All-solid waste spraying mortar and preparation method thereof
By forming gelling materials by fly ash, industrially produced gypsum, steel slag powder and ore dressing tailings, combined with crushed waste stone as aggregate, fully solid waste spray mortar is prepared, which solves the problems of high cost and complex processes of traditional mortar, and realizes the The preparation of spray mortar with low cost and excellent performance has improved the utilization rate of solid waste.
Patent Information
- Application Number
- CN202310184224.1
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2023-03-01
- Publication Date
- 2024-11-12
- Estimated Expiration
- 2043-03-01
AI Technical Summary
The preparation of existing jet mortars usually depends on high-cost raw materials such as cement, cement clinker, and slag. The process is complicated and the utilization rate of solid waste is low, which limits its wide application.
Fly ash, industrially produced gypsum, steel slag powder and ore dressing tailings sand are used as gelling materials, and crushed waste stones of ore dressing tailings sand are used as aggregates. All-solid waste spray mortar is prepared through screening and excitation to replace traditional glue Coagulation materials simplify processes and reduce costs.
It realizes the preparation of all-solid waste spray mortar with low cost, simple processes and excellent performance, improves solid waste utilization, avoids the high-price dependence and process complexity of traditional mortar aggregates, and meets the needs of widespread application.
Smart Images

Figure CN116354682B_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of solid waste resource utilization, and in particular to a full-solid waste spraying mortar and a preparation method thereof. Background Art
[0002] Shotcrete is a type of concrete that is sprayed onto the sprayed surface using high-pressure air with the help of a pressure spray gun or other device.
[0003] Chinese application CN 115124314 A discloses a shotcrete and a preparation method thereof, wherein the shotcrete is prepared according to the weight ratio of 16-20 parts of sulphoaluminate cement, 2-6 parts of modified gypsum, 1-3 parts of admixture, 38-44 parts of sand, 32-38 parts of gravel, 0.15-0.3 parts of water reducer, and 8-12 parts of water. The process still uses traditional building materials such as sulphoaluminate cement or ordinary silicate cement, gravel, sand, etc., which have limited sources and high costs, limiting their application; in addition, although solid waste materials such as lithium slag and fly ash are also added, the utilization ratio is not high, and there are more components, the process is more complicated, and the cost is higher.
[0004] Chinese application CN 113636812 A discloses a shotcrete and its preparation method, which prepares concrete according to the weight components of cement 400-500 parts, water 100-180 parts, gravel 1200-1300 parts, sand 500-600 parts, expansion agent 10-30 parts, water reducer 0.5-2.5 parts, waterproof nano powder 10-30 parts. This process still uses traditional building materials such as cement, gravel, sand, etc., which have limited sources, high costs, more components, more complex processes, and higher costs, which limits its application.
[0005] Chinese application CN 112408912 A discloses a low-cost shotcrete and its preparation method, which uses desert sand instead of machine-made sand, and prepares mortar according to 180-220 parts of water, 425-455 parts of Portland cement, 922-960 parts of crushed stone, 496-640 parts of desert sand, 7-10 parts of accelerator, 14-20 parts of viscosity enhancer and 3-6 parts of water reducer. Although this process uses desert sand instead of machine-made sand, it still needs to use Portland cement as a cementitious material and crushed stone as an aggregate, which is relatively expensive. In addition, desert sand is subject to relatively large geographical restrictions and limited raw material sources, which limits its promotion and application.
[0006] Chinese application CN 112047666 A discloses an alkali-activated blast furnace nickel-iron slag shotcrete, which is prepared by 300-600 parts of blast furnace nickel-iron slag powder, 200-400 parts of zeolite powder, 50-100 parts of carbide slag, 30-90 parts of sodium hydroxide, 20-60 parts of sodium silicate, 30-50 parts of setting agent, 10-20 parts of ASA resin emulsion, 600-1100 parts of machine-made sand, 100-300 parts of water slag, 3-6 parts of thickener, 1-20 parts of steel fiber, and 170-300 parts of water. The process uses sodium hydroxide and sodium silicate to activate blast furnace nickel-iron slag powder, and adds a certain amount of water slag to improve activity to prepare a binder. Its aggregate uses machine-made sand and steel fiber is added. The technology has many components, a relatively complex process, and a relatively high cost.
