (c) is a graph showing the results of the first experiment.

[0041] Fig.14 (a) and Fig.14 (b) is a graph showing the results of the second experiment.

[0042] Fig.15 This is a graph showing the results of the second experiment.

[0043] Fig.16 (a) is a diagram for explaining the required reduction amount of each sample in the third experiment, Fig.16 (b) is a table showing the required reduction amount of each sample in the third experiment.

[0044] Fig.17 is a flowchart showing a method according to yet another embodiment.

[0045] Fig.18 It is an application Fig.17 An enlarged cross-sectional view of a portion of a workpiece in the method shown.

[0046] Fig.19 Yes means Fig.17 A cross-sectional view showing a state of a portion of a workpiece during execution of the method shown.

[0047] Fig. 20 Yes means Fig.17 A cross-sectional view showing a state of a portion of a workpiece during execution of the method shown.

[0048] Fig.21 Yes means Fig.17 A cross-sectional view showing a state of a portion of a workpiece during execution of the method shown.

[0049] Fig. 22 Yes means Fig.17 A cross-sectional view showing a state of a portion of a workpiece during execution of the method shown.

[0050] Fig.23 Yes means Fig.17 A cross-sectional view showing a state of a portion of a workpiece after execution of the method shown.

[0051] Fig.24 It is detailed Fig.17 A flow chart showing the steps of a portion of a method is shown.

[0052] Fig.25 (a) and Fig.25 (b) is a detailed representation of Fig.17 A flow chart showing the steps of a portion of a method is shown.

[0053] Description of Reference Numerals

[0054] 10 Plasma treatment device

[0055] 12 Chamber body

[0056] 12c Chamber

[0057] 14 units

[0058] 16 Electrostatic chuck

[0059] 18 Lower electrode

[0060] 30 High frequency power supply

[0061] 44 Gas supply unit

[0062] 50 Antenna

[0063] 70A, 70B High Frequency Power Supply

[0064] 80 Control Department

[0065] W Workpiece

[0066] R1 First Area

[0067] R2 Second Area

[0068] R3 Third Area

[0069] MR1 Modified Region

[0070] MR3 oxidation region. DETAILED DESCRIPTION

[0071] Hereinafter, various embodiments will be described in detail with reference to the accompanying drawings. In addition, in each of the drawings, the same or corresponding parts are marked with the same reference numerals.

[0072] Figure 1 is a flow chart representing a method of one embodiment. Figure 1 The method MT shown is a method for selectively etching a first region formed of silicon nitride relative to a second region formed of silicon oxide. In one embodiment, the method MT selectively etches the first region relative to the second region and a third region formed of silicon. In the method MT, first, in step STP, a workpiece is prepared in a chamber provided by a chamber body of a plasma processing apparatus.

[0073] Figure 2 This is an enlarged cross-sectional view showing a part of an example of a workpiece obtained by applying a method according to one embodiment. Figure 2 The workpiece W shown in FIG. 1 has a first region R1 and a second region R2. The workpiece W may also have a third region R3. The first region R1 is formed of silicon nitride, the second region R2 is formed of silicon oxide, and the third region R3 is formed of silicon. The third region R3 is formed of polycrystalline silicon, for example. Figure 2 In the workpiece W shown in the figure, the first region R1, the second region R2 and the third region R3 are arranged on the base layer UL. The layout of the first region R1, the second region R2 and the third region R3 in the workpiece W is not limited to Figure 2 Layout shown.

[0074] Figure 3 This is an enlarged cross-sectional view showing a portion of a workpiece of another example obtained by applying a method according to one embodiment. Figure 3 The workpiece W shown in FIG. Figure 2The workpiece W shown also has a first region R1, a second region R2, and a third region R3. The second region R2 is disposed on both sides of the third region R3, and the third region R3 is disposed in a manner of being raised relative to the second region R2. The first region R1 is disposed in a manner of covering the second region R2 and the third region R3. In addition, Figure 3 The workpiece W shown is an intermediate product obtained in the manufacturing process of the FinFET, and the third region R3 is used as a fin region for providing a source region, a drain region, and a gate region.

[0075] Figure 4 FIG. 1 is a diagram schematically showing a plasma processing apparatus that can be used in the methods of various embodiments. Figure 4 The plasma processing device 10 shown has an ICP (Inductively Coupled Plasma) type plasma source. The plasma processing device 10 has a chamber body 12. The chamber body 12 is formed of a metal such as aluminum, for example. The chamber body 12 has a substantially cylindrical shape, for example. The chamber body 12 provides its internal space as a chamber 12c. The chamber 12c is used as a space for plasma processing.

[0076] A table 14 is provided at the bottom of the chamber body 12. The table 14 holds the workpiece W mounted thereon. The table 14 can be supported by a support portion 13. The support portion 13 extends upward from the bottom of the chamber body 12 in the chamber 12c. The support portion 13 has, for example, a substantially cylindrical shape. The support portion 13 can be formed of, for example, an insulating material such as quartz.

[0077] The stage 14 has an electrostatic chuck 16 and a lower electrode 18. The lower electrode 18 includes a first plate 18a and a second plate 18b. The first plate 18a and the second plate 18b can be formed of a metal such as aluminum, for example. The first plate 18a and the second plate 18b can have a substantially disc shape, for example. The second plate 18b is disposed on the first plate 18a. The second plate 18b is electrically connected to the first plate 18a.

[0078] The electrostatic chuck 16 is provided on the second plate 18b. The electrostatic chuck 16 has an insulating layer and a film-shaped electrode provided in the insulating layer. The DC power supply 22 is electrically connected to the electrode of the electrostatic chuck 16 via a switch 23. The electrostatic chuck 16 generates an electrostatic force generated by the DC power supply from the DC power supply 22. The workpiece W is attracted to the electrostatic chuck 16 by the electrostatic force and is held by the electrostatic chuck 16.

[0079] When the plasma processing apparatus 10 is used, the focus ring FR is disposed on the outer peripheral edge of the second plate 18b so as to surround the edge of the workpiece W and the edge of the electrostatic chuck 16. The focus ring FR is used to improve the uniformity of plasma processing. The focus ring FR can be formed of quartz, for example.

[0080] A flow path 24 is formed in the second plate 18b. A heat exchange medium, such as a refrigerant, for adjusting the temperature of the stage 14 is supplied to the flow path 24 from a temperature regulator (e.g., a cooling unit) provided outside the chamber body 12. The temperature regulator is a device for adjusting the temperature of the heat exchange medium. The heat exchange medium is supplied to the flow path 24 from the temperature regulator via a pipe 26a. The heat exchange medium supplied to the flow path 24 is returned to the temperature regulator via a pipe 26b. The heat exchange medium whose temperature is adjusted is supplied to the flow path 24 of the stage 14 by the heat exchange regulator, thereby adjusting the temperature of the stage 14 and, in turn, the temperature of the workpiece W. In the plasma processing apparatus 10, a gas supply line 28 extends through the stage 14 to the upper surface of the electrostatic chuck 16. A heat transfer gas, such as He gas, from a heat transfer gas supply mechanism is supplied to a space between the upper surface of the electrostatic chuck 16 and the back surface of the workpiece W via the gas supply line 28. Thus, heat exchange between the stage 14 and the workpiece W is promoted.

[0081] A heater HT may also be provided in the stage 14. The heater HT is a heating element. The heater HT is embedded in, for example, the second plate 18b or the electrostatic chuck 16. The heater HT is connected to a heater power supply HP. The temperature of the stage 14 is adjusted by supplying power from the heater power supply HP to the heater HT, thereby adjusting the temperature of the workpiece.

