A quasi-solid electrolyte based on boron nitride nanosheets and its preparation method and application
By using boron nitride nanosheets mixed with polyvinyl carbonate and lithium salt to form a quasi-solid electrolyte in lithium batteries, the problems of poor toughness and high processing difficulty of existing solid electrolytes are solved, realizing a high-performance lithium battery electrolyte with high lithium-ion conductivity, wide electrochemical window and good mechanical properties.
Patent Information
- Application Number
- CN202210250223.8
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2022-03-15
- Publication Date
- 2024-11-22
- Estimated Expiration
- 2042-03-15
AI Technical Summary
Existing solid electrolyte materials in lithium batteries suffer from problems such as poor toughness, difficulty in processing, poor contact with electrodes, sensitivity to air and water, and low lithium-ion conductivity, which affect the safety and performance of lithium batteries.
Boron nitride nanosheets are used as inorganic fillers and mixed with a liquid component consisting of polyvinyl carbonate and lithium salt. Through thermal polymerization, a quasi-solid electrolyte is formed. The boron nitride nanosheets promote the rapid transport of lithium ions, while the polyvinyl carbonate improves mechanical properties and stability, thus forming a high-performance electrolyte system.
It achieves high lithium-ion conductivity, high lithium-ion transference number, wide electrochemical operating window, good mechanical properties and flame retardancy, improves the safety and cycle stability of lithium batteries, is compatible with commercial cathodes, and has excellent processability and flexibility.
Smart Images

Figure CN114649587B_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to the technical field of solid electrolytes, and in particular to a quasi-solid electrolyte based on boron nitride nanosheets, and a preparation method and application thereof. Background Art
[0002] With the popularity of personal mobile electronic devices and the promotion of new energy vehicles in recent years, lithium batteries have become an increasingly indispensable part of life. However, the liquid organic electrolytes used in traditional lithium-ion batteries have safety hazards such as flammability, easy leakage, and poor thermal stability, which is one of the main causes of lithium battery deflagration and explosion. Therefore, the development of solid electrolytes has become one of the most promising solutions to improve the safety and comprehensive performance of lithium batteries.
[0003] Solid electrolytes do not have the characteristics of liquid flow, have higher thermal stability and better mechanical properties, are non-flammable and non-leaky, and are currently one of the research hotspots in the energy storage system based on lithium batteries. At present, solid electrolytes can be mainly divided into two types: inorganic solid electrolytes and organic solid electrolytes. Inorganic solid electrolytes mainly include oxides and sulfides. Among them, oxides include Li 3x La 2 / 3-x TiO3(LLTO), NASICON type Li1+xAl x Ti 2-x (PO4)3(LATP), Li1+xAl x Ge2-x(PO4)3(LAGP), garnet-type Li7La3Zr2O 12 (LLZO), etc., which usually have the advantages of high lithium ion conductivity and high hardness, but also have disadvantages such as poor toughness, poor contact between electrodes, and high processing difficulty. Sulfides mainly include Li 3.25 Ge 0.25 P 0.75 S4, Li 9.54 Si 1.74 P 1.44 S 11.7 Cl 0.3etc., also have high lithium ion conductivity, but are usually very sensitive to air and water, and have poor stability, which has adverse effects on processing, assembly and practical use. The most mature organic solid electrolytes are PEO (polyethylene oxide), which have good film-forming properties and good interface contact, but low lithium ion conductivity at room temperature and a narrow electrochemical working window; there are also organic solid electrolytes based on PAN (polyacrylonitrile) and PVDF (polyvinylidene fluoride), which, in addition to the similar advantages and disadvantages to PEO, have performance effects caused by solvent residues that also hinder their practical application [SCHNELL J, GüNTHERT, KNOCH ET, et al. All-solid-state lithium-ion and lithium metal batteries-paving the way to large-scale production [J]. 2018, 382 (160-75).].
[0004] In general, all types of solid electrolytes have defects and disadvantages that cannot be ignored. Therefore, developing solid electrolytes with high safety, high ionic conductivity and high battery performance is still a research goal and hot topic for researchers. Summary of the invention
[0005] The object of the present invention is to provide a quasi-solid electrolyte based on boron nitride nanosheets and a preparation method and application thereof, wherein the quasi-solid electrolyte has good mechanical properties, appropriate flame retardancy, high lithium ion conductivity, high lithium ion transference number and wide electrochemical working window.
[0006] In order to achieve the above-mentioned object of the invention, the present invention provides the following technical solutions:
[0007] The present invention provides a quasi-solid electrolyte, comprising polyvinylene carbonate, a liquid component and boron nitride nanosheets; the liquid component comprises vinylene carbonate and a lithium salt; the liquid component and the boron nitride nanosheets are dispersed in the framework of the polyvinylene carbonate.
[0008] Preferably, in terms of mass percentage, the quasi-solid electrolyte comprises 74.8-84.8 wt % of polyvinylene carbonate, 15-25 wt % of liquid components and 0.2-0.8 wt % of boron nitride nanosheets.
[0009] Preferably, the boron nitride nanosheets are hexagonal boron nitride, and the particle size of the boron nitride nanosheets is 20 nm to 5000 nm.
