A chelated organotin catalyst and its application in storage-resistant dealcoholization type RTV-1 silicone rubber
By using a combination of chelated organotin catalysts and dehydration catalysts, the problem of decreased curing performance of de-alcoholized RTV-1 silicone rubber during storage was solved, achieving high stability and environmental friendliness.
Patent Information
- Application Number
- CN202211686085.4
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2022-12-27
- Publication Date
- 2024-11-29
- Estimated Expiration
- 2042-12-27
AI Technical Summary
Existing de-alcoholized RTV-1 silicone rubber undergoes an equilibrium reaction with polysiloxane in the presence of free alcohol and organometallic catalysts during storage, resulting in decreased curing performance and the presence of irritating alcohol odors and corrosion problems.
A chelated organotin catalyst containing phosphate ester ligands, combined with a dehydration catalyst and a methanol carrier, is used to accelerate the hydrolysis of the crosslinking agent and the azeotropic removal of free alcohol, thereby reducing the equilibrium reaction between alcohols and the base rubber. The chelated organotin catalyst with phosphate ester ligands is used to catalyze the condensation reaction of silicone rubber.
It significantly improves the storage stability of the dealcoholized RTV-1 silicone rubber, avoids the equilibration reaction of alcohols, reduces irritating odor and corrosion risk, and maintains the performance of silicone rubber.
Smart Images

Figure QLYQS_1 
Figure QLYQS_2 
Figure BDA0004021064610000061
Abstract
Description
Technical Field
[0001] The invention relates to the field of dealcoholization RTV-1 silicone rubber catalysts, and in particular to a chelated organotin catalyst and application thereof in storage-resistant dealcoholization RTV-1 silicone rubber. Background Art
[0002] According to the vulcanization mechanism, silicone rubber can be divided into two systems: addition type and condensation type. The former must have a catalyst to react, while the condensation type is a spontaneous reaction, but the reaction speed is too slow, and it is generally assisted by organic or titanate and its complex catalysts; according to the different condensation products, condensation-type one-component room temperature curing (RTV-1) silicone rubber is mainly divided into deketoxime type, dealcoholization type, deacetic acid type, deamidation type, dehydroxylamine type, dehydrogenation type, and deacetone type.
[0003] During the curing process, the dealcohol-type one-component room temperature curing silicone rubber releases alcohols, has no irritating odor, has good comprehensive performance, and its environmental protection is in line with the future market application prospects; however, its storage performance is poor, and the curing performance gradually decreases with the extension of storage time or even does not cure. The main reason is that the free alcohol in the dealcohol-type room temperature curing silicone rubber reacts with polysiloxane in a balanced manner in the presence of an organic metal catalyst to form (CH3O)(CH3)2SiO 1 / 2 End group.
[0004] Chinese patent document CN102911198B discloses a hydroxyl scavenger, which can remove a certain amount of methanol, water or silanol, improve the storage stability of silicone rubber, and improve the mechanical properties of silicone rubber prepared from fillers treated with the compound; however, ammonia released by alcoholysis of the compound can corrode copper, and excessive addition can affect the deep curing performance of dealcoholization-type room temperature curing silicone rubber.
[0005] Chinese patent document CN102875591B discloses a tetra-tert-butyl titanate complex, which can be used as a catalyst for RTV silicone rubber. The tetra-tert-butyl titanate complex has relatively stable quality and can be used to prepare transparent dealcoholized RTV silicone rubber; however, the free alcohol in the system is prone to equilibrium reaction of polysiloxane in the presence of the catalyst, resulting in a decrease in the curing performance of the silicone rubber. Summary of the invention
[0006] In order to solve the deficiencies in the prior art, the purpose of the present invention is to provide a chelated organotin catalyst and its application in storage-resistant dealcoholization RTV-1 silicone rubber. The present invention provides a chelated organotin catalyst containing a phosphate ligand, which has a good catalytic effect on the condensation reaction of the rubber material, but has an extremely low catalytic efficiency for the equilibrium reaction of methanol and the base rubber. The present invention also utilizes a dehydration catalyst to accelerate the hydrolysis of the cross-linking agent in the production process, deeply removes the water in the system and generates methanol, and then utilizes a methanol carrier to azeotropically remove the free methanol in the system, thereby reducing or even inhibiting the equilibrium reaction of the methanol synergistic catalyst and the base rubber, greatly prolonging the storage stability of the prepared dealcoholization RTV-1 silicone rubber.