[0082] The high frequency power supply 30 is connected to the lower electrode 18 of the stage 14 via the matching device 32. The high frequency from the high frequency power supply 30 can be supplied to the lower electrode 18. The high frequency power supply 30 generates a high frequency for guiding ions to the workpiece W mounted on the stage 14, that is, a high frequency for bias. The high frequency for bias has a frequency in the range of 400 [kHz] to 40.68 [MHz], and in one example, a frequency of 13.56 [MHz]. The matching device 32 has a circuit for matching the output impedance of the high frequency power supply 30 with the output impedance of the load end (the lower electrode 18 end). In addition, in the plasma processing device 10, by supplying the high frequency for bias to the lower electrode 18, plasma can be generated without using other high frequencies for plasma.

[0083] In the plasma processing apparatus 10, a shield 34 is detachably provided along the inner wall of the chamber body 12. The shield 34 is also provided on the outer periphery of the support portion 13. The shield 34 is a component for preventing the etching byproducts from being attached to the chamber body 12. The shield 34 may be formed by coating the surface of an aluminum substrate with a ceramic such as Y2O3.

[0084] An exhaust passage is formed between the stage 14 and the side wall of the chamber body 12. The exhaust passage is connected to an exhaust port 12e formed at the bottom of the chamber body 12. An exhaust device 38 is connected to the exhaust port 12e via a pipe 36. The exhaust device 38 includes a pressure regulator and a vacuum pump such as a turbomolecular pump. A buffer plate 40 is provided in the exhaust passage, that is, between the stage 14 and the side wall of the chamber body 12. The buffer plate 40 has a plurality of through holes penetrating the buffer plate 40 in the thickness direction thereof. The buffer plate 40 can be formed, for example, by coating a ceramic such as Y2O3 on the surface of an aluminum substrate.

[0085] The chamber body 12 has an opening at the top. The opening is closed by a window member 42. The window member 42 is made of a dielectric such as quartz. The window member 42 has a plate shape, for example.

[0086] A gas inlet 12i is formed on the side wall of the chamber body 12. The gas supply unit 44 is connected to the gas inlet 12i via a pipe 46. The gas supply unit 44 supplies the first gas and the second gas described later to the chamber 12c. The gas supply unit 44 includes a gas source group 44a, a flow controller group 44b and a valve group 44c. The gas source group 44a includes a plurality of gas sources. The plurality of gas sources include: a source of one or more gases including the first gas; and a source of one or more gases including the second gas. The flow controller group 44b includes a plurality of flow controllers. The plurality of flow controllers are all mass flow controllers or pressure-controlled flow controllers. The valve group 44c includes a plurality of valves. The plurality of gas sources of the gas source group 44a are connected to the gas inlet 12i via corresponding flow controllers among the plurality of flow controllers of the flow controller group 44b and corresponding valves among the plurality of valves of the valve group 44c. In addition, the gas inlet 12i may be formed not on the side wall of the chamber body 12 but on other parts such as the window member 42.

[0087] An opening 12p is formed in the side wall of the chamber body 12. The opening 12p is a passage through which the workpiece W passes when the workpiece W is carried into the chamber 12c from the outside of the chamber body 12 and when the workpiece W is carried out from the chamber 12c to the outside of the chamber body 12. A gate valve 48 for opening and closing the opening 12p is installed in the side wall of the chamber body 12.

[0088] An antenna 50 and a shielding member 60 are provided on the top of the chamber body 12 and on the window member 42. The antenna 50 and the shielding member 60 are provided on the outside of the chamber body 12. In one embodiment, the antenna 50 has an inner antenna element 52A and an outer antenna element 52B. The inner antenna element 52A is a spiral coil extending on the central portion of the window member 42. The outer antenna element 52B is a spiral coil extending on the window member 42 and outside the inner antenna element 52A. The inner antenna element 52A and the outer antenna element 52B are each formed of a conductor such as copper, aluminum, or stainless steel.

[0089] The inner antenna element 52A and the outer antenna element 52B are sandwiched and supported by a plurality of sandwiching bodies 54. The plurality of sandwiching bodies 54 are all in a rod shape. The plurality of sandwiching bodies 54 extend radially from the vicinity of the center of the inner antenna element 52A to the outside of the outer antenna element 52B.

[0090] The shielding member 60 covers the antenna 50. The shielding member 60 includes an inner shielding wall 62A and an outer shielding wall 62B. The inner shielding wall 62A has a cylindrical shape. The inner shielding wall 62A is provided between the inner antenna element 52A and the outer antenna element 52B in a manner of surrounding the inner antenna element 52A. The outer shielding wall 62B has a cylindrical shape. The outer shielding wall 62B is provided outside the outer antenna element 52B in a manner of surrounding the outer antenna element 52B.

[0091] The inner antenna element 52A is provided with a disk-shaped inner shield plate 64A to close the opening of the inner shield wall 62A. The outer antenna element 52B is provided with a ring-shaped outer shield plate 64B to close the opening between the inner shield wall 62A and the outer shield wall 62B.

[0092] In addition, the shapes of the shielding wall and the shielding plate of the shielding member 60 are not limited to the above-mentioned shapes. The shape of the shielding wall of the shielding member 60 may also be other shapes such as a square tube shape.

[0093] The inner antenna element 52A and the outer antenna element 52B are connected to the high-frequency power supply 70A and the high-frequency power supply 70B, respectively. High frequencies having the same frequency or different frequencies are supplied to the inner antenna element 52A and the outer antenna element 52B from the high-frequency power supply 70A and the high-frequency power supply 70B, respectively. When the high frequency from the high-frequency power supply 70A is supplied to the inner antenna element 52A, an induced magnetic field is generated in the chamber 12c, and the gas in the chamber 12c is excited by the induced magnetic field. Thus, plasma is generated above the central area of ​​the workpiece W. In addition, when the high frequency from the high-frequency power supply 70B is supplied to the outer antenna element 52B, an induced magnetic field is generated in the chamber 12c, and the gas in the chamber 12c is excited by the induced magnetic field. Thus, a ring-shaped plasma is generated above the peripheral area of ​​the workpiece W.

[0094] In addition, it is necessary to adjust the electrical lengths of the inner antenna element 52A and the outer antenna element 52B according to the high frequencies outputted from the high frequency power supplies 70A and 70B, respectively. Therefore, the height positions of the inner shielding plate 64A and the outer shielding plate 64B can be independently adjusted by the actuators 68A and 68B.

[0095] The plasma processing device 10 further includes a control unit 80. The control unit 80 can be a computer having a storage unit such as a processor and a memory, an input device, a display device, and the like. The control unit 80 can operate according to the control program and the recipe data stored in the storage unit to control various main parts of the plasma processing device 10. Specifically, the control unit 80 controls various main parts of the plasma processing device such as the plurality of flow controllers of the flow controller group 44b, the plurality of valves of the valve group 44c, the exhaust device 38, the high-frequency power supply 70A, the high-frequency power supply 70B, the high-frequency power supply 30, the matching device 32, and the heater power supply HP. In addition, when executing the methods of various embodiments, the control unit 80 can control various main parts of the plasma processing device 10 according to the control program and the recipe data.

[0096] Below, refer to Figure 1 , the method MT is described in detail. In addition, in the following description, reference is made to Figure 5 (a) Figure 5 (b) Figure 6 (a) Figure 6 (b) Figure 6 (c) Figure 7 (a) Figure 7 (b) and Figure 7 (c). Figure 5 (a) is a diagram for explaining step ST1 of a method of one embodiment, Figure 5(b) is a diagram showing a state of the workpiece after execution of step ST1 of the method according to one embodiment. Figure 6 (a) is a diagram for explaining step ST2 of a method of one embodiment, Figure 6 (b) is a diagram showing a state of a workpiece after execution of step ST2 of a method according to one embodiment of the present invention. Figure 6 (c) is a diagram showing a state of a workpiece when a method according to one embodiment is completed. Figure 7 (a) is a diagram showing a state of a workpiece after execution of step ST1 of a method according to one embodiment, Figure 7 (b) is a diagram showing a state of a workpiece after execution of step ST2 of a method according to one embodiment of the present invention. Figure 7 (c) is a diagram showing a state of a workpiece when a method according to one embodiment is completed.

