A low-carbon sound insulation floor mortar

By using ore powder and acid to treat waste tire particles and high-strength fibers in sound insulation mortar, the existing sound insulation mortar has solved the problems of high cost and large carbon emissions, and achieved low-carbon and environmentally friendly sound insulation effect, significantly reducing noise through the building The problem of things.

CN116102296BActive Publication Date: 2024-11-05HENAN JIAFANG IND CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202211531533.3
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2022-12-01
Publication Date
2024-11-05
Estimated Expiration
2042-12-01

AI Technical Summary

Technical Problem

The existing sound insulation mortar is costly and has a large carbon emission, making it difficult to effectively reduce noise pollution and carbon emissions during construction.

Method used

Use mineral powder instead of cement, use waste tire particles instead of rubber blocks, and improve its binding capacity through acid leaching and shape improvement, add high-strength fibers to improve strength and sound insulation performance, reduce cement usage and use mineral powder, combined with hollow tubular glass Fiber to improve sound insulation.

Benefits of technology

It effectively reduces the production cost and carbon emissions of mortar, improves the sound insulation performance and strength, significantly reduces the problem of noise passing through floor slabs and walls, and uses waste tire resources to achieve a low-carbon and environmentally friendly sound insulation effect.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN116102296B_ABST
    Figure CN116102296B_ABST
Patent Text Reader

Abstract

The invention discloses a low-carbon sound insulation floor mortar, which relates to the technical field of cement mortar. The mortar comprises the following raw materials in parts by weight: 0-100 parts of cement, 35-40 parts of anhydrite, 250-350 parts of mineral powder, 12-16 parts of latex powder, 80-120 parts of river sand, 2-4 parts of water reducer, 5-7 parts of calcium formate, 120-150 parts of waste tire particles, and 20-50 parts of high-strength fiber. The shape of the waste tire particles includes granular and strip-shaped. The weight ratio of the granular in the waste tire particles is 20%-40%, wherein the high-strength fiber is steel fiber or glass fiber, preferably hollow tubular glass fiber. The invention produces good sound insulation and noise reduction effects by adding waste tire particles and hollow tubular high-strength fibers, and the cost is much lower than that of the existing floor sound insulation mortar, and the cement content in the mortar is significantly lower than that of the existing products, which can greatly reduce the carbon emissions during the construction process.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of cement mortar, in particular to a low-carbon sound insulation floor mortar. Background Art

[0002] The sound insulation effect of buildings has an important impact on people's life, sleep and work quality. According to the provisions of GB50118-2010 "Civil Building Sound Insulation Design Code", the sound insulation standard of household walls and floor slabs of residential buildings should be greater than 53dB. However, the measurement point for indoor noise in this standard is located in the center of the room and is 1.2m or more above the ground. Buildings built according to this standard have good sound insulation effect for airborne sound sources, that is, when the sound source is not in contact with the building wall or the ground, most of the noise will be blocked, reflected or absorbed by the wall and floor slab. However, for some noise caused by collision, moving objects, and running, since the sound source is located on the wall or ground surface, and the transmission ability of concrete and steel bars to sound waves is stronger than air, it is easy to penetrate the walls and floors, causing interference to neighbors. The resulting neighborhood conflicts have been frequently reported in the newspapers in recent years.

[0003] CN102249614A discloses a lightweight thermal insulation and sound-insulating damping floor mortar, which uses inorganic silicate as a cementitious material, and therefore has good compatibility with cement mortar and concrete base, strong bonding, avoids hollowing phenomenon, and adapts to various base conditions. In the case of poor flatness, it can also have a leveling function, and the construction is very simple. It can be scraped and used after adding water and stirring evenly. The entire sound insulation layer is a whole, which greatly reduces the existence of sound bridges, has moderate compressive strength, is not easy to deform, and will not significantly increase the load of the building. It has a very low thermal conductivity, so that the floor has a thermal insulation effect while being soundproof. However, a higher proportion of rubber powder needs to be added in this scheme, and rubber is expensive. Whether it is natural rubber or synthetic rubber, the price is dozens of times that of ordinary cement, thereby greatly increasing the production cost of mortar.

[0004] In addition, cement accounts for a large proportion of the existing cement mortar. During the solidification process of cement, calcium carbonate decomposes and produces a large amount of CO2 gas. Therefore, a large amount of carbon emissions will be generated during the construction process. Infrastructure construction occupies an important part of my country's economic activities. Reducing carbon emissions during the construction process is an important way to achieve carbon reduction goals. Summary of the invention

[0005] The purpose of the present invention is to provide a low-carbon sound insulation floor mortar, which has the advantages of low carbon and environmental protection, good sound insulation effect and low cost, so as to solve the problems of high cost and large carbon emission of existing sound insulation mortar.

