A thermal field system and process method for reducing oxygen content in silicon crystals

By adjusting the heater structure and process parameters, the reaction between the quartz crucible and molten silicon is reduced, and the oxygen content in single crystal silicon is reduced, which solves the problem of excessive oxygen content in CZ production, and improves the quality of single crystal silicon and components. Yield rate.

CN115198350BActive Publication Date: 2024-12-06MCL ELECTRONICS MATERIALS
View PDF 12 Cites 0 Cited by

Patent Information

Application Number
CN202210829510.4
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2022-07-15
Publication Date
2024-12-06
Estimated Expiration
2042-07-15

AI Technical Summary

Technical Problem

During the CZ method, the reaction between the quartz crucible and the molten silicon leads to excessive oxygen content in the silicon crystal, forming oxygen precipitates, reducing the yield of the component.

Method used

By adjusting the structure of the main heater and the bottom heater, the coverage of the central high-efficiency heating zone of the main heater is reduced, and the reaction between the quartz crucible and molten silicon is weakened. The longitudinal circumferential heating zone and the U-shaped bottom heating zone of the bottom heater are designed. Combined with argon flow rate and furnace pressure control, the amount of oxygen entering the silicon melt is reduced.

Benefits of technology

Effectively reduce the oxygen content in single crystal silicon, improve crystal quality, enhance the reliability of components, and meet the production needs of high-quality single crystals.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN115198350B_ABST
    Figure CN115198350B_ABST
Patent Text Reader

Abstract

The invention relates to a thermal field system and a process method capable of reducing the oxygen content of silicon crystals. The invention effectively solves the problem that the oxygen content in silicon melt is high during the Czochralski method for producing single crystals, resulting in poor quality of generated silicon single crystal rods. The technical solution comprises: the solution adjusts the structures of a main heater and a bottom heater to reduce the coverage of a central efficient heating zone of a main heater for providing heat demand during the crystal pulling process, so that the contact area between the crystal, molten silicon and the inner wall of a quartz crucible during the growth process is not entirely between the central efficient heating zone of the main heater, thereby reducing the heat radiation to the quartz crucible, thereby reducing the degree of reaction between the inner wall of the quartz crucible and the molten silicon, and reducing the amount of oxygen entering the molten silicon.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the technical field of semiconductor single crystal silicon production, and in particular to a thermal field system and a process method capable of reducing the oxygen content of silicon crystals. Background Art

[0002] In the industry, more than 98% of electronic component materials are made of single crystal silicon, which is mainly produced by FZ (FloatZone, zone melting method) and CZ (Czochralski, straight pulling method), and CZ method is the most commonly used method. In CZ method production, quartz crucible is one of the most important materials, because the quartz crucible contains molten polysilicon, and the reaction between the two will directly affect the quality of the grown single crystal rod;

[0003] The quartz crucible (main component SiO2) used in CZ silicon has been improved in various ways to increase its purity and slow down the reaction with molten silicon, but the quartz itself will inevitably react with molten silicon at high temperatures (SiO2+Si→2SiO), resulting in a high concentration of oxygen in the grown silicon crystal rod. The oxygen concentration entering the silicon crystal forms oxygen precipitates during the subsequent processing and heat treatment process, and the oxygen precipitates in the component area will also reduce the minority carrier lifetime. In severe cases, defects such as stacking faults and dislocation loops will be formed along with the oxygen precipitates, greatly reducing the component yield. Therefore, reducing the oxygen content in CZ silicon has become an urgent problem to be solved;

[0004] In view of the above, we provide a thermal field system and process method that can reduce the oxygen content of silicon crystals to solve the above problems. Summary of the invention

[0005] In view of the above situation, the present invention provides a thermal field system and a process method for reducing the oxygen content of silicon crystals. This scheme adjusts the structure of the main heater and the bottom heater to reduce the coverage of the central high-efficiency heating zone of the main heater used to provide heat requirements during the crystal pulling process, so that the contact area between the crystal and the molten silicon and the inner wall of the quartz crucible during the growth process is not entirely between the central high-efficiency heating zone of the main heater, thereby reducing the thermal radiation to the quartz crucible, thereby reducing the degree of reaction between the inner wall of the quartz crucible and the molten silicon, and reducing the amount of oxygen entering the molten silicon.