[0010] Preferably, the lithium salt comprises lithium difluorooxalatoborate or lithium perchlorate.
[0011] The present invention provides a method for preparing the quasi-solid electrolyte described in the above technical solution, comprising the following steps:
[0012] mixing lithium salt, vinylene carbonate and boron nitride nanosheets to obtain a polymer precursor;
[0013] The polymerization precursor and the initiator are mixed and thermally polymerized to obtain a quasi-solid electrolyte.
[0014] Preferably, the mixing of the lithium salt, vinylene carbonate and boron nitride nanosheets comprises: first mixing the lithium salt and vinylene carbonate to obtain a liquid component; and second mixing the liquid component and the boron nitride nanosheets to obtain a polymer precursor.
[0015] Preferably, the ratio of the mass of the lithium salt to the volume of vinylene carbonate is (0.4-1.7) g:(8-12) mL; and the ratio of the mass of the boron nitride nanosheets to the volume of the liquid component is (18-25) mg:(3-4) mL.
[0016] Preferably, the initiator includes azobisisobutyronitrile, and the ratio of the mass of the initiator to the volume of the polymerization precursor is (6-8.5) mg:3.5 mL.
[0017] Preferably, the thermal polymerization pressure is 30-50 kPa, the temperature is 55-65° C., and the time is 700-900 min.
[0018] The present invention provides the use of the quasi-solid electrolyte described in the above technical solution or the quasi-solid electrolyte prepared by the preparation method described in the above technical solution in a lithium battery.
[0019] The present invention provides a quasi-solid electrolyte, comprising polyvinylene carbonate, a liquid component and boron nitride nanosheets; the liquid component comprises vinylene carbonate and a lithium salt; the liquid component and the boron nitride nanosheets are dispersed in the framework of the polyvinylene carbonate.
[0020] In the quasi-solid electrolyte provided by the present invention, the liquid phase component has a higher ability to transmit lithium ions, and the boron nitride nanosheets can promote the rapid transmission of lithium ions. Therefore, the inorganic filler boron nitride nanosheets and the liquid phase component can improve the poor intrinsic lithium ion conductivity of the organic skeleton, enhance the lithium ion transmission capacity of the electrolyte, and make the quasi-solid electrolyte have a higher lithium ion conductivity and a higher lithium ion migration number; the organic skeleton (polyvinyl carbonate) itself has good mechanical properties and stability, the organic skeleton and the liquid phase component can improve the interface contact, and improve the toughness and processability of the electrolyte; the inorganic filler and the organic skeleton can improve the safety and stability of the liquid phase component, and the three work in coordination to achieve the construction of a high-performance electrolyte system. The boron nitride nanosheet filler in the quasi-solid electrolyte provided by the present invention has a rapid transmission mechanism for lithium ions, reduces the transmission barrier of lithium ions, and improves its diffusion coefficient, so that the quasi-solid electrolyte has a high lithium ion migration number (the ratio of the charge transferred by lithium ions to the total charge). The closer the lithium ion migration number is to 1, the better the deposition effect of lithium ions on the negative electrode, the fewer side reactions between the electrode and the electrolyte, the longer the cycle life that the electrolyte can maintain, and the better the cycle performance of the battery.
[0021] The quasi-solid electrolyte provided by the present invention has a wide electrochemical working window, can stably cycle within 0 to 5V, is well compatible with commercial lithium iron phosphate positive electrodes and ternary positive electrodes, and has a stable working state. This is because polyvinyl carbonate and vinyl carbonate themselves have a wide electrochemical stability window and good oxidation resistance. In addition, boron nitride nanosheets have high chemical stability, which further improves the stability of the electrolyte.
[0022] The quasi-solid electrolyte provided by the present invention has quasi-solid characteristics, and the liquid phase component improves the elasticity of the electrolyte, so that the quasi-solid system in which the organic skeleton and the liquid phase component coexist has good elasticity, thereby having higher elongation at break and deformation recovery ability, and thus has excellent mechanical properties, the elongation at break of stretching is greater than 200%, and it can be folded and twisted 180 degrees without damage; it has good processability and can be easily cut by ordinary knives; it has the ability of large-scale preparation, and its size can be changed according to the size of the molding mold.
[0023] The quasi-solid electrolyte provided by the present invention has high lithium ion conductivity and high lithium ion migration number, and the boron nitride nanosheets are helpful to construct a good electrolyte-electrode contact layer. A lithium nitride contact layer will be formed at the contact interface. Lithium nitride itself has high mechanical strength and high lithium ion conductivity, which helps to stabilize the surface of the lithium metal negative electrode to reduce side reactions, inhibit the growth of lithium dendrites to improve safety and cycle life, balance the surface charge distribution to avoid uneven deposition of lithium, and thus improve the electrical performance of the lithium battery: good cycle stability, in a lithium-lithium symmetrical battery, it can stably cycle for more than 5600 hours; good rate performance, can support the lithium iron phosphate electrode to be quickly charged and discharged at a rate of 2C, and the specific capacity is maintained at 100mAh g -1 Above; the capacity retention rate is high. After 120 cycles of the assembled lithium iron phosphate full battery, the capacity retention rate is as high as 96%.
