A highly stable tensile conductive sealing strip and its application

By using a conductive structure composed of materials such as silicone rubber and graphene of a specific proportion in the conductive seal strip, combined with the tensile structure, the problems of poor sealing effect of the existing conductive seal strip and the peeling of the adhesive layer are solved, and high stability is achieved and excellent electromagnetic shielding performance.

CN115413213BActive Publication Date: 2024-11-22PINGHU ALLIED IND
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202111264981.7
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2021-10-28
Publication Date
2024-11-22
Estimated Expiration
2041-10-28

AI Technical Summary

Technical Problem

The sealing effect of existing conductive seal strips is poor, and it is prone to deformation due to external forces, resulting in electromagnetic radiation leakage and the bonding layer falling off, and it is unable to effectively play the role of sealing and electromagnetic shielding.

Method used

Tensile conductive seal strips including sealing body, tensile structure and conductive structure are adopted. The conductive structure consists of a specific proportion of silicone rubber, silicone compounds, graphene, conductive powder, processing aids and crosslinking agents, and are coextruded. Process molding forms arched structures and protrusions, enhancing mechanical properties and electromagnetic shielding properties.

Benefits of technology

It achieves a high-stable tensile conductive sealing effect, enhances the weather resistance and mechanical properties of the sealing strip, ensures excellent electromagnetic shielding performance, avoids permanent deformation and fall-off, and continuously and effectively seals and anti-interference.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN115413213B_ABST
    Figure CN115413213B_ABST
Patent Text Reader

Abstract

The present invention relates to the technical field of sealing strips, and more specifically to a highly stable tensile conductive sealing strip and its application, comprising a sealing body, a tensile structure, and a conductive structure, wherein the sealing body is coated with the tensile structure, and the conductive structure is arranged on the sealing body, and the raw materials of the conductive structure include 100 parts of silicone rubber, 4-6 parts of siloxane compounds, 3-5 parts of graphene, 230-280 parts of conductive powder, 2-5 parts of processing aids, 2-4 parts of coupling agents, and 5-7 parts of cross-linking agents, in terms of weight. The conductive part formed by the present invention by selecting specific components and proportions not only enables the sealing strip to play an electromagnetic shielding role for a long time, but also has certain weather resistance and aging resistance, ensuring that the sealing strip has high stability under various environmental conditions, and in addition, through the coordinated cooperation with the anti-stretching part and the main body, the sealing strip plays a stable and continuous sealing and anti-interference effect.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the technical field of sealing strips, in particular to IPC classification number H05K9 / 00, and more particularly to a highly stable tensile conductive sealing strip and application thereof. Background Art

[0002] Electrically powered components such as electronic devices will generate electromagnetic radiation. If they are not electromagnetically shielded, they will interfere with the normal operation of adjacent components.

[0003] At present, some conductive sealing strips on the market have poor sealing effects, resulting in leakage of electromagnetic radiation. In addition, their mechanical properties are insufficient and they are easily deformed by external forces. Patent CN201820945922 discloses a conductive sealing strip, including a sealing strip, an adhesive layer and a conductive layer, so that it has excellent sealing and environmental isolation functions, as well as aesthetics and comfort. However, due to the addition of an adhesive layer, the sealing strip may fall off due to changes in the environment or the action of external forces, and thus cannot play a sealing role. Summary of the invention

[0004] In response to the above-mentioned technical problems, on the one hand, the present invention provides a highly stable tensile conductive sealing strip, including a sealing body, a tensile structure, and a conductive structure. The sealing body is coated with the tensile structure, and the conductive structure is arranged on the sealing body. The raw materials of the conductive structure include 100 parts of silicone rubber, 4-6 parts of siloxane compounds, 3-5 parts of graphene, 230-280 parts of conductive powder, 2-5 parts of processing aids, 2-4 parts of coupling agents, and 5-7 parts of cross-linking agents, in parts by weight.

