A Te-doped Rb 2 SnCl 6 Preparation method and application of vacancy-ordered double perovskite phosphor
Preparation of Te-doped Rb2SnCl6 vacant ordered double perovskite phosphor by aqueous precipitation method, solving the toxicity and instability of lead-based perovskites, improving fluorescence performance and stability, and achieving suitable for large-scale production The green and low-cost process is used in white light-emitting diode devices, improving the color rendering index and color temperature.
Patent Information
- Application Number
- CN202211611604.0
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2022-12-14
- Publication Date
- 2024-11-22
- Estimated Expiration
- 2042-12-14
AI Technical Summary
In the prior art, the toxicity and instability of lead-based perovskite materials hinder their large-scale commercial applications. At the same time, the fluorescence performance of traditional Rb2SnCl6 perovskites is poor, and their synthesis methods are complex and not suitable for large-scale production.
Using simple aqueous precipitation method, Te-doped Rb2SnCl6 vacant order double perovskite phosphor was prepared through low-temperature reaction. Using tin, tellurium and rubidium compounds as raw materials, effective doping of Te doping was achieved and improved The stability and fluorescence properties of the material are achieved.
The prepared Te doped Rb2SnCl6 phosphor exhibits yellow-green light emission and high photoluminescence quantum efficiency (60-74.2%), and is used in white light-emitting diode devices, achieving high color development index and suitable color temperature, solving the stability of the material and the problem of fluorescence performance, simple process and low cost, suitable for large-scale production.
Smart Images

Figure CN116285979B_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to the technical field of luminescent materials, and in particular to a preparation method and application of a doped Rb2SnCl6 vacancy-ordered double perovskite phosphor. Background Art
[0002] With the rapid development of information technology and the increasingly serious energy crisis, people's demand for more efficient, energy-saving, stable and low-cost terminal display devices and lighting equipment has increased sharply. Light-emitting diodes (LEDs) have attracted widespread attention as an important development of full-color display technology and solid-state lighting. Based on InGaN blue light LED chips stimulating Ce 3+ :Y3Al5O 12 White light LEDs with yellow phosphors have the advantages of environmental protection, energy saving, high light efficiency and long life, and are an ideal choice to replace traditional incandescent lamps. However, the excess blue light components in white light LEDs can easily cause irreversible damage to the human eye, especially the retina of children, namely "blue damage". In addition, a large amount of strategic rare earth materials are used as raw materials. Therefore, the development of a new generation of new single-matrix white fluorescent materials to avoid "blue damage" and the use of rare earth elements is of great significance to achieve green lighting and sustainable energy development.
[0003] Lead halide perovskite materials have optoelectronic properties such as wide emission spectrum, large Stokes shift, and high quantum efficiency (PLQY≈100%), making them ideal materials for new single-matrix white fluorescent materials. However, the toxicity of lead and its poor stability under light, humidity, and heat hinder the large-scale commercial application of lead-based halide perovskites.
[0004] Pb for lead-based perovskites 2+ In order to solve the toxicity problem of Sn ions, researchers have explored new methods to replace lead-based perovskites, including equivalent substitution, non-equivalent substitution, monovalent / trivalent co-substitution and tetravalent / vacancy co-substitution. Since the physical properties of Sn and Pb are similar, lead-free RbSnCl3 perovskite has become an ideal choice to replace lead halide perovskite. However, Sn 2+ Sn is easily oxidized 4+ , resulting in poor stability. Therefore, through a Sn 4+ Replace two Pb 2+ It can form a stable vacancy-ordered double perovskite (Rb2SnCl6), which has excellent stability, high carrier mobility and high absorption coefficient, making it an ideal optoelectronic material. However, due to the large number of vacancies in Rb2SnCl6 perovskite, its fluorescence performance is poor, but its luminescence performance can be greatly improved by doping. For example: Bi 3+ Doped lead-free Rb2SnCl6 perovskite, due to Bi 3+ and Sn 4+The unequal valence states between them lead to defective complexes [Bi Sn +V Cl ], thereby improving the fluorescence performance. However, the anion vacancies generated by heterovalent doping hinder the further improvement of the fluorescence quantum yield of lead-free Rb2SnCl6 perovskite phosphors.