[0024] The quasi-solid electrolyte provided by the present invention has excellent flame retardancy, can be ignited directly by a lighter, has the phenomenon of self-extinguishing, has improved stability to the fire source, and is beneficial to improving the safety of the battery. This is because the quasi-solid electrolyte provided by the present invention has quasi-solid characteristics, the organic skeleton is less likely to ignite than the liquid phase, and the boron nitride inorganic filler has high thermal stability and high thermal conductivity, which helps to evenly disperse local high heat, is non-flammable itself, and plays a decisive role in improving the flame retardancy of the electrolyte as a whole. Compared with a simple liquid phase component or a traditional organic electrolyte, it has significantly improved safety and stability, and has a higher ignition point.
[0025] The present invention uses boron nitride nanosheets as inorganic fillers, polyvinyl carbonate as an organic skeleton, and vinyl carbonate as a liquid phase component, and can obtain a high-performance quasi-solid electrolyte with good mechanical properties, appropriate flame retardancy, high lithium ion conductivity, high lithium ion migration number and a wide electrochemical working window, which is helpful to develop a solid electrolyte system that improves the actual performance of lithium batteries.
[0026] The results of the examples show that the boron nitride nanosheets used in the present invention are hexagonal (PDF#45-0894); the lithium ion conductivity of the quasi-solid electrolyte is 1.1 mS cm -1 , the lithium ion transfer number is 0.78, the electrochemical working window is 0-5V, the tensile elastic modulus is >7MPa, and the tensile elongation at break is >230%. BRIEF DESCRIPTION OF THE DRAWINGS
[0027] Figure 1 This is the XRD pattern of the boron nitride nanosheets used in Example 1;
[0028] Figure 2 This is the Raman spectrum of the boron nitride nanosheets used in Example 1;
[0029] Figure 3 TEM image of the boron nitride nanosheets used in Example 1;
[0030] Figure 4 50×50 mm obtained in Example 1 2 Photo of the quasi-solid electrolyte membrane (PVCA-BNNF QSE);
[0031] Figure 5 The original photo of the PVCA-BNNF QSE prepared in Example 1 and the photos under twisting, stretching and folding conditions;
[0032] Figure 6 This is a cross-sectional SEM image of the PVCA-BNNF QSE prepared in Example 1;
[0033] Figure 7 This is a photo of the PVCA-BNNF QSE prepared in Example 1 after being ignited by a lighter;
[0034] Figure 8 The electrochemical impedance spectroscopy of the PVCA-BNNF QSE prepared in Example 1;
[0035] Fig. 9 The transient current test results of the PVCA-BNNF QSE prepared in Example 1 are built-in as electrochemical impedance spectra before and after polarization;
[0036] Fig.10 This is the full cell performance diagram of the PVCA-BNNF QSE prepared in Example 1;
[0037] Fig.11 Electrochemical stability test diagram of PVCA-BNNF QSE prepared in Example 1 and PVCA QSE prepared in Comparative Example 1;
[0038] Fig.12 TEM image of the boron nitride nanosheets used in Example 2;
[0039] Fig.13 This is a digital photo of the PVCA-BNNF QSE prepared in Example 2;
[0040] Fig.14 The photos are of the PVCA-BNNF QSE prepared in Example 2 and the PVCA QSE prepared in Comparative Example 1 after being ignited with a lighter;
[0041] Fig.15 Voltage curves of the PVCA-BNNF QSE prepared in Example 2 and the PVCA QSE prepared in Comparative Example 1 at different current densities;
[0042] Fig.16 The symmetrical cell of PVCA-BNNF QSE prepared in Example 2 and PVCA QSE prepared in Comparative Example 1 was 0.5 mA cm -2 The current density and 0.5 mAh cm -2 Voltage curve under surface capacity;
[0043] Fig.17 The performance curve of the full battery assembled with PVCA-BNNF QSE, NCM811 and lithium sheet prepared in Example 2;
[0044] Fig.18 This is a digital picture of the PVCA-BNNF QSE prepared in Example 3 after folding;
[0045] Fig.19 Symmetrical battery cycle performance diagram of PVCA-BNNF QSE prepared in Example 3;
[0046] Fig. 20 The rate performance diagram of the PVCA-BNNF QSE prepared in Example 3 and the PVCA QSE prepared in Comparative Example 1 after being assembled into a full battery with a lithium iron phosphate pole piece and a lithium sheet;
[0047] Fig.21 The charge and discharge curves of the PVCA-BNNF QSE prepared in Example 3 and the PVCA QSE prepared in Comparative Example 1 at 0.1C after being assembled into full batteries with lithium iron phosphate;
[0048] Fig. 22 The stress-strain curve of the PVCA-BNNF QSE prepared in Example 3;
[0049] Fig.23 This is a picture of the PVCA QSE prepared in Comparative Example 1 being ignited by a direct lighter. DETAILED DESCRIPTION
[0050] The present invention provides a quasi-solid electrolyte, comprising polyvinylene carbonate, a liquid component and boron nitride nanosheets; the liquid component comprises vinylene carbonate and a lithium salt; the liquid component and the boron nitride nanosheets are dispersed in the framework of the polyvinylene carbonate.
[0051] In the present invention, unless otherwise specified, the required raw materials or reagents are commercially available products well known to those skilled in the art.