[0007] Chinese application CN 112094081 A discloses a mortar and a preparation method thereof, wherein the technology uses steel slag powder of different particle sizes to mix, and uses a certain aggregate forming agent to prepare the mortar, wherein the mortar is prepared according to 15-25 parts of alkali slag, 35-45 parts of steel slag, 3-6 parts of waste gypsum mold, 30-35 parts of cementitious material (cement clinker), and 0-1.5 parts of additives (enhancer / grinding aid). The process uses steel slag of different particle sizes as aggregate, and uses cement clinker as a cementitious material to prepare an aggregate forming agent, wherein the steel slag has potential activity, but its activity is not fully utilized after being crushed as an aggregate, and cement clinker is used as a cementitious material, and cement clinker is used as a cementitious material, and cement clinker is the main raw material of cement, and its cost is equivalent to that of cement, and it does not have an advantage.
[0008] Chinese application CN113135700A discloses a solid waste-based polymer mortar dry mix, which is prepared by 10% to 30% of volcanic ash cementitious material, 10% to 20% of phosphorus slag powder, 30% to 60% of sand, 0% to 10% of vermiculite powder, 0% to 10% of diatomite, 0% to 10% of magnesium borate whisker, 0% to 5% of modified nano titanium oxide, and 0.02% to 0.2% of polyvinyl alcohol and 2% to 6% of alkali activator in total raw materials. The process uses kaolin, river silt and soda ash waste residue to calcine at high temperature in a certain proportion, cool and grind, and then add a certain amount of sodium hydroxide and sodium silicate as alkali activators to prepare volcanic ash cementitious material to replace cement. The high-temperature calcination is not only complex in process, but also extremely costly. At the same time, the addition of sodium hydroxide and sodium silicate chemical reagents further increases the cost, and the advantages are not obvious.
[0009] Chinese application CN 110357556 A discloses a dry-mixed mortar made of all solid waste and its preparation method. The dry-mixed mortar is prepared according to the weight ratio of fly ash 10% to 15%, steel slag 5% to 10%, slag 5% to 10%, gypsum 3% to 5%, ceramic waste 30% to 40%, and slag 30% to 40%. The process uses mixed and crushed ceramic waste and slag as aggregates, and uses fly ash, steel slag, slag and gypsum mixed in proportion as cementitious materials. Among them, slag is currently widely used as a mineral admixture or slag cement raw material, and its price has soared, even exceeding that of cement, with high cost and complicated procedures.
[0010] In summary, the inventors of the present application have found that the preparation of the above-mentioned sprayed mortar is usually based on conventional cementitious materials, conventional aggregates, or prepared using a small amount of solid waste, and there are problems such as high cost, multiple components or underutilization, complex procedures, and limited application. How to design a sprayed mortar with low cost, simple preparation process, meeting performance requirements, and can be widely promoted and applied is a technical problem that urgently needs to be solved. In response to the above findings and understandings, the inventors of the present application have further studied and improved to provide a formula and process for all-solid waste sprayed mortar. Summary of the invention
[0011] According to one embodiment of the present invention, the purpose is to provide a full-solid waste spraying mortar and a preparation method thereof, so as to solve the problems of high cost, complicated process, limited application, low solid waste utilization rate, etc. in preparing mortar using cement, cement clinker, slag, etc. as cementitious material raw materials, and using traditional mortar aggregates such as river sand, machine-made sand, and gravel.
[0012] The above purpose can be achieved by implementing the following technical solutions:
[0013] According to one aspect of the present invention, the present invention provides an all-solid waste spraying mortar, which is a cementitious material composed of fly ash, industrial by-product gypsum, steel slag powder and tailings powder in mineral processing tailings, and uses other parts of the mineral processing tailings and crushed waste rock as aggregates; wherein, in the mineral processing tailings, the ultrafine particle part with a particle size of ≤20μm is used as tailings powder, and this part accounts for more than 30% of the mineral processing tailings; the particle size of the crushed waste rock is ≤16mm.