[0007] In order to achieve the above object, the present invention adopts the following technical solution:
[0008] A chelated organotin catalyst, comprising the following components in parts by weight:
[0009] Dibutyltin diacetoacetate 13-30 servings; Ethylene glycol methyl ether 25-60 servings; Chelating agents 50-100 copies; Diisobutylamine 20 to 40 servings.
[0010] Preferably, the chelating agent is di(2-ethylhexyl) phosphate and / or 2-ethylhexyl phosphate mono-2-ethylhexyl ester.
[0011] The present invention also claims a storage-resistant dealcoholization RTV-1 silicone rubber prepared by using the chelated organotin catalyst, which comprises the following components in parts by weight:
[0012] Alkoxy-terminated polydimethylsiloxane 100 copies; Plasticizers 0-30 servings; filler 8-20 servings; Crosslinking agent 3 to 10 servings; Interface agent 0.1~0.5 parts; Dehydration catalyst 0.05~0.5 parts; Methanol Carrier 0.1~5 parts; Coupling agent 0.6~4 parts; Crab-compounded organotin catalyst 0.1 to 2 servings.
[0013] Preferably, the alkoxy-terminated polydimethylsiloxane is methyldimethylsilane-terminated polydimethylsiloxane and / or vinyldimethoxy-terminated polydimethylsiloxane, and the viscosity of the alkoxy-terminated polydimethylsiloxane at 25° C. is 2000 to 50000 mPa·s.
[0014] Preferably, the plasticizer is one or more of alkyl aromatic hydrocarbons, mineral oil or dimethyl silicone oil.
[0015] Preferably, the filler is fumed silica, and the specific surface area of the filler is 90 to 300 m 2 / g.
[0016] Preferably, the crosslinking agent is one or more of methyltrimethoxysilane, methyltriethoxysilane, vinyltrimethoxysilane, vinyltriethoxysilane, methyl orthosilicate or ethyl orthosilicate.
[0017] Preferably, the interfacial agent is ethylene glycol methyl ether and / or propylene glycol methyl ether.
[0018] Preferably, the dehydration catalyst is diethylamine.
[0019] Preferably, the methanol carrier is isopropyl acetate.
[0020] Preferably, the coupling agent is one or more of γ-aminopropyltrimethoxysilane, γ-aminopropyltriethoxysilane, β-aminoethyl-γ-aminopropyltrimethoxysilane or γ-glycidoxypropyltrimethoxysilane.
[0021] The present invention also claims protection for a method for preparing the storage-resistant dealcoholization RTV-1 silicone rubber, comprising the following steps: weighing alkoxy-terminated polydimethylsiloxane, a cross-linking agent, an interfacial agent, and a dehydration catalyst by weight and mixing them evenly, then adding a methanol carrier, a filler, and a plasticizer, controlling the rotation speed to 500 to 800 rpm, stirring at 65 to 75° C. and -0.06 to -0.099 MPa for 60 to 120 min, adding a coupling agent and a chelated organic tin catalyst after mixing evenly, and vacuum degassing and mixing for 30 to 60 min to obtain the storage-resistant dealcoholization RTV-1 silicone rubber.
[0022] Compared with the prior art, the present invention has the following beneficial effects:
[0023] 1) Alcohols can react with the base rubber polysiloxane in an equilibrium reaction in the presence of a metal catalyst to form some end groups without cross-linking function, so that the rubber gradually loses its vulcanization performance during storage; the present invention provides a chelated organic tin catalyst containing a phosphate ligand, which has a good catalytic effect on the condensation reaction of silicone rubber and basically does not cause an equilibrium reaction between alcohols and the base rubber, and can significantly improve the storage stability of dealcoholization RTV-1 silicone rubber.