[0005] In addition, the main methods for synthesizing Rb2SnCl6 are solvothermal and hot injection methods, but the above methods require expensive equipment, harsh reaction conditions, and complex operations, which are not conducive to the large-scale production of phosphors and limit the development of lead-free halide perovskite phosphors. Therefore, it is still an urgent problem to develop a simple, green and scalable synthesis method to prepare high-efficiency, high-stability lead-free halide perovskite phosphors and construct white light-emitting diode devices with high color rendering index and color temperature. Summary of the invention
[0006] The purpose of the present invention is to overcome the shortcomings of the prior art and provide a method for preparing a Te-doped Rb2SnCl6 vacancy-ordered double perovskite phosphor. The Te-doped Rb2SnCl6 vacancy-ordered double perovskite phosphor is prepared at low temperature by a simple aqueous precipitation method using tin-containing compounds, tellurium-containing compounds, and rubidium-containing compounds as raw materials. Another purpose of the present invention is to provide an application of the above-mentioned Te-doped Rb2SnCl6 vacancy-ordered double perovskite phosphor.
[0007] The purpose of the present invention is achieved through the following technical solutions:
[0008] The present invention provides a method for preparing a Te-doped Rb2SnCl6 vacancy-ordered double perovskite phosphor, comprising the following steps:
[0009] (1) adding a tin-containing compound and a tellurium-containing compound to concentrated hydrochloric acid at a molar ratio of tin:tellurium = 0.750-0.999:0.001-0.250, stirring and dissolving, to obtain a solution A with a concentration of 0.1-0.5 mol / L;
[0010] (2) adding the rubidium-containing compound to concentrated hydrochloric acid, stirring and dissolving to obtain a solution B with a concentration of 0.5 to 2 mol / L;
[0011] (3) adding the solution B to the solution A at a molar ratio of rubidium:tin+tellurium=2:1, reacting at a temperature of 80-160°C for 0.1-4h to obtain a light yellow precipitate product;
[0012] (4) The product is cooled to room temperature, and after centrifugation or filtration, washing and drying, a Te-doped Rb2SnCl6 vacancy-ordered double perovskite phosphor is obtained.
[0013] Furthermore, the tin-containing compound of the present invention is tin tetrachloride, tin dichloride, tin tetrachloride pentahydrate, tin oxide, or stannous oxide; the tellurium-containing compound is tellurium tetrachloride, sodium tellurite, or tellurium dioxide; the rubidium-containing compound is rubidium chloride or rubidium carbonate. The drying step (4) is carried out at a temperature of 40 to 70° C. for 30 to 120 minutes.
[0014] Another object of the present invention is achieved by the following technical solutions:
[0015] The product obtained by the preparation method of the above-mentioned Te-doped Rb2SnCl6 vacancy-ordered double perovskite phosphor exhibits yellow-green light emission, with a wavelength coverage range of 450 to 700 nm, a peak position of 546 to 552 nm, an emission peak line width of 97 to 105 nm, and a photoluminescence quantum efficiency (PLQY) of 60 to 74.2%.
[0016] The product of the present invention is used in a white light-emitting diode device. The material obtained by mixing the Te-doped Rb2SnCl6 phosphor with the blue phosphor and the red phosphor is mixed with silica gel and then coated on an LED chip. After curing, a white light-emitting diode device with a color rendering index of 73.3 to 97.1 and a color temperature of 4580 to 5656 K is obtained. Preferably, the materials are mixed according to a mass ratio of Te-doped Rb2SnCl6 phosphor: blue phosphor: red phosphor = 1: 0.5 to 2: 0.5 to 2.
[0017] The present invention has the following beneficial effects:
[0018] (1) The present invention adopts a simple aqueous precipitation method and a chemical reaction at low temperature to prepare a pure phase Te-doped Rb2SnCl6 vacancy-ordered double perovskite phosphor, achieving high efficiency, high stability, and broadband emission. It solves the toxicity and instability problems of lead halide perovskites in the prior art, overcomes the problems of high synthesis temperature and harsh reaction conditions of Rb2SnCl6 perovskite phosphors prepared by solvent thermal and hot injection methods, realizes effective doping of equivalent elements, and enhances the fluorescence performance and stability of Rb2SnCl6 perovskite phosphors.
[0019] (2) The Te-doped Rb2SnCl6 vacancy-ordered double perovskite phosphor prepared by the present invention exhibits yellow-green light emission, with a wavelength coverage range of 450-700nm, a peak position of 546-552nm, an emission peak line width of 97-105nm, and a PLQY of 60-74.2%. 4+ Doping induces lattice distortion, thereby enhancing electro-acoustic coupling, promoting self-trapped exciton emission, and combining with Te 4 +The phosphor is used to prepare a white light emitting diode device, and the device exhibits a high color rendering index (73.3-97.1) and a color temperature (4580-5656K).