[0005] Preferably, in parts by weight, the raw materials of the conductive structure include 100 parts of silicone rubber, 4.5 parts of siloxane compounds, 4.5 parts of graphene, 255 parts of conductive powder, 3.5 parts of processing aids, 3 parts of coupling agents, and 6 parts of cross-linking agents.

[0006] In some embodiments, the sealing body is an arched structure, the conductive structure is disposed in the middle of the arched structure, and the conductive structure is disposed through the middle of the sealing body.

[0007] In some embodiments, protrusions are provided on both sides of the arch bridge structure of the sealing body along the outer contour, and the number of the protrusions is 8-16.

[0008] Preferably, the number of the protrusions is twelve.

[0009] In some embodiments, the tensile structure includes two parts, which are respectively arranged inside the two sides of the arch bridge.

[0010] In some embodiments, the silicone rubber includes methyl vinyl silicone rubber or fluorosilicone rubber.

[0011] Preferably, the methyl vinyl silicone rubber has a molecular weight of 400,000-800,000 and a vinyl content of 0.13-0.2 mol%, and is purchased from Shenzhen Chuangyou Silicone Rubber Technology Co., Ltd. with a model number of 110-2.

[0012] In some embodiments, the weight ratio of the siloxane compound to the graphene is 1:(0.8-1.2).

[0013] Preferably, the weight ratio of the siloxane compound to graphene is 1:1.

[0014] In some embodiments, the siloxane compound includes a mixture of hydrogen silicone oil and methyl silicone oil in a weight ratio of 1:(0.5-1).

[0015] Preferably, the siloxane compound comprises a mixture of hydrogenated silicone oil and methyl silicone oil in a weight ratio of 1:0.75.

[0016] In some embodiments, the kinematic viscosity of the methyl silicone oil is 80-120 mm 2 / s.

[0017] Preferably, the kinematic viscosity of the methyl silicone oil is 90-110 mm 2 / s, purchased from Shandong Kepler Biotechnology Co., Ltd., model 201.

[0018] In some embodiments, the conductive powder includes nickel-coated aluminum powder and / or silver-coated glass microbead powder.

[0019] Preferably, the conductive powder comprises nickel-coated aluminum powder and silver-coated glass microbead powder in a weight ratio of (1-1.5):1.

[0020] More preferably, the conductive powder includes nickel-coated aluminum powder and silver-coated glass microbead powder in a weight ratio of 1.2:1.

[0021] In some embodiments, the hydrogen-containing silicone oil has a viscosity of 10-70 cps at 25° C. and a hydrogen content of 0.1-1.5 wt.%.

[0022] In some embodiments, the surface area of ​​the graphene is 250 to 380 m 2 / g, particle size D50<10μm.

[0023] Preferably, the surface area of ​​the graphene is 260 to 350 m 2 / g, particle size D50<10μm, purchased from Shanghai Fuqi Industry and Trade Co., Ltd., model FQ-62.

[0024] In some embodiments, the cross-linking agent includes a mixture of benzoyl peroxide and di-tert-butyl peroxide in a weight ratio of (0.75-1.2):1.

[0025] Preferably, the cross-linking agent comprises a combination of benzoyl peroxide and di-tert-butyl peroxide in a weight ratio of 1:1.

[0026] In some embodiments, the coupling agent includes at least one of vinyltrimethoxysilane and vinyltriethoxysilane.