[0024] 2) The chelated organic tin catalyst prepared by the present invention has a very strong P=O bond energy of the chelating agent, and phosphorus tends to generate a tetracoordinate compound containing a P=O bond, which can provide many metal multi-structure chelated ligands; diisobutylamine can neutralize phosphate esters, remove acidic groups that are not conducive to the curing of dealcoholized RTV-1 silicone rubber, and does not affect the performance of the dealcoholized RTV-1 silicone rubber; ethylene glycol methyl ether is used as a solvent to avoid agglomeration and encapsulation of phosphate esters during neutralization.
[0025] 3) The present invention discloses a storage-resistant dealcoholization RTV-1 silicone rubber. In the production process, a dehydration catalyst diethylamine is added to accelerate the hydrolysis of a crosslinking agent, deeply remove the water in the system and generate methanol, and then a methanol carrier isopropyl acetate is used to azeotropically remove free alcohol in the system, thereby reducing or even inhibiting the equilibrium reaction between the methanol synergistic catalyst and the base rubber, significantly improving the storage stability of the dealcoholization RTV-1 silicone rubber, and not affecting the performance of the dealcoholization RTV-1 silicone rubber after production.
[0026] 4) Compared with the prior art, the methanol carrier added in the present invention will not produce irritating odors such as NH3 while removing free alcohol in the system, and thus will not cause corrosion to the coating substrate; the dehydration catalyst added in the present invention will not have a negative impact on the mechanical properties and thermal stability of RTV-1 silicone rubber. DETAILED DESCRIPTION
[0027] In order to make the purpose, technical solution and advantages of the present invention clearer, the present invention is further described in detail below in conjunction with the embodiments. Of course, the specific embodiments described here are only used to explain the present invention and are not used to limit the present invention.
[0028] The term "and / or" as used herein refers to and encompasses any and all possible combinations of one or more of the associated listed items.
[0029] Unless otherwise specified, the chemical reagents and materials in the present invention are purchased from the market or synthesized from raw materials purchased from the market.
[0030] Example 1
[0031] A method for preparing a chelated organotin catalyst, the specific steps are as follows:
[0032] 13.3 g of dibutyltin diacetoacetate was added to 26.6 g of ethylene glycol methyl ether, and then 44.2 g of di(2-ethylhexyl)phosphate and 17.3 g of diisobutylamine were added and mixed evenly to obtain the chelated organotin catalyst; A method for preparing a storage-resistant dealcoholization RTV-1 silicone rubber, the specific steps of which are as follows:
[0033] 100 g of vinyl dimethoxy-terminated polydimethylsiloxane with a viscosity of 25000 mPa·s, 4 g of methyltrimethoxysilane, 0.25 g of ethylene glycol methyl ether, and 0.25 g of diethylamine were added to a planetary mixer and mixed evenly. Then, 10 g of dimethyl silicone oil with a viscosity of 400 mPa·s and 10 g of a specific surface area of 150 m 2 / g of fumed silica and 0.3g of isopropyl acetate were added, the rotation speed was controlled to 500rpm, and the low-boiling substances were removed by stirring for 90min under a vacuum degree of -0.06Mpa. Then, 1.2g of γ-aminopropyltrimethoxysilane and 1.92g of chelated organotin catalyst were added, and the mixture was stirred for 30min under a vacuum degree of -0.09Mpa to obtain a storage-resistant dealcoholization RTV-1 silicone rubber.
