Electroslag mixing method for inhibiting the burning of boron element in boron-containing and nitrogen-containing heat-resistant steel

By adding boron nitride and carbon powder to the electroslag remelting process, combining protection atmosphere and process parameter optimization, the problem of boron element burning in heat-resistant steel is solved, and the stable harvest of boron element is achieved to rate and component control.

CN116144937BActive Publication Date: 2024-11-22CHENGDU ADVANCED METAL MATERIALS IND TECH RES INST CO LTD +1
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202310007916.9
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2023-01-04
Publication Date
2024-11-22
Estimated Expiration
2043-01-04

AI Technical Summary

Technical Problem

In the process of steel metallurgy, boron elements in boron-containing nitrogen-resistant heat-resistant steels are prone to burning during the electroslag remelting process, resulting in unstable component control and it is difficult to achieve a stable rate of boron elements.

Method used

Using an electroslag slag mixing method, boron nitride and carbon powder are added to the heat-resistant steel ingot, and electroslag remelting is carried out under a protective atmosphere to control the electroslag melting rate and process parameters, and use CaF2, Al2O3, CaO, etc. Combining as slag mixing ensures a low oxygen atmosphere and an appropriate electroslag melting rate, heat treatment is performed to stabilize the distribution of boron elements.

Benefits of technology

The reception rate of boron element is significantly improved, from 40 to 70% to 70% to 80%, reducing the amount of alloy used in smelting and the introduction of impurities, and achieving stable control of boron element.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN116144937B_ABST
    Figure CN116144937B_ABST
Patent Text Reader

Abstract

The present invention discloses an electroslag mixing method for inhibiting the burning of boron element in boron-containing and nitrogen-containing heat-resistant steel. The method comprises: adding electroslag mixing to a heat-resistant steel ingot, wherein the electroslag mixing comprises boron nitride and carbon powder; electroslag remelting is performed in a protective atmosphere, and the filling ratio d=(0.6-0.8)D, where D is the diameter of the crystallizer; and the electroslag melting rate is controlled at 7-11 kg / min. The present invention optimizes the settings of the electroslag remelting voltage, current and melting rate according to the characteristics of the steel grade, the specifications of the billet and the filling ratio. For large-size and large-filling ratio billets, the melting rate is appropriately reduced to inhibit component segregation. For the burning of the B element, the whole process process is optimized, starting from the aspects of component optimization, billet solidification (including heat treatment) and electroslag remelting process, the B recovery rate is effectively stabilized and improved, and the stable control of the composition of the boron-containing and nitrogen-containing heat-resistant steel during smelting is achieved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of iron and steel metallurgy, and in particular to an electroslag mixing method for inhibiting the burning of boron elements in boron-containing and nitrogen-containing heat-resistant steel. Background Art

[0002] The loss of a large amount of element B that is easily burned during the electroslag remelting process of the boron- and nitrogen-containing martensitic heat-resistant steel for turbine blades is a key common problem that affects the composition control during the smelting process. In the production practice of heat-resistant steel, it is found that some B content is relatively high, especially heat-resistant steel grades containing both boron and nitrogen. The B content is prone to large fluctuations during the smelting process, and the B receipt rate is extremely unstable in several key technical links (such as refining outside the furnace and electroslag remelting). The B content in the billet may fluctuate between the upper and lower limits of the control range. It is difficult to achieve stable control of the B element by reserving a burn-loss margin in the ingredients alone (it is easy for the B content to exceed the upper limit or fall below the lower limit). Effectively stabilizing the B receipt rate is an effective way to achieve stable composition control.

[0003] First, through field research, we found out the key nodes of composition control. Secondly, we sorted out the burning loss mechanism of element B in smelting, and on this basis, formulated a process plan for B stability control.

[0004] 1. Key process nodes

[0005] The production of boron-nitrogen-containing heat-resistant steel 10Cr11Co3W3NiMoVNbNB (vacuum induction furnace + ESR (electroslag remelting)) was followed throughout the production process, and the composition changes of the easily burned elements in each process link were recorded (such as Figure 1 ). Figure 1 The figure shows the changes in the contents of easily burned elements in each stage of vacuum induction + ESR smelting of boron-nitrogen-containing heat-resistant steel (without process adjustment) (burden composition - induction furnace steel composition - electrode rod composition - electroslag ingot composition). In the figure, the B content drops significantly after ESR treatment; there is a significant increase in Si; there is an increase in Al after ESR; and the Nb content remains relatively stable.