[0020] (3) The present invention has the advantages of simple preparation method, greenness, low cost, and easy large-scale industrial production, and has broad application prospects in the field of environmental protection lighting. BRIEF DESCRIPTION OF THE DRAWINGS
[0021] The present invention will be further described in detail below with reference to the embodiments and accompanying drawings:
[0022] Figure 1 This is the XRD spectrum of the phosphor prepared in Example 1 of the present invention;
[0023] Figure 2 The PLE and PL spectra of the phosphor prepared in Example 1 of the present invention;
[0024] Figure 3 These are the electroluminescent spectrum and color coordinates of the white light LED device prepared in Example 6 of the present invention. DETAILED DESCRIPTION
[0025] Embodiment 1:
[0026] This embodiment is a Te-doped Rb2SnCl6 vacancy ordered double perovskite phosphor, and the steps are as follows:
[0027] (1) adding tin tetrachloride and tellurium tetrachloride to hydrochloric acid at a molar ratio of tin:tellurium = 0.950:0.050, stirring and dissolving at 80° C. to obtain a solution A with a concentration of 0.25 mol / L;
[0028] (2) adding rubidium chloride to concentrated hydrochloric acid, stirring and dissolving to obtain a solution B with a concentration of 1 mol / L;
[0029] (3) adding the above solution B to solution A at a molar ratio of rubidium:tin+tellurium = 2:1, reacting at 110°C for 1 hour to obtain a light yellow precipitate product;
[0030] (4) The product is cooled to room temperature, centrifuged or filtered, washed with anhydrous ethanol for 4 to 5 times, and dried at 60° C. for 60 min to obtain a Te-doped Rb2SnCl6 vacancy-ordered double perovskite phosphor.
[0031] like Figure 1 As shown, the diffraction peak of the phosphor prepared in this embodiment can correspond to the standard diffraction peak of Rb2SnCl6, and no other impurity phases are found.
[0032] like Figure 2As shown, the phosphor prepared in this embodiment exhibits dual excitation bands of 200-360nm and 360-500nm, the emission wavelength can cover 450-700nm, the peak position is 550nm, the emission peak line width is 98nm, and the PLQY is 74.2%.
[0033] Embodiment 2:
[0034] This embodiment is a Te-doped Rb2SnCl6 vacancy ordered double perovskite phosphor, and the steps are as follows:
[0035] (1) adding tin dichloride and tellurium dioxide to concentrated hydrochloric acid at a molar ratio of tin:tellurium = 0.850:0.150, stirring and dissolving at 80° C. to obtain a solution A with a concentration of 0.25 mol / L;
[0036] (2) adding rubidium chloride to concentrated hydrochloric acid, stirring and dissolving to obtain a solution B with a concentration of 1 mol / L;
[0037] (3) adding the above solution B to solution A at a molar ratio of rubidium:tin+tellurium=2:1, reacting at 140°C for 0.5h to obtain a light yellow precipitate product;
[0038] (4) The product is cooled to room temperature, centrifuged or filtered, washed with anhydrous ethanol for 4 to 5 times, and dried at 60° C. for 60 min to obtain a Te-doped Rb2SnCl6 vacancy-ordered double perovskite phosphor.
[0039] Embodiment three:
[0040] This embodiment is a Te-doped Rb2SnCl6 vacancy ordered double perovskite phosphor, and the steps are as follows:
[0041] (1) adding tin tetrachloride pentahydrate and sodium tellurite to concentrated hydrochloric acid at a molar ratio of tin:tellurium = 0.900:0.100, stirring and dissolving at 80° C. to obtain a solution A with a concentration of 0.25 mol / L;
[0042] (2) adding rubidium carbonate to concentrated hydrochloric acid, stirring and dissolving to obtain a solution B with a concentration of 1 mol / L;
[0043] (3) adding the above solution B to solution A at a molar ratio of rubidium:tin+tellurium=2:1, reacting at 120°C for 0.5h to obtain a light yellow precipitate product;
[0044] (4) The product is cooled to room temperature, centrifuged or filtered, washed with anhydrous ethanol for 4 to 5 times, and dried at 50° C. for 120 min to obtain a Te-doped Rb2SnCl6 vacancy-ordered double perovskite phosphor.
[0045] Embodiment 4:
[0046] This embodiment is a Te-doped Rb2SnCl6 vacancy ordered double perovskite phosphor, and the steps are as follows:
[0047] (1) adding stannous oxide and tellurium dioxide to concentrated hydrochloric acid at a molar ratio of tin:tellurium = 0.750:0.250, stirring and dissolving at 80° C. to obtain a solution A with a concentration of 0.25 mol / L;
[0048] (2) adding rubidium carbonate to concentrated hydrochloric acid, stirring and dissolving to obtain a solution B with a concentration of 1 mol / L;
[0049] (3) adding the above solution B to solution A at a molar ratio of rubidium:tin+tellurium = 2:1, reacting at 80°C for 1 hour to obtain a light yellow precipitate product;
[0050] (4) The product is cooled to room temperature, centrifuged or filtered, washed with n-hexane for 4 to 5 times, and dried at 60° C. for 90 min to obtain a Te-doped Rb2SnCl6 vacancy-ordered double perovskite phosphor.