[0097] like Figure 1 As shown, in step STP of method MT, in a chamber provided by a chamber body of a plasma processing apparatus, a Figure 2 or Figure 3 The workpiece W is shown. The workpiece W is placed on a table having a lower electrode. When the plasma processing apparatus 10 is used, the workpiece W is placed on a table 14 and held by an electrostatic chuck 16 .

[0098] In method MT, step ST1 and step ST2 are sequentially performed with the workpiece W placed on stage 14. In step ST1, plasma PL1 of a first gas is generated in the chamber. The first gas includes a hydrogen-containing gas. The hydrogen-containing gas may be, for example, H2 gas and / or NH3 gas.

[0099] In step ST1, if Figure 5 As shown in (a), active species of hydrogen, such as hydrogen ions, are irradiated from plasma PL1 onto the surface of the workpiece W. Figure 5 In (a), the circular figure surrounding the letter "H" represents the active species of hydrogen. When the active species of hydrogen are irradiated onto the surface of the workpiece W, Figure 5 As shown in (b), a portion of the first region R1, that is, a portion of the first region R1 including the surface is modified to become a modified region MR1. Figure 3 The workpiece W, such as Figure 7 As shown in (a), the modified region MR1 is formed. The modified region MR1 can be easily removed by the active species of fluorine. On the other hand, the second region R2 is stable and is not modified by the active species of hydrogen.

[0100] In step ST1 of one embodiment, a high frequency for bias is supplied to the lower electrode of the stage. In step ST1 of one embodiment, plasma can be generated only by the high frequency for bias. When the high frequency for bias is supplied to the lower electrode, hydrogen ions are strongly guided to the workpiece W, which can promote the modification of the first region R1, and the thickness of the modified region MR1 increases in the film thickness direction of the first region R1. In addition, the power of the high frequency for bias supplied to the lower electrode in step ST1 is set so that etching by sputtering cannot occur.

[0101] When the workpiece W has the third region R3, the first gas may include an oxygen-containing gas. The oxygen-containing gas may be, for example, any one of O2 gas, CO gas, CO2 gas, NO gas, NO2 gas, N2O gas, SO2 gas, or a mixed gas containing two or more of the above gases. Figure 5 As shown in (a), active species of oxygen such as oxygen ions are irradiated onto the surface of the workpiece W. Figure 5 In (a), the circular figure surrounding the letter "O" represents the active species of oxygen. When the active species of oxygen are irradiated onto the surface of the workpiece W, Figure 5 As shown in (b), a portion of the third region R3, that is, a portion of the third region R3 including the surface is oxidized to form an oxidized region MR3. When the surface of the third region R3 is oxidized in this way, etching of the third region R3 in step ST2 described later can be suppressed.

[0102] In one embodiment, the ratio of the flow rate of the oxygen-containing gas in the first gas to the flow rate of the hydrogen-containing gas in the first gas may be greater than 3 / 100 and less than 9 / 100. As described above, by setting the ratio of the flow rate of the oxygen-containing gas in the first gas to the flow rate of the hydrogen-containing gas in the first gas, the etching of the third region R3 including the oxidized region MR3 can be further suppressed in the step ST2 described later. In addition, the reduction in the etching rate of the first region R1 in the step ST2 described later can be suppressed.

[0103] When the plasma processing apparatus 10 is used, in step ST1, a first gas containing a hydrogen-containing gas is supplied from the gas supply unit 44 to the chamber 12c. The first gas supplied to the chamber 12c may also contain an oxygen-containing gas. The flow rates of one or more gases contained in the first gas are respectively controlled by corresponding flow controllers of the flow controller group 44b. In addition, the pressure of the chamber 12c is set to a specified pressure by the exhaust device 38. In addition, a high frequency for biasing from the high frequency power supply 30 may also be supplied to the lower electrode 18. In step ST1, in order to generate plasma, high frequencies may be supplied from the high frequency power supply 70A and the high frequency power supply 70B to the inner antenna element 52A and the outer antenna element 52B, respectively, but they may not be supplied. That is, in step ST1, since a high frequency for biasing is supplied to the lower electrode 18, plasma may be generated without using other high frequencies.

[0104] In the next step ST2, a plasma PL2 of a second gas is generated in the chamber. The second gas includes a fluorine-containing gas. The fluorine-containing gas can be any fluorine-containing gas. For example, the fluorine-containing gas can be any one of NF3 gas, SF6 gas, and fluorocarbon gas (e.g., CF4 gas) or a mixed gas containing two or more of the above gases. In addition to the fluorine-containing gas, the second gas can also contain other gases, such as rare gases such as O2 gas and Ar gas.

[0105] In step ST2, if Figure 6 As shown in (a), the active species of fluorine are irradiated from the plasma PL2 to the surface of the workpiece W. Figure 6 In (a), the circular figure surrounding the letter "F" represents the active species of fluorine. When the active species of fluorine are irradiated onto the surface of the workpiece W, as shown in FIG. Figure 6 As shown in (b), the modified region MR1 is selectively etched and removed using active species of fluorine. Figure 3 The workpiece W, such as Figure 7 As shown in (b), the modified area is removed.

[0106] In step ST2 of one embodiment, high frequency for biasing is not supplied to the lower electrode of the stage. In step ST2, when high frequency for biasing is not supplied to the lower electrode of the stage, the active species of fluorine is not fluorine ions, but etching is mainly performed using fluorine radicals. That is, pattern etching is not performed using ions, but etching is performed using radicals. Thus, etching of the second region R2 and the third region R3 including the oxidized region MR3 can be suppressed. In addition, the modified region MR1 is removed by chemical reaction between the modified region MR1 and the active species of fluorine.

[0107] In step ST2 of one embodiment, the second gas may contain hydrogen. When the second gas contains hydrogen, the ratio of the number of hydrogen atoms in the second gas to the number of fluorine atoms in the second gas is 8 / 9 or more. In addition, when the fluorine-containing gas in the second gas is NF3 gas and the hydrogen-containing gas is H2 gas, the ratio of the flow rate of H2 gas in the second gas to the flow rate of NF3 gas in the second gas is 3 / 4 or more. When the ratio of the number of hydrogen atoms in the second gas to the number of fluorine atoms in the second gas or the ratio of the flow rate of H2 gas in the second gas to the flow rate of NF3 gas in the second gas is set in the above manner, silicon nitride, silicon oxide and silicon are hardly etched. However, silicon nitride modified with hydrogen can be etched. That is, the modified region MR1 is etched. Therefore, the etching selectivity of the first region R1 can be further improved.

[0108] When the plasma processing apparatus 10 is used, in step ST2, a second gas containing a fluorine-containing gas is supplied from the gas supply unit 44 to the chamber 12c. The second gas supplied to the chamber 12c may not contain a hydrogen-containing gas. The flow rates of one or more gases contained in the second gas are respectively controlled by corresponding flow controllers of the flow controller group 44b. In addition, the pressure of the chamber 12c is set to a specified pressure using the exhaust device 38. In addition, a high frequency from the high frequency power supply 70A is supplied to the internal antenna element 52A, and a high frequency from the high frequency power supply 70B is supplied to the external antenna element 52B. The high frequency for biasing from the high frequency power supply 30 is not supplied to the lower electrode 18, or its power is relatively small.

[0109] like Figure 1 As shown, in the next step STJ, it is determined whether the stop condition is satisfied. The stop condition is determined to be satisfied when the number of executions of the process including step ST1 and step ST2 reaches a predetermined number of times. In step STJ, if it is determined that the stop condition is not satisfied, step ST1 is executed again. On the other hand, if it is determined that the stop condition is satisfied, the method MT ends. At the end of the method MT, Figure 6 As shown in (c), from Figure 2 The workpiece W shown in FIG. 1 is free of the first region R1. Alternatively, Figure 7 As shown in (c), from Figure 3 The workpiece W shown is obtained by removing the first region R1.