[0006] The B element remains relatively stable during the refining process, but drops sharply after electroslag remelting.

[0007] The survey found that B and N elements are often added in the form of alloys in the late stage of refining outside the furnace (LF or VD) or before steelmaking, at which time the composition can be fine-tuned. At this time, the relative content of B is relatively stable, while the N content changes over time (when the N content is low, there may be an increase in N, and when the content is too high, it gradually decreases over time).

[0008] After electroslag remelting, the B content decreases significantly, and the B recovery rate usually fluctuates between 40% and 70%. In some cases, B is not burned at all. It can be seen that the key process node that affects the final recovery rate of B element is electroslag remelting.

[0009] 2. Burning of element B

[0010] Clarify the role, existence form and main burning mechanism of B (including N) elements in heat-resistant steel:

[0011] (1) The main functions of B and N elements in heat-resistant steel:

[0012] The solubility of B in Fe is low, and a small amount of B (≤8ppm) dissolved in the matrix can improve the hardenability of the material. The B content in boron-containing heat-resistant steel is relatively high (0.03% ≥ B% ≥ 0.01%), and most of the B will be concentrated at the grain boundary in the form of free state or compound. Among them, free B combines with intergranular carbides to form boron-carbon compounds (such as M23 (C, B) 6, etc.), which can inhibit the Ostwald ripening of intergranular carbides and significantly improve the high-temperature durability and high-temperature creep properties of the material.

[0013] The N element can replace part of the precious metals and improve the yield strength of the steel. At the same time, it has little effect on plasticity and toughness when combined with nitrogen-fixing elements such as V, Nb, and Al. As an austenite-forming element, it can inhibit the formation of harmful phase delta ferrite and improve the uniformity of the structure. In addition, adding N to heat-resistant steel can improve the corrosion resistance of the material.

[0014] The BN precipitate phase generated by the reaction of B and N in steel has similar properties to MnS. When the content is low and the size is small, it has almost no effect on the performance of the steel billet; but when the content is high and the size is large, it can improve the cutting performance of the material.

[0015] (2) Existence forms of B and N

[0016] The forms of B in heat-resistant steel include solid solution, free state or compound form concentrated at grain boundaries. At high temperatures, B has high chemical activity and can react with N and O in steel to generate structurally stable nitrides and oxides. The following formula is the Gibbs free energy corresponding to several oxidation reactions. In smelting, the oxidation activity of B is higher than that of Mn and Si, but lower than that of Ti and AI. During the smelting process, B reacts with O before Mn and Si to produce oxides. If the oxide of boron cannot be reduced in time, it is easily adsorbed by the slag, resulting in the loss of boron. The oxidation reaction of B is directly affected by the oxygen content in the molten steel. When the oxygen content exceeds a certain threshold, as the oxygen content increases, the proportion of B oxide in the total boron content gradually increases.

[0017] [Mn] + [O] = [MnO] s ΔG θ=-244300+107.6T

[0018] 1 / 2[Si]+[O]=1 / 2[SiO2] s ΔG θ =-288220+109.1T

[0019] 2 / 3[Al]+[O]=1 / 3[Al2O3] s ΔG θ =-408333+131.3T

[0020] 1 / 2[Ti]+[O]=1 / 2[TiO2] s ΔG θ =-330960+114T

[0021] 2 / 3[B]+[O]=1 / 3[B2O3] s ΔG θ =-254806.5+95.5T

[0022] B reacts with N to form a stable compound BN. At relatively low temperatures (≤1700℃), the binding ability of B and N is higher than that of Al (on the contrary at >1700℃), and lower than that of Ti and Zr, as shown in the Gibbs free energy of the reaction. BN is easy to precipitate gradually with the movement of grain boundaries during the non-equilibrium solidification of the steel billet. Therefore, the content and morphology of BN are affected by the B and N contents in the steel and the solidification rate of the steel billet. If there are a large number of large-sized BN or BN cluster structures in the heat-resistant steel electrode rod, these precipitation structures are easily adsorbed by the slag during the electroslag process, resulting in a significant decrease in the total B content.