[0052] The quasi-solid electrolyte provided by the present invention comprises polyvinylene carbonate; the polyvinylene carbonate is formed by polymerization of vinylene carbonate, and the molecular weight of the polyvinylene carbonate is preferably 200,000 to 800,000, more preferably 400,000.
[0053] The quasi-solid electrolyte provided by the present invention includes a liquid component, and the liquid component includes vinylene carbonate and a lithium salt. In the present invention, the purity of the vinylene carbonate is preferably >96%; the lithium salt preferably includes lithium difluorooxalatoborate (LiODFB, purity >97%) or lithium perchlorate (LiClO4, purity >97%). In the present invention, the lithium salt is dissolved in vinylene carbonate to form a liquid component. In the present invention, the concentration of the liquid component (i.e., the concentration of the lithium salt in vinylene carbonate) is preferably 0.3 to 1.5 mol L -1 , more preferably 0.95 to 1 mol L -1 .
[0054] The quasi-solid electrolyte provided by the present invention includes boron nitride nanosheets. In the present invention, the boron nitride nanosheets are preferably hexagonal boron nitride (h-BN, purity>98%), and the particle size of the boron nitride nanosheets is preferably 20nm to 5000nm, more preferably 100nm to 1000nm. Hexagonal boron nitride has many excellent properties, including low density, high chemical stability, good thermal conductivity, non-flammability, good mechanical properties, etc., and has the potential to improve the interface of the electrolyte and the lithium ion transport in the electrolyte.
[0055] In the present invention, the quasi-solid electrolyte preferably includes 74.8-84.8wt% of polyvinyl carbonate, 15-25wt% of liquid component and 0.2-0.8wt% of boron nitride nanosheets, in terms of mass percentage. The polyvinyl carbonate is more preferably 71.8-87.8wt%, and further preferably 75.2-79.9wt%. The liquid component is preferably 12-24.2wt%, and more preferably 19.7-22.3wt%. The boron nitride nanosheets are 0.4-0.6wt%, and further preferably 0.5wt%.
[0056] The present invention provides a method for preparing the quasi-solid electrolyte described in the above technical solution, comprising the following steps:
[0057] mixing lithium salt, vinylene carbonate and boron nitride nanosheets to obtain a polymer precursor;
[0058] The polymerization precursor and the initiator are mixed and thermally polymerized to obtain a quasi-solid electrolyte.
[0059] The invention mixes lithium salt, vinylene carbonate and boron nitride nanosheets to obtain a polymerization precursor.
[0060] In the present invention, the mixing of the lithium salt, vinylene carbonate and boron nitride nanosheets preferably includes: first mixing the lithium salt and vinylene carbonate to obtain a liquid component; second mixing the liquid component and boron nitride nanosheets to obtain a polymer precursor. In the present invention, the first mixing is preferably carried out under stirring conditions, and the temperature of the first mixing is preferably 15 to 40°C, more preferably 25°C; the time is preferably 1 to 24 hours, more preferably 12 to 15 hours. The present invention does not have any special restrictions on the stirring rate, and the lithium salt can be completely dissolved according to the process well known in the art.
[0061] In the present invention, the ratio of the mass of the lithium salt to the volume of vinylene carbonate is preferably (0.4-1.7) g:(8-12) mL, more preferably (1.06-1.42) g:(10-12) mL, and further preferably 1.37 g:(10-12) mL; when the lithium salt is lithium difluorooxalatoborate, the ratio of the mass of the lithium salt to the volume of vinylene carbonate is preferably (0.5-1.7) g:(8-12) mL; more preferably 1.42 g:(8-12) mL; when the lithium salt is lithium perchlorate, the ratio of the mass of the lithium salt to the volume of vinylene carbonate is preferably (0.4-1.5) g:(8-12) mL; more preferably 1.06 g:(8-12) mL.
[0062] In the present invention, the ratio of the mass of the boron nitride nanosheets to the volume of the liquid component is preferably (18-25) mg:(3-4) mL, more preferably (20-22) mg:3.5 mL, and further preferably 21 mg:3.5 mL.
[0063] In the present invention, the temperature of the second mixing is preferably 15-40°C, more preferably 25°C; the time is preferably 1-10 hours, more preferably 2-4 hours; the second mixing is preferably carried out under ultrasonic conditions; the present invention preferably adjusts the time of the second mixing according to the mass and particle size of the boron nitride nanosheets so that the boron nitride nanosheets are uniformly dispersed. The present invention has no special restrictions on the ultrasonic conditions, and the boron nitride nanosheets can be uniformly dispersed according to the process well known in the art.
[0064] After obtaining the polymer precursor, the present invention mixes the polymer precursor and an initiator, performs thermal polymerization, and obtains a quasi-solid electrolyte. In the present invention, the initiator preferably includes azobisisobutyronitrile (AIBN, purity>99%), and the ratio of the mass of the initiator to the volume of the polymer precursor is preferably (6-8.5) mg:3.5 mL, more preferably (7.2-7.7) mg:3.5 mL, and further preferably 7.5 mg:3.5 mL.