[0006] A thermal field system capable of reducing the oxygen content of silicon crystals comprises a furnace body and a quartz crucible is arranged in the furnace body, characterized in that a main heater cooperating with the quartz crucible is arranged in the furnace body, a bottom heater is arranged vertically in the furnace body below the main heater, and the bottom heater comprises a horizontally arranged U-shaped bottom heating zone and a vertically arranged longitudinal circumferential heating zone.

[0007] Preferably, the height of the heating area of ​​the main heater is one third to two thirds of the height of the quartz crucible.

[0008] The above technical solution has the following beneficial effects:

[0009] (1) This solution achieves the purpose of safe material processing and reducing the reaction between the quartz crucible and molten silicon by adjusting the structure of the main heater and the bottom heater. It can simply reduce the oxygen content in the single crystal silicon crystal by controlling the argon flow rate, furnace pressure and crucible rotation process during the crystal pulling process, thereby improving the quality of the crystal and meeting the production and social needs of high-quality single crystals.

[0010] (2) By reducing the coverage of the central efficient heating zone of the main heater used to provide heat for the crystal pulling process, the contact area between the crystal and the molten silicon and the inner wall of the quartz crucible during the growth process is not entirely between the central efficient heating zone of the main heater, thereby reducing the heat radiation to the quartz crucible, thereby reducing the degree of reaction between the inner wall of the quartz crucible and the molten silicon, and reducing the amount of oxygen entering the silicon melt;

[0011] (3) The design of the longitudinal circumferential heating zone of the bottom heater in this solution combines the characteristic of shortening the central high-efficiency heating zone of the main heater of this application, and designs a corresponding height to compensate for the problem of too low temperature in this area during the material processing. At the same time, combined with the design of the U-shaped bottom heating zone, the circumferential side and bottom of the quartz crucible are heated to achieve the material processing effect. BRIEF DESCRIPTION OF THE DRAWINGS

[0012] Figure 1 It is a schematic cross-sectional view of the overall structure of the present invention;

[0013] Figure 2 This is a schematic diagram of the structure of the main heater of the present invention;

[0014] Figure 3 This is a schematic diagram of the bottom heater structure of the present invention;

[0015] Figure 4 It is a top view schematic diagram of the matching relationship between the main heater, the bottom heater and the exhaust duct of the present invention;

[0016] Figure 5 This is a schematic structural diagram of the bottom heater of the present invention from another perspective;

[0017] Figure 6 This is a structural schematic diagram of the main heater of the present invention from another viewing angle;

[0018] Figure 7 It is a schematic diagram of the internal structure of the furnace body after the cross section of the present invention;

[0019] Figure 8 This is a schematic diagram of the position relationship between the bottom heater and the exhaust duct of the present invention;

[0020] Fig. 9It is a structural schematic diagram of another viewing angle of the internal structure of the furnace body of the present invention after being cut away;

[0021] Fig.10 Schematic diagram of oxygen content in silicon single crystal rods produced in this embodiment and comparative example of the present invention. DETAILED DESCRIPTION

[0022] The above and other technical contents, features and effects of the present invention are described in detail below with reference to the attached Figures 1 to 10 It can be clearly presented in the detailed description of the embodiments that the structural contents mentioned in the following embodiments are all referenced to the drawings in the specification.