[0110] In method MT, a portion of the first region R1 is modified by the active species of hydrogen generated in step ST1 to form a modified region MR1 that can be easily removed by the active species of fluorine. On the other hand, the second region R2 formed by silicon oxide is stable and is therefore not modified by the active species of hydrogen. Therefore, in step ST2, the modified region MR1 is selectively removed relative to the second region R2. Therefore, according to method MT, the first region R1 is selectively etched relative to the second region R2. In addition, the active species in the plasma generated in steps ST1 and ST2 have a relatively low accumulation property, or substantially no accumulation property, compared to the active species in the plasma of hydrofluorocarbon gas. Therefore, according to method MT, the generation of deposits can be suppressed.

[0111] In addition, when the workpiece W has the third region R3, as described above, the first gas contains an oxygen-containing gas. Therefore, in step ST1, the surface of the third region R3 is oxidized by the active species of oxygen, and in the etching of step ST2, the etching of the third region R3 including the oxidized region MR3 can be suppressed. Therefore, the first region R1 can be selectively etched relative to the second region R2 and the third region R3.

[0112] In addition, as described above, in one embodiment, the ratio of the flow rate of the oxygen-containing gas in the first gas to the flow rate of the hydrogen-containing gas in the first gas is set to be greater than 3 / 100 and less than 9 / 100. In this embodiment, in step ST2, the etching of the third region R3 including the oxidized region MR3 can be further suppressed. In addition, the reduction in the etching rate of the first region R1 in step ST2 can be suppressed. As a result, the first region R1 can be etched with a higher selectivity relative to the third region R3.

[0113] Hereinafter, a method according to another embodiment will be described. Figure 8 is a flow chart showing a method of another embodiment. Figure 8 The method MTA shown can be applied to Figure 3 The workpiece W shown is a workpiece in which the second region R2 and the third region R3 are covered by the first region R1.

[0114] The method MTA includes a step STP identical to the step STP of the method MT. The method MTA also includes a plurality of procedures SQ executed in sequence. Each of the plurality of procedures SQ includes a step ST1 identical to the step ST1 of the method MT and a step ST2 identical to the step ST2 of the method MT.

[0115] The plurality of processes SQ include one or more first processes SQ1 and one or more second processes SQ2. The one or more first processes SQ1 are one or more processes including the processes that are first executed among the plurality of processes. The one or more second processes SQ2 are processes that are executed after the one or more first processes SQ1 among the plurality of processes SQ. The one or more second processes SQ2 are processes including step ST1 for oxidizing the surface of the third region R3.

[0116] Method MTA includes step STJ1 and step STJ2. In step STJ1, it is determined whether the stop condition is satisfied. In step STJ1, the stop condition is determined to be satisfied when the number of executions of the first process SQ1 reaches a specified number of times. In step STJ1, when it is determined that the stop condition is not satisfied, the first process SQ1 is executed again. On the other hand, in step STJ1, when it is determined that the stop condition is satisfied, the processing proceeds to the execution of the second process SQ2.

[0117] In step STJ2, it is determined whether the stop condition is satisfied. In step STJ2, the stop condition is determined to be satisfied when the number of executions of the second process SQ2 reaches a specified number of times. In step STJ2, when it is determined that the stop condition is not satisfied, the second process SQ2 is executed again. On the other hand, when it is determined that the stop condition is satisfied, the execution of method MTA is terminated.

[0118] Fig. 9 (a) Fig. 9 (b) are used to illustrate Figure 8 FIG. 1 is a diagram showing step ST1 of the first process in the first example of the method shown, and step ST1 of the second process, Fig. 9 (c) is a diagram showing a state where the surface of the third region is oxidized by executing step ST1 in the second process. In the first example of the method MTA, one or more first processes SQ1 are executed until the third region R3 is exposed. In the first example of the method MTA, the first gas used in one or more steps ST1 of the first process SQ1 does not contain an oxygen-containing gas. Therefore, Fig. 9 As shown in (a) of FIG. 1 , in one or more steps ST1 of the first process SQ1 , the workpiece W is not irradiated with active species of oxygen, but is irradiated with active species of hydrogen.

[0119] In the first example of the method MTA, one or more second processes SQ2 are performed immediately after the third region R3 is exposed. In step ST1 of one or more second processes SQ2, the first gas contains an oxygen-containing gas in addition to the hydrogen-containing gas. Fig. 9 As shown in (b), immediately after the third region R3 is exposed, in step ST1, active species of hydrogen and active species of oxygen are irradiated to the workpiece W. As a result, Fig. 9 As shown in (c), after the surface of the third region R3 is exposed, the surface of the third region R3 is oxidized to form an oxidized region R3. Therefore, the third region R3 is protected by etching with active species of fluorine in step ST2. According to the first example of the above-mentioned method MTA, the first region R1 can be selectively etched relative to the second region R2 and the third region R3.

[0120] Fig.10 (a) Fig.10 (b) are used to illustrate Figure 8 FIG. 2 is a diagram showing step ST1 in the first flow and step ST1 in the second flow of the second example of the method shown. Fig.10 (c) is a diagram showing the state after the surface of the third region is oxidized by executing step ST1 in the second process. In the second example of the method MTA, one or more first processes SQ1 are executed until the third region R3 is about to be exposed. That is, one or more first processes SQ1 are executed until a state is formed in which only the first region R1 remains in a manner covering the third region R3. In the second example of the method MTA, the first gas used in step ST1 of one or more first processes SQ1 does not contain an oxygen-containing gas. Therefore, Fig.10 As shown in (a) of FIG. 1 , in one or more steps ST1 of the first sequence SQ1 , the workpiece W is not irradiated with active species of oxygen, but is irradiated with active species of hydrogen.

[0121] In one or more second steps SQ2 of the second example of the method MTA, the first gas includes an oxygen-containing gas in addition to the hydrogen-containing gas. Therefore, in the second example of the method MTA, after the third region R3 is about to be exposed, as shown in FIG. Fig.10 As shown in (b), the workpiece W is irradiated with active species of oxygen. Fig.10 As shown in (c), the surface of the third region R3 is oxidized immediately after the surface of the third region R3 is exposed. Therefore, immediately after the surface of the third region R3 is exposed, the third region R3 is protected by etching with active species of fluorine in step ST2. According to the second example of the method MTA, the first region R1 is selectively etched relative to the second region R2 and the third region R3.

[0122] Hereinafter, a method according to still another embodiment will be described. Fig.11 is a flowchart showing a method according to yet another embodiment. Fig.11 The method MTB shown can be applied in the same way as the method MTA. Figure 3The method MTB includes step STP, one or more first processes SQ1, step STJ1, one or more second processes SQ2 and step STJ2, and one or more third processes SQ3 and step STJ3.

[0123] In method MTB, one or more second processes SQ2 are terminated after the surface of the third region R3 is oxidized. In method MTB, when it is determined in step STJ2 that the stop condition is satisfied, the processing proceeds to the execution of the third process SQ3. In step STJ3, it is determined whether the stop condition is satisfied. The stop condition is determined to be satisfied when the number of executions of the third process SQ3 reaches a specified number of times. In step STJ3, when it is determined that the stop condition is not satisfied, the third process SQ2 is executed again. On the other hand, in step STJ3, when it is determined that the stop condition is satisfied, the operation of method MTB ends.

[0124] Fig.12 (a) Fig.12 (b) Fig.12 (c) are used to illustrate Fig.11 FIG. 1 shows step ST1 of the first process, step ST1 of the second process, and step ST1 of the third process of the method shown in FIG. In the method MTB, one or more first processes SQ1 are performed before or until the third region R3 is exposed. In one or more steps ST1 of the first processes SQ1, the first gas does not contain an oxygen-containing gas. Therefore, Fig.12 As shown in (a), in one or more steps ST1 of the first process SQ1, active species of hydrogen are irradiated to the workpiece W instead of active species of oxygen. In one or more steps ST1 of the first process SQ1, the first gas may include an oxygen-containing gas.