[0023] [Ti]+[N]=[TiN] s ΔG θ =-291000+107.9T

[0024] [B]+[N]=[BN] s ΔG θ =-267486+100.3T

[0025] [Al]+[N]=[AlN] s ΔG θ =-129626+19.72T

[0026] 3. Inhibit B burning

[0027] According to the analysis of the burning mechanism, the loss of B element in the smelting process must be controlled from the two aspects of oxygen control and nitrogen fixation. At present, conventional treatment often focuses on optimizing the deoxidation system and strengthening the deoxidation. However, insufficient attention is paid to the nitriding burning of B. For heat-resistant steel containing both boron and nitrogen, the loss of B caused by nitriding burning may be no less than the impact caused by oxidation burning. Summary of the invention

[0028] The object of the present invention is to provide an electroslag mixing method for inhibiting the burning of boron element in boron-containing and nitrogen-containing heat-resistant steel. To achieve the above object, the present invention provides the following technical solutions:

[0029] An electroslag mixing method for inhibiting the burning of boron element in boron-containing and nitrogen-containing heat-resistant steel, the method comprising:

[0030] Adding electroslag mixed slag into a heat-resistant steel ingot, wherein the electroslag mixed slag includes boron nitride and carbon powder;

[0031] The electroslag remelting is carried out in a protective atmosphere, the filling ratio d=(0.6-0.8)D, D is the diameter of the crystallizer; the electroslag melting rate is controlled at 7-11 kg / min.

[0032] Furthermore, the electroslag mixture also includes one or more of CaF2, Al2O3, and CaO.

[0033] Furthermore, in the electroslag mixed slag, the content of boron nitride is 0.01-0.02%, and the content of carbon powder is 0.1-0.15%.

[0034] Further, electroslag remelting is performed using a protective atmosphere, including

[0035] When using protective atmosphere for electroslag remelting, a large flow rate of inert gas is introduced into the crystallizer for 10 to 15 minutes before arc initiation, and the flow rate of inert gas is gradually reduced after the electroslag remelting process becomes stable.

[0036] After the flow rate of the inert gas is reduced, the O2 content in the electroslag remelting process is ≤0.02%.

[0037] Furthermore, the average voltage of the electroslag remelting stable stage is 45-46V.

[0038] Furthermore, for heat-resistant steel ingots with a total weight of ≤3t, the electroslag melting rate is controlled at 7-9kg / min, and for heat-resistant steel ingots with a total weight of ≥3t, the electroslag melting rate is controlled at 9-11kg / min.

[0039] Furthermore, the method further comprises:

[0040] After electroslag remelting, the electroslag ingot is left to stand in the crystallizer for 1 to 2 hours before being tapped, hood-cooled for 24 to 36 hours, and then annealed at 750 to 800°C for 24 to 30 hours.

[0041] Furthermore, obtaining the heat-resistant steel ingot includes:

[0042] Raw material pretreatment: Shot blast the alloy raw materials to completely remove the oxide scale, and weigh them for later use;

[0043] Loading and melting: Load the alloy raw materials into the crucible in a loose upper and tight lower manner, close the furnace and evacuate, wait until the vacuum degree of the melting chamber is lower than 20Pa, then turn on the power to start melting, take samples for analysis after the alloy is completely melted, and fine-tune the composition in the furnace;

[0044] Vacuum carbon deoxidation refining: heat up to the refining temperature, refining for 50 to 80 minutes in a vacuum environment, add deoxidizer, take samples for analysis after melting, then add Nb-Fe and V-Fe respectively and stir;

[0045] Add ferroboron and cast steel: Add N-Cr and sponge Ti and stir, add B-Fe and Mn after they are melted, fill in inert gas to increase the pressure in the furnace and control the steel tapping temperature range at 1550-1650℃, and cast to obtain heat-resistant steel ingots.

[0046] Furthermore, the raw material components of the heat-resistant steel ingot include, by mass percentage (%): C: 0.09-0.11, Mn: 0.4-0.5, Si: ≤0.1, P: ≤0.015, S: ≤0.01, Cr: 11-11.5, Ni: 0.3-0.7, Mo: 0.1-0.4, Co: 2.5-3.5, W: 2.4-3, V: 0.2-0.24, Nb: 0.08-0.14, N: 0.012-0.02, B: 0.015-0.02, Al: 0.01-0.015, Ti: 0.01-0.02, and the rest is Fe except for a small amount of impurity elements.

[0047] Furthermore, during the vacuum carbon deoxidation refining process, the oxygen content in the electrode base material is controlled to be ≤30ppm.

[0048] Furthermore, after the heat-resistant steel ingot is obtained by casting, when the B content at the head and tail of the electrode rod is at the lower limit of control, the electrode base material is subjected to a homogenization treatment at 1050-1150° C. for not less than 10 hours;

[0049] After heat treatment, the riser and nozzle ends of the electrode rod are removed and the surface is polished or turned.