[0027] The applicant discovered in the study that the raw materials of the conductive structure not only affect the sealing effect and electromagnetic shielding performance of the sealing strip, but also have an important impact on its mechanical properties and weather resistance. At present, there is a certain difficulty in balancing various performances. The applicant unexpectedly discovered that the raw materials of the conductive structure in the present system are added with methyl vinyl silicone rubber and siloxane compounds with a specific vinyl content, especially the methyl vinyl silicone rubber with a vinyl content of 0.13-0.2 mol%, and the siloxane compound includes hydrogenated silicone oil and methyl silicone oil in a weight ratio of 1: (0.5-1), which can make the conductive structure part have better weather resistance and mechanical properties. The applicant believes that the possible reason The reason is that methyl vinyl silicone rubber can react with hydrogen-containing silicone oil and methyl silicone oil, thereby increasing the complexity of the silicone rubber three-dimensional network and increasing the stability of the conductive structure. In addition, since the molecular chains of hydrogen-containing silicone oil and methyl silicone oil are relatively short, the interaction between the silicone rubber molecular chains is reduced, and the flexibility and resilience of the molecules are improved, thereby reducing the probability of permanent deformation of the sealing strip in actual use. At the same time, the conductive powder and graphene can be evenly distributed in the three-dimensional network, and the two produce a good synergistic effect, so that the electromagnetic shielding performance of the sealing strip is excellent. Through the coordinated cooperation with the tensile part and the main body, the sealing strip can achieve stable and continuous sealing and anti-interference effects.

[0028] In some embodiments, the processing aid is zinc stearate.

[0029] In some embodiments, the material of the main body includes 100 parts of silicone rubber containing vinyl, 55 parts of filler, 8 parts of anti-structuring agent, 1.5 parts of metal complex, 2.5 parts of regulator, and 5 parts of vulcanizer.

[0030] In some embodiments, the silicone rubber containing vinyl groups includes methyl vinyl silicone rubber and methyl phenyl vinyl silicone rubber, and the weight ratio is 1:(0.2-0.5), preferably 1:0.35.

[0031] In some embodiments, the methyl vinyl silicone rubber has a molecular weight of 400,000-800,000 and a vinyl content of 0.13-0.2 mol%, and can be purchased from Shenzhen Chuangyou Silicone Rubber Technology Co., Ltd., model 110-2.

[0032] In some embodiments, the methylphenyl vinyl silicone rubber has a molecular weight of 400,000-800,000 and is purchased from Anhui IOTA Silicone Oil Co., Ltd. with a model number of IOTA120.

[0033] In some embodiments, the filler material includes kaolin and white carbon.

[0034] In some embodiments, the white carbon black comprises a mixture of fumed white carbon black and precipitated white carbon black, and the weight ratio is 1: (0.6-1), preferably 1: 0.8; the average particle size of the fumed white carbon black is 12nm, and the specific surface area is 175-225m 2 / g, brand name is Degussa A200; the particle size of the precipitated silica is 4-10 μm, and the specific surface area is 200-240 m 2 / g, can be purchased from Boai County Xiangsheng Silica Powder Co., Ltd.

[0035] In some embodiments, the kaolin is modified calcined kaolin with a particle size of 6250 mesh, which can be purchased from Shanghai Huijing Sub-Nano New Materials Co., Ltd.

[0036] In some embodiments, the regulator is one of vinyl silicone oil and vinyl silicone resin, preferably vinyl silicone oil, and the vinyl content of the vinyl silicone oil is 0.22-0.26 wt.%.

[0037] In some embodiments, the anti-structuring agent is dihydroxy polydimethylsiloxane.

[0038] In some embodiments, the metal complex is a complex of titanium and cerium with diphenylsilanediol.

[0039] In some embodiments, the vulcanizing agent includes 35 wt % of a catalyst and 65 wt % of a cross-linking agent.

[0040] In some embodiments, the catalyst includes 0.5 wt % of platinum catalyst and 99.5 wt % of methyl vinyl silicone rubber; the crosslinking agent includes 40 wt % of hydrogenated silicone oil, 59 wt % of methyl vinyl silicone rubber, and 1 wt % of ethynyl cyclohexanol.

[0041] In some embodiments, the material of the anti-stretching part is the same as that of the main body, except that the filler is 60 parts.

[0042] In some embodiments, the sealing body, the tensile structure and the conductive structure are formed by a co-extrusion process.

[0043] Another aspect of the present invention provides an application of a highly stable tensile conductive sealing strip for sealing and electromagnetic shielding at an interface of electronic equipment.