[0014] Preferably, the raw materials, calculated by weight, include: 820 to 1100 parts of ore dressing tailings; 920 to 960 parts of crushed waste rock; 90 to 140 parts of fly ash; 6 to 10 parts of industrial by-product gypsum; 4 to 10 parts of steel slag powder; 3 to 6 parts of water reducer; 6 to 12 parts of accelerator; 10 to 20 parts of thickener; and 160 to 240 parts of water.
[0015] Preferably, the industrial by-product gypsum and steel slag powder are mixed into a composite activator, and the weight ratio of the two is in the range of 1:1 to 2:1.
[0016] Preferably, the particle size distribution of the beneficiation tailings is, by weight: -20 μm>30%; 20-30 μm 10%-25%; 30-74 μm 20%-31%; 74-150 μm 5%-11%; +150 μm 5%-15%.
[0017] Preferably, the main chemical components of the beneficiation tailings include SiO2, Al2O3, CaO and MgO, etc., and the contents by weight percentage are: SiO2>55%; Al2O3 4%~12%; CaO 3%~7%; MgO<6%.
[0018] Preferably, the industrial by-product gypsum is one or more of desulfurized gypsum, fluorinated gypsum, and phosphogypsum; and its SO3 content is greater than 30%; the fineness is less than 10% on a 45μm sieve. The steel slag is converter slag, the fineness is less than 10% on a 45μm sieve, and the CaO content is greater than 40%. The fly ash is Class I or Class II fly ash.
[0019] Preferably, the crushed waste rock is solid waste generated during ore mining, which is crushed by a crusher into waste rock with a particle size not greater than 16 mm, and the mud content is not greater than 3%.
[0020] Preferably, the water reducer is a polycarboxylic acid water reducer; the quick-setting agent is an inorganic salt quick-setting agent; the thickener is one or more of bentonite, attapulgite, aluminum silicate, etc. Further, the inorganic salt quick-setting agent is one of Red Star Type I, Type 7II, Type 782, and Type 8604.
[0021] Preferably, the rebound rate of the all-solid waste spraying mortar is less than 10%.
[0022] According to another aspect of the present invention, the present invention provides a method for preparing the above-mentioned all-solid waste spraying mortar, comprising: weighing raw materials according to weight proportions; screening and dressing tailings, taking the ultrafine particle part with a particle size ≤20 μm as tailings powder, and taking the part with a particle size >20 μm as mortar fine aggregate, mixing the tailings powder, desulfurized gypsum, steel slag powder, and fly ash to form a cementitious material; taking the mortar fine aggregate and crushed waste rock as aggregates, and mixing them evenly with the cementitious material, water reducer, accelerator and thickener to prepare mortar dry material; adding water to the mortar dry material, stirring evenly with a mixer to prepare spraying mortar.
[0023] Beneficial effects: According to one embodiment of the present invention, the cementitious material is composed of fly ash, industrial by-product gypsum, steel slag powder and tailings powder in ore dressing tailings, and other coarse particles screened from ore dressing tailings and crushed waste rock are used as aggregates, thereby achieving the full solid waste preparation of spray mortar that meets the performance requirements. In the cementitious material system composed of fly ash, industrial by-product gypsum, steel slag powder and tailings powder in ore dressing tailings, tailings powder is used as an active material, fly ash is used as tailings powder as a modifying material to improve and supplement the activity of tailings powder, desulfurized gypsum is used as a sulfate activator, and steel slag powder is used as both an alkaline activator and a modifying material for tailings powder, thereby replacing conventional cementitious materials such as cement. In addition, the present application does not use high-priced raw materials such as blast furnace slag and cement clinker, nor does it use traditional mortar aggregates such as river sand, machine-made sand, and gravel.
[0024] In addition, compared with the prior art, some preferred embodiments of the present application also have the following advantages:
[0025] 1) Utilizing the potential activity