[0006] The technical solution adopted by the present invention is as follows:

[0007] A low-carbon sound insulation floor mortar comprises the following raw materials in parts by weight: 0-100 parts of cement, 35-40 parts of anhydrite, 250-350 parts of mineral powder, 12-16 parts of latex powder, 80-120 parts of river sand, 2-4 parts of water reducing agent, 5-7 parts of calcium formate, 120-150 parts of waste tire particles, and 20-50 parts of high-strength fiber. The waste tire particles have a shape of granules and strips, and the weight ratio of the granules in the waste tire particles is 20%-40%.

[0008] Preferably, the amount of cement used does not exceed 25% of the amount of mineral powder used.

[0009] Preferably, the waste tire particles are treated with acid leaching.

[0010] Preferably, the waste tire particles are in the form of strips, and among the waste tire particles, the cross-sectional shape of the strip-shaped particles is H-shaped, O-shaped, or square with a V-shaped groove.

[0011] Preferably, the high-strength fiber is steel fiber or glass fiber.

[0012] Preferably, the acid leaching process of the waste tire particles is to soak them in carboxylic acid with a concentration of 10% to 30% at room temperature for 10 hours or longer, and then wash them with water and dry them.

[0013] Preferably, the high-strength fiber is glass fiber, the glass fiber is in the shape of a hollow tube with both ends closed, and the surface of the glass fiber is treated with a silane coupling wetting agent.

[0014] Preferably, the carboxylic acid is acetic acid, oxalic acid, citric acid or a mixture thereof.

[0015] In summary, due to the adoption of the above technical solution, the beneficial effects of the present invention are:

[0016] (1) Using mineral powder instead of cement reduces the calcium carbonate content in the mortar, which can effectively reduce CO2 emissions during the mortar solidification process. Using waste tires instead of commercially available rubber blocks effectively reduces the cost of mortar.

[0017] (2) By acid leaching the waste tire particles, the bonding ability between the tire particles and other components in the mortar is effectively improved, thus avoiding the problems of loose structure and decreased strength of the mortar after solidification. In addition, the shape of the waste tire particles is improved to improve their sound insulation performance.

[0018] (3) High-strength fibers are added to improve strength, which can improve the strength reduction problem caused by mineral powder. The use of hollow tubular glass fibers further improves the sound insulation performance and reduces the amount of rubber particles used. BRIEF DESCRIPTION OF THE DRAWINGS

[0019] Figure 1 The waste tire particles are long strips with different cross-sectional shapes, wherein a, b, c, and d are H-shaped, O-shaped, square with 2 V-shaped grooves, and square with 4 V-shaped grooves, respectively. DETAILED DESCRIPTION

[0020] The present invention mainly provides a low-carbon sound insulation floor mortar, which can be used for floor and wall construction during the decoration of residential buildings, and can reduce carbon emissions during the construction process. The floors and walls after construction have good sound insulation effects and can significantly reduce the noise penetration caused by object collisions.

[0021] In order to make the purpose, technical solutions and advantages of the present invention more clearly understood, the present invention is further described in detail below in conjunction with the accompanying drawings and embodiments. It should be understood that the specific embodiments described herein are only used to explain the present invention and are not intended to limit the present invention.

[0022] Since the amount of waste tires generated each year is very considerable, the price of waste tires is much lower than that of commercially available rubber blocks. Waste tires can be used to replace rubber particles in mortar to reduce costs. However, after experiments, the applicant directly crushed the waste tires into 10-80 mesh particles, mixed them into cement mortar, and made blocks. The compression and flexural properties of the blocks after solidification were significantly lower than those of the particles made by adding rubber blocks. This is because carbon black, sulfur, vulcanization accelerators, softeners and other ingredients are added during the tire production process. The rubber powder composed of multiple materials such as rubber, carbon black, vulcanization accelerators and softeners is an inert vulcanized rubber with a cross-linked structure on the surface. It is different from the properties of the surface of the blended material and has poor compatibility. At the same time, because waste tires have been used in outdoor environments for a long time, they are often exposed to the sun and high temperature, and are severely aged. It is difficult to form a good bonding interface at the interface by direct mixing, which leads to a significant decrease in the mechanical properties of the composite material and fails to achieve the expected effect.