[0125] In the method MTB, after one or more processes SQ1, one or more second processes SQ2 are performed to oxidize the surface of the third region R3. In step ST1 of one or more second processes SQ2, the first gas contains an oxygen-containing gas in addition to the hydrogen-containing gas. Therefore, according to one or more second processes SQ2 of the method MTB, Fig.12 As shown in (b), immediately after the third region R3 is exposed, active species of oxygen are irradiated onto the workpiece W. In the method MTB, one or more second steps SQ2 are terminated after the surface of the third region R3 is oxidized.

[0126] In the method MTB, after one or more processes SQ2, one or more third processes SQ3 are performed. In step ST1 of one or more third processes SQ3, the first gas does not contain an oxygen-containing gas. Fig.12 As shown in (c), in step ST1 of one or more third processes SQ3, active species of oxygen are not irradiated to the workpiece W, but active species of hydrogen are irradiated to the workpiece W. In method MTB, in one or more second processes SQ2, the surface of the third region R3 is oxidized immediately after it is exposed, so even if the first gas does not contain an oxygen-containing gas in step ST1 of one or more third processes SQ3, the third region R3 can be protected by etching with active species of fluorine in step ST2. According to the above method MTB, the first region R1 is selectively etched relative to the second region R2 and the third region R3.

[0127] Various experimental results are described below, but the present invention is not limited to these experiments.

[0128] (First Experiment)

[0129] The first experiment is an experiment conducted to guide the following conditions: when silicon nitride is not modified by hydrogen active species, it cannot be etched by active species from the plasma of the second gas. In the first experiment, in the chamber of the plasma processing device 10, the silicon nitride film, the silicon oxide film and the silicon film are processed by the plasma of the second gas. The second gas used in the first experiment is a gas containing NF3 gas, H2 gas, O2 gas and Ar gas. In the first experiment, the flow rate of H2 gas in the second gas is set to various flow rates. The following shows other parameters of the first experiment.

[0130] <Parameters of the first experiment>

[0131] ·Pressure of chamber 12c: 400 [mTorr] (53.33 [Pa])

[0132] High frequency of high frequency power supplies 70A and 70B: 27 [MHz], 600 [W]

[0133] · High frequency for bias: 0[W]

[0134] NF3 gas flow rate: 45[sccm]

[0135] O2 gas flow rate: 300[sccm]

[0136] Ar gas flow rate: 100 [sccm]

[0137] Processing time: 10 [seconds]

[0138] In the first experiment, the reduction amount (length) of the film thickness (that is, the etching amount) of each of the silicon nitride film, the silicon oxide film, and the silicon film obtained by the treatment using the plasma of the second gas was measured. Fig.13 (a) Fig.13 (b) and Fig.13 (c) shows a graph showing the results of the first experiment. Fig.13 (a) Fig.13 (b) and Fig.13 In each of the graphs (c), the horizontal axis represents the flow rate of the H 2 gas in the second gas. Fig.13 The vertical axis of the graph (a) represents the etching amount of the silicon nitride film. Fig.13 The vertical axis of the graph (b) represents the etching amount of the silicon oxide film. Fig.13 The vertical axis of the graph of (c) represents the etching amount of the silicon film.

[0139] Depend on Fig.13 (a) Fig.13 (b) and Fig.13 (c) shows that when the flow rate of H2 gas in the second gas is 60 sccm or more, the silicon nitride film, silicon oxide film and silicon film are basically not etched in the plasma treatment of the second gas. Therefore, in the treatment of the second gas plasma using the ratio of the flow rate of H2 gas in the second gas to the flow rate of NF3 gas in the second gas being 3 / 4 or more, it is confirmed that silicon nitride, silicon oxide and silicon are not etched. Thus, when the ratio of the number of oxygen atoms in the second gas to the number of fluorine atoms in the second gas is 8 / 9 or more, in the treatment using the plasma of the second gas, it is confirmed that silicon nitride, silicon oxide and silicon are not etched. .

[0140] (Second experiment)

[0141] In the second experiment, the method MT was applied to the silicon nitride film, the silicon oxide film, and the silicon film using the plasma processing apparatus 10, and the relationship between the ratio of the O2 gas in the first gas to the H2 gas in the first gas and the etching selectivity of the silicon nitride film to the silicon oxide film and the silicon film was obtained. The number of executions of the process including step ST1 and step ST2 in the second experiment was 6 times. The following shows other parameters of the second experiment.

[0142] <Parameters of Step ST1 in the Second Experiment>

[0143] ·Pressure of chamber 12c: 30 [mTorr] (4 [Pa])

[0144] High frequency of high frequency power sources 70A and 70B: 0 [W]

[0145] · High frequency for bias: 13.56[MHz], 50[W]

[0146] ·H2 gas flow rate: 100[sccm]

[0147] Processing time: 15 [seconds]

[0148] <Parameters of Step ST2 in the Second Experiment>

[0149] ·Pressure of chamber 12c: 400 [mTorr] (53.33 [Pa])

[0150] High frequency of high frequency power supplies 70A and 70B: 27 [MHz], 600 [W]

[0151] · High frequency for bias: 0[W]

[0152] NF3 gas flow rate: 45[sccm]

[0153] ·H2 gas flow rate: 60[sccm]

[0154] O2 gas flow rate: 300[sccm]

[0155] Ar gas flow rate: 100 [sccm]

[0156] Processing time: 10 [seconds]

[0157] In the second experiment, the reduction in film thickness (length) (i.e., etching amount) of each of the silicon nitride film, silicon oxide film, and silicon film was measured. Furthermore, based on the etching amount of the silicon nitride film and the etching amount of the silicon film, the ratio of the etching amount of the silicon film to the etching amount of the silicon nitride film, i.e., the etching selectivity of the silicon film to the silicon nitride film, was calculated. Fig.14 (a) Fig.14 (b) and Fig.15 The results are shown in Fig.14 (a) Fig.14 (b) and Fig.15 In each graph, the horizontal axis represents the ratio of the flow rate of O 2 gas to the flow rate of H 2 gas. Fig.14 In the graph (a), the vertical axis represents the etching amount of the silicon nitride film. Fig.14 In the graph of (b), the vertical axis represents the etching amount of the silicon oxide film and the etching amount of the silicon film. Fig.15 In the graph of FIG. 1 , the vertical axis represents the etching selectivity of the silicon film to the silicon nitride film.

[0158] from Fig.14 As can be seen from the graph (b), when the ratio of the flow rate of O2 gas in the first gas to the flow rate of H2 gas in the first gas is 3 / 100 or more (a ratio of 3% or more), it is confirmed that the etching amount of the silicon film is reduced, that is, the etching of the silicon film can be suppressed. Fig.14As can be seen from the graph (a), when the ratio of the flow rate of O2 gas in the first gas to the flow rate of H2 gas in the first gas is less than 9 / 100 (less than 9%), the etching amount of the silicon nitride film is approximately equal to the etching amount of the nitride film when the ratio of the flow rate of O2 gas in the first gas to the flow rate of H2 gas in the first gas is 0. That is, when the ratio of the flow rate of O2 gas in the first gas to the flow rate of H2 gas in the first gas is less than 9 / 100, the etching amount of the nitride film does not substantially decrease. Therefore, as Fig.15 As shown, when the ratio of the flow rate of O 2 gas in the first gas to the flow rate of H 2 gas in the first gas is greater than 3 / 100 and less than 9 / 100, it is confirmed that the etching selectivity of the silicon film to the silicon nitride film becomes a high selectivity.

