Production equipment for melt-coated lithium metal / lithium alloy composite strip
By setting up feeding devices and cold air channels in the metal lithium/lithium alloy composite belt production equipment, we block molten metal from contacting with metal foil and control the temperature of the cooling and molding area, we solve the problem of metal foil breaking and forming quality, and improve the product tensile strength and safety.
Patent Information
- Application Number
- CN202110334443.4
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2021-03-29
- Publication Date
- 2024-11-22
- Estimated Expiration
- 2041-03-29
AI Technical Summary
When the existing composite metal belt continuous production equipment is used to produce metal lithium/lithium alloy composite belts, the metal foil is easily pulled out, and the cooling time and temperature in the cooling zone affect the forming quality, resulting in lithium dendrites growth and cracks, affecting storage. Safety of equipment.
A melt-coated metal lithium/lithium alloy composite belt production equipment is designed. By setting a feeding device and a cold air passage on the feed side of the control roller group, a melt-coated composite area and a cooling shaping area are formed, and an inner baffle and an outer baffle are used. It prevents the direct contact between the molten metal and the metal foil, destroys the surface tension of the molten metal, and controls the temperature and time of the cooling shaping area through the cooling medium to reduce the friction force of the tension balance roller group.
It effectively avoids the metal foil being pulled out, improves the equipment stability and product quality, ensures the tensile strength and molding quality of the metal lithium/lithium alloy composite belt, and avoids the emergence of cracks and lithium dendrites.
Smart Images

Figure CN115138824B_ABST
Abstract
Description
Technical Field
[0001] The invention relates to a metal strip production device, in particular to a melt-coated metal lithium / lithium alloy composite strip production device. Background Art
[0002] A Chinese patent application with publication number CN111822662A discloses a continuous production device for composite metal strips, comprising: an unwinding mechanism: for continuously unwinding a substrate; an extrusion molding device: for extruding a metal layer on at least one side of the substrate and obtaining a composite metal strip; a winding mechanism: for winding the prepared composite metal strip; the extrusion molding device comprises an extrusion roller group, the extrusion roller group comprises two extrusion rollers whose axes are parallel to each other; a feeding device for adding molten metal material is provided on the feed side of the two extrusion rollers; a high-temperature zone for keeping the molten metal material in a molten state is provided on the feed side of the extrusion roller group, and a cooling zone for cooling and shaping the composite metal strip is provided on the discharge side of the extrusion roller group; a guide mechanism for allowing the substrate to pass through between the two extrusion rollers is provided between the unwinding mechanism and the winding mechanism.
[0003] Although the composite metal strip continuous production equipment can meet the continuous production requirements of the composite metal strip to a certain extent, it still has the following problems when used to produce metal lithium / lithium alloy composite strips:
[0004] 1. Lithium metal / lithium alloy composite tape is generally used as the electrode of energy storage equipment, and its thickness is strictly controlled; specifically, the thickness of metal foil is generally 6um, and the melting point of lithium metal is 180℃. To achieve the technical purpose of making molten lithium metal or molten lithium alloy flow through two extrusion rollers, the molten lithium metal or molten lithium alloy must have a certain fluidity, and its temperature must be at least 200℃. The molten lithium metal or lithium alloy is in contact with the metal foil for a long time, which causes the metal foil to heat up and reduce its tensile strength. In addition, in the continuous production equipment of the composite metal tape, the tension of the metal foil when passing through the two extrusion rollers is relatively large, which can easily break the metal foil, resulting in production interruption;
[0005] 2. The cooling time and cooling temperature in the cooling zone affect the forming quality of the metal lithium / lithium alloy composite belt. In the continuous production equipment of the composite metal belt, if the cooling time of the metal lithium / lithium alloy composite belt in the cooling zone is too long, cracks will be generated in the metal lithium layer or the lithium alloy layer. The existence of cracks will easily lead to the growth of lithium dendrites, affecting the safety of the energy storage equipment.
[0006] 3. The molten lithium metal or molten lithium alloy droplets have a strong surface tension. It is impossible to coat the molten lithium metal or molten lithium alloy onto the metal foil simply by using an extrusion roller, that is, the quality of the produced lithium metal / lithium alloy composite strip cannot be guaranteed. Summary of the invention
[0007] In view of this, the object of the present invention is to provide a production device for melt-coated metal lithium / lithium alloy composite strips, which can prevent the metal foil from being broken and improve the stability of the equipment.
[0008] In order to achieve the above object, the present invention provides the following technical solutions:
[0009] A production device for melt-coated lithium metal / lithium alloy composite strip, comprising:
[0010] Unwinding mechanism: used for continuously unwinding metal foil;
[0011] Melt coating composite forming device: used for melt coating and composite forming of a metal lithium layer or a lithium alloy layer on at least one side of a metal foil to obtain a metal lithium / lithium alloy composite strip;
[0012] Winding mechanism: used for winding the prepared metal lithium / lithium alloy composite strip;
[0013] The melt-coating composite forming device comprises a control roller group for controlling the thickness of the melt-coated composite lithium metal layer or lithium alloy layer, wherein the control roller group comprises two control rollers whose axes are parallel to each other;
[0014] The feeding side of the two control rollers is provided with a feeding device for adding molten metal lithium or molten lithium alloy, and the discharging side is provided with a cooling zone for cooling and shaping the metal lithium / lithium alloy composite belt;
[0015] The feeding device includes a feeding channel, and the feeding channel includes an upper inner baffle plate arranged close to the metal foil and an upper outer baffle plate located on the side of the upper inner baffle plate facing away from the metal foil. A melt-coating composite zone is formed below the feeding channel and between the metal foil and the corresponding control roller. A melt-coating composite roller is provided in the melt-coating composite zone for destroying the surface tension of molten lithium metal or molten lithium alloy and compounding the molten lithium metal or molten lithium alloy with the metal foil.
[0016] Furthermore, a cold air channel is provided in the cooling zone, and the cold air channel includes a lower inner baffle plate arranged close to the metal foil and a lower outer baffle plate located on the side of the lower inner baffle plate facing away from the metal foil. A cooling and molding zone is formed above the cold air channel and between the metal lithium / lithium alloy composite strip and the corresponding control roller. The cooling medium blown in through the cold air channel reaches the cooling and molding zone and cools and molds the metal lithium / lithium alloy composite strip.
[0017] Furthermore, a roll gap adjusting mechanism for adjusting the roll gap is provided between the two control rolls.
[0018] Furthermore, the distance between the melt-coated composite roller and the metal foil is adjustable.
[0019] Furthermore, the melt-coated composite roller is a brush roller or a scraper roller.
[0020] Furthermore, when the metal foil is always in contact with one of the control rollers, the feeding channel is provided as one and is located on the side of the metal foil facing the other control roller.