[0050] Technical effects and advantages of the present invention:

[0051] (1) Optimization of ingredients

[0052] First, the alloy composition is optimized, especially the content of B, N, and various nitrogen-fixing elements. The relationship between B and N content is based on the empirical formula lg[B] = -2.45lg[N]-6.81 (where [B] and [N] are the mass percentages of B and N, respectively). Figure 2 shown), Figure 2 The relationship between the mass percentage of B and N in heat-resistant steel and the precipitation and morphology of BN (large frame: the agreement range of B and N content in the alloy; small frame: the optimized B and N content). The upper right corner of the formula in the figure corresponds to the B and N composition range, which is easy to generate BN; while the lower right corner of the formula corresponds to the composition range, which is generally not easy to generate BN. When the logarithmic relationship between N and B is close to the empirical formula at 1050-1150℃, the BN in the steel is mainly dispersed small-sized particles; when lg[B]>-2.45lg[N]-6.81, BN is mostly large-sized cluster structure; and when lg[B]<-2.45lg[N]-6.81, BN is almost not precipitated in the steel. It is possible to consider increasing the proportion of nitrogen-fixing elements in steel, such as appropriately increasing the relative content of V, Nb, and Al (residual Al in steel) in heat-resistant steel.

[0053] (2) Increase strong nitrogen-fixing elements

[0054] Increase the content of certain strong nitrogen-fixing elements (Ti, Zr). BMKapadia et al. proposed an effective boron estimation formula (as shown below), which reflects the relationship between nitrogen-fixing elements and effective boron (acid-soluble boron) (where 0.002 is the weight of nitrogen-fixing elements such as Al and V).

[0055]

[0056] Since Ti reacts with N to form TiN with a cubic structure, this type of structure easily forms a crack source and has a negative impact on the fatigue properties of the material. Ti in heat-resistant steel is often used as an impurity element, but the content can be appropriately increased and controlled according to the lower and middle limits of the composition.

[0057] (3) Enhanced deoxidation

[0058] Strengthen the deoxidation process in the smelting process and control the oxygen content in the molten steel below 30ppm before tapping. Some types of heat-resistant steel need to examine the impact performance, put forward higher requirements for inclusion control, and strictly control the Al and Si content. During smelting, Al can reduce SiO2 in the slag to cause Si increase in the steel billet. Therefore, C and Al are usually used as the main deoxidizers, and the total amount of Al is strictly controlled. However, the residual Al content in the steel billet is moderately increased to prevent oxygen increase during the smelting process.

[0059] After deoxidation, B-containing and N-containing alloys are added respectively. Such alloys often contain more impurities and inclusions. It is best to purify them before use to reduce the content of impurity elements.

[0060] (4) Billet solidification rate

[0061] The morphology and size of BN are directly affected by the solidification rate. When the solidification rate is high, BN presents a dispersed small-sized particle structure; when the solidification rate is low, BN particles tend to agglomerate to form a large-sized cluster structure. Increasing the solidification rate of the billet (such as appropriately reducing the casting temperature, using auxiliary cooling methods, etc.) can avoid the appearance of BN with a large-sized cluster structure.

[0062] (5) Heat treatment

[0063] For some large-sized heat-resistant steel billets, the composition segregation is serious, and it is difficult to suppress the large-scale appearance of BN with cluster structure through rapid solidification. It is possible to consider reducing the relative content of BN through homogenization heat treatment. The heat treatment temperature is controlled at 1050-1150℃ to increase the diffusion rate of residual Al in the steel and use Al to reduce BN.

[0064] (6) Optimization scheme of electroslag mixing

[0065] The electroslag remelting process needs to start from optimizing the protective atmosphere, slag system and mixed slag raw materials, and process parameters, among which the focus is on the adjustment of the protective atmosphere and mixed slag composition.

[0066] First, it is necessary to ensure that the O2 and N2 content in the crystallizer is low enough to avoid serious element burnout of the billet during electroslag remelting. Before ESR treatment, the air tightness of the equipment should be tested to avoid air infiltration; high-purity Ar should be used as the protective atmosphere; before arc initiation, Ar should be introduced into the crystallizer at a large flow rate for more than 10 minutes to try to remove the air in the crystallizer; after arc initiation, Ar should be continuously introduced at a large flow rate to try to avoid the protective atmosphere from expanding due to heat, forming convection with the air in the exhaust pipe, and entraining impurity gases; after the process is stable, the Ar flow rate should be gradually reduced.