[0065] In the present invention, the polymerization precursor and the initiator are preferably mixed by adding the initiator to the polymerization precursor and ultrasonicating for 10 minutes to 1 hour until the initiator is completely dissolved. The present invention has no particular limitation on the ultrasonic conditions, and the initiator can be completely dissolved according to the process well known in the art.
[0066] After the mixing is completed, the present invention preferably adds the obtained mixed solution into a polytetrafluoroethylene mold, places the mold under pressure conditions, and performs thermal polymerization. The present invention has no special limitation on the polytetrafluoroethylene mold and its size, which can be selected according to actual needs; in the embodiment of the present invention, the size of the polytetrafluoroethylene mold is specifically 5cm×5cm×0.1cm.
[0067] In the present invention, the pressure of the thermal polymerization is preferably 30-50 kPa, more preferably 35-40 kPa, and further preferably 37-38 kPa; the temperature is preferably 55-65°C, more preferably 58-60°C; the time is preferably 700-900 min, more preferably 850-860 min. The method of applying the pressure in the present invention is not particularly limited, and any method known in the art that can achieve the above pressure can be used.
[0068] During the thermal polymerization process, vinylene carbonate monomers are polymerized to form a polyvinylene carbonate polymer skeleton, and the liquid component and the boron nitride nanosheets are physically mixed in the polyvinylene carbonate polymer skeleton.
[0069] After the thermal polymerization is completed, the present invention preferably cools the obtained product naturally to room temperature, and after demolding, obtains a quasi-solid electrolyte; the quasi-solid electrolyte is in the form of a film. The present invention has no special limitation on the demolding process, and it can be carried out according to a process well known in the art.
[0070] The present invention provides the use of the quasi-solid electrolyte described in the above technical solution or the quasi-solid electrolyte prepared by the preparation method described in the above technical solution in a lithium battery. The present invention has no special limitation on the method of the application, and the application can be carried out according to methods well known in the art.
[0071] The technical solutions in the present invention will be described clearly and completely below in conjunction with the embodiments of the present invention. Obviously, the described embodiments are only a part of the embodiments of the present invention, not all of them. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0072] Example 1
[0073] The composition of the quasi-solid electrolyte membrane: 77.2wt% polyvinylene carbonate (molecular weight is about 420,000), 22.3wt% liquid component and 0.5wt% boron nitride nanosheets;
[0074] At room temperature (25°C), 1.37 g of lithium difluorooxalatoborate (LiODFB, purity > 97%) was added to 10 mL of vinylene carbonate monomer (purity > 96%) liquid and stirred for 12 h to obtain a concentration of 0.95 mol L -1 A monomer-lithium salt solution;
[0075] At room temperature (25°C), 22 mg of boron nitride nanosheets (h-BN, purity >98%, particle size 100 nm) were added to 3.5 mL of monomer-lithium salt solution and ultrasonically dispersed for 2 h to obtain a polymerization precursor;
[0076] 7.5 mg of azobisisobutyronitrile (AIBN, purity>99%) was added to the polymerization precursor and ultrasonically dissolved for 10 minutes. 3 mL of the obtained solution was added to a 5 cm×5 cm×0.1 cm polytetrafluoroethylene mold. The mold was placed in an environment with a pressure of 40 kPa and a temperature of 60°C, kept warm for 850 minutes, and naturally cooled to room temperature. After demolding, a quasi-solid electrolyte membrane was obtained, which was recorded as PVCA-BNNF QSE.
[0077] Example 2
[0078] The composition of the quasi-solid electrolyte membrane: 75.2wt% polyvinylene carbonate (molecular weight about 370,000), 24.2wt% liquid component and 0.6wt% boron nitride nanosheets;
[0079] At room temperature (25°C), add 1.06 g of lithium perchlorate (LiClO4, purity> 97%) to 10 mL of vinylene carbonate monomer (purity> 96%) liquid and stir for 15 h to obtain a concentration of 1 mol L -1 A monomer-lithium salt solution;
[0080] At room temperature (25°C), 21 mg of boron nitride nanosheets (h-BN, purity >98%, particle size 100 nm) were added to 3.5 mL of monomer-lithium salt solution and ultrasonically dispersed for 4 h to obtain a polymer precursor;
[0081] 7.7 mg of azobisisobutyronitrile (AIBN, purity>99%) was added to the polymerization precursor and ultrasonically dissolved for 10 minutes. 3.1 mL of the obtained solution was added to a 5 cm×5 cm×0.1 cm polytetrafluoroethylene mold. The mold was placed in an environment with a pressure of 35 kPa and a temperature of 60°C, kept warm for 850 minutes, naturally cooled to room temperature, and demolded to obtain a quasi-solid electrolyte membrane PVCA-BNNF QSE.