[0021] Furthermore, the melt coating composite roller is provided as one and is located in the melt coating composite zone, and a pressure roller is provided on the side of the metal foil material facing away from the melt coating composite zone corresponding to the melt coating composite roller.
[0022] Furthermore, when a melting coating gap is provided between the metal foil and the two control rollers respectively, the feeding channels are provided in two and are respectively located on two sides of the metal foil.
[0023] Furthermore, the number of the melt-coated composite rollers is two and they are respectively arranged on two sides of the metal foil.
[0024] Furthermore, an overflow trough is provided in the feeding channel, and an overflow port is provided in the overflow trough for allowing the molten metal lithium or the molten lithium alloy to overflow to the corresponding melt-coated composite roller.
[0025] Furthermore, a guide plate extending into the cooling and molding area is provided in the cold air channel, and the guide plate divides the cold air channel into an air inlet channel and an air outlet channel, and the air inlet channel and the air outlet channel are connected through the cooling and molding area.
[0026] Furthermore, it also includes a control roller heating device for heating the control roller; the control roller heating device uses a heating element arranged in the control roller; or, the control roller heating device uses an eddy current heating device or a radiation heating device for heating the surface of the control roller, and the control roller heating device is arranged between the upper outer baffle plate and the lower outer baffle plate.
[0027] Furthermore, it also includes a scraper for scraping off the molten metal lithium or molten lithium alloy attached to the control roller; a collection box is provided below the scraper.
[0028] Furthermore, it also includes two groups of tension balancing roller groups. Among the two groups of tension balancing roller groups, one group of the tension balancing roller groups is arranged on the side of the melt-coating composite zone facing away from the cooling and forming zone and is used to apply a friction force to the metal foil to balance its tension, and the other group of the tension balancing roller groups is arranged on the side of the cooling and forming zone facing away from the melt-coating composite zone and is used to apply a friction force to the metal lithium / lithium alloy composite strip to balance its tension.
[0029] Furthermore, at least one thickness control section for controlling the thickness of the metal lithium layer or the lithium alloy layer is provided between the cooling and shaping section and the winding mechanism, and the thickness control section includes a thickness control area, and the thickness control area is provided with thickness control rollers respectively located on both sides of the metal lithium / lithium alloy composite strip;
[0030] The thickness control zone is divided into a first temperature zone and a second temperature zone with the metal lithium / lithium alloy composite belt as the interface; when controlling the thickness of the metal lithium layer or the lithium alloy layer facing the first temperature zone, the first temperature zone is set as a high temperature zone and the second temperature zone is set as a low temperature zone; when controlling the thickness of the metal lithium layer or the lithium alloy layer facing the second temperature zone, the second temperature zone is set as a high temperature zone and the first temperature zone is set as a low temperature zone; the temperature in the high temperature zone is higher than the temperature in the low temperature zone, and a roller heating device for heating the corresponding thickness control roller is provided in the high temperature zone.
[0031] Furthermore, the roller heating device adopts a heating element arranged in the thickness control roller; or, the roller heating device adopts an eddy current heating device or a radiation heating device for heating the surface of the thickness control roller, and a rolling insulation plate is provided between the roller heating device and the metal lithium / lithium alloy composite strip.
[0032] Furthermore, the thickness control section also includes a temperature control transition zone located in front of the thickness control zone.
[0033] Furthermore, a heat preservation section is provided between the thickness control section and the cooling and shaping area.
[0034] Furthermore, a finishing section for finishing the metal lithium / lithium alloy composite strip is provided between the thickness control section and the winding mechanism.
[0035] Furthermore, at least one finishing zone is provided in the finishing section, and finishing rollers are provided in the finishing zone respectively located on both sides of the metal lithium / lithium alloy composite belt, and finishing heating devices are also provided in the finishing zone respectively located on both sides of the metal lithium / lithium alloy composite belt and used to heat the corresponding finishing rollers.
[0036] Furthermore, the finishing roller in the finishing zone at the rear end is a surface finishing roller used to control the surface finish of the metal lithium / lithium alloy composite strip.
[0037] Furthermore, the finishing heating device adopts a heating element arranged in the finishing roller; or, the finishing heating device adopts an eddy current heating device or a radiation heating device for heating the surface of the finishing roller, and a finishing insulation plate is provided between the finishing heating device and the metal lithium / lithium alloy composite strip.
[0038] Furthermore, a tempering section for eliminating the internal stress of the metal lithium / lithium alloy composite strip is provided between the finishing section and the winding mechanism.
[0039] Furthermore, a covering film laminating mechanism for laminating covering films on both side edges of the metal foil is provided between the unwinding mechanism and the feeding channel.
[0040] Furthermore, a covering film winding mechanism is provided in front of the winding mechanism, and the covering film winding mechanism comprises a knife roller, and a cutting knife facing the inner edge of the covering film is provided on the knife roller.
[0041] Furthermore, a strip sticking mechanism for sticking covering strips at intervals on the metal foil is provided between the unwinding mechanism and the feeding channel; or, a covering film sticking mechanism for sticking a covering film on the metal foil and a covering film winding mechanism for peeling the covering film off the metal foil so that the covering strips arranged at intervals on the covering film are stuck to the metal foil are provided between the unwinding mechanism and the feeding channel.
[0042] Furthermore, a brush roller mechanism for brushing molten metal lithium or molten lithium alloy on the metal foil is provided between the unwinding mechanism and the feeding channel.
[0043] Furthermore, a membrane winding composite mechanism for compositely winding a membrane on the surface of the metal lithium / lithium alloy composite belt is provided in front of the winding mechanism.
[0044] Furthermore, the upper inner baffle and the lower inner baffle are made of insulation boards, the upper outer baffle is made of insulation boards or plates made of temperature-resistant materials; and the lower outer baffle is made of insulation boards or plates made of low-temperature-resistant materials.
[0045] Furthermore, the metal foil is copper foil, aluminum foil, steel foil, nickel foil, silver foil or gold foil.
[0046] Furthermore, the feeding sides of the two control rollers are provided with clamping mechanisms for clamping the edges of both ends of the metal foil respectively, and the clamping mechanisms include clamping grooves, and sealing strips are respectively provided between the two side walls of the clamping groove and the metal foil.
[0047] Furthermore, the clamping plate mechanism includes two clamping plates, the clamping groove is formed between the two clamping plates, and a clamping adjustment mechanism for controlling the clamping force between the sealing strip and the metal foil is provided between the two clamping plates.
[0048] Furthermore, a side surface of the clamping plate close to the control roller is configured as an arc-shaped surface matching the control roller.