[0023] Embodiment 1: This embodiment provides a thermal field system that can reduce the oxygen content of silicon crystals. Figure 1 As shown, including the furnace body (as shown in the attached Figure 1 As shown, the furnace body is provided with a plurality of heat-insulating components 2 from top to bottom, and a quartz crucible 3 is provided in the furnace body, and an exhaust channel 8 for exhaust is provided at the bottom of the quartz crucible 3 (in the process of crystal pulling, argon gas with a certain flow rate needs to be transported into the furnace body, and the exhaust channel 8 allows the argon gas transported into the furnace body to take away oxygen, carbon and other high-temperature volatile impurity gases in the furnace and discharge the furnace body), and a lower shaft head 6 for lifting the quartz crucible 3 and making it rise and fall in the furnace body (in the process of crystal pulling, the height position of the quartz crucible 3 in the furnace body changes, and the lower shaft head 6 is connected to a lifting mechanism), the generated silicon single crystal rod 1 is in the middle position of the quartz crucible 3, and the silicon single crystal rod 1 is slowly pulled upward during its growth, and the crystal grows at the contact surface between the lower end of the silicon single crystal rod 1 and the silicon melt 4 (that is, at the solid-liquid interface). Since the above-mentioned structural components are all existing technologies, and the improvement of this scheme does not lie in this, the structure thereof will not be described in detail. The improvement of this scheme lies in:

[0024] A main heater 5 is provided in the furnace body to cooperate with the quartz crucible 3 (used to provide the heat required in the single crystal pulling process), and a bottom heater 7 is vertically spaced in the furnace body below the main heater 5 (mainly used in the material processing of block polycrystalline silicon in the quartz crucible 3. Before the crystal pulling production process, the block polycrystalline silicon needs to be placed in the quartz crucible 3 and heated to turn it into silicon melt 4). The top of the bottom heater 7 and the bottom of the main heater 5 are spaced a certain distance apart (as shown in the attached figure). Figure 7 , 9 ), as shown in the attached Figure 5 As shown, the bottom heater 7 includes a circumferential longitudinal heating zone and a U-shaped bottom heating zone 7-1, and the circumferential longitudinal heating zone and the U-shaped bottom heating zone 7-1 are integrally arranged. Figure 3As shown, the area size of the center 7-2 of the U-shaped bottom heating zone of the bottom heater 7 is designed to be larger than the maximum diameter of the lower shaft head 6, so that when the block polysilicon is initially melted, the melting of the material at a low crucible level is guaranteed as much as possible (at this time, the quartz crucible 3 is at the lowest limit in the furnace body, and the lower shaft head 6 is also at the lowest limit), which can avoid the risk of the bottom being too cold during the melting process, and can also better avoid the risk of arcing or heating overcurrent caused by the lower shaft head 6 being too close to the U-shaped bottom heating zone 7-1 of the bottom heater 7 (because the bottom heater 7 and the main heater 5 are both made of graphite, and the heating principle is: graphite as a heater itself acts as a resistor to generate heat, and a certain amount of heat is passed into it After the current is passed, it quickly heats up and generates heat, thereby achieving a heating effect. The lower shaft head 6 is also made of graphite and is too close to the bottom heater. Due to the volatilization of impurities in the furnace, it is easy to cause an arc between the two, which may cause an overcurrent risk in severe cases). When the quartz crucible 3 is at the lowest limit of the furnace body and the block polysilicon inside it is being melted (at this time, the lower shaft head 6 is also at the lowest end position), the center 7-2 of the U-shaped bottom heating zone is larger than the maximum diameter of the lower shaft head 6, which can better avoid the U-shaped bottom heating zone 7-1 of the bottom heater 7 from touching the lower shaft head 6 due to the failure of the lower limit, thereby avoiding the occurrence of a short circuit in the heater;

[0025] The U-shaped bottom heating zone 7-1 and the longitudinal circumferential heating zone 7-3 are designed according to the distribution of the electrode positions and the exhaust duct 8 positions arranged on the bottom wall of the furnace body. Figure 6 As shown, the main heater 5 includes a central high-efficiency heating area 5-1 of the main heater 5 and a main heater support body 5-2 (both of which are made of graphite). Fig. 9 As shown, a main heater electrode 5-3 is provided at the bottom of the furnace body and the main heater support 5-2 is fixed to the main heater electrode 5-3 by screw connection. Figure 4 , 7 As shown in the figure, a bottom heater electrode 7-4 is provided at the bottom of the furnace body and the bottom heater electrode 7-4 is connected to the bottom heater 7, and the main heater electrode 5-3 and the bottom heater electrode 7-4 are respectively connected to external electrical circuits, as shown in the attached figure. Figure 4 , 8 As shown in the figure, the U-shaped bottom heating zone 7-1 is arranged to avoid the exhaust duct 8, the main heater electrode 5-3, and the bottom heater electrode 7-4 arranged at the bottom of the furnace body, so as to realize the synchronous coordination design of the U-shaped bottom heating zone 7-1 and the longitudinal circumferential heating zone 7-3;