[0034] Example 2
[0035] A method for preparing a chelated organotin catalyst, the specific steps are as follows:
[0036] 13.7 g of dibutyltin diacetoacetate was added to 27.4 g of ethylene glycol methyl ether, and then 41.3 g of 2-ethylhexyl phosphate mono-2-ethylhexyl ester and 17.6 g of diisobutylamine were added and mixed uniformly to obtain the chelated organotin catalyst;
[0037] A method for preparing a storage-resistant dealcoholization type RTV-1 silicone rubber, the specific steps are as follows:
[0038] 100 g of methyldimethylsilane-terminated polydimethylsiloxane with a viscosity of 50000 mPa·s, 4 g of methyltrimethoxysilane, 0.25 g of ethylene glycol methyl ether, and 0.25 g of diethylamine were added to a planetary mixer and mixed evenly. Then, 10 g of dimethyl silicone oil with a viscosity of 400 mPa·s and 10 g of a specific surface area of 150 m 2 / g of fumed silica and 0.3g of isopropyl acetate were added, the rotation speed was controlled at 600rpm, and the low-boiling substances were removed by stirring for 100min under a vacuum degree of -0.08Mpa. Then, 1.2g of γ-aminopropyltrimethoxysilane and 1.89g of a chelated organotin catalyst were added, and the mixture was stirred for 30min under a vacuum degree of -0.09Mpa to obtain a storage-resistant dealcoholization RTV-1 silicone rubber.
[0039] Example 3
[0040] A method for preparing a chelated organotin catalyst, the specific steps are as follows:
[0041] 13.7g of dibutyl tin diacetoacetate was added to 27.4g of ethylene glycol methyl ether, and then 21.4g of di(2-ethylhexyl) phosphate, 20.65g of 2-ethylhexyl phosphate mono-2-ethylhexyl fat, and 17.45g of diisobutylamine were added and mixed uniformly to obtain the chelated organotin catalyst;
[0042] A method for preparing a storage-resistant dealcoholization type RTV-1 silicone rubber, the specific steps are as follows:
[0043] 100 g of vinyl dimethoxy-terminated polydimethylsiloxane with a viscosity of 25000 mPa·s, 4 g of methyltrimethoxysilane, 0.25 g of ethylene glycol methyl ether, and 0.25 g of diethylamine were added to a planetary mixer and mixed evenly. Then, 10 g of dimethyl silicone oil with a viscosity of 400 mPa·s and 10 g of a specific surface area of 150 m 2 / g of fumed silica and 0.3g of isopropyl acetate were added, the rotation speed was controlled to 800rpm, and the low-boiling substances were removed by stirring for 120min under a vacuum degree of -0.09Mpa. Then, 1.2g of γ-aminopropyltrimethoxysilane and 1.86g of chelated organotin catalyst were added, and the mixture was stirred for 30min under a vacuum degree of -0.09Mpa to obtain a storage-resistant dealcoholization RTV-1 silicone rubber.
[0044] Comparative Example 1
[0045] A method for preparing dealcoholized RTV-1 silicone rubber, the specific steps are as follows:
[0046] 100 g of vinyl dimethoxy-terminated polydimethylsiloxane with a viscosity of 25000 mPa·s, 4 g of methyltrimethoxysilane, 0.25 g of ethylene glycol methyl ether, and 0.25 g of diethylamine were added to a planetary mixer and mixed evenly. Then, 10 g of dimethyl silicone oil with a viscosity of 400 mPa·s and 10 g of a specific surface area of 150 m 2 / g of fumed silica and 0.3g of isopropyl acetate were added, the rotation speed was controlled to 500rpm, and the low-boiling substances were removed by stirring for 90min under a vacuum degree of -0.06Mpa. Then, 1.2g of γ-aminopropyltrimethoxysilane and 0.25g of dibutyltin diacetoacetate were added, and the mixture was stirred for 30min under a vacuum degree of -0.09Mpa to obtain dealcoholized RTV-1 silicone rubber.