[0049] The beneficial effects of the present invention are:
[0050] The melt-coated metal lithium / lithium alloy composite belt production equipment of the present invention provides a feeding device on the feed side of the control roller group, and provides a feeding channel in the feeding device and forms a melt-coated composite zone between the metal foil and the corresponding control roller below the feeding channel. The upper inner baffle plate can prevent the molten metal lithium or the molten lithium alloy from directly contacting the metal foil, so that the molten metal lithium or the molten lithium alloy contacts the metal foil only in the melt-coated composite zone, thereby reducing the contact time between the metal foil and the high-temperature molten metal lithium or the molten lithium alloy, so as to avoid the problem that the tensile strength of the metal foil is reduced and it is pulled apart due to the long-term contact between the metal foil and the molten metal lithium or the molten lithium alloy; the surface tension of the molten metal lithium or the molten lithium alloy is destroyed by providing a melt-coated composite roller, so that the molten metal lithium or the molten lithium alloy can be better coated on the metal foil, thereby improving the production quality of the metal lithium / lithium alloy composite belt.
[0051] By arranging a cold air channel on the discharge side of the control roller group, and forming a cooling and shaping zone between the metal lithium / lithium alloy composite belt and the corresponding control roller above the cold air channel, the cooling medium contacts the metal lithium / lithium alloy composite belt only in the cooling and shaping zone to cool and shape it, thereby controlling the cooling and shaping temperature and time of the metal lithium / lithium alloy composite belt, avoiding defects such as cracks in the metal lithium layer or the lithium alloy layer, and improving product quality.
[0052] By arranging tension balancing roller groups on the opposite sides of the melt coating composite zone and the cooling and forming zone, respectively, the tension balancing roller group located on the side of the melt coating composite zone facing away from the cooling and forming zone applies friction force to the metal foil and is used to balance the tension required for unwinding the metal foil; the tension balancing roller group located on the side of the cooling and forming zone facing away from the melt coating composite zone applies friction force to the metal foil and is used to balance the tension required for subsequent winding of the metal lithium / lithium alloy composite strip; in this way, the tension of the metal foil and the metal lithium / lithium alloy composite strip between the two groups of tension balancing roller groups can be reduced, thereby preventing the metal foil from being broken. BRIEF DESCRIPTION OF THE DRAWINGS
[0053] In order to make the purpose, technical solution and beneficial effects of the present invention clearer, the present invention provides the following drawings for illustration:
[0054] Figure 1 This is a schematic structural diagram of Embodiment 1 of the production equipment for melt-coated lithium metal / lithium alloy composite strips of the present invention;
[0055] Figure 2 for Figure 1 Detailed drawing A;
[0056] Figure 3 for Figure 2 Detail B of
[0057] Figure 4 for Figure 1Detailed drawing C;
[0058] Figure 5 It is a structural schematic diagram when a covering film laminating mechanism is provided;
[0059] Figure 6 It is a schematic diagram of the structure after the masking film is attached to the two side edges of the metal foil;
[0060] Figure 7 It is a structural schematic diagram when a strip sticking mechanism is provided;
[0061] Figure 8 It is a schematic diagram of the structure when a covering film laminating mechanism is provided;
[0062] Fig. 9 It is a schematic diagram of the structure after the masking strips are laminated on the metal foil at intervals;
[0063] Fig.10 It is a structural schematic diagram when a brush roller mechanism is provided;
[0064] Fig.11 It is a structural schematic diagram of the splint mechanism;
[0065] Fig.12 for Fig.11 Left view of
[0066] Fig.13 This is a schematic structural diagram of Embodiment 2 of the production equipment for melt-coated lithium metal / lithium alloy composite strips of the present invention;
[0067] Fig.14 for Fig.13 D detailed drawing.
[0068] Description of reference numerals:
[0069] 1-metal foil; 2-metal lithium / lithium alloy composite strip; 3-masking film; 4-masking strip; 5-covering film; 6-rolled diaphragm;
[0070] 10-unwinding mechanism; 11-covering film laminating mechanism; 12-strip laminating mechanism; 13-covering film laminating mechanism; 14-covering film rewinding mechanism; 15-brush roller mechanism;
[0071] 20-melt coating composite forming device; 21-control roller; 22-upper inner baffle; 23-upper outer baffle; 24-melt coating composite area; 25-melt coating composite roller; 26-lower inner baffle; 27-lower outer baffle; 28-cooling and shaping area; 29-overflow trough; 30-overflow port; 31-guide plate; 32-air inlet channel; 33-air outlet channel; 34-control roller heating device; 35-scraper; 36-collection box; 37-tension balance roller group; 38-pressure roller;
[0072] 40-rewinding mechanism; 41-covering film rewinding mechanism; 42-knife roller; 43-rewinding diaphragm composite mechanism;
[0073] 50-thickness control section; 51-first temperature zone; 52-second temperature zone; 53-rolling heat insulation board; 54-temperature control transition zone; 55-roller heating device;
[0074] 60- Insulation section;
[0075] 70-finishing section; 71-finishing roller; 72-finishing heating device; 73-finishing heat insulation board;
[0076] 80- clamping plate mechanism; 81- clamping groove; 82- sealing strip; 83- clamping plate; 84- arc surface; 85- pressing adjustment mechanism;
[0077] 90-Tempering section. DETAILED DESCRIPTION
[0078] The present invention is further described below in conjunction with the accompanying drawings and specific embodiments so that those skilled in the art can better understand the present invention and implement it, but the embodiments are not intended to limit the present invention.
[0079] Example 1
[0080] like Figure 1 The figure is a schematic diagram of the structure of the embodiment 1 of the production equipment for melt-coated metal lithium / lithium alloy composite strip of the present invention. The production equipment for melt-coated metal lithium / lithium alloy composite strip of the present embodiment comprises:
[0081] Unwinding mechanism 10: used for continuously unwinding the metal foil material 1;
[0082] The melt coating composite forming device 20 is used to melt-coat and composite a metal lithium layer or a lithium alloy layer on at least one side of the metal foil 1 to obtain a metal lithium / lithium alloy composite strip 2;
[0083] The winding mechanism 40 is used for winding the prepared metal lithium / lithium alloy composite strip 2.
[0084] The melt coating composite forming device 20 includes a control roller group for controlling the thickness of the melt coating composite metal lithium layer or lithium alloy layer, and the control roller group includes two control rollers 21 whose axes are parallel to each other;
[0085] The upper end of the two control rollers 21 is the feeding side, and the lower end is the discharging side. The upper feeding side is provided with a feeding device for adding molten metal lithium or molten lithium alloy, and the lower discharging side is provided with a cooling zone for cooling and shaping the metal lithium / lithium alloy composite strip 2.
[0086] like Figure 2 and Figure 3As shown, the feeding device of this embodiment includes a feeding channel, and the feeding channel includes an upper inner baffle 22 arranged close to the metal foil 1 and an upper outer baffle 23 located on the side of the upper inner baffle 22 facing away from the metal foil 1. A melt-coating composite area 24 is formed below the feeding channel and between the metal foil 1 and the corresponding control roller 21. A melt-coating composite roller 25 is provided in the melt-coating composite area 24 for destroying the surface tension of the molten lithium metal or the molten lithium alloy and compounding the molten lithium metal or the molten lithium alloy with the metal foil.