[0159] (Third Experiment)

[0160] In a third experiment, using the plasma processing apparatus 10, the method MT was applied to Figure 3 The experimental sample 1 and the experimental sample 2 are the same as the workpiece W shown in FIG. In the method MT applied to the experimental sample 1, the first gas does not contain O2 gas. In the method MT applied to the experimental sample 2, the first gas does not contain O2 gas. In addition, the plasma processing apparatus 10 is used to process the Figure 3 The comparative sample having the same workpiece W as shown was subjected to plasma treatment with a treatment gas containing a hydrofluorocarbon gas. The following shows the parameters of the method MT applied to the experimental sample 1, the parameters of the method MT applied to the experimental sample 2, and the parameters of the plasma treatment applied to the comparative sample. In addition, in the method MT applied to the experimental sample 1 and the method MT applied to the experimental sample 2, the treatment was performed until the first region R1 was removed, and the number of executions of the process including step ST1 and step ST2 was 33 times. Similarly, in the plasma treatment of the comparative sample, the treatment was also performed until the first region R1 was removed.

[0161] <Parameters of Step ST1 of Method MT for Experimental Sample 1 of Third Experiment>

[0162] ·Pressure of chamber 12c: 30 [mTorr] (4 [Pa])

[0163] High frequency of high frequency power sources 70A and 70B: 0 [W]

[0164] · High frequency for bias: 13.56[MHz], 50[W]

[0165] ·H2 gas flow rate: 100[sccm]

[0166] O2 gas flow rate: 0 [sccm]

[0167] Processing time: 15 [seconds]

[0168] <Parameters of Step ST2 of Method MT for Experimental Sample 1 of Third Experiment>

[0169] ·Pressure of chamber 12c: 400 [mTorr] (53.33 [Pa])

[0170] High frequency of high frequency power supplies 70A and 70B: 27 [MHz], 600 [W]

[0171] · High frequency for bias: 0[W]

[0172] NF3 gas flow rate: 45[sccm]

[0173] ·H2 gas flow rate: 60[sccm]

[0174] O2 gas flow rate: 300[sccm]

[0175] Ar gas flow rate: 100 [sccm]

[0176] Processing time: 10 [seconds]

[0177] <Parameters of Step ST1 of Method MT for Experimental Sample 2 of Third Experiment>

[0178] ·Pressure of chamber 12c: 30 [mTorr] (4 [Pa])

[0179] High frequency of high frequency power sources 70A and 70B: 0 [W]

[0180] · High frequency for bias: 13.56[MHz], 50[W]

[0181] ·H2 gas flow rate: 100[sccm]

[0182] O2 gas flow rate: 9[sccm]

[0183] Processing time: 15 [seconds]

[0184] <Parameters of Step ST2 of Method MT for Experimental Sample 2 of Third Experiment>

[0185] ·Pressure of chamber 12c: 400 [mTorr] (53.33 [Pa])

[0186] High frequency of high frequency power supplies 70A and 70B: 27 [MHz], 600 [W]

[0187] · High frequency for bias: 0[W]

[0188] NF3 gas flow rate: 45[sccm]

[0189] ·H2 gas flow rate: 60[sccm]

[0190] O2 gas flow rate: 300[sccm]

[0191] Ar gas flow rate: 100 [sccm]

[0192] Processing time: 10 [seconds]

[0193] <Parameters of Plasma Treatment Applied to Comparative Samples>

[0194] ·Pressure of chamber 12c: 50 [mTorr] (6.666 [Pa])

[0195] High frequency of high frequency power supplies 70A and 70B: 27 [MHz], 200 [W]

[0196] · High frequency for bias: 50[W]

[0197] · CH3F gas flow rate: 30 [sccm]

[0198] O2 gas flow rate: 15[sccm]

[0199] He gas flow rate: 500[sccm]

[0200] Fig.16 (a) is a diagram for explaining the reduction amount required for each sample in the third experiment. Fig.16 In (a), the second region R2 and the third region R3 of each sample before treatment are indicated by double-dashed lines, and the second region R2 and the third region R3 of each sample after treatment are indicated by solid lines. Fig.16 As shown in (a), the reduction amount ΔL2 of the second region R2 and the reduction amount ΔL3 of the third region R3 were obtained for each sample. The results are shown in Fig.16 From the table (b). Fig.16 The results of the comparative sample shown in (b) show that, in the plasma treatment using the hydrofluorocarbon gas, not only the first region R1 is etched, but also the second region R2 and the third region R3 are etched. Fig.16From the results of the experimental sample 1 shown in the table (b), it can be seen that in the method MT, by modifying the plasma using the first gas containing hydrogen gas, it is confirmed that the second region R2 is not etched, and the first region R1 is selectively etched. However, in the method MT applied to the experimental sample 1, the first gas does not contain oxygen-containing gas, and therefore, the third region R3 is etched. In the experimental sample 2 to which the method MT using the first gas containing oxygen-containing gas is applied, it is confirmed that the first region R1 can be selectively etched without etching both the second region R2 and the third region R3.

[0201] Hereinafter, a method according to another embodiment will be described. Fig.17 is a flow chart showing another embodiment of the method. Fig.17 Together, refer to Figure 18 to Figure 25 .exist Fig.17 In the method MTC shown, after the workpiece having the first region is formed into the second region, the process including the above-mentioned step ST1 and step ST2 is performed one or more times. Hereinafter, the method MTC performed using the plasma device 10 is described, but the method MTC can also be performed using a plasma processing device other than the plasma processing device 10.

[0202] In step STP of method MTC, a plasma processing device 10 is provided with a substrate such as Fig.18 The workpiece W is shown. Fig.18 The workpiece W shown has a base layer UL and a region EL. The region EL is provided on the base layer UL. The surface of the base layer UL includes a main surface UL1. The main surface UL1 is a surface perpendicular to the direction DR. When the workpiece W is placed on the stage 14 (on the electrostatic chuck 16), the direction DR corresponds to the vertical direction.

[0203] The region EL includes a plurality of convex regions (e.g., convex region PJ1 and convex region PJ2). Each of the plurality of convex regions of the region EL extends upward from the main surface UL11. Each of the plurality of convex regions of the region EL has an end face. The convex region PJ1 has an end face TE1. The convex region PJ2 has an end face TE2. Fig.18 In the workpiece W shown, the end faces of the plurality of convex regions of the region EL are exposed. The end face TE1 of the convex region PJ1 and the end face TE2 of the convex region PJ2 are exposed.

[0204] The height of each of the plurality of convex regions is the distance between the end face and the main face UL1. The height TT1 of the convex region PJ1 is the distance between the end face TE1 and the main face UL1. The height TT2 of the convex region PJ2 is the distance between the end face TE2 and the main face UL1. The heights of the plurality of convex regions of the region EL are different from each other. The convex region PJ1 is lower than the convex region PJ2. That is, the value of the height TT1 of the convex region PJ1 is smaller than the value of the height TT2 of the convex region PJ2.

[0205] The base layer UL is formed of Si (silicon), for example. The region EL is formed of silicon nitride, for example. That is, the entire region EL may be a first region formed of silicon nitride. Alternatively, the plurality of convex regions may be formed of materials different from each other. For example, a portion of the plurality of convex regions may be formed of a material different from that of the other convex regions. For example, the convex region PJ1 may be formed of silicon nitride, and the other convex regions may be formed of one or more other materials such as silicon. In this case, the convex region PJ1 is a first region formed of silicon nitride.

[0206] The ends of the plurality of convex regions (convex region PJ1, convex region PJ2, etc.) of the region EL (parts of the end surfaces including the end surfaces TE1, TE2, etc.) may be formed so that their widths are narrowed according to the size of the distance from the main surface UL1. That is, the ends of the plurality of convex regions of the region EL may have a gradually tapering shape. When the end surfaces of the plurality of convex regions of the region EL have a gradually tapering shape, the width of the opening defined by the ends of the plurality of convex regions becomes relatively large, and therefore, the deposits formed at the ends of the convex regions can be suppressed to a great extent.