[0067] Optimize the composition of electroslag mixed slag: Use a ternary slag system with better inclusion removal effect (such as CaF2:Al2O3:CaO=60:20:20), add a small amount of BN powder and carbon powder as a deoxidizer to form a mixed slag. BN can increase the B content in the slag. 3+ The proportion of ions can inhibit the oxidation or nitridation reaction of free B between slag and metal during ESR. Carbon powder can inhibit the oxidation and burning of billet elements during arc initiation, and reduce the burning of C elements in the billet.

[0068] Adjustment of electroslag process parameters: Optimize the electroslag remelting voltage, current and melting speed settings according to the characteristics of steel grade, billet specifications and filling ratio. For large-sized and large-filling ratio billets, appropriately reduce the melting speed to suppress component segregation.

[0069] In response to the burning of element B, full-process process optimization is carried out, starting from composition optimization, billet solidification (including heat treatment) and electroslag remelting process, to effectively stabilize and improve the B recovery rate and achieve stable composition control of boron and nitrogen-containing heat-resistant steel during smelting.

[0070] The present invention starts from two aspects: inhibiting the precipitation of B compounds in steel and reducing the loss of B through slag during smelting. By optimizing the composition, adding nitrogen-fixing elements, appropriately reducing the pouring temperature to increase the solidification rate of the steel billet, performing solid solution treatment on the electrode rod, and performing electroslag remelting in an Ar atmosphere and low O2 environment, especially using an electroslag mixed slag scheme of CaF2 / Al2O3+BN+carbon powder for electroslag remelting treatment. It has a significant effect on improving the boron element recovery rate in the electroslag remelting process of boron-containing and nitrogen-containing steel (especially steel with relatively high boron content) and achieving stable control of the B element.

[0071] The present invention achieves stable control of the B element in the electroslag remelting process of boron-containing steel (B% is 0.01-0.03%) by adding a small amount of BN to the mixed slag. The proportion of BN added in each furnace is low, which hardly affects the ESR smelting cost. The B recovery rate can be increased from 40-50% to 70-80%, reducing the amount of boron-containing alloys used in smelting and reducing impurities introduced with such alloys.

[0072] Other features and advantages of the present invention will be described in the following description, and partly become obvious from the description, or be understood by implementing the present invention. The purpose and other advantages of the present invention can be realized and obtained by the structures pointed out in the description and the drawings. BRIEF DESCRIPTION OF THE DRAWINGS

[0073] Figure 1 The composition changes of Al, Si, B and Nb in each process of smelting of boron- and nitrogen-containing heat-resistant steel;

[0074] Figure 2 The relationship between the B and N contents and BN precipitation in heat-resistant steel (1050-1150℃);

[0075] Figure 3 A flow chart of an electroslag mixing method for inhibiting the burning of boron element in boron-containing and nitrogen-containing heat-resistant steel according to the present invention. DETAILED DESCRIPTION

[0076] The following will be combined with the drawings in the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0077] In order to solve the deficiencies of the prior art, the present invention discloses an electroslag mixing method for inhibiting the burning of boron element in boron-containing and nitrogen-containing heat-resistant steel, such as Figure 3 As shown, the method comprises the following steps:

[0078] Raw material pretreatment: Shot blast the alloy raw materials to completely remove the oxide scale, and weigh them for later use;

[0079] Loading and melting: Load the alloy raw materials into the crucible in a loose upper and tight lower manner, close the furnace and evacuate, wait until the vacuum degree of the melting chamber is lower than 20Pa, then turn on the power to start melting, take samples for analysis after the alloy is completely melted, and fine-tune the composition in the furnace;

[0080] Vacuum carbon deoxidation refining: heat up to the refining temperature, refining for 50 to 80 minutes in a vacuum environment, add deoxidizer, take samples for analysis after melting, then add Nb-Fe and V-Fe respectively and stir;

[0081] Add ferroboron and cast steel: Add N-Cr and sponge Ti and stir, add B-Fe and Mn after they are melted, fill in inert gas to increase the pressure in the furnace and control the steel tapping temperature range at 1550-1600℃, and cast to obtain heat-resistant steel ingots.