[0023] To solve this problem, the applicant adopted the following method to process waste tires: the waste tires were cleaned with a high-pressure water gun to remove surface attachments, and then cut into small pieces not exceeding 50 mm square, and then poured into a crusher to crush into 10-80 mesh particles, and the particles were poured into acid solution for soaking to improve the compatibility of their surface. After soaking, they were washed with water, dried or baked, and then made into blocks with other raw materials in the same proportion for performance testing.

[0024] Acid leaching test:

[0025] Different types of acidic substances were made into aqueous solutions with concentrations of 5%, 10%, 20%, and 30% (m / m), and soaked for 0.5h-72h according to the mass ratio of waste tire particles: acid solution = 1:20-1:5, and then washed with water until the washing liquid was neutral, and then made into cement mortar blocks. The cement mortar blocks contained 350 parts of cement, 38 parts of anhydrite, 15 parts of latex powder, 100 parts of river sand, 4 parts of water reducer, 5 parts of calcium formate, and 200 parts of waste tire particles. After curing, the compressive strength and tensile bonding strength were tested, and compared with the waste tire particles and commercially available rubber block particles treated with deionized water under the same conditions. The data showed that among the acidic substances used, the blocks made of waste tire particles treated with hydrochloric acid, sulfuric acid, oxalic acid, citric acid, and acetic acid had different degrees of improvement in compressive strength and tensile bonding strength compared with the waste tire particles not treated with acid leaching. The specific data are shown in the following table:

[0026] Table 1 Effects of different acid leaching treatments

[0027]

[0028] As shown in the table above, blocks made from waste tire particles treated with hydrochloric acid and citric acid have the highest compressive strength and tensile bond strength. However, if the chloride ions in the cement mortar penetrate into the concrete layer, they are likely to corrode the steel bars in the concrete, which will affect the structural strength of the building in the long run.

[0029] According to the above test results, oxalic acid, citric acid and acetic acid are preferred as acid leaching agents.

[0030] According to the "Code for Measurement of Building Sound Insulation" and GB / T19889.8-2022 "Measurement of Sound Insulation of Acoustic Buildings and Building Components", the test frequency range is 100Hz, 125Hz, 160Hz, 200Hz, 250Hz, 315Hz, 400Hz, 500Hz, 630Hz, 800Hz, 1000Hz, 1250Hz, 1600Hz, 2000Hz, 2500Hz, and 3150Hz. The single value evaluation values ​​of the impact sound when using oxalic acid, citric acid, and acetic acid as acid leaching reagents are 63dB, 67dB, and 59dB respectively. The single value evaluation value of the impact sound of blocks with commercially available rubber block particles is 62dB.

[0031] At present, the rubber particles added to the sound insulation floor mortar are mostly particles of about 10-50 mesh, which are close to spherical in shape. The specific surface area of ​​solid spherical particles is the smallest among all shapes. In order to investigate the effect of the shape of rubber particles on the sound insulation ability, waste tires were crushed into spherical particles of 10 mesh, 30 mesh, 50 mesh, 80 mesh, and 100 mesh using a crusher, and cut into H-shaped, O-shaped, and square strips using special-shaped cutters. The surface of the square strip contains at least 2 V-shaped grooves with an angle of no more than 40°, and the cross-sectional area of ​​the strip does not exceed 0.5mm 2 , length not exceeding 5mm.

[0032] According to 350 parts of cement, 38 parts of anhydrite, 15 parts of latex powder, 100 parts of river sand, 4 parts of water reducer, 5 parts of calcium formate, and 200 parts of waste tire particles, blocks were made using waste tire particles of different shapes. These waste tire particles were soaked in citric acid (concentration 30%, mass ratio 1:5, duration 10h), washed and dried, and the sound insulation performance of the blocks was tested after curing, as shown in the following table:

[0033] Table 2 Effect of particle shape on noise reduction performance

[0034]

[0035] As shown in the table above, when used alone, making waste tires into special-shaped strips is more conducive to improving the sound insulation performance. However, the applicant also found that when spherical particles and special-shaped strip particles are mixed in a certain proportion, a better sound insulation effect can be achieved. Some data are as follows:

[0036] Table 3 Effect of mixing particles of different shapes on noise reduction performance

[0037]

[0038]

[0039] As shown in the table above, when H-shaped and square slotted strips are mixed with spherical particles in a certain proportion, the sound insulation effect of the blocks is better than when used alone, and the sound insulation effect is best when mixed with 80-mesh spherical particles. However, the effect is not obvious when O-shaped strips are mixed with spherical particles of different mesh sizes.