[0087] like Figure 3 As shown, a cold air channel is provided in the cooling zone of the present embodiment, and the cold air channel includes a lower inner baffle 26 arranged near the metal foil and a lower outer baffle 27 located on the side of the lower inner baffle 26 facing away from the metal foil 1. A cooling and shaping zone 28 is formed above the cold air channel and between the metal lithium / lithium alloy composite belt 2 and the corresponding control roller 21. The cooling medium blown in through the cold air channel reaches the cooling and shaping zone 28 and cools and shapes the metal lithium / lithium alloy composite belt 2. By arranging a cold air channel on the discharge side of the control roller group, and forming a cooling and shaping zone above the cold air channel and between the metal lithium / lithium alloy composite belt and the corresponding control roller, the cooling medium contacts the metal lithium / lithium alloy composite belt only in the cooling and shaping zone to cool and shape it, thereby controlling the temperature and time of cooling and shaping the metal lithium / lithium alloy composite belt, avoiding defects such as cracks in the metal lithium layer or the lithium alloy layer, and improving product quality.
[0088] Specifically, the upper inner baffle 22 and the lower inner baffle 26 are made of heat insulation plates, the upper outer baffle 23 is made of heat insulation plates or plates made of temperature-resistant materials; the lower outer baffle 27 is made of heat insulation plates or plates made of low-temperature resistant materials. The upper inner baffle 22, the upper outer baffle 23, the lower inner baffle 26 and the lower outer baffle 27 of this embodiment are all made of heat insulation plates, which can exchange heat with the outside through the side walls of the feeding channel and the cold air channel, thereby avoiding the heating of the metal foil 1 and causing the metal lithium / lithium alloy composite belt 2 to cool down for too long. Specifically, the metal foil 1 can be made of copper foil, aluminum foil, steel foil, nickel foil, silver foil or gold foil. The metal foil 1 of this embodiment can be made of copper foil, which will not be repeated.
[0089] Furthermore, a roll gap adjustment mechanism for adjusting the roll gap is provided between the two control rolls 21. The roll gap adjustment mechanism can be implemented by using a variety of existing structural methods, which will not be described in detail. By providing the roll gap adjustment mechanism to adjust the distance between the two control rolls 21, the coating thickness of the metal lithium layer or the lithium alloy layer can be controlled.
[0090] Furthermore, the distance between the melt-coated composite roller 25 and the metal foil can be adjusted, thereby increasing the pressure between the melt-coated composite roller 25 and the metal foil 1, and better destroying the surface tension of the molten metal lithium or molten lithium alloy. The melt-coated composite roller 25 can be a brush roller or a scraper roller. The melt-coated composite roller 25 of this embodiment is a brush roller. Those skilled in the art should know that the brush of the brush roller should be made of a high temperature resistant material.
[0091] In this embodiment, a coating gap is provided between the metal foil and the two control rollers, that is, both sides of the metal foil 1 in this embodiment are coated with a metal lithium layer or a lithium alloy layer. At this time, two feeding channels are provided and are respectively located on both sides of the metal foil. Of course, two coating composite rollers 25 are provided and are respectively provided on both sides of the metal foil 1. The two coating composite rollers 25 are provided on both sides of the metal foil 1. At this time, the two coating composite rollers 25 can be adjusted to move toward or away from each other at the same time, so that the pressure applied by the two coating composite rollers 25 to the metal foil 1 is equal and balanced.
[0092] Furthermore, an overflow groove 29 is provided in the feeding channel, and an overflow port 30 is provided in the overflow groove 29 for allowing the molten metal lithium or molten lithium alloy to overflow to the corresponding melt-coated composite roller. By providing the overflow groove 29, the problem of uneven feeding in the axial direction of the control roller 21 can be avoided. At the same time, under the action of the cooling zone below, three different temperature zones are formed between the feeding channel and the melt-coated composite zone 24, that is, the temperature of the molten metal lithium or molten lithium alloy located above the overflow groove 29 is higher, the temperature of the molten metal lithium or molten lithium alloy located below the melt-coated composite roller 25 is lower, and the temperature of the molten metal lithium or molten lithium alloy located between the melt-coated composite roller 25 and the overflow groove 29 is in the middle. In this way, it can be ensured that the molten metal lithium or molten lithium alloy above the overflow groove 29 has sufficient fluidity to overflow to the melt-coated composite roller 25, and the molten metal lithium or molten lithium alloy can be gradually cooled down to increase viscosity, and coated on the metal foil 1 under the action of the melt-coated composite roller 25.
[0093] Furthermore, in the cold air channel of the present embodiment, a guide plate 31 extending into the cooling and shaping area 28 is provided, and the guide plate 31 divides the cold air channel into an air inlet channel 32 and an air outlet channel 33, and the air inlet channel 32 and the air outlet channel 33 are connected through the cooling and shaping area 28. Specifically, the air inlet channel 32 is formed between the guide plate 31 and the lower outer baffle 27, and the air outlet channel 33 is formed between the guide plate 31 and the lower inner baffle 26. Of course, those skilled in the art should know that the air outlet channel 33 can also be formed between the guide plate 31 and the lower outer baffle 27, and the air inlet channel 32 can also be formed between the guide plate 31 and the lower inner baffle 26, which will not be repeated. By providing the guide plate 31 for guiding, the air wall effect formed by directly blowing the cooling medium on the metal lithium / lithium alloy composite strip 2 can be avoided, thereby improving the cooling effect.
[0094] Further, the production equipment of the melt-coated metal lithium / lithium alloy composite strip of the present embodiment further comprises a control roller heating device 34 for heating the control roller; the control roller heating device 34 adopts a heating element arranged in the control roller; or the control roller heating device 34 adopts an eddy current heating device or a radiation heating device for heating the surface of the control roller, and the control roller heating device is arranged between the upper outer baffle 23 and the lower outer baffle 27. The control roller heating device 34 of the present embodiment adopts an eddy current heating device for heating the surface of the control roller. By heating the control roller 21, it is possible to prevent the control roller 21 from cooling the molten metal lithium or the molten lithium alloy.
[0095] Furthermore, the production equipment of the melt-coated lithium metal / lithium alloy composite strip of the present embodiment further includes a scraper 35 for scraping off the molten lithium metal or molten lithium alloy attached to the control roller 21 ; a collecting box 36 is provided below the scraper 35 .