[0026] The heating height of the conventional heater usually covers the entire quartz crucible 3. During the growth of the single crystal, the contact area between the silicon melt 4 and the inner wall of the quartz crucible 3 can always be kept between the wider central high-efficiency heating area 5-1 of the main heater 5. That is, during the crystal pulling process, the reaction degree between the silicon melt 4 and the inner wall of the quartz crucible 3 is always relatively intense. During the crystal pulling process, a large amount of oxygen enters the silicon melt 4, which leads to a higher oxygen content in the single crystal.

[0027] As attached Figure 1 As shown, in this scheme, when the main heater 5 is set, it is made not to completely cover the quartz crucible 3 (the height of the heating area of ​​the main heater 5 is one-third to two-thirds of the height of the quartz crucible 3), that is, the main heater 5 adopts the method of reducing the height of the heating area of ​​the heater to reduce the height range covered by the central efficient heating area of ​​the heater itself, so that the contact area between the silicon melt 4 and the inside of the quartz crucible 3 during the growth of the crystal is not completely between the central efficient heating area 5-1 of the main heater 5, so as to reduce the degree of heat radiation to the quartz crucible 3, thereby reducing the degree of reaction between the inner wall of the quartz crucible 3 and the silicon melt 4, and reducing the amount of oxygen entering the silicon melt 4;

[0028] Although the height of the heating area of ​​the main heater 5 is reduced, this solution combines the characteristic of shortening the heating area of ​​the main heater 5 in the present application when setting the bottom heater 7, by setting the longitudinal circumferential heating zone 7-3, as shown in the attached Figure 7 As shown in , the problem of low temperature in the heating area of ​​the main heater 5 during the process of initiating the material can be effectively compensated, and the problem of failure to initiate initiation or poor initiation effect when the quartz crucible 3 is at a low crucible position can be avoided. When the initiation of initiation is basically completed and before the crystal pulling is started, the bottom heater 7 is gradually turned off and only the main heater 5 is kept working to provide the heat required in the process of crystal pulling, which can further reduce the heat radiation to the body of the quartz crucible 3, thereby further reducing the oxygen content entering the silicon melt 4 during the process of crystal pulling;

[0029] As attached Figure 3 As shown, in the present scheme, a total of 4 groups of U-shaped bottom heating zones 7-1 are arranged and distributed along a circular array, and the longitudinal circumferential heating zone 7-3 avoids the main heater electrode 5-3, the position of the bottom heater electrode 7-4 and the position of the exhaust hole and is also designed to be symmetrically distributed. After the polycrystalline material block collapses during the material processing, the crucible is rotated at 1-2rpm to ensure uniform heating. In this embodiment, a main heater 5 heating area height range (230-260mm) and an interval distance (30-40mm) between the top of the longitudinal circumferential heating zone 7-3 and the bottom of the main heater 5 are given to ensure a safe and effective height design. In addition, the structural design of the bottom heater 7 is not limited to the structure given in the drawings of the specification, and its specific design needs to be designed accordingly in combination with the chassis structural characteristics of different single crystal furnace bodies.

[0030] Embodiment 2, a process method for reducing the oxygen content of silicon crystals, using a thermal field system for reducing the oxygen content of silicon crystals in Embodiment 1, including chemical processing and crystal pulling, specifically comprising the following steps:

[0031] S1: Install the bottom heater and main heater in the furnace body;

[0032] S2: During the process of chemical reaction, the main heater and the bottom heater are turned on at the same time. The bottom heater uses 20-25kw, and the main heater uses 80-90kw. During the process, the given argon flow rate is 70-90slpm and the furnace pressure is 15-20torr.