[0044] Beneficial effects:

[0045] (1) The raw materials of the conductive structure in this system are added with methyl vinyl silicone rubber and siloxane compounds with a specific vinyl content, especially the vinyl content of the methyl vinyl silicone rubber is 0.13-0.2 mol%, and the siloxane compound includes hydrogen-containing silicone oil and methyl silicone oil in a weight ratio of 1: (0.5-1), which can make the conductive structure part have better weather resistance and mechanical properties;

[0046] (2) The conductive powder and graphene used in the present invention can be evenly distributed in a three-dimensional network, and the two produce a good synergistic effect, so that the electromagnetic shielding performance of the sealing strip is excellent; through the coordinated cooperation with the tensile part and the main body, the sealing strip can achieve stable and continuous sealing and anti-interference effects. BRIEF DESCRIPTION OF THE DRAWINGS

[0047] Figure 1 is a schematic diagram of the cross-sectional structure of a highly stable tensile conductive sealing strip provided in Example 1;

[0048] Figure 2 is a schematic diagram of the cross-sectional structure of a highly stable tensile conductive sealing strip provided in Example 2;

[0049] Figure 3 It is a schematic diagram of the cross-sectional structure of a highly stable tensile conductive sealing strip provided in Example 3.

[0050] 1. Sealed body; 2. Tensile-resistant structure; 3. Conductive structure. DETAILED DESCRIPTION

[0051] Example 1

[0052] Please refer to Figure 1 On the one hand, this embodiment provides a highly stable tensile conductive sealing strip, including a sealing body 1, a tensile structure 2, and a conductive structure 3. The sealing body 1 is arranged to cover the tensile structure 2. In terms of weight, the raw materials of the conductive structure 3 include 100 parts of silicone rubber, 4.5 parts of siloxane compounds, 4.5 parts of graphene, 255 parts of conductive powder, 3.5 parts of processing aids, 3 parts of coupling agents, and 6 parts of cross-linking agents.

[0053] The sealing body 1 is an arched structure, and the conductive structure 3 is arranged in the middle of the arched structure. The conductive structure 3 runs through the middle of the sealing body 1 .

[0054] The silicone rubber is methyl vinyl silicone rubber purchased from Shenzhen Chuangyou Silicone Rubber Technology Co., Ltd., with a model of 110-2, a molecular weight of 400,000-800,000, and a vinyl content of 0.13-0.2 mol%.

[0055] The siloxane compound includes a mixture of hydrogen silicone oil and methyl silicone oil in a weight ratio of 1:0.75.

[0056] The kinematic viscosity of the methyl silicone oil is 90-110 mm 2 / s, purchased from Shandong Kepler Biotechnology Co., Ltd., model 201.

[0057] The conductive powder includes nickel-coated aluminum powder and silver-coated glass microbead powder, with a weight ratio of 1.2:1.

[0058] The nickel-coated aluminum powder was purchased from Wuhan Beichenxing High-tech Materials Technology Co., Ltd., and the silver-coated glass microbead powder was purchased from Huizhou Tenghui Technology Co., Ltd., model JC-20.

[0059] The hydrogen-containing silicone oil was purchased from Qingdao Xingye Organic Silicone New Materials Co., Ltd., with a viscosity of 10-70 cps at 25° C. and a hydrogen content of 0.1-1.5 wt.%.

[0060] The graphene was purchased from Shanghai Fuqi Industry and Trade Co., Ltd., model FQ-62, with a surface area of ​​260-350m 2 / g, particle size D50<10μm.

[0061] The cross-linking agent comprises a compound of benzoyl peroxide and di-tert-butyl peroxide, with a weight ratio of 1:1.

[0062] The coupling agent is vinyltrimethoxysilane.

[0063] The processing aid is zinc stearate.

[0064] The material of the main body includes 100 parts of silicone rubber containing vinyl, 55 parts of filler, 8 parts of anti-structuring agent, 1.5 parts of metal complex, 2.5 parts of regulator, and 5 parts of vulcanizer.