[0207] like Fig.17 As shown, step STP includes step ST11 and step ST12. In step ST11, Fig.18 In the state where the workpiece W is placed on the stage 14, the first film SF1 is conformally formed on the surface of the workpiece W. The first film SF1 is formed of silicon oxide. The film forming method in step ST11 is the ALD (Atomic Layer Deposition) method. Fig.24 Detailed flowchart of step ST11 is shown. Fig.24 As shown, step ST11 includes step ST11a, step ST11b, step ST11c, and step ST11d. Step ST11a, step ST11b, step ST11c, and step ST11d constitute flow SQ11. In step ST11, flow SQ11 is executed one or more times.

[0208] In step ST11a, a third gas is supplied from the gas supply unit 44 to the chamber 12c containing the workpiece W. The third gas contains an aminosilane-type gas, for example, an organic aminosilane-type gas. The organic aminosilane-type gas uses, for example, an aminosilane monomer (H3-Si-R (R is an organic amino group)). In step ST11a, plasma of the third gas is not generated. In step ST11a, molecules in the third gas (for example, aminosilane monomers) are attached to the surface of the workpiece W as precursors. In addition, the aminosilane-type gas contained in the third gas may contain aminosilanes having 1 to 3 silicon atoms in addition to the aminosilane monomer. In addition, the aminosilane-type gas contained in the third gas may also contain aminosilanes having 1 to 3 amino groups.

[0209] In the next step ST11b, the chamber 12c is purged. That is, in step ST11b, the third gas is exhausted. In step ST11b, an inactive gas such as nitrogen or a rare gas may be supplied to the chamber 12c as a purge gas. In step ST11b, molecules excessively attached to the workpiece W can be removed. By executing step ST11b, the layer of the precursor on the workpiece W becomes an extremely thin layer (e.g., a monomolecular layer).

[0210] In step ST11c, a plasma of a fourth gas is generated in the chamber 12c. The fourth gas includes an oxygen-containing gas. The fourth gas may be, for example, an oxygen-containing gas. In step ST11c, the fourth gas is supplied from the gas supply unit 44 to the chamber 12c. In addition, the pressure of the chamber 12c is set to a specified pressure using the exhaust device 38. In addition, high frequencies are supplied from the high-frequency power supply 70A and the high-frequency power supply 70B to the inner antenna element 52A and the outer antenna element 52B, respectively. In addition, a high frequency for biasing from the high-frequency power supply 30 may also be supplied to the lower electrode 18. In step ST11c, the fourth gas is excited to generate plasma. Then, the layer of the precursor is exposed to the active species of oxygen formed by the plasma. Thus, a silicon oxide film (the first film SF1 or a portion thereof) of the layer of the precursor is formed.

[0211] In the next step ST11d, the chamber 12c is purged. That is, in step ST11d, the fourth gas is exhausted. In step ST11d, an inert gas such as nitrogen or a rare gas is supplied to the chamber 12c as a purge gas.

[0212] In the next step ST11e, it is determined whether to terminate the execution of process SQ11. Specifically, in step ST11e, it is determined whether the execution number of process SQ11 has reached a preset number of times. In step ST11e, if it is determined that the execution number of process SQ11 has not reached the preset number of times, process SQ11 is executed again. On the other hand, in step ST11e, if it is determined that the execution number of process SQ11 has reached the preset number of times, the execution of step ST11 is terminated. By executing this step ST11, as shown in FIG. Fig.19 As shown, the first film SF1 is conformally formed on the surface of the workpiece W. The film thickness of the first film SF1 is determined by the number of executions of the process SQ11. That is, the film thickness of the first film SF1 is represented by the product of the film thickness of the silicon oxide film formed by executing the process SQ11 once and the number of executions of the process SQ11. The number of executions of the process SQ11 is set according to the desired film thickness of the first film SF1.

[0213] Back to Fig.17 In the method MTC, next, step ST12 is performed. In step ST12, a second film SF2 is formed on the first film SF1. The second film SF2 is formed of silicon oxide. In step ST12, the second film SF2 is formed in such a manner that the greater the distance from the main surface UL1 at the formation position, the greater the film thickness. For example, Fig. 20 As shown, the film thickness of the second film SF2 formed on the first film SF1 on the end surface TE2 of the convex region PJ2 is greater than the film thickness of the second film SF2 formed on the first film SF1 on the end surface TE1 of the convex region PJ1.

[0214] In the film forming process of step ST12, the following can be used: Fig.25 Step ST12A shown in (a) or Fig.25 Step ST12B shown in (b) of FIG. 1A and step ST12B are described below.

[0215] Step ST12A includes step ST121 and step ST122. In step ST121, plasma of the fifth gas is generated in the chamber 12c. The fifth gas contains silicon atoms and contains chlorine atoms or hydrogen atoms. The fifth gas contains SiCl4 gas or SiH4 gas. The fifth gas is, for example, a mixed gas of SiCl4 gas or SiH4 gas, Ar gas, and oxygen-containing gas. In step ST121, the fifth gas is supplied to the chamber 12c from the gas supply unit 44. In addition, the pressure of the chamber 12c is set to a specified pressure by the exhaust device 38. In addition, high frequencies are supplied to the inner antenna element 52A and the outer antenna element 52B from the high frequency power supply 70A and the high frequency power supply 70B, respectively. In addition, high frequencies for biasing from the high frequency power supply 30 may also be supplied to the lower electrode 18. In step ST121, the fifth gas is excited to generate plasma. Then, the second film SF2 is formed on the first film SF1 using silicon and oxygen from the plasma. In the next step ST122, the chamber 12c is purged. The purge in step ST122 is the same as the purge in step STST11b (should be ST11b).

[0216] Step ST12B includes step ST125, step ST126, step ST127, and step ST128. Step ST125, step ST126, step ST127, and step ST128 constitute flow SQ12. In step ST12B, flow SQ12 is executed one or more times.

[0217] In step ST125, the sixth gas is supplied to the chamber 12c. The sixth gas contains silicon atoms or chlorine atoms. The sixth gas can be a mixed gas containing SiCl4 gas and Ar gas. In step ST125, the sixth gas is supplied to the chamber 12c from the gas supply unit 44. In addition, the pressure of the chamber 12c is set to a specified pressure using the exhaust device 38. In step ST125, no plasma is generated. In step ST125, the silicon-containing molecules in the sixth gas are attached to the surface of the first film SF1 as precursors. In the next step ST126, the chamber 12c is purged. The purging of step ST126 is the same as the purging of step ST11b. By executing step ST126, the molecules excessively attached to the first film SF1 can be removed.

[0218] In the next step ST127, plasma of the seventh gas is generated in the chamber 12c. The seventh gas includes an oxygen-containing gas. The seventh gas is, for example, a mixed gas including an oxygen-containing gas and an Ar gas. In step ST127, the seventh gas is supplied from the gas supply unit 44 to the chamber 12c. In addition, the pressure of the chamber 12c is set to a specified pressure by the exhaust device 38. In addition, high frequencies are supplied from the high-frequency power supply 70A and the high-frequency power supply 70B to the inner antenna element 52A and the outer antenna element 52B, respectively. In addition, high frequencies for biasing from the high-frequency power supply 30 may also be supplied to the lower electrode 18. In step ST127, the seventh gas is excited to generate plasma. Then, the layer of the precursor is exposed to the active species of oxygen formed by the plasma. Thus, the layer of the precursor forms a silicon oxide film (the second film SF2 or a part thereof). In the next step ST128, the chamber 12c is purged. The purging of step ST128 is the same as the purging of step ST11b.

[0219] In the next step ST129, it is determined whether to terminate the execution of process SQ12. Specifically, in step ST129, it is determined whether the number of executions of process SQ12 has reached a preset number of times. In step ST129, when it is determined that the number of executions of process SQ12 has not reached a preset number of times, process SQ12 is executed again. On the other hand, in step ST129, when it is determined that the number of executions of process SQ12 has reached a preset number of times, the execution of step ST12B is terminated. The film thickness of the second film SF2 is determined by the number of executions of process SQ12. That is, the film thickness of the second film SF2 increases as the number of executions of process SQ12 increases. The number of executions of process SQ12 is set according to the desired film thickness of the second film SF2.