[0082] Electroslag remelting: In the present invention, the mixed slag preferably adopts a ternary slag system of CaF2:Al2O3:CaO=60:20:20 (or a binary slag system of CaF2:Al2O3=70:30), and pre-melted slag is used as much as possible. The total slag amount depends on the specifications of the crystallizer and is within the lower and middle limits of the equipment allowable range; the content of boron nitride in the slag is 0.01-0.02%, and the content of carbon powder is 0.1-0.15%. In the present invention, preferably, 0.02% BN and 0.1% carbon powder are added to form a mixed slag, and the mixed slag system and BN are fully baked at 800±20℃ for 6-8h before use. The preferred mixed slag process parameters of the present invention are as follows: filling ratio d=(0.6-0.8)D, where D is the diameter of the crystallizer; high-purity Ar is used as the protective atmosphere during the electroslag process, and is introduced into the crystallizer at a large flow rate before arc initiation (10-15 minutes), and the Ar flow rate is gradually reduced after the ESR processing is stable to ensure that the O2 content in the electroslag process is ≤0.02%; the average voltage in the ESR stable stage is 45-46V; for electrode rods ≤3t, the electroslag melting rate is controlled at 7-9kg / min, and for ingots ≥3t, it is 9-11kg / min; after the electroslag remelting treatment, the electroslag ingot is left to stand in the crystallizer for 1-2 hours before tapping, and then hood-cooled for 24-36 hours, and then annealed at 750-800°C for 24-30 hours.

[0083] In a specific embodiment of the present invention, the raw material components of the boron-nitrogen-containing heat-resistant steel are as follows in mass percentage (%): C: 0.08-0.12, Mn: 0.35-0.6, Si: ≤0.1, P: ≤0.015, S: ≤0.01, Cr: 10-12.5, Ni: 0.3-0.7, Mo: 0.1-0.4, Co: 2.5-3.5, W: 2.4-3, V: 0.15-0.25, Nb: 0.05-0.15, N: 0.01-0.4, B: 0.01-0.03Al: ≤0.02, Ti: ≤0.04, and the rest is Fe except for a small amount of impurity elements. By smelting boron-nitrogen-containing heat-resistant steel with vacuum induction furnace + ESR or electric furnace + ESR, the composition optimization scheme for inhibiting B burning includes: N takes the middle lower limit of the composition (0.012-0.02%), B takes the middle limit of the composition (0.015-0.02%), V is controlled at the middle upper limit (0.2-0.24%), Nb is controlled at the middle upper limit (0.08-0.14%); Cr and Mn are controlled at the middle upper limit (11-11.5% and 0.4-0.5% respectively); C is controlled at the middle lower limit (0.09-0.11%); an appropriate amount of strong nitrogen-fixing element Ti (0.01-0.02) is added, and the residual Al in the steel is controlled at the middle upper limit (0.01-0.015%).

[0084] In a specific embodiment of the present invention, Al deoxidation is used to ensure that the residual Al in the molten steel before steel casting is within the range of 0.01-0.015%; and the oxygen content in the electrode base material is controlled to be ≤30ppm.

[0085] In a specific embodiment of the present invention, B is added in the form of Fe-B alloy before steelmaking, and Fe-B is remelted before use to make B in the alloy uniform and remove impurity elements and inclusions as much as possible; N is added in the form of nitrogen-containing alloy, and alloy raw materials with fewer impurities and more uniform composition are selected as much as possible; B and N are added separately, and it must be ensured that the added alloys are completely dissolved.

[0086] In a specific embodiment of the present invention, the casting temperature is designed according to the furnace loading, and the tapping temperature of the above steel grades is controlled within the range of 1550-1600°C. The casting temperature is adjusted as low as possible under the premise of conditions permitting (to avoid casting to death); if the B content at the head and tail of the electrode rod is relatively low (the B content is at the lower control limit), the electrode base material is subjected to homogenization treatment at 1050-1150°C for not less than 10 hours. After the heat treatment, the riser and nozzle ends of the electrode rod are removed, and the surface is polished or turned.

[0087] The scheme of the present invention is further described below in conjunction with examples, but the present invention is not limited thereto.