[0065] The silicone rubber containing vinyl includes methyl vinyl silicone rubber and methyl phenyl vinyl silicone rubber, and the weight ratio is 1:0.35.

[0066] The methyl vinyl silicone rubber has a molecular weight of 400,000-800,000 and a vinyl content of 0.13-0.2 mol%, and is purchased from Shenzhen Chuangyou Silicone Rubber Technology Co., Ltd. with a model number of 110-2.

[0067] The molecular weight of the methylphenyl vinyl silicone rubber is 400,000-800,000 and it is purchased from Anhui IOTA Silicone Oil Co., Ltd. with the model number of IOTA120.

[0068] The filler materials include kaolin and white carbon black.

[0069] The white carbon black comprises a mixture of gas phase white carbon black and precipitated white carbon black, and the weight ratio is 1:0.8; the average particle size of the gas phase white carbon black is 12nm, and the specific surface area is 175-225m 2 / g, brand name is Degussa A200; the particle size of the precipitated silica is 4-10 μm, and the specific surface area is 200-240 m 2 / g, can be purchased from Boai County Xiangsheng Silica Powder Co., Ltd.

[0070] The kaolin is modified calcined kaolin with a particle size of 6250 mesh, which can be purchased from Shanghai Huijing Suba-Nano New Materials Co., Ltd.

[0071] The regulator is vinyl silicone oil, and the vinyl content is 0.22-0.26wt.%.

[0072] The anti-structuring agent is dihydroxy polydimethylsiloxane.

[0073] The metal complex is a complex of titanium, cerium and diphenylsilanediol.

[0074] The vulcanizing agent includes 35 wt % of a catalyst and 65 wt % of a cross-linking agent.

[0075] The catalyst comprises 0.5 wt % of platinum catalyst and 99.5 wt % of methyl vinyl silicone rubber; the cross-linking agent comprises 40 wt % of hydrogenated silicone oil, 59 wt % of methyl vinyl silicone rubber and 1 wt % of ethynyl cyclohexanol.

[0076] The material of the anti-stretching part is the same as that of the main body, except that the filler is 60 parts.

[0077] The sealing body, the tensile structure and the conductive structure are formed by a co-extrusion process.

[0078] Another aspect of the present embodiment provides an application of a highly stable tensile conductive sealing strip for use in sealing and electromagnetic shielding at interfaces of electronic equipment.

[0079] Example 2

[0080] Please refer to Figure 2 On the one hand, this embodiment provides a highly stable tensile conductive sealing strip, including a sealing body 1, a tensile structure 2, and a conductive structure 3. The sealing body 1 is provided to cover the tensile structure 2. In terms of weight, the raw materials of the conductive structure 3 include 100 parts of silicone rubber, 4 parts of siloxane compounds, 5 parts of graphene, 230 parts of conductive powder, 3.5 parts of processing aids, 3 parts of coupling agents, and 6 parts of cross-linking agents.

[0081] The sealing body 1 is an arched structure, and the conductive structure 3 is arranged in the middle of the arched structure. The conductive structure 3 runs through the middle of the sealing body 1 .

[0082] Both sides of the arch bridge structure of the sealing body are provided with protrusions along the outer contour, and the number of the protrusions is 12.

[0083] The silicone rubber is methyl vinyl silicone rubber purchased from Shenzhen Chuangyou Silicone Rubber Technology Co., Ltd., with a model of 110-2, a molecular weight of 400,000-800,000, and a vinyl content of 0.13-0.2 mol%.

[0084] The siloxane compound includes a mixture of hydrogen silicone oil and methyl silicone oil in a weight ratio of 1:0.5.

[0085] The kinematic viscosity of the methyl silicone oil is 90-110 mm 2 / s, purchased from Shandong Kepler Biotechnology Co., Ltd., model 201.