[0096] Furthermore, the production equipment of the melt-coated metal lithium / lithium alloy composite strip in this embodiment also includes two groups of tension balancing roller groups 37. Among the two groups of tension balancing roller groups 37, one group of tension balancing roller groups 37 is arranged on the side of the melt-coated composite zone 24 facing away from the cooling and molding zone 28 and is used to apply a friction force to the metal foil 1 to balance its tension, and the other group of tension balancing roller groups is arranged on the side of the cooling and molding zone 28 facing away from the melt-coated composite zone 24 and is used to apply a friction force to the metal lithium / lithium alloy composite strip 2 to balance its tension. By arranging tension balancing roller groups on the opposite sides of the melt coating composite zone and the cooling and forming zone, respectively, the tension balancing roller group located on the side of the melt coating composite zone facing away from the cooling and forming zone applies friction force to the metal foil and is used to balance the tension required for unwinding the metal foil; the tension balancing roller group located on the side of the cooling and forming zone facing away from the melt coating composite zone applies friction force to the metal foil and is used to balance the tension required for subsequent winding of the metal lithium / lithium alloy composite strip; in this way, the tension of the metal foil and the metal lithium / lithium alloy composite strip between the two groups of tension balancing roller groups can be reduced, thereby preventing the metal foil from being broken.
[0097] Furthermore, at least one thickness control section 50 for controlling the thickness of the metal lithium layer or the lithium alloy layer is provided between the cooling and shaping area 28 and the winding mechanism 40. The thickness control section 50 includes a thickness control area, and the thickness control area is provided with thickness control rollers 51 respectively located on both sides of the metal lithium / lithium alloy composite strip.
[0098] The thickness control zone is divided into a first temperature zone 51 and a second temperature zone 52 with the metal lithium / lithium alloy composite strip as the interface; when controlling the thickness of the metal lithium layer or lithium alloy layer facing the first temperature zone 51, the first temperature zone 51 is set as a high temperature zone and the second temperature zone 52 is set as a low temperature zone; when controlling the thickness of the metal lithium layer or lithium alloy layer facing the second temperature zone 52, the second temperature zone 52 is set as a high temperature zone and the first temperature zone 51 is set as a low temperature zone; the temperature in the high temperature zone is higher than the temperature in the low temperature zone, and a roller heating device for heating the corresponding thickness control roller is provided in the high temperature zone. The roller heating device adopts a heating element arranged in the thickness control roller; or, the roller heating device 55 adopts an eddy current heating device or a radiation heating device for heating the surface of the thickness control roller, and a rolling insulation plate 53 is provided between the roller heating device and the metal lithium / lithium alloy composite strip. The roller heating device of this embodiment adopts an eddy current heating device for heating the surface of the thickness control roller, and a rolling insulation plate 53 is provided between the roller heating device and the metal lithium / lithium alloy composite strip. Specifically, when controlling the thickness of the metal lithium layer or lithium alloy layer in the first temperature zone 51, the temperature of the second temperature zone 52 is set to be relatively low, and the temperature in the first temperature zone 51 is set to a temperature suitable for the plastic deformation of the metal lithium layer or lithium alloy layer, so that when the thickness control roller 51 is rolled, only the thickness of the metal lithium layer or lithium alloy layer located in the first temperature zone 51 is greatly changed, and the thickness of the metal lithium layer or lithium alloy layer located in the second temperature zone 52 does not change or produces a slight change that does not affect the product quality. On the contrary, when controlling the thickness of the metal lithium layer or lithium alloy layer in the second temperature zone 52, the temperature of the first temperature zone 53 is set to be relatively low. The thickness control section 50 of this embodiment is set to two sections, and the two thickness control sections 50 are used to control the thickness of the metal lithium layer or lithium alloy layer on both sides of the metal foil 1 respectively. Preferably, the thickness control section 50 also includes a temperature control transition zone 54 located in the front side of the thickness control zone, which is used to achieve the transition of temperature change.
[0099] Furthermore, a heat preservation section 60 is provided between the thickness control section 50 and the cooling and molding area 28, so that the metal lithium / lithium alloy composite strip rapidly cooled in the cooling and molding area 28 can gradually return to a suitable temperature to eliminate internal stress and improve product quality.
[0100] Furthermore, a finishing section 70 for finishing the metal lithium / lithium alloy composite strip is provided between the thickness control section 50 and the winding mechanism 40. Figure 4As shown, at least one finishing zone is provided in the finishing section 70, and finishing rollers 71 are provided in the finishing zone, which are respectively located on both sides of the metal lithium / lithium alloy composite belt 2, and finishing heating devices 72 are also provided in the finishing zone, which are respectively located on both sides of the metal lithium / lithium alloy composite belt and are used to heat the corresponding finishing rollers. The finishing heating device 72 uses a heating element arranged in the finishing roller; or, the finishing heating device 72 uses an eddy current heating device or a radiation heating device for heating the surface of the finishing roller, and a finishing heat insulation plate 73 is provided between the finishing heating device 72 and the metal lithium / lithium alloy composite belt. Preferably, the finishing roller in the finishing zone at the rear end of this embodiment is a surface finishing roller used to control the surface finish of the metal lithium / lithium alloy composite belt, so as to control the surface roughness of the metal lithium / lithium alloy composite belt and improve the product quality.
[0101] Furthermore, a tempering section 90 for eliminating the internal stress of the metal lithium / lithium alloy composite strip is provided between the finishing section 70 and the winding mechanism 40, so as to eliminate the internal stress, prevent the metal lithium / lithium alloy composite strip from deforming, and improve product quality.
[0102] Furthermore, in order to use the produced metal lithium / lithium alloy composite strip for energy storage devices, it is also necessary to reserve an area for setting the tabs on the metal foil 1. There are many ways to reserve an area for setting the tabs on the metal foil 1, such as:
[0103] The first type: Figure 5 As shown, a covering film laminating mechanism 11 is provided between the unwinding mechanism 10 and the feeding channel for laminating the covering film 3 on both side edges of the metal foil 1. The covering film 3 is used to cover the both side edges of the metal foil 1 to prevent metal lithium or lithium alloy from being coated on both side edges of the metal foil 1, and to reserve both side areas for the tabs. The covering film 3 can be removed when manufacturing the energy storage device, or it can be removed before winding. That is, a covering film winding mechanism 41 is provided in front of the winding mechanism 40 of this embodiment. The covering film winding mechanism 41 includes a knife roller 42, and the knife roller 42 is provided with a cutter facing the inner edge of the covering film 3. Figure 6 , which is a schematic structural diagram after the covering films 3 are attached to the two side edges of the metal foil 1 .