[0051] Embodiment five:
[0052] This embodiment is a Te-doped Rb2SnCl6 vacancy ordered double perovskite phosphor, and the steps are as follows:
[0053] (1) adding stannous oxide and tellurium tetrachloride to concentrated hydrochloric acid at a molar ratio of tin:tellurium = 0.920:0.080, stirring and dissolving at 80° C. to obtain a solution A with a concentration of 0.25 mol / L;
[0054] (2) adding rubidium chloride to concentrated hydrochloric acid, stirring and dissolving to obtain a solution B with a concentration of 1 mol / L;
[0055] (3) adding the above solution B to solution A at a molar ratio of rubidium:tin+tellurium = 2:1, reacting at 100°C for 3 hours to obtain a light yellow precipitate product;
[0056] (4) The product is cooled to room temperature, centrifuged or filtered, washed with isopropanol for 4 to 5 times, and dried at 70° C. for 30 min to obtain a Te-doped Rb2SnCl6 vacancy-ordered double perovskite phosphor.
[0057] Embodiment six:
[0058] The Te-doped Rb2SnCl6 vacancy-ordered double perovskite phosphor prepared in Example 1 of the present invention was mixed with commercial BaMgAl 10 O 17 :Eu blue phosphor and K2SiF6:Mn 2+The material obtained by mixing red phosphor (the three are in a mass ratio of 1:1:1) and silica gel (in a mass ratio of silica gel: material = 1:1) is coated on a 395nm LED chip and cured at 150°C for 1h to obtain a white light-emitting diode device. Figure 3 As shown, the device exhibits a high color rendering index (97.1) and color temperature (4739K), and the color coordinates are (0.3522, 0.3526).
Claims
1. A Te-doped Rb 2 SnCl 6 Preparation method of vacancy ordered double perovskite phosphor, Features The following steps are involved: (1) adding a tin-containing compound and a tellurium-containing compound to concentrated hydrochloric acid at a molar ratio of tin:tellurium = 0.750-0.999:0.001-0.250, stirring and dissolving, to obtain a solution A with a concentration of 0.1-0.5 mol / L; (2) adding the rubidium-containing compound to concentrated hydrochloric acid, stirring and dissolving to obtain a solution B with a concentration of 0.5 to 2 mol / L; (3) adding the solution B to the solution A at a molar ratio of rubidium:tin+tellurium=2:1, reacting at a temperature of 80-160°C for 0.1-4 h to obtain a light yellow precipitate product; (4) The product is cooled to room temperature, centrifuged or filtered, washed, and dried at 40 to 70° C. for 30 to 120 min to obtain Te-doped Rb with yellow-green light emission, a wavelength coverage range of 450 to 700 nm, a peak position of 546 to 552 nm, an emission peak line width of 97 to 105 nm, and a photoluminescence quantum efficiency of 60 to 74.2%. 2 SnCl 6 Vacancy ordered double perovskite phosphor; doping the Te with Rb 2 SnCl 6 Phosphor is doped with Te and Rb according to the mass ratio 2 SnCl 6 Phosphor: blue phosphor: red phosphor = 1: 0.5-2: 0.5-2, the material obtained by mixing the blue phosphor and the red phosphor is mixed with silica gel, and then coated on the LED chip, and after curing, a white light emitting diode device with a color rendering index of 73.3-97.1 and a color temperature of 4580-5656 K is obtained.
2. Te-doped Rb according to claim 1 2 SnCl 6 Preparation method of vacancy ordered double perovskite phosphor, Features: The tin-containing compound is tin tetrachloride, tin dichloride, tin tetrachloride pentahydrate, tin oxide, or stannous oxide; the tellurium-containing compound is tellurium tetrachloride, sodium tellurite, or tellurium dioxide; and the rubidium-containing compound is rubidium chloride or rubidium carbonate.
3. Using the Te doped Rb as claimed in claim 1 or 2 2 SnCl 6 The product is obtained by the preparation method of vacancy ordered double perovskite phosphor.
4. Use of the product according to claim 3, Features: Applicable to white light emitting diode devices.
Citation Information
Patent Citations
Te-doped A2SnCl6 perovskite material and preparation method thereof
CN110803711A
White-light fluorescent powder as well as preparation method and application thereof
CN111876156A
Single-phase fluorescent material for white-light LED as well as preparation method and application of single-phase fluorescent material
CN113372915A
Bi / Sb co-doped tin-based perovskite crystal and preparation method and application thereof