[0040] In order to reduce the amount of cement in the mortar and reduce carbon emissions during the mortar solidification process, 350 parts of cement, 38 parts of anhydrite, 15 parts of latex powder, 100 parts of river sand, 4 parts of water reducer, 5 parts of calcium formate, 200 parts of waste tire particles (80 mesh spherical particles + square strips, ratio 7:13, square strips with a cross-sectional area of ​​0.32mm 2, 4 V-shaped grooves are symmetrically set with an angle of 35°) by weight ratio. Under the condition that other components remain unchanged, mineral powder is used as the substitute for cement in mortar, and the compressive strength under different amounts of mineral powder is tested to see if it is qualified, as follows:

[0041] Table 4 Effect of cement content on compressive strength

[0042] Cement content Mineral powder quantity Compressive strength / MPa 300 50 6.42 200 150 6.27 100 250 6.15 0 350 5.78

[0043] The compressive strength of the blocks with added mineral powder is lower than that of the blocks without added mineral powder. This is due to the weak hydration strength of the mineral powder. To improve this problem, a certain proportion of high-strength fibers such as glass fiber or steel fiber is added to the mortar. The specific composition is 350 parts of mineral powder, 38 parts of hard gypsum, 15 parts of latex powder, 100 parts of river sand, 4 parts of water reducer, 5 parts of calcium formate, 200 parts of waste tire particles (80 mesh spherical particles + square strips, ratio 7:13, square strips with a cross-sectional area of ​​0.32mm2, 4 V-shaped grooves are symmetrically arranged, with an angle of 35°), and 20-50 parts of high-strength fiber. The surface of the glass fiber used is treated with a silane coupling wetting agent. The final block strength data is as follows:

[0044] Table 5 Effect of high-strength fiber type and addition amount on strength

[0045] Fiber Type Fiber content Compressive strength / MPa Steel Fiber 20 6.13 Steel Fiber 30 6.51 Steel Fiber 50 6.89 Fiberglass 20 6.09 Fiberglass 30 6.35 Fiberglass 50 6.78

[0046] As shown in the table above, when mineral powder is used to completely replace cement, adding high-strength fibers such as steel fiber or glass fiber can improve the compressive strength of mortar blocks.

[0047] The sound insulation performance of the blocks with high-strength fibers was tested, and the data are as follows:

[0048] Table 6 Effect of high-strength fiber type and addition amount on noise reduction performance

[0049] Fiber Type Fiber content Impact sound single value evaluation quantity / dB Steel Fiber 20 56 Steel Fiber 30 59 Steel Fiber 50 64 Fiberglass 20 52 Fiberglass 30 53 Fiberglass 50 52

[0050] The applicant has found that if the glass fiber used is in the shape of a hollow tube, the sound insulation performance of the block can be improved well, and the amount of rubber particles can be reduced while maintaining the same sound insulation performance, as follows:

[0051] Table 7 Effect of glass fiber shape and addition amount on waste tire particle dosage and noise reduction performance

[0052] Glass fiber type Fiber content Quantity of waste tire particles Impact sound single value evaluation quantity / dB Hollow tube 20 150 52 Hollow tube 30 120 51 Hollow tube 50 80 52 solid 20 150 54 solid 30 120 55 solid 50 80 57

[0053] In addition, sealing both ends of the hollow tubular glass fiber can prevent other components of the mortar from entering the internal cavity of the glass fiber during construction and produce better sound insulation effect:

[0054] Table 8 Effect of glass fiber shape and addition amount on waste tire particle dosage and noise reduction performance

[0055] Glass fiber type Fiber content Quantity of waste tire particles Impact sound single value evaluation quantity / dB Hollow tube 20 150 52 Hollow tube 30 120 51 Hollow tube 50 80 52 Hollow tube, closed at both ends 20 150 50 Hollow tube, closed at both ends 30 120 48 Hollow tube, closed at both ends 50 80 47

[0056] The following are embodiments of the present invention:

[0057] Example 1

[0058] 350 parts of mineral powder, 38 parts of anhydrite, 15 parts of latex powder, 100 parts of river sand, 4 parts of water reducer, 5 parts of calcium formate, 150 parts of waste tire particles (80 mesh spherical particles + rectangular strips, ratio 7:13, cross-sectional area of ​​the rectangular strips 0.32mm 2 , 4 V-shaped grooves are symmetrically arranged with an angle of 35°), 20 parts of hollow tubular glass fibers, waste tire particles are soaked in 20% concentration oxalic acid solution for 10 hours and washed and dried, both ends of the glass fibers are sealed and the surface is treated with a silane coupling wetting agent to make cement mortar blocks.