[0047] Comparative Example 2
[0048] A method for preparing a catalyst mixture sample, the specific steps are as follows:
[0049] 13.3 g of dibutyltin diacetoacetate was added to 26.6 g of ethylene glycol methyl ether, and then 42.8 g of di(2-ethylhexyl)phosphate was added and mixed evenly to obtain a catalyst mixture sample;
[0050] A method for preparing dealcoholized RTV-1 silicone rubber, the specific steps are as follows:
[0051] 100 g of vinyl dimethoxy-terminated polydimethylsiloxane with a viscosity of 25000 mPa·s, 4 g of methyltrimethoxysilane, 0.25 g of ethylene glycol methyl ether, and 0.25 g of diethylamine were added to a planetary mixer and mixed evenly. Then, 10 g of dimethyl silicone oil with a viscosity of 400 mPa·s and 10 g of a specific surface area of 150 m 2 / g of fumed silica and 0.3g of isopropyl acetate were added, the rotation speed was controlled to 500rpm, and low boiling points were removed by stirring for 90min under a vacuum degree of -0.06Mpa. Then, 1.2g of γ-aminopropyltrimethoxysilane and 1.92g of the catalyst were added and the mixture was stirred for 30min under a vacuum degree of -0.09Mpa to obtain dealcoholized RTV-1 silicone rubber.
[0052] First, the performance of the dehydration catalyst used in the present invention is tested, and the specific steps are as follows:
[0053] Sample 1: 20 g of water was added to 100 g of methyltrimethoxysilane at room temperature, and the mixture was allowed to stand in the air after mixing;
[0054] Sample 2: Add 20 g of water and 10 g of ethylene glycol methyl ether to 90 g of methyltrimethoxysilane at room temperature, mix and let stand in air;
[0055] Sample 3, at room temperature, 20g of water, 10g of ethylene glycol methyl ether and 10g of diethylamine were added to 80g of methyltrimethoxysilane, and the mixture was allowed to stand in the air after mixing. The specific experimental results are shown in Table 1.
[0056] Table 1
[0057] Standing time Sample 1 Sample 2 Sample 3 3min Spherical droplet interface is clear Two-phase stratification Fever and turbidity 10min Droplet two-phase aggregation Two-phase homogenization White particles generated 1h Two-phase stratification 24h Two-phase stratification 72h Mild fusion of interface layer
[0058] The observation results of samples 1 and 2 in Table 1 show that the direct dehydration effect of the cross-linking agent methyltrimethoxysilane is very poor. First, methyltrimethoxysilane and water are not miscible, and the contact area is insufficient, so an interfacial agent is required to promote miscibility. Secondly, under a neutral environment, the hydrolysis rate of methyltrimethoxysilane is very slow, which cannot meet the requirement of rapid dehydration in production. The observation results of sample 3 show that under the joint action of the interfacial agent and the dehydration catalyst, the cross-linking agent methyltrimethoxysilane hydrolyzes very quickly. The dehydration catalyst disclosed in the present invention plays a good role in accelerating the hydrolysis of the cross-linking agent, can quickly consume the water in the system, and can greatly improve the storage performance of the dealcoholized RTV-1 silicone rubber.
[0059] Next, the performance of the dealcoholized RTV-1 silicone rubber prepared in Examples 1 to 3 and Comparative Examples 1 to 2 was tested. The specific process is as follows: the surface drying time of the dealcoholized RTV-1 silicone rubber was tested using the national standard GB / T 13477.5-2002; the hardness of the dealcoholized RTV-1 silicone rubber was tested using the national standard GB / T 531.1-2008; the prepared dealcoholized RTV-1 silicone rubber was aged at 100°C for 24h, 72h and 168h, respectively, and then the performance of the dealcoholized RTV-1 silicone rubber was tested. The specific experimental results are shown in Table 2.
[0060] Table 2
[0061]
[0062] Examples 1 to 3 and Comparative Examples 1 to 2 all use a methanol carrier and a dehydration catalyst, so the water and free alcohol in the system are greatly reduced, thereby alleviating or even inhibiting the equilibrium reaction between the free alcohol and the base rubber in the system; the difference is that Examples 1 to 3 also use the chelated organic tin catalyst disclosed in the present invention, Comparative Example 1 uses a common condensation catalyst, and Comparative Example 2 uses a catalyst mixture without adding diisobutylamine; according to the performance data tested in Table 2, it can be seen that the initial performance of the dealcoholized RTV-1 silicone rubber prepared in Examples 1 to 3 and Comparative Examples 1 to 2 is The performance of the dealcoholized RTV-1 silicone rubber prepared in Examples 1 to 3 and Comparative Examples 1 to 2 was not significantly degraded even after the accelerated aging test at 100°C for 24 hours and 72 hours. However, after the accelerated aging test at 100°C for 168 hours, it was found that the dealcoholized RTV-1 silicone rubber prepared in Examples 1 to 3 still had better performance, but the dealcoholized RTV-1 silicone rubber prepared in Comparative Examples 1 to 2 could not be cured. This shows that the chelated organotin catalyst disclosed in the present invention can significantly improve the storage stability of the dealcoholized RTV-1 silicone rubber.