[0086] The conductive powder includes nickel-coated aluminum powder and silver-coated glass microbead powder, with a weight ratio of 1:1.

[0087] The nickel-coated aluminum powder was purchased from Wuhan Beichenxing High-tech Materials Technology Co., Ltd., and the silver-coated glass microbead powder was purchased from Huizhou Tenghui Technology Co., Ltd., model JC-20.

[0088] The hydrogen-containing silicone oil was purchased from Qingdao Xingye Organic Silicone New Materials Co., Ltd., with a viscosity of 10-70 cps at 25° C. and a hydrogen content of 0.1-1.5 wt.%.

[0089] The graphene was purchased from Shanghai Fuqi Industry and Trade Co., Ltd., model FQ-62, with a surface area of ​​260-350m 2 / g, particle size D50<10μm.

[0090] The cross-linking agent comprises a compound of benzoyl peroxide and di-tert-butyl peroxide, with a weight ratio of 0.75:1.

[0091] The coupling agent is vinyltrimethoxysilane.

[0092] The processing aid is zinc stearate.

[0093] The material of the main body includes 100 parts of silicone rubber containing vinyl, 55 parts of filler, 8 parts of anti-structuring agent, 1.5 parts of metal complex, 2.5 parts of regulator, and 5 parts of vulcanizer.

[0094] The silicone rubber containing vinyl includes methyl vinyl silicone rubber and methyl phenyl vinyl silicone rubber, and the weight ratio is 1:0.35.

[0095] The methyl vinyl silicone rubber has a molecular weight of 400,000-800,000 and a vinyl content of 0.13-0.2 mol%, and is purchased from Shenzhen Chuangyou Silicone Rubber Technology Co., Ltd. with a model number of 110-2.

[0096] The molecular weight of the methylphenyl vinyl silicone rubber is 400,000-800,000 and it is purchased from Anhui IOTA Silicone Oil Co., Ltd. with the model number of IOTA120.

[0097] The filler materials include kaolin and white carbon black.

[0098] The white carbon black comprises a mixture of gas phase white carbon black and precipitated white carbon black, and the weight ratio is 1:0.8; the average particle size of the gas phase white carbon black is 12nm, and the specific surface area is 175-225m 2 / g, brand name is Degussa A200; the particle size of the precipitated silica is 4-10 μm, and the specific surface area is 200-240 m 2 / g, can be purchased from Boai County Xiangsheng Silica Powder Co., Ltd.

[0099] The kaolin is modified calcined kaolin with a particle size of 6250 mesh, which can be purchased from Shanghai Huijing Suba-Nano New Materials Co., Ltd.

[0100] The regulator is vinyl silicone oil, and the vinyl content is 0.22-0.26wt.%.

[0101] The anti-structuring agent is dihydroxy polydimethylsiloxane.

[0102] The metal complex is a complex of titanium, cerium and diphenylsilanediol.

[0103] The vulcanizing agent includes 35 wt % of a catalyst and 65 wt % of a cross-linking agent.

[0104] The catalyst comprises 0.5 wt % of platinum catalyst and 99.5 wt % of methyl vinyl silicone rubber; the cross-linking agent comprises 40 wt % of hydrogenated silicone oil, 59 wt % of methyl vinyl silicone rubber and 1 wt % of ethynyl cyclohexanol.

[0105] The material of the anti-stretching part is the same as that of the main body, except that the filler is 60 parts.

[0106] The sealing body, the tensile structure and the conductive structure are formed by a co-extrusion process.

[0107] Another aspect of the present embodiment provides an application of a highly stable tensile conductive sealing strip for use in sealing and electromagnetic shielding at interfaces of electronic equipment.

[0108] Example 3

[0109] Please refer to Figure 3 On the one hand, this embodiment provides a highly stable tensile conductive sealing strip, including a sealing body 1, a tensile structure 2, and a conductive structure 3. The sealing body 1 is provided to cover the tensile structure 2. In terms of weight, the raw materials of the conductive structure 3 include 100 parts of silicone rubber, 6 parts of siloxane compounds, 5 parts of graphene, 280 parts of conductive powder, 5 parts of processing aids, 4 parts of coupling agents, and 7 parts of cross-linking agents.