[0082] Example 3
[0083] The composition of the quasi-solid electrolyte membrane: 79.9wt% polyvinylene carbonate (molecular weight about 480,000), 19.7wt% liquid component and 0.4wt% boron nitride nanosheets;
[0084] At room temperature (25°C), 1.42 g of lithium difluorooxalatoborate (LiODFB, purity > 97%) was added to 10 mL of vinylene carbonate monomer (purity > 96%) liquid and stirred for 15 h to obtain a concentration of 1 mol L -1 A monomer-lithium salt solution;
[0085] At room temperature (25°C), 20 mg of boron nitride nanosheets (h-BN, purity >98%, particle size 100 nm) were added to 3.5 mL of monomer-lithium salt solution and ultrasonically dispersed for 4 h to obtain a polymerization precursor;
[0086] 7.2 mg of azobisisobutyronitrile (AIBN, purity>99%) was added to the polymerization precursor and ultrasonically dissolved for 10 minutes. 3 mL of the resulting solution was added to a 5 cm×5 cm×0.1 cm polytetrafluoroethylene mold. The mold was placed in an environment with a pressure of 37 kPa and a temperature of 58°C, kept warm for 860 minutes, naturally cooled to room temperature, and demolded to obtain a quasi-solid electrolyte membrane PVCA-BNNF QSE.
[0087] Comparative Example 1
[0088] The composition of the quasi-solid electrolyte membrane: 76.4wt% polyvinylene carbonate (molecular weight about 400,000), 23.6wt% liquid component;
[0089] At room temperature (25°C), 1.43 g of lithium difluorooxalatoborate (LiODFB, purity > 97%) was added to 10 mL of vinylene carbonate monomer (purity > 96%) liquid and stirred for 15 h to obtain a concentration of 1 mol L -1 A monomer-lithium salt solution;
[0090] 7.5 mg of azobisisobutyronitrile (AIBN, purity>99%) was added to the monomer-lithium salt solution and dissolved by ultrasound for 10 min. 3 mL of the obtained solution was added to a 5 cm×5 cm×0.1 cm polytetrafluoroethylene mold. The mold was placed in an environment with a pressure of 35 kPa and a temperature of 60°C, kept warm for 850 minutes, and then naturally cooled to room temperature. After demolding, a quasi-solid electrolyte membrane was obtained, which was recorded as PVCA QSE.
[0091] Characterization and performance testing
[0092] In the following test process, when assembling the battery, the C2032 button battery was assembled in a glove box, and the glove box was filled with argon gas so that the water and oxygen contents were less than 0.1 ppm.
[0093] 1) XRD test was performed on the boron nitride nanosheets used in Example 1, and the obtained spectrum is shown in Figure 1 ;Depend on Figure 1 It can be seen that the boron nitride nanosheets are hexagonal boron nitride with high purity and good crystallinity.
[0094] 2) The boron nitride nanosheets used in Example 1 were subjected to Raman testing, and the resulting spectrum is shown in Figure 2 ;Depend on Figure 2 It can be seen that at 1370cm -1 The peak at shows that the boron nitride nanosheets are hexagonal boron nitride, with fewer layers and thinner overall.
[0095] 3) The boron nitride nanosheets used in Example 1 were subjected to TEM testing, and the resulting spectrum is shown in Figure 3 ;Depend on Figure 3 It can be seen that the boron nitride nanosheets present a thin flake morphology, and the diameter of the boron nitride nanosheets is about 100 nm.
[0096] 4) Figure 4 50×50 mm obtained in Example 1 2 Photo of the quasi-solid electrolyte membrane (PVCA-BNNF QSE), Figure 4 The inset in the upper right corner is a SEM image of the upper surface of the quasi-solid electrolyte membrane. Figure 4 It can be seen that the prepared quasi-solid electrolyte membrane has high overall uniformity, a smooth surface and clear edges, indicating good formability.
[0097] 5) Figure 5 The original photo of PVCA-BNNF QSE prepared in Example 1 and the photos under twisting, stretching and folding conditions are shown in Figure 1. Figure 5 It can be seen that the quasi-solid electrolyte has high bending and stretching capabilities, strong processability, has the potential to be used in flexible electronic devices, and is easy to produce and transfer.
[0098] 6) Figure 6 This is a cross-sectional SEM image of the PVCA-BNNF QSE prepared in Example 1. Figure 6 It can be seen that the thickness of the quasi-solid electrolyte is about 500 microns, and the thickness is relatively uniform.
[0099] 7) Figure 7 This is a photo of the PVCA-BNNF QSE prepared in Example 1 after being ignited by a lighter; Figure 7It can be seen that the flame automatically extinguished within 0.2 seconds, proving that the quasi-solid electrolyte has self-extinguishing and good flame retardancy, confirming its high safety. This is because the boron nitride nanosheets BNNF themselves have good thermal conductivity and thermal stability.
[0100] 8) The PVCA-BNNF QSE prepared in Example 1 was assembled into a blocking cell, stainless steel gaskets were placed on both sides of the quasi-solid electrolyte membrane, and an AC impedance test was performed. The obtained spectrum is shown in Figure 8 ,Depend on Figure 8 Calculation shows that the lithium ion conductivity of PVCA-BNNF QSE at room temperature (25°C) is 1.1 mS cm -1 .
[0101] 9) A lithium sheet was placed on one side of the PVCA-BNNF QSE prepared in Example 1 and a stainless steel gasket was placed on the other side. The lithium ion migration number was measured using the transient current method. The results are shown in Fig. 9 ; Fig. 9 The middle inset is the electrochemical impedance spectrum of the corresponding battery before and after polarization; the lithium ion migration number of PVCA-BNNF QSE measured by transient current method is 0.78, which is greater than the lithium ion migration number in conventional liquid electrolyte (<0.5), which is due to the addition of boron nitride nanosheets. The larger the lithium ion migration number, the more stable the performance.