[0220] Back to Fig.17 In the method MTC, next, step ST13 is performed. In step ST13, anisotropic etching of the first film SF1 and the second film SF2 is performed. Thus, the first film SF1 and the second film SF2 on one or more convex regions among the plurality of convex regions are removed. For example, Fig.12 As shown, the first film SF1 and the second film SF2 on the end surface TE1 of the convex region PJ1 are removed.

[0221] In step ST13, plasma of the eighth gas is generated in the chamber 12c. The eighth gas may include a fluorocarbon-based gas. The fluorocarbon-based gas includes a fluorocarbon (C x F y ) and / or hydrofluorocarbons (C x H y F z). The fluorocarbon gas may include, for example, one or more of CF4, C4F8, and CHF3. In step ST13, a fourth gas is supplied from the gas supply unit 44 to the chamber 12c. In addition, the pressure of the chamber 12c is set to a specified pressure by the exhaust device 38. In addition, high frequencies are supplied from the high frequency power supply 70A and the high frequency power supply 70B to the inner antenna element 52A and the outer antenna element 52B, respectively. Moreover, a high frequency for biasing is supplied from the high frequency power supply 30 to the lower electrode 18. Thus, particles from the plasma are guided to the workpiece W to perform anisotropic etching of the first film SF1 and the second film SF2.

[0222] The composite film including the first film SF1 and the second film SF2 formed at a position with a short distance from the main surface UL1 is thinner, and the composite film including the first film SF1 and the second film SF2 formed at a position with a long distance from the main surface UL1 is thicker. Therefore, in step ST13, the composite film on a portion of the end surfaces of the plurality of convex regions with a short distance from the main surface UL1 can be removed. For example, Fig.21 As shown, the first film SF1 and the second film SF2 on the end face TE1 of the convex region PJ1 are removed. The second film SF2 on the end face TE2 of the convex region PJ2 is thin but remains. The remaining first film SF1 and the second film SF2 form the second region.

[0223] In the next step ST14, the first region, i.e., the convex region with the end face exposed among the plurality of convex regions, is selectively etched relative to the first film SF1 and the second film SF2, i.e., the second region. In step ST14, the process including the above-mentioned steps ST1 and ST2 is performed one or more times. In step ST1, a part of the end face of the convex region with the end face exposed among the plurality of convex regions is modified. For example, Fig. 22 As shown in FIG. 1 , a portion of the convex region PJ1 including the end face TE1 is modified to become a modified region MX. Fig.23 As shown, the modified region MX is selectively removed.

[0224] This method MTC can not only be used for Fig.18The etching of the convex area of ​​a portion of the workpiece W shown can also be used, for example, in the manufacture of a fin field effect transistor. In the manufacture of a fin field effect transistor, the workpiece has a fin region and multiple gate regions. The fin region provides a source region, a drain region, and a channel region. Multiple gate regions are arranged on the fin region. Between adjacent gate regions, the fin region is covered with a silicon nitride film. In the manufacture of a fin field effect transistor, while protecting multiple gate regions, a process of removing the silicon nitride film and exposing the fin region (source region and drain region) is performed between adjacent gate regions. This process is performed to form a connection with the fin region (source region and drain region). To achieve this process, method MTC can be used.

[0225] Various embodiments have been described above, but the present invention is not limited to the above embodiments, and various modified forms can be formed. The above-mentioned plasma processing device 10 is an inductively coupled plasma processing device, but the plasma processing device that can be used in each of the various embodiments and the methods of its modified forms can also be an ECR (Electron Cyclotron Resonance) type plasma processing device, a capacitively coupled plasma processing device, or a plasma processing device that uses surface waves such as microwaves to generate plasma.

Claims

1. An etching device, characterized in that: include: a chamber having a gas inlet and an exhaust port; a substrate support portion disposed in the chamber, the substrate support portion including an electrode to which a high frequency bias power can be supplied; A plasma generating unit; and A control unit that performs the following a control to c control, a, placing a substrate including a first region formed of silicon nitride and a second region formed of silicon oxide on the substrate support portion, b controls, supplies the high frequency bias power, generates a first plasma from a first gas containing hydrogen to modify the first region, c control, stopping the supply of the high frequency bias power, generating a second plasma from a second fluorine-containing gas to remove the modified first region, The first region has a plurality of convex regions with different heights from each other, The a control includes: a1 control, conformally forming a first film formed of silicon oxide on the surfaces of the plurality of convex regions; a2 controls to form a second film formed of silicon oxide on the first film, the second film being formed in such a manner that the film thickness increases as the distance from the main surface of the base layer of the substrate increases; and a3 controls the first film and the second film to be anisotropically etched to remove the first film and the second film on one or more convex regions among the plurality of convex regions, and the remaining first film and the second film form the second region.

2. The etching device according to claim 1, characterized in that: The control unit executes a plurality of sequence controls, each of which includes b control and c control in sequence.

3. The etching device according to claim 2, characterized in that: The control unit also performs the following d control and e control: d control, when the number of repetitions of the plurality of sequence controls reaches a specified number, it is determined that a stop condition is met, e control, when the number of repetitions of the plurality of sequence controls does not reach a prescribed number of times, it is determined that the stop condition is not satisfied.

4. The etching device according to claim 1, characterized in that: The control unit supplies high frequency power to the inductively coupled plasma antenna in the b control.

5. The etching device according to claim 1, characterized in that: The plasma generating unit includes an inductively coupled plasma antenna, The control unit supplies high frequency power to the inductively coupled plasma antenna in the b control.

6. The etching device according to claim 1, characterized in that: The plasma generating unit includes an inductively coupled plasma antenna, The control unit supplies high frequency power to the inductively coupled plasma antenna in c control.

7. The etching device according to claim 1, characterized in that: In the c control, the control unit supplies H2 gas and NF3 gas through the gas inlet port, The ratio of the flow rate of the H 2 gas in the second gas to the flow rate of the NF 3 gas in the second gas is 4 / 3 or more.

8. The etching device according to claim 1, characterized in that: In the c-control, the ratio of the number of hydrogen atoms in the second gas to the number of fluorine atoms in the second gas is 8 / 9 or more.

9. The etching device according to claim 1, characterized in that: In the b-control, the control unit supplies H 2 gas through the gas inlet.

10. The etching device according to claim 1, characterized in that: In the b-control, the control unit supplies oxygen through the gas introduction port.

11. An etching device for selectively etching a first region formed of silicon nitride relative to a second region formed of silicon oxide on a substrate, the etching device comprising: a chamber having a gas inlet and an exhaust port; A substrate support portion disposed in the chamber, the substrate support portion comprising an electrode; a gas supply device for supplying gas to the chamber; an RF supply unit for supplying an RF signal to the electrode; and A control unit that performs the following a control to e control, a control, placing the substrate on the substrate support, b controlling, using an RF signal to form a first plasma from a first gas containing hydrogen, c, exposing the substrate to the first plasma to modify the first region, d controlling to form a second plasma from a second fluorine-containing gas without using the RF signal, e, exposing the substrate to the second plasma to remove the modified first region, The first region has a plurality of convex regions with different heights from each other, The a control includes: a1 control, conformally forming a first film formed of silicon oxide on the surfaces of the plurality of convex regions; a2 controls to form a second film formed of silicon oxide on the first film, the second film being formed in such a manner that the film thickness increases as the distance from the main surface of the base layer of the substrate increases; and a3 controls the first film and the second film to be anisotropically etched to remove the first film and the second film on one or more convex regions among the plurality of convex regions, and the remaining first film and the second film form the second region.

Citation Information

Patent Citations

  • Method of etching

    JP2003229418A

  • Plasma immersion ion implantation process

    US20050191830A1

  • Film formation method and apparatus for forming silicon oxide film

    US20080081104A1

  • Etch process for reducing silicon recess

    US20110318936A1

  • Selective ETCH of silicon by way of metastable hydrogen termination

    US20130089988A1