[0110] The sealing body 1 is an arched structure, and the conductive structure 3 is arranged in the middle of the arched structure. The conductive structure 3 runs through the middle of the sealing body 1 .

[0111] Both sides of the arch bridge structure of the sealing body are provided with protrusions along the outer contour, and the number of the protrusions is 12.

[0112] The tensile structure comprises two parts, which are respectively arranged inside the two sides of the arch bridge.

[0113] The silicone rubber is methyl vinyl silicone rubber purchased from Shenzhen Chuangyou Silicone Rubber Technology Co., Ltd., with a model of 110-2, a molecular weight of 400,000-800,000, and a vinyl content of 0.13-0.2 mol%.

[0114] The siloxane compound includes a mixture of hydrogen silicone oil and methyl silicone oil in a weight ratio of 1:0.5.

[0115] The kinematic viscosity of the methyl silicone oil is 90-110 mm 2 / s, purchased from Shandong Kepler Biotechnology Co., Ltd., model 201.

[0116] The conductive powder includes nickel-coated aluminum powder and silver-coated glass microbead powder, with a weight ratio of 1:1.

[0117] The nickel-coated aluminum powder was purchased from Wuhan Beichenxing High-tech Materials Technology Co., Ltd., and the silver-coated glass microbead powder was purchased from Huizhou Tenghui Technology Co., Ltd., model JC-20.

[0118] The hydrogen-containing silicone oil was purchased from Qingdao Xingye Organic Silicone New Materials Co., Ltd., with a viscosity of 10-70 cps at 25° C. and a hydrogen content of 0.1-1.5 wt.%.

[0119] The graphene was purchased from Shanghai Fuqi Industry and Trade Co., Ltd., model FQ-62, with a surface area of ​​260-350m 2 / g, particle size D50<10μm.

[0120] The cross-linking agent comprises a compound of benzoyl peroxide and di-tert-butyl peroxide, with a weight ratio of 0.75:1.

[0121] The coupling agent is vinyltrimethoxysilane.

[0122] The processing aid is zinc stearate.

[0123] The material of the main body includes 100 parts of silicone rubber containing vinyl, 55 parts of filler, 8 parts of anti-structuring agent, 1.5 parts of metal complex, 2.5 parts of regulator, and 5 parts of vulcanizer.

[0124] The silicone rubber containing vinyl includes methyl vinyl silicone rubber and methyl phenyl vinyl silicone rubber, and the weight ratio is 1:0.35.

[0125] The methyl vinyl silicone rubber has a molecular weight of 400,000-800,000 and a vinyl content of 0.13-0.2 mol%, and is purchased from Shenzhen Chuangyou Silicone Rubber Technology Co., Ltd. with a model number of 110-2.

[0126] The molecular weight of the methylphenyl vinyl silicone rubber is 400,000-800,000 and it is purchased from Anhui IOTA Silicone Oil Co., Ltd. with the model number of IOTA120.

[0127] The filler materials include kaolin and white carbon black.

[0128] The white carbon black comprises a mixture of gas phase white carbon black and precipitated white carbon black, and the weight ratio is 1:0.8; the average particle size of the gas phase white carbon black is 12nm, and the specific surface area is 175-225m 2 / g, brand name is Degussa A200; the particle size of the precipitated silica is 4-10 μm, and the specific surface area is 200-240 m 2 / g, can be purchased from Boai County Xiangsheng Silica Powder Co., Ltd.

[0129] The kaolin is modified calcined kaolin with a particle size of 6250 mesh, which can be purchased from Shanghai Huijing Suba-Nano New Materials Co., Ltd.

[0130] The regulator is vinyl silicone oil, and the vinyl content is 0.22-0.26wt.%.