[0088] Example 1

[0089] An electroslag mixing scheme for inhibiting the burning of boron element in boron-containing and nitrogen-containing heat-resistant steel comprises the following steps:

[0090] 1) Raw material pretreatment: The alloy raw materials are shot blasted to remove the surface oxide scale, weighed according to the composition range and then loaded into the vacuum induction furnace respectively. The composition is shown in the table (V-Fe and B-Fe are remelted in the vacuum induction furnace before use):

[0091] Table 1 Control range of components of boron- and nitrogen-containing heat-resistant steel (wt%)

[0092]

[0093]

[0094] 2) First, Fe, Fe-Ni, Fe-Cr, Co, Mo-Fe, and W-Fe alloy materials are loaded into the crucible; the furnace is evacuated to below 20Pa and power is supplied;

[0095] 3) After the alloy is melted, take samples for analysis and make fine adjustments to the composition in the furnace to ensure that the main components are within the control range;

[0096] 4) Refining is performed for 50 to 60 minutes in a vacuum environment, and a deoxidizer is added after the refining is completed. Samples are taken for analysis after melting, and then Nb-Fe and V-Fe are added respectively and stirred;

[0097] 5) Add N-Cr and sponge Ti and stir, add B-Fe and Mn after they are melted, fill with Ar gas to increase the pressure in the furnace and measure the temperature;

[0098] 6) The tapping temperature range is controlled at 1550-1600°C, and the cast steel billet is about 3 tons; the steel billet is homogenized at 1050-1150°C for 10 hours.

[0099] 7) After the billet solidifies, the riser end and the nozzle end are removed and the surface is processed, and then the false electrode is welded to make the electrode rod, and the electroslag furnace is charged;

[0100] 8) Before electroslag remelting, check the air tightness of the equipment, use high-purity Ar as the protective atmosphere, and continuously pass it into the crystallizer at a large flow rate for 10 minutes before arcing to ensure that the O2 content in the crystallizer is less than 0.03% under the Ar protective atmosphere;

[0101] 9) Using CaF2:Al2O3:CaO=60:20:20 ternary slag system with a total slag amount of 150kg, 0.02% BN and 0.1% carbon powder are added to the slag to form a mixed slag, wherein the mixed slag system and BN are baked at 800±20℃ for 6-8h before use; the mixed slag is temporarily stored in an oven at 100℃ and quickly taken out.

[0102] 10) Using Benxi Steel materials as base pads and arc starters to carry out electroslag remelting treatment, the voltage in the stable stage is controlled at 45-46V, and the average electroslag melting rate is controlled at 7-9kg / min;

[0103] 11) The steel billet is cooled in the furnace for 1 to 2 hours before being tapped out, hood cooled for 24 to 36 hours, and then annealed at 750 to 800°C for 24 to 30 hours.

[0104] Example 2

[0105] The electroslag remelting test of 150kg 10Cr11Co3W3NiMoVNbNB electrode rod was carried out in the laboratory. The changes of easily burned elements in the steel billet before and after treatment were compared, and the element recovery rate was calculated.

[0106] The diameter of the electrode rod is Φ150mm, and the inner diameter of the crystallizer is Φ220mm; the electroslag slag system is a ternary slag system of CaF2:Al2O3:CaO=60:20:20, and the total slag amount is 15kg; carbon powder and BN are added to the slag to form a mixed slag, and two mixed slag schemes are adopted respectively: 0.1% carbon powder + 0.02% BN, 0.1% carbon powder + 0.04% BN; the electroslag melting rate is 6-7kg / min (for small ingots, the melting rate is further reduced).

[0107] The composition comparison and element recovery rate of the easily burned elements before and after electroslag treatment of the steel billet are shown in Table 2. Among them, the B recovery rate reaches 94.44% and the Nb recovery rate is close to 100% when the mixed slag scheme with 0.02% BN is adopted; the B recovery rate is 77.27% and the Nb recovery rate is 92.23% when the mixed slag scheme with 0.04% BN is adopted. In both mixed slag schemes, the Si content in the steel billet decreases to varying degrees, and there is an increase in Al.

[0108] Table 2 Yield of 10Cr11Co3W3NiMoVNbNB billet B before and after electroslag remelting

[0109]

[0110] Finally, it should be noted that the above is only a preferred embodiment of the present invention and is not intended to limit the present invention. Although the present invention has been described in detail with reference to the aforementioned embodiments, it is still possible for those skilled in the art to modify the technical solutions described in the aforementioned embodiments or to make equivalent substitutions for some of the technical features therein. Any modifications, equivalent substitutions, improvements, etc. made within the spirit and principles of the present invention should be included in the protection scope of the present invention.