[0033] S3: After the smelting is basically completed, the bottom heater is gradually turned off, and only the main heater is kept to provide the power and temperature requirements in the late stage of smelting and the crystal pulling process, so as to reduce the large-area reaction between the inner wall of the crucible and the silicon melt caused by the heat radiation of the main heater to the quartz crucible, thereby increasing the oxygen entering the silicon melt;

[0034] S4: After the material is oxidized, the crystal pulling process begins, including stabilization - seeding - shoulder placement - equal diameter - finishing. During the stabilization process, the stabilization time is increased by 0.5-1h compared with the usual time. That is, after the temperature fluctuation is ±1°C during the process, the high argon flow rate and low furnace pressure (60-80slpm / 15-20torr) are maintained to fully remove the oxygen and other impurities volatilized during the high-power oxidization process;

[0035] During the process of seeding, shoulder placement, equal diameter and finishing, a high argon flow rate (60-80slpm) is maintained, and the crucible speed and furnace pressure are controlled to complete the entire single crystal pulling process.

[0036] The following is a detailed description of this solution in conjunction with a specific embodiment, and the specific process is as follows:

[0037] The effect of this solution is verified by setting a comparative example and comparing the present embodiment. The comparative example and the present embodiment are carried out under the condition that a 20-inch heat field is installed in a CZ single crystal furnace and 70 kg of polysilicon material is loaded;

[0038] (1) In this embodiment, the main heater and bottom heater described above are used, and the process method described above is adopted at the same time, and the crystal orientation is obtained through the steps of evacuation - leak detection - material processing - stabilization - seeding - shoulder release - shoulder rotation - equal diameter - finishing. <100> Lightly boron-doped silicon single crystal;

[0039] (2) In the comparative example, a thermal field system with a common bottom heater (flat plate design, providing only bottom longitudinal heat) and a conventional main heater (heating zone covered with quartz crucible) was configured to obtain the same crystal orientation. <100> Lightly boron-doped silicon single crystal;

[0040] In the comparative analysis of the embodiments and comparative examples of the present invention, the description of other operation processes and control parameters in all links of single crystal pulling is omitted, that is, the operations and related control parameters in the embodiments and comparative examples are the same;

[0041] This embodiment:

[0042] The thermal field system used in the material processing is the bottom heater and the main heater described in the present invention. The specific process is as follows:

[0043] (1) During the chemical process, a chemical power of 20kw+85kw, an argon flow rate of 70slpm, a pressure of 20torr, and a gradual increase in the crucible position of the quartz crucible are used;

[0044] (2) After the material is basically oxidized, gradually turn off the bottom heater, rise to the seeding crucible position, reduce the main heater to the seeding power, continue to stabilize for 3 hours, maintain the argon flow rate of 70slpm and the pressure of 20torr, and complete the shouldering operation;

[0045] (3) During the equal diameter process, the argon flow rate is maintained at 60-80slpm, the furnace pressure is 30-50torr, and the crucible speed is 8-12rpm to complete the entire single crystal pulling process;

[0046] (4) The thermal field configuration used in this embodiment does not affect the execution of the process conditions, and a complete crystal orientation is obtained. <100> The overall oxygen content of the dislocation-free lightly doped boron silicon single crystal is distributed in the range of 7.32-11.53 ppma. Fig.10 shown.

[0047] Comparative Example:

[0048] During the material processing, a common bottom heater (flat plate design, only providing bottom longitudinal heat) and a conventional main heater (heating zone covers the quartz crucible) are configured, and the same process as in Example 1 is adopted, as follows:

[0049] (1) During the chemical process, a chemical power of 20kw+85kw, an argon flow rate of 70slpm, a pressure of 20torr, and a gradual increase in the crucible position of the quartz crucible are used;

[0050] (2) After the chemistry is basically completed, gradually turn off the bottom heater, reduce the main heater to the seeding power, continue stabilizing for 3 hours, maintain the argon flow rate at 70slpm and the pressure at 20torr, and complete the seeding and shouldering operation;

[0051] (3) During the equal diameter process, the argon flow rate is maintained at 60-80slpm, the furnace pressure is 30-50torr, and the crucible speed is 8-12rpm to complete the entire single crystal pulling process;

[0052] (4) Comparative Example 1 uses the above thermal field configuration and process technology to obtain a complete crystal orientation <100> The overall oxygen content of the dislocation-free lightly doped boron silicon single crystal is distributed in the range of 8.94-12.67 ppma. Fig.10 shown.