[0131] The anti-structuring agent is dihydroxy polydimethylsiloxane.

[0132] The metal complex is a complex of titanium, cerium and diphenylsilanediol.

[0133] The vulcanizing agent includes 35 wt % of a catalyst and 65 wt % of a cross-linking agent.

[0134] The catalyst comprises 0.5 wt % of platinum catalyst and 99.5 wt % of methyl vinyl silicone rubber; the cross-linking agent comprises 40 wt % of hydrogenated silicone oil, 59 wt % of methyl vinyl silicone rubber and 1 wt % of ethynyl cyclohexanol.

[0135] The material of the anti-stretching part is the same as that of the main body, except that the filler is 60 parts.

[0136] The sealing body, the tensile structure and the conductive structure are formed by a co-extrusion process.

[0137] Another aspect of the present embodiment provides an application of a highly stable tensile conductive sealing strip for use in sealing and electromagnetic shielding at interfaces of electronic equipment.

[0138] Example 4

[0139] This embodiment provides a highly stable tensile conductive sealing strip, and the specific implementation method is the same as that of Embodiment 1, except that the siloxane compound does not include graphene.

[0140] Example 5

[0141] This embodiment provides a highly stable tensile conductive sealing strip, and the specific implementation is the same as that of Embodiment 1, except that the conductive powder does not include nickel-coated aluminum powder.

[0142] Performance Testing

[0143] 1. Volume resistivity

[0144] The volume resistivity of the tensile conductive sealing strips described in Examples 1-5 was tested according to the MIL-DTL-83528 standard. The results are shown in Table 1.

[0145] Table 1

[0146] serial number Volume resistivity / Ω﹒cm Example 1 0.03 Example 2 0.07 Example 3 0.05 Example 4 0.2 Example 5 0.16

Claims

1. A highly stable tensile conductive sealing strip, characterized in that: It comprises a sealing body, a tensile structure and a conductive structure, wherein the sealing body covers the tensile structure, and the conductive structure is arranged on the sealing body. The raw materials of the conductive structure include 100 parts of silicone rubber, 4-6 parts of siloxane compounds, 3-5 parts of graphene, 230-280 parts of conductive powder, 2-5 parts of processing aids, 2-4 parts of coupling agents, and 5-7 parts of cross-linking agents in parts by weight. The sealing body is an arched structure, the conductive structure is arranged in the middle of the arched structure, and the conductive structure is arranged through the middle of the sealing body; The silicone rubber comprises methyl vinyl silicone rubber, the vinyl content of the methyl vinyl silicone rubber is 0.13-0.2 mol%, and the siloxane compound comprises hydrogen-containing silicone oil and methyl silicone oil in a weight ratio of 1:(0.5-1); The weight ratio of the siloxane compound to the graphene is 1:(0.8-1.2), and the conductive powder includes nickel-coated aluminum powder and silver-coated glass microbead powder, and the weight ratio is (1-1.5):

1.

2. The highly stable tensile conductive sealing strip according to claim 1, characterized in that: Both sides of the arch bridge structure of the sealing body are provided with protrusions along the outer contour, and the number of the protrusions is 8-16.

3. The highly stable tensile conductive sealing strip according to claim 1, characterized in that: The tensile structure comprises two parts, which are respectively arranged inside the two sides of the arch bridge.

4. The highly stable tensile conductive sealing strip according to claim 3, characterized in that: The kinematic viscosity of the methyl silicone oil is 80-120 mm 2 / s.

5. The highly stable tensile conductive sealing strip according to claim 1, characterized in that: The conductive powder includes nickel-coated aluminum powder and / or silver-coated glass microbead powder.

6. The highly stable tensile conductive sealing strip according to claim 1, characterized in that: The sealing body, the tensile structure and the conductive structure are formed by a co-extrusion process.

7. An application of a highly stable tensile conductive sealing strip according to any one of claims 1 to 6, characterized in that: Used for sealing and electromagnetic shielding at interfaces of electronic equipment.