Claims

1. An electroslag mixing method for inhibiting the burning of boron element in boron-containing and nitrogen-containing heat-resistant steel, characterized in that: The method comprises, The raw materials are sequentially subjected to pretreatment, charging, melting, vacuum carbon deoxidation refining, addition of ferroboron, and steel pouring to obtain a heat-resistant steel ingot; wherein the raw material components of the heat-resistant steel ingot include, by mass percentage (%): C: 0.09-0.11, Mn: 0.4-0.5, Si: ≤0.1, P: ≤0.015, S: ≤0.01, Cr: 11-11.5, Ni: 0.3-0.7, Mo: 0.1-0.4, Co: 2.5-3.5, W: 2.4-3, V: 0.2-0.24, Nb: 0.08-0.14, N: 0.012-0.02, B: 0.015-0.02, Al: 0.01-0.015, Ti: 0.01-0.02, and the rest is Fe except for a small amount of impurity elements; Vacuum carbon deoxidation refining: Heat to refining temperature, refining for 50 to 80 minutes in vacuum environment, add deoxidizer, take samples for analysis after melting, then add Nb-Fe and V-Fe respectively, and stir; during vacuum carbon deoxidation refining, the oxygen content in the electrode base material is controlled at ≤30ppm; Add ferroboron and cast steel: Add N-Cr and sponge Ti and stir them, add B-Fe and Mn after they are melted, fill in inert gas to increase the pressure in the furnace and control the steel tapping temperature range at 1550-1650℃, and cast to obtain heat-resistant steel ingots; After pouring and obtaining the heat-resistant steel ingot, when the B content at the head and tail of the electrode rod is at the control lower limit, the electrode base material is subjected to homogenization treatment at 1050-1150°C for not less than 10 hours; Adding electroslag mixed slag to the heat-resistant steel ingot, wherein the electroslag mixed slag includes boron nitride and carbon powder, wherein the content of boron nitride is 0.01-0.02%, and the content of carbon powder is 0.1-0.15%; the electroslag mixed slag also includes one or more of CaF2, Al2O3, and CaO; The electroslag remelting is carried out in a protective atmosphere, the filling ratio d=(0.6-0.8)D, D is the diameter of the crystallizer; the electroslag melting rate is controlled at 7-11kg / min; wherein, the electroslag remelting is carried out in a protective atmosphere, including: When using protective atmosphere for electroslag remelting, a large flow rate of inert gas is introduced into the crystallizer for 10 to 15 minutes before arc initiation, and the flow rate of inert gas is gradually reduced after the electroslag remelting process becomes stable. After the flow rate of the inert gas is reduced, the O2 content in the electroslag remelting process is ≤0.02%.

2. The electroslag mixing method for inhibiting the burning loss of boron element in boron-containing and nitrogen-containing heat-resistant steel according to claim 1, characterized in that: The average voltage in the stable stage of electroslag remelting is 45-46V.

3. The electroslag mixing method for inhibiting the burning loss of boron element in boron-containing and nitrogen-containing heat-resistant steel according to claim 1, characterized in that: For heat-resistant steel ingots with a total weight of ≤3t, the electroslag melting rate is controlled at 7-9kg / min; for heat-resistant steel ingots with a total weight of ≥3t, the electroslag melting rate is controlled at 9-11kg / min.

4. The electroslag mixing method for inhibiting the burning loss of boron element in boron-containing and nitrogen-containing heat-resistant steel according to claim 1, characterized in that: The method further comprises, After electroslag remelting, the electroslag ingot is left to stand in the crystallizer for 1 to 2 hours before being tapped, hood-cooled for 24 to 36 hours, and then annealed at 750 to 800°C for 24 to 30 hours.

5. The electroslag mixing method for inhibiting the burning loss of boron element in boron-containing and nitrogen-containing heat-resistant steel according to claim 1, characterized in that: The acquisition of the heat-resistant steel ingot comprises: Raw material pretreatment: Shot blast the alloy raw materials to completely remove the oxide scale, and weigh them for later use; Charging and melting: Load the alloy raw materials into the crucible in a loose-up and tight-down manner, close the furnace and evacuate the chamber. When the vacuum degree in the smelting chamber is lower than 20Pa, power on and start smelting. After the alloy is completely melted, take samples for analysis and make fine adjustments to the composition in the furnace.

6. The electroslag mixing method for inhibiting the burning loss of boron element in boron-containing and nitrogen-containing heat-resistant steel according to claim 1, characterized in that: After heat treatment, the riser and nozzle ends of the electrode rod are removed and the surface is polished or turned.