[0063] The above description is only a preferred specific implementation manner of the present invention, but the protection scope of the present invention is not limited thereto. Any technician familiar with the technical field can make equivalent replacements or changes according to the technical scheme and inventive concept of the present invention within the technical scope disclosed by the present invention, which should be covered by the protection scope of the present invention.
Claims
1. A chelated organotin catalyst, characterized in that: In parts by weight, it contains the following components: The chelating agent is di(2-ethylhexyl) phosphate and / or 2-ethylhexyl phosphate mono-2-ethylhexyl ester.
2. The storage-resistant dealcoholization type RTV-1 silicone rubber prepared by the chelated organotin catalyst according to claim 1, characterized in that: In parts by weight, it contains the following components:
3. The storage-resistant dealcoholization type RTV-1 silicone rubber according to claim 2, characterized in that: The alkoxy-terminated polydimethylsiloxane is methyldimethylsilane-terminated polydimethylsiloxane and / or vinyldimethoxy-terminated polydimethylsiloxane, and the viscosity of the alkoxy-terminated polydimethylsiloxane at 25° C. is 2000-50000 mPa·s.
4. The storage-resistant dealcoholization type RTV-1 silicone rubber according to claim 2, characterized in that: The plasticizer is one or more of alkyl aromatic hydrocarbons, mineral oil or dimethyl silicone oil; the filler is fumed silica, and the specific surface area of the filler is 90-300 m 2 / g.
5. The storage-resistant dealcoholization type RTV-1 silicone rubber according to claim 2, characterized in that: The crosslinking agent is one or more of methyltrimethoxysilane, methyltriethoxysilane, vinyltrimethoxysilane, vinyltriethoxysilane, methyl orthosilicate or ethyl orthosilicate.
6. The storage-resistant dealcoholization type RTV-1 silicone rubber according to claim 2, characterized in that: The interface agent is ethylene glycol methyl ether and / or propylene glycol methyl ether.
7. The storage-resistant dealcoholization type RTV-1 silicone rubber according to claim 2, characterized in that: The dehydration catalyst is diethylamine; the methanol carrier is isopropyl acetate.
8. The storage-stable dealcoholization type RTV-1 silicone rubber according to claim 2, characterized in that: The coupling agent is one or more of γ-aminopropyltrimethoxysilane, γ-aminopropyltriethoxysilane, β-aminoethyl-γ-aminopropyltrimethoxysilane or γ-glycidoxypropyltrimethoxysilane.
9. A method for preparing the storage-resistant dealcoholization type RTV-1 silicone rubber according to any one of claims 2 to 8, characterized in that: The method comprises the following steps: weighing alkoxy-terminated polydimethylsiloxane, a crosslinking agent, an interface agent and a dehydration catalyst by weight and mixing them evenly; then adding a methanol carrier, a filler and a plasticizer; controlling the rotation speed to 500-800 rpm; stirring for 60-120 minutes at 65-75°C and -0.06-0.099 MPa; adding a coupling agent and a chelated organic tin catalyst after mixing evenly; and vacuum degassing and mixing for 30-60 minutes to obtain the storage-resistant dealcoholization RTV-1 silicone rubber.
Citation Information
Patent Citations
Method for preparing tetra-tert-butyl orthotitanate composite
CN102875591B
A hydroxyl scavenging compound, its preparation method and its uses
CN102911198B
Single-component dealcoholization type room-temperature vulcanized silicone sealant and preparation method thereof
CN109762511A
Flame-retardant organic polysiloxane composition and preparation method thereof
CN110204900A