[0104] The second type: a strip pasting mechanism 12 for pasting the covering strip 4 on the metal foil 1 is provided between the unwinding mechanism 10 and the feeding channel, that is, the covering strip 4 is pasted directly on the metal foil 1 at intervals, such as Figure 7 As shown; or, a covering film laminating mechanism 13 for laminating the covering film 5 on the metal foil 1 and a covering film reeling mechanism 14 for peeling the covering film 5 off the metal foil 1 so that the covering strips 4 arranged at intervals on the covering film are attached to the metal foil 1 are provided between the unwinding mechanism 10 and the feeding channel, as shown in FIG. Figure 8That is, the masking strips 4 are first pasted on the covering film 5 at intervals, and then the covering film 5 is compounded on the metal foil 1 so that the masking strips 4 are pasted on the metal foil 1 at intervals, and then the covering film 5 is removed and the masking strips 4 are left on the metal foil 1. Fig. 9 , which is a schematic structural diagram after the covering strips 4 are laminated on the metal foil 1 at intervals.
[0105] Of course, in order to enhance the melting coating effect, a brush roller mechanism 15 for brushing molten lithium metal or molten lithium alloy on the metal foil 1 can also be provided between the unwinding mechanism 10 and the feeding channel, such as Fig.10 After a layer of metal lithium or lithium alloy is pre-coated on the metal foil 1, the metal lithium or lithium alloy is melt-coated by the melt-coating composite molding device 20, so as to improve the bonding performance between the molten metal lithium or molten lithium alloy and the metal foil 1.
[0106] Furthermore, a membrane winding composite mechanism 43 for compositely winding the membrane 6 on the surface of the metal lithium / lithium alloy composite strip is provided in front of the winding mechanism 10 to prevent the metal lithium layers or lithium alloy layers between adjacent winding layers from sticking together after winding.
[0107] Furthermore, the feeding sides of the two control rollers 21 of this embodiment are provided with clamping plate mechanisms 80 for clamping the edges of both ends of the metal foil material 1. Fig.11 As shown, the clamping mechanism 80 includes a clamping groove 81, and sealing strips 82 are respectively provided between the two side walls of the clamping groove 81 and the metal foil 1. Specifically, the clamping mechanism of this embodiment includes two clamping plates 83, and the clamping groove 81 is formed between the two clamping plates 83, and a clamping adjustment mechanism 85 for controlling the clamping force between the sealing strip 82 and the metal foil 1 is provided between the two clamping plates 83. The clamping adjustment mechanism can be implemented in a variety of existing ways, which will not be repeated. The side surface of the clamping plate 83 of this embodiment close to the control roller 21 is set as an arc surface 84 matching the control roller 21, which can prevent molten metal lithium or molten lithium alloy from flowing out from both ends of the control roller 21.
[0108] The melt-coated metal lithium / lithium alloy composite belt production equipment of this embodiment is provided with a feeding device on the feed side of the control roller group, and a feeding channel is provided in the feeding device, and a melt-coated composite zone is formed between the metal foil and the corresponding control roller below the feeding channel. The upper inner baffle plate can prevent the molten metal lithium or molten lithium alloy from directly contacting the metal foil, so that the molten metal lithium or molten lithium alloy is in contact with the metal foil only in the melt-coated composite zone, thereby reducing the contact time between the metal foil and the high-temperature molten metal lithium or molten lithium alloy, so as to avoid the problem of the metal foil being broken due to the decrease of tensile strength due to the long-term contact between the metal foil and the molten metal lithium or molten lithium alloy; the surface tension of the molten metal lithium or molten lithium alloy is destroyed by providing a melt-coated composite roller, so that the molten metal lithium or molten lithium alloy can be better coated on the metal foil, thereby improving the production quality of the metal lithium / lithium alloy composite belt.
[0109] Example 2
[0110] like Fig.13 The figure is a schematic diagram of the structure of the embodiment 1 of the production equipment for melt-coated metal lithium / lithium alloy composite strip of the present invention. The production equipment for melt-coated metal lithium / lithium alloy composite strip of the present embodiment comprises:
[0111] Unwinding mechanism 10: used for continuously unwinding the metal foil material 1;
[0112] The melt coating composite forming device 20 is used to melt-coat and composite a metal lithium layer or a lithium alloy layer on at least one side of the metal foil 1 to obtain a metal lithium / lithium alloy composite strip 2;
[0113] The winding mechanism 40 is used for winding the prepared metal lithium / lithium alloy composite strip 2.
[0114] The melt coating composite forming device 20 includes a control roller group for controlling the thickness of the melt coating composite metal lithium layer or lithium alloy layer, and the control roller group includes two control rollers 21 whose axes are parallel to each other;
[0115] The upper end of the two control rollers 21 is the feeding side, and the lower end is the discharging side. The upper feeding side is provided with a feeding device for adding molten metal lithium or molten lithium alloy, and the lower discharging side is provided with a cooling zone for cooling and shaping the metal lithium / lithium alloy composite strip 2.
[0116] The feeding device of this embodiment includes a feeding channel, which includes an upper inner baffle 22 arranged close to the metal foil 1 and an upper outer baffle 23 located on the side of the upper inner baffle 22 facing away from the metal foil 1. A melt-coating composite area 24 is formed below the feeding channel and between the metal foil 1 and the corresponding control roller 21. A melt-coating composite roller 25 is provided in the melt-coating composite area 24 for destroying the surface tension of molten lithium metal or molten lithium alloy and compounding the molten lithium metal or molten lithium alloy with the metal foil.
[0117] In the cooling zone of the present embodiment, a cold air channel is provided, and the cold air channel includes a lower inner baffle 26 arranged near the metal foil and a lower outer baffle 27 located on the side of the lower inner baffle 26 facing away from the metal foil 1. A cooling and shaping zone 28 is formed above the cold air channel and between the metal lithium / lithium alloy composite belt 2 and the corresponding control roller 21. The cooling medium blown in through the cold air channel reaches the cooling and shaping zone 28 and cools and shapes the metal lithium / lithium alloy composite belt 2. By providing a cold air channel on the discharge side of the control roller group, and forming a cooling and shaping zone above the cold air channel and between the metal lithium / lithium alloy composite belt and the corresponding control roller, the cooling medium only contacts the metal lithium / lithium alloy composite belt in the cooling and shaping zone to cool and shape it, thereby being able to control the temperature and time of cooling and shaping the metal lithium / lithium alloy composite belt, avoiding defects such as cracks in the metal lithium layer or the lithium alloy layer, and improving product quality.
[0118] Furthermore, the metal foil 1 of this embodiment always maintains contact and cooperation with one of the control rollers 21, that is, in this embodiment, a metal lithium layer or a lithium alloy layer is only melt-coated on one side of the metal foil 1, and at this time, one feeding channel is provided and is located on the side of the metal foil 1 facing the other control roller 21. Specifically, in this embodiment, one melt-coated composite roller 25 is provided and is located in the melt-coated composite area 24, and a pressure roller 38 is provided on the side of the metal foil 1 facing away from the melt-coated composite area 24 corresponding to the melt-coated composite roller 25, and the pressure roller 38 is mainly used to balance the pressure applied by the melt-coated composite roller 25 to the metal foil 1.