[0102] 10) The PVCA-BNNF QSE electrolyte membrane prepared in Example 1 was matched with a lithium metal negative electrode and a lithium iron phosphate positive electrode, respectively, wherein the surface capacity density of the lithium iron phosphate positive electrode was 2 mAh cm -2 Then, the Xinwei battery test system is used to perform constant current charge and discharge tests on the battery within the matching test voltage range and at different charge and discharge rates to test the full battery performance. The results are shown in Fig.10 ;Depend on Fig.10 It can be seen that at a current density of 0.1C, it can be stably cycled for 100 cycles with a capacity retention rate of up to 96.8%, showing excellent cycle stability.
[0103] 11) The electrochemical stability test of the PVCA-BNNF QSE prepared in Example 1 and the PVCA QSE prepared in Comparative Example 1 was carried out by linear sweep voltammetry with a scan rate of 1 mV / s and a voltage range of 0 to 6.3 V. The results are shown in Fig.11 ;Depend on Fig.11 It can be seen that the electrochemical working windows of both are greater than 5 V, and after the addition of boron nitride nanosheets, the ability of PVCA-BNNF QSE to resist electrochemical oxidation is improved to a certain extent.
[0104] 12) Fig.12 TEM image of the boron nitride nanosheets used in Example 2. Fig.12 The measured interplanar spacing of the (002) crystal plane is 0.34 nm, which is consistent with the parameters of hexagonal boron nitride. Moreover, a single nanosheet is composed of only four layers of hexagonal boron nitride, confirming that it has thin-sheet properties.
[0105] 13) Fig.13 This is a digital photo of the PVCA-BNNF QSE electrolyte prepared in Example 2, showing clear edges, a size of up to 50 mm×50 mm, and uniform dispersion of the inorganic filler.
[0106] 14) Fig.14 The PVCA-BNNF QSE prepared in Example 2 and the PVCA QSE prepared in Comparative Example 1 were ignited with a lighter; Fig.14 It can be seen that PVCA-BNNF QSE was not ignited, but PVCA was ignited and continued to burn, indicating that the flame retardant properties of the electrolyte were significantly improved after the addition of boron nitride nanosheets.
[0107] 15) Fig.15 The voltage curves of the PVCA-BNNF QSE prepared in Example 2 and the PVCA QSE prepared in Comparative Example 1 at different current densities. Fig.15 It can be seen that at the same low current density, PVCA exhibits a higher overpotential; with the increase of current density, PVC at 3 mA cm -2 Around, the voltage value overflows, while the PVCA-BNNF QSE is at 5mA cm -2 At a current density of 1.5 volts, the overpotential is still maintained at no more than 2 V, and the cycle is stable. This result shows that after adding boron nitride nanosheets, PVCA-BNNF QSE has strong lithium ion transmission ability and high rate charge and discharge capability.
[0108] 16) Lithium sheets were placed on both sides of the PVCA-BNNF QSE prepared in Example 2 and the PVCA QSE prepared in Comparative Example 1 to assemble into symmetrical batteries; Fig.16 The symmetrical cell of PVCA-BNNF QSE prepared in Example 2 and PVCA QSE prepared in Comparative Example 1 was 0.5 mA cm -2 The current density and 0.5 mAh cm -2 The voltage curve under the surface capacity. Fig.16 It can be seen that the PVCA QSE symmetric battery fails after about 500 hours of cycling, while the PVCA-BNNF QSE can be stably cycled for more than 1800 hours with an overpotential not exceeding 0.4 V, reflecting the excellent cycling stability of PVCA-BNNF QSE for large currents and large capacities.
[0109] 17) Fig.17This is the performance curve of the full battery assembled with PVCA-BNNF QSE, NCM811 and lithium sheet prepared in Example 2. Fig.17 It can be seen that at high capacity (3 mAh cm -2 ) after being matched with the high-nickel positive electrode NCM811, the PVCA-BNNF QSE electrolyte still performed stably, indicating that it can work normally in the high voltage range (4V-5V), reflecting its good compatibility with the two mainstream types of lithium battery positive electrodes and great potential application prospects.
[0110] 18) Fig.18 This is a digital picture of the PVCA-BNNF QSE prepared in Example 3 after folding, showing good flexibility and processability.
[0111] 19) Fig.19 This is the symmetrical battery cycle performance diagram of the PVCA-BNNF QSE prepared in Example 3. Fig.19 It can be seen that at 0.1 mA cm -2 The current density and 0.1 mAh cm -2 At the surface capacity of 100 MW, PVCA-BNNF QSE can be stably cycled for more than 5600 hours. In addition, high-rate tests were added during the cycling process. When the current density was increased to 1 mA cm -2 Then it is reduced to 0.1mAcm -2 After the reaction, it can still maintain a low overpotential for more than 2500 h, and the overpotential does not exceed 0.2 V. This proves the excellent cycling stability and high rate performance of PVCA-BNNF QSE.