[0059] Example 2

[0060] 50 parts of cement, 300 parts of mineral powder, 35 parts of anhydrite, 12 parts of latex powder, 80 parts of river sand, 3 parts of water reducer, 6 parts of calcium formate, 150 parts of waste tire particles (50 mesh spherical particles + square strips, ratio 2:3, square strips with a cross-sectional area of ​​0.32mm 2 , 4 V-shaped grooves are symmetrically arranged with an angle of 35°), 20 parts of hollow tubular glass fibers, waste tire particles are soaked in 30% concentration citric acid solution for 10 hours and washed and dried, both ends of the glass fibers are sealed and the surface is treated with a silane coupling wetting agent to make cement mortar blocks.

[0061] Example 3

[0062] 100 parts of cement, 250 parts of mineral powder, 40 parts of anhydrite, 16 parts of latex powder, 120 parts of river sand, 2 parts of water reducing agent, 7 parts of calcium formate, 120 parts of waste tire particles (50 mesh spherical particles + square strips, ratio 2:3, square strips with a cross-sectional area of ​​0.32mm 2 , 4 V-shaped grooves are symmetrically arranged with an angle of 35°), 50 parts of hollow tubular glass fibers, waste tire particles are soaked in 30% concentration acetic acid solution for 10 hours and washed and dried, both ends of the glass fibers are sealed and the surface is treated with a silane coupling wetting agent to make cement mortar blocks.

[0063] The single-value evaluation values ​​of compressive strength, tensile bonding strength, and impact sound of Examples 1-3 are as follows:

[0064] Table 9 Performance data of Examples 1-3

[0065] Example Compressive strength / MPa Tensile bonding strength / MPa Impact sound single value evaluation quantity / dB 1 6.07 0.67 53 2 6.34 0.65 50 3 6.67 0.69 48

[0066] In summary, the low-carbon sound-insulating floor mortar proposed in the present invention has good compressive strength, tensile bonding strength and sound insulation performance, can effectively solve the problem of noise caused by impact being transmitted through floors and walls, and reduce noise pollution in residential buildings. It also utilizes waste tire resources, has low cost, and can reduce pollution caused by discarded waste tires.

[0067] The above description is only a preferred embodiment of the present invention and is not intended to limit the present invention. Any modifications, equivalent substitutions and improvements made within the spirit and principles of the present invention should be included in the protection scope of the present invention.

Claims

1. A low-carbon sound insulation floor mortar, characterized in that: The invention comprises the following raw materials in parts by weight: 0-100 parts of cement, 35-40 parts of anhydrite, 250-350 parts of mineral powder, 12-16 parts of latex powder, 80-120 parts of river sand, 2-4 parts of water reducing agent, 5-7 parts of calcium formate, 120-150 parts of waste tire particles, and 20-50 parts of high-strength fiber. The shapes of the waste tire particles include granular and strip-shaped. The mass ratio of spherical particles to square particles with V-shaped grooves in the cross section of the waste tire particles is 7:

13.

2. A low-carbon sound insulation floor mortar according to claim 1, characterized in that: The amount of cement used shall not exceed 25% of the amount of mineral powder used.

3. The low-carbon sound insulation floor mortar according to claim 1, characterized in that: The waste tire particles are treated with acid leaching.

4. The low-carbon sound insulation floor mortar according to claim 1, characterized in that: The high-strength fiber is steel fiber or glass fiber.

5. The low-carbon sound insulation floor mortar according to claim 3, characterized in that: The acid leaching process of the waste tire particles is to soak them in carboxylic acid with a concentration of 10% to 30% at room temperature for 10 hours or longer, then wash them with water and dry them.

6. The low-carbon sound insulation floor mortar according to claim 4, characterized in that: The high-strength fiber is glass fiber, which is in the shape of a hollow tube with closed ends, and the surface of the glass fiber is treated with a silane coupling wetting agent.

7. The low-carbon sound insulation floor mortar according to claim 5, characterized in that: The carboxylic acid is acetic acid, oxalic acid, citric acid or a mixture thereof.