[0119] Of course, in this embodiment, at least one thickness control section 50 for controlling the thickness of the metal lithium layer or the lithium alloy layer is provided between the cooling and shaping area 28 and the winding mechanism 40. The thickness control section 50 includes a thickness control area, and the thickness control area is provided with thickness control rollers 51 respectively located on both sides of the metal lithium / lithium alloy composite strip.
[0120] The thickness control zone is divided into a first temperature zone 51 and a second temperature zone 52 with the metal lithium / lithium alloy composite strip as the interface; when controlling the thickness of the metal lithium layer or lithium alloy layer facing the first temperature zone 51, the first temperature zone 51 is set as a high temperature zone and the second temperature zone 52 is set as a low temperature zone; when controlling the thickness of the metal lithium layer or lithium alloy layer facing the second temperature zone 52, the second temperature zone 52 is set as a high temperature zone and the first temperature zone 51 is set as a low temperature zone; the temperature in the high temperature zone is higher than the temperature in the low temperature zone, and a roller heating device for heating the corresponding thickness control roller is provided in the high temperature zone. The roller heating device adopts a heating element arranged in the thickness control roller; or, the roller heating device adopts an eddy current heating device or a radiation heating device for heating the surface of the thickness control roller, and a rolling insulation plate 53 is provided between the roller heating device and the metal lithium / lithium alloy composite strip. The roller heating device of this embodiment adopts an eddy current heating device for heating the surface of the thickness control roller, and a rolling insulation plate 53 is provided between the roller heating device and the metal lithium / lithium alloy composite strip. Specifically, when controlling the thickness of the metal lithium layer or lithium alloy layer in the first temperature zone 51, the temperature of the second temperature zone 52 is set to be relatively low, so that when the thickness control roller 51 is rolling, only the thickness of the metal lithium layer or lithium alloy layer in the first temperature zone 51 is greatly changed, and the thickness of the metal lithium layer or lithium alloy layer in the second temperature zone 52 is unchanged or slightly changed without affecting the product quality. The thickness control section 50 of this embodiment is set as one section, and the thickness control section 50 is used to control the thickness of the metal lithium layer or lithium alloy layer coated on one side of the metal foil 1. Preferably, the thickness control section 50 also includes a temperature control transition zone 54 located in front of the thickness control zone, which is used to achieve the transition of temperature change.
[0121] The other implementations of this embodiment are the same as those of Embodiment 1 and are not described one by one.
[0122] Note: The meaning of "metal lithium / lithium alloy" mentioned herein is "metal lithium" or "lithium alloy". According to the different added raw materials, the melt-coated metal lithium / lithium alloy composite belt production equipment of the present invention can produce "metal lithium composite belt" or "lithium alloy composite belt". The "melt coating" mentioned herein refers to melting metal lithium or lithium alloy and then coating it on the metal foil. The temperature of the molten metal lithium and the molten lithium alloy is between its melting point and boiling point.
[0123] The above-described embodiments are only preferred embodiments for fully illustrating the present invention, and the protection scope of the present invention is not limited thereto. Equivalent substitutions or changes made by those skilled in the art based on the present invention are within the protection scope of the present invention. The protection scope of the present invention shall be subject to the claims.
Claims
1. A production equipment for melt-coated lithium metal / lithium alloy composite strip, characterized in that: include: Unwinding mechanism: used for continuously unwinding metal foil; Melt coating composite forming device: used for melt coating and composite forming of a metal lithium layer or a lithium alloy layer on at least one side of a metal foil to obtain a metal lithium / lithium alloy composite strip; Winding mechanism: used for winding the prepared metal lithium / lithium alloy composite strip; The melt-coating composite forming device comprises a control roller group for controlling the thickness of the melt-coated composite lithium metal layer or lithium alloy layer, wherein the control roller group comprises two control rollers whose axes are parallel to each other; The feeding side of the two control rollers is provided with a feeding device for adding molten metal lithium or molten lithium alloy, and the discharging side is provided with a cooling zone for cooling and shaping the metal lithium / lithium alloy composite belt; The feeding device comprises a feeding channel, the feeding channel comprises an upper inner baffle plate arranged close to the metal foil and an upper outer baffle plate located on the side of the upper inner baffle plate facing away from the metal foil, a melt-coating composite zone is formed between the lower part of the feeding channel and the metal foil and the corresponding control roller, and a melt-coating composite roller is arranged in the melt-coating composite zone for destroying the surface tension of the molten metal lithium or the molten lithium alloy and compounding the molten metal lithium or the molten lithium alloy with the metal foil; A cold air channel is provided in the cooling zone, and the cold air channel includes a lower inner baffle plate arranged close to the metal foil and a lower outer baffle plate located on the side of the lower inner baffle plate facing away from the metal foil. A cooling and shaping zone is formed between the upper part of the cold air channel and the metal lithium / lithium alloy composite strip and the corresponding control roller. The cooling medium blown in through the cold air channel reaches the cooling and shaping zone and cools and shapes the metal lithium / lithium alloy composite strip. The cold air channel is provided with a guide plate extending into the cooling and shaping area, the guide plate divides the cold air channel into an air inlet channel and an air outlet channel, and the air inlet channel and the air outlet channel are connected through the cooling and shaping area; It also includes two groups of tension balancing roller groups. Among the two groups of tension balancing roller groups, one group of the tension balancing roller groups is arranged on the side of the melt-coating composite zone facing away from the cooling and forming zone and is used to apply a friction force to the metal foil to balance its tension, and the other group of the tension balancing roller groups is arranged on the side of the cooling and forming zone facing away from the melt-coating composite zone and is used to apply a friction force to the metal lithium / lithium alloy composite strip to balance its tension.
2. The metal lithium / lithium alloy composite belt production equipment according to claim 1, characterized in that: The distance between the melt-coated composite roller and the metal foil is adjustable.
3. The metal lithium / lithium alloy composite belt production equipment according to claim 1, characterized in that: The melt-coated composite roller is a brush roller or a scraper roller.
4. The metal lithium / lithium alloy composite belt production equipment according to claim 1, characterized in that: When the metal foil material is always in contact with one of the control rollers, the feeding channel is provided as one and is located on the side of the metal foil material facing the other control roller.
5. The metal lithium / lithium alloy composite belt production equipment according to claim 4, characterized in that: The melt coating composite roller is provided as one and is located in the melt coating composite area. A pressure roller is provided corresponding to the melt coating composite roller on the side of the metal foil material facing away from the melt coating composite area.
6. The metal lithium / lithium alloy composite belt production equipment according to claim 1, characterized in that: When a melting coating gap is respectively arranged between the metal foil and the two control rollers, the number of the feeding channels is two and they are respectively located at two sides of the metal foil.
7. The metal lithium / lithium alloy composite belt production equipment according to claim 6, characterized in that: The melt-coated composite rollers are provided in two numbers and are respectively arranged at two sides of the metal foil.