[0112] 20) Fig. 20 The rate performance test of the PVCA-BNNF QSE prepared in Example 3 and the PVCAQSE prepared in Comparative Example 1 after being assembled with lithium iron phosphate pole pieces and lithium sheets into full batteries. Fig. 20 It can be seen that PVCA-BNNF QSE can support better capacity release at all rates compared with PVCA without adding boron nitride nanosheets. When the charge and discharge rate increases, the capacity retention rate of PVCA-BNNF QSE is higher, and it can still be maintained above 100mAh g-1 at 2C, reflecting good fast charging and discharging potential.
[0113] twenty one) Fig.21 The charge and discharge curves of the PVCA-BNNF QSE prepared in Example 3 and the PVCA QSE prepared in Comparative Example 1 at 0.1C after being assembled into a full battery with lithium iron phosphate. Fig.21It can be seen that PVCA-BNNF QSE has a flat platform, which proves that the reaction process is good and there are few side reactions. At the same time, the voltage difference of PVCA-BNNF QSE between the charge and discharge curve platforms is significantly smaller than that of PVCA, which proves that PVCA-BNNF QSE has a higher lithium ion transmission capacity.
[0114] twenty two) Fig. 22 The stress-strain curve of PVCA-BNNF QSE prepared in Example 3 is shown in Figure 2. Fig. 22 It can be concluded that the prepared PVCA-BNNF QSE has a high tensile modulus of 7.3 MPa and an elongation at break of 230%, reflecting good device performance and processability.
[0115] twenty three) Fig.23 This is a picture of the PVCA QSE direct lighter ignited by the comparative example 1. Fig.23 It can be seen that after it comes into contact with the flame, it continues to burn until it is completely burned, reflecting its flammability, which reflects that the flame retardancy of PVCA-BNNFQSE is greatly improved after the addition of boron nitride nanosheets.
[0116] The above is only a preferred embodiment of the present invention. It should be pointed out that for ordinary technicians in this technical field, several improvements and modifications can be made without departing from the principle of the present invention. These improvements and modifications should also be regarded as the scope of protection of the present invention.
Claims
1. A quasi-solid electrolyte, It is characterized in that It includes polyvinylene carbonate, liquid components and boron nitride nanosheets; the liquid components include vinylene carbonate and lithium salt; the liquid components and boron nitride nanosheets are dispersed in the framework of the polyvinylene carbonate; The method for preparing the quasi-solid electrolyte comprises the following steps: mixing lithium salt, vinylene carbonate and boron nitride nanosheets to obtain a polymer precursor; The polymerization precursor and the initiator are mixed and thermally polymerized to obtain a quasi-solid electrolyte.
2. The quasi-solid electrolyte according to claim 1, It is characterized in that Calculated by mass percentage, the quasi-solid electrolyte comprises 74.8-84.8wt% of polyvinylene carbonate, 15-25wt% of liquid components and 0.2-0.8wt% of boron nitride nanosheets.
3. The quasi-solid electrolyte according to claim 1, It is characterized in that The boron nitride nanosheet is hexagonal boron nitride, and the particle size of the boron nitride nanosheet is 20nm-5000nm.
4. The quasi-solid electrolyte according to claim 1, It is characterized in that The lithium salt includes lithium difluorooxalatoborate or lithium perchlorate.
5. A method for preparing the quasi-solid electrolyte according to any one of claims 1 to 4, It is characterized in that The following steps are involved: mixing lithium salt, vinylene carbonate and boron nitride nanosheets to obtain a polymer precursor; The polymerization precursor and the initiator are mixed and thermally polymerized to obtain a quasi-solid electrolyte.
6. The preparation method according to claim 5, It is characterized in that The mixing of the lithium salt, vinylene carbonate and boron nitride nanosheets comprises: first mixing the lithium salt and vinylene carbonate to obtain a liquid component; and second mixing the liquid component and the boron nitride nanosheets to obtain a polymer precursor.
7. The preparation method according to claim 6, It is characterized in that The ratio of the mass of the lithium salt to the volume of vinylene carbonate is (0.4-1.7) g: (8-12) mL; the ratio of the mass of the boron nitride nanosheets to the volume of the liquid component is (18-25) mg: (3-4) mL.
8. The preparation method according to claim 5, It is characterized in that The initiator includes azobisisobutyronitrile, and the ratio of the mass of the initiator to the volume of the polymerization precursor is (6-8.5) mg:3.5 mL.
9. The preparation method according to claim 5, It is characterized in that The thermal polymerization pressure is 30-50 kPa, the temperature is 55-65° C., and the time is 700-900 min.
10. Use of the quasi-solid electrolyte according to any one of claims 1 to 4 or the quasi-solid electrolyte prepared by the preparation method according to any one of claims 5 to 9 in a lithium battery.
Citation Information
Patent Citations
Polymer-based solid electrolyte with high room-temperature ionic conductance as well as preparation method and application thereof
CN112436188A
Polymer composite solid electrolyte and preparation method and application thereof
CN113381065A
Battery, electrolyte layer, battery pack, electronic apparatus, electric vehicle, power storage device, and electric power system
US20160043429A1
Lithium metal secondary battery containing an electrochemically stable anode-protecting layer
US20190393495A1
Electrolyte functional additive for lithium ion battery, lithium ion battery electrolyte and lithium ion battery
WO2021243953A1