[0053] It can be easily concluded from the data structure of this embodiment and the comparative example that the arrangement of the main heater and the bottom heater in this solution can significantly reduce the overall oxygen content compared with the traditional arrangement of the main heater and the bottom heater, thereby improving the yield of the electronic components produced in subsequent processing.

[0054] The above is only for illustrating the present invention. It should be understood that the present invention is not limited to the above embodiments, and various variations that conform to the concept of the present invention are within the protection scope of the present invention.

Claims

1. A thermal field system capable of reducing the oxygen content of silicon crystals, comprising a furnace body and a quartz crucible (3) arranged in the furnace body, characterized in that: The furnace body is provided with a main heater (5) matched with the quartz crucible (3), and a bottom heater (7) is vertically spaced in the furnace body below the main heater (5), wherein the bottom heater (7) comprises four groups of U-shaped bottom heating zones (7-1) arranged horizontally and a longitudinal circumferential heating zone (7-3) arranged vertically, wherein the four groups of U-shaped bottom heating zones (7-1) are arranged in a circular array, and there is a gap between two adjacent groups of U-shaped bottom heating zones (7-1); the longitudinal circumferential heating zone (7-3) is located above the gap between two adjacent groups of U-shaped bottom heating zones (7-1); the main heater (5) comprises a central high-efficiency heating zone (5-1) of the main heater (5) and a main heater support body (5-2); the area size of the center (7-2) of the U-shaped bottom heating zone of the bottom heater 7 is designed to be larger than the maximum diameter of the lower shaft head (6); When the main heater (5) is set, the height of the heating area of ​​the main heater (5) is one third to two thirds of the height of the quartz crucible (3). The main heater (5) reduces the height of the heating area of ​​the heater to reduce the height range covered by the central high-efficiency heating area (5-1) of the heater itself, so that during the growth of the crystal, the contact area between the silicon melt (4) and the inside of the quartz crucible (3) is not completely between the central high-efficiency heating area (5-1) of the main heater (5), thereby reducing the degree of heating radiation to the quartz crucible (3), thereby reducing the degree of reaction between the inner wall of the quartz crucible (3) and the silicon melt (4), and reducing the amount of oxygen entering the silicon melt (4).

2. A process for reducing the oxygen content of silicon crystals, using a thermal field system for reducing the oxygen content of silicon crystals as claimed in claim 1, characterized in that: The process includes chemical processing and crystal pulling, and specifically includes the following steps: S1: Install the bottom heater and main heater in the furnace body; S2: During the process of chemical reaction, the main heater and the bottom heater are turned on at the same time. The bottom heater uses 20-25kw, and the main heater uses 80-90kw. During the process, the given argon flow rate is 70-90slpm and the furnace pressure is 15-20torr. S3: After the smelting is basically completed, the bottom heater is gradually turned off, and only the main heater is kept to provide the power and temperature requirements of the crystal pulling process after the smelting is completed; S4: After the material is oxidized, the crystal pulling process is carried out; The crystal pulling process in S4 includes stabilization, seeding, shoulder release, equal diameter, and finishing, which specifically includes the following steps: S4-1: Stabilization process: After the completion of the material sintering, continue to maintain a high argon flow rate of 60-80slpm and a low furnace pressure of 15-20torr. This stabilization process lasts for 0.5-1h. S4-2: Seeding, shoulder placement, equal diameter, and finishing process; maintain a high argon flow rate of 60-80slpm, and coordinate with the quartz crucible speed and furnace pressure control to complete the entire single crystal pulling process.

Citation Information

Patent Citations

  • Heater and monocrystalline silicon production method applying heater

    CN107460539A

  • Single crystal furnace capable of reducing crystal defects

    CN109680330A

  • Single crystal furnace heating device, single crystal furnace and heating method of single crystal furnace

    CN111733447A

  • Crystal pulling furnace for semiconductor monocrystalline silicon

    CN113061983A

  • Combined heater for single crystal furnace

    CN203923445U