8. The metal lithium / lithium alloy composite belt production equipment according to claim 1, characterized in that: An overflow groove is provided in the feeding channel, and an overflow port is provided in the overflow groove for allowing molten metal lithium or molten lithium alloy to overflow to the corresponding melt-coated composite roller.
9. The metal lithium / lithium alloy composite belt production equipment according to claim 1, characterized in that: It also includes a control roller heating device for heating the control roller; the control roller heating device uses a heating element arranged in the control roller; or the control roller heating device uses an eddy current heating device or a radiation heating device for heating the surface of the control roller, and the control roller heating device is arranged between the upper outer baffle plate and the lower outer baffle plate.
10. The metal lithium / lithium alloy composite belt production equipment according to claim 1, characterized in that: It also includes a scraper for scraping off the molten metal lithium or molten lithium alloy attached to the control roller; a collecting box is provided below the scraper.
11. The metal lithium / lithium alloy composite belt production equipment according to claim 1, characterized in that: At least one thickness control section is provided between the cooling and shaping section and the winding mechanism for controlling the thickness of the metal lithium layer or the lithium alloy layer, and the thickness control section includes a thickness control area, and the thickness control area is provided with thickness control rollers respectively located on both sides of the metal lithium / lithium alloy composite strip; The thickness control zone is divided into a first temperature zone and a second temperature zone with the metal lithium / lithium alloy composite belt as the interface; when controlling the thickness of the metal lithium layer or the lithium alloy layer facing the first temperature zone, the first temperature zone is set as a high temperature zone and the second temperature zone is set as a low temperature zone; when controlling the thickness of the metal lithium layer or the lithium alloy layer facing the second temperature zone, the second temperature zone is set as a high temperature zone and the first temperature zone is set as a low temperature zone; the temperature in the high temperature zone is higher than the temperature in the low temperature zone, and a roller heating device for heating the corresponding thickness control roller is provided in the high temperature zone.
12. The metal lithium / lithium alloy composite belt production equipment according to claim 11, characterized in that: The roller heating device adopts a heating element arranged in the thickness control roller; or, the roller heating device adopts an eddy current heating device or a radiation heating device for heating the surface of the thickness control roller, and a rolling insulation plate is provided between the roller heating device and the metal lithium / lithium alloy composite strip.
13. The metal lithium / lithium alloy composite belt production equipment according to claim 11, characterized in that: The thickness control section also includes a temperature control transition zone located in front of the thickness control zone.
14. The metal lithium / lithium alloy composite belt production equipment according to claim 11, characterized in that: A heat preservation section is also provided between the thickness control section and the cooling and shaping area.
15. The metal lithium / lithium alloy composite belt production equipment according to claim 11, characterized in that: A finishing section for finishing the metal lithium / lithium alloy composite strip is provided between the thickness control section and the winding mechanism.
16. The metal lithium / lithium alloy composite belt production equipment according to claim 15, characterized in that: At least one finishing zone is provided in the finishing section, and finishing rollers are provided in the finishing zone respectively located on both sides of the metal lithium / lithium alloy composite belt, and finishing heating devices are also provided in the finishing zone respectively located on both sides of the metal lithium / lithium alloy composite belt and used to heat the corresponding finishing rollers.
17. The metal lithium / lithium alloy composite belt production equipment according to claim 16, characterized in that: The finishing roller in the finishing zone at the rearmost end is a surface finishing roller used to control the surface finish of the metal lithium / lithium alloy composite strip.
18. The metal lithium / lithium alloy composite belt production equipment according to claim 16, characterized in that: The finishing heating device adopts a heating element arranged in the finishing roller; or, the finishing heating device adopts an eddy current heating device or a radiation heating device for heating the surface of the finishing roller, and a finishing insulation plate is provided between the finishing heating device and the metal lithium / lithium alloy composite strip.
19. The metal lithium / lithium alloy composite belt production equipment according to claim 15, characterized in that: A tempering section for eliminating the internal stress of the metal lithium / lithium alloy composite strip is provided between the finishing section and the winding mechanism.
20. The metal lithium / lithium alloy composite belt production equipment according to claim 1, characterized in that: A covering film laminating mechanism for laminating covering films on both side edges of the metal foil is provided between the unwinding mechanism and the feeding channel.
21. The metal lithium / lithium alloy composite belt production equipment according to claim 20, characterized in that: A covering film winding mechanism is arranged in front of the winding mechanism, and the covering film winding mechanism comprises a knife roller, and a cutting knife facing the inner edge of the covering film is arranged on the knife roller.
22. The metal lithium / lithium alloy composite belt production equipment according to claim 1, characterized in that: A strip sticking mechanism for sticking covering strips on the metal foil at intervals is provided between the unwinding mechanism and the feeding channel; or, a covering film sticking mechanism for sticking a covering film on the metal foil and a covering film winding mechanism for peeling the covering film off the metal foil so that the covering strips arranged at intervals on the covering film are stuck to the metal foil are provided between the unwinding mechanism and the feeding channel.
23. The metal lithium / lithium alloy composite belt production equipment according to claim 1, characterized in that: A brush roller mechanism for brushing molten metal lithium or molten lithium alloy on the metal foil is provided between the unwinding mechanism and the feeding channel.
24. The metal lithium / lithium alloy composite belt production equipment according to claim 1, characterized in that: A membrane winding composite mechanism for compositely winding a membrane on the surface of the metal lithium / lithium alloy composite belt is also provided in front of the winding mechanism.
25. The metal lithium / lithium alloy composite belt production equipment according to claim 1, characterized in that: The upper inner baffle and the lower inner baffle are made of heat insulation plates, the upper outer baffle is made of heat insulation plates or plates made of temperature-resistant materials; the lower outer baffle is made of heat insulation plates or plates made of low-temperature-resistant materials.
26. The metal lithium / lithium alloy composite belt production equipment according to claim 1, characterized in that: The metal foil material is copper foil, aluminum foil, steel foil, nickel foil, silver foil or gold foil.
27. The metal lithium / lithium alloy composite belt production equipment according to claim 1, characterized in that: The feeding sides of the two control rollers are provided with clamping mechanisms respectively used to clamp the edges of both ends of the metal foil. The clamping mechanisms include clamping grooves, and sealing strips are respectively provided between the two side walls of the clamping groove and the metal foil.
28. The metal lithium / lithium alloy composite belt production equipment according to claim 27, characterized in that: The clamping plate mechanism comprises two clamping plates, the clamping groove is formed between the two clamping plates, and a pressing adjustment mechanism for controlling the pressing force between the sealing strip and the metal foil is arranged between the two clamping plates.
29. The metal lithium / lithium alloy composite belt production equipment according to claim 28, characterized in that: A side surface of the clamping plate close to the control roller is configured as an arc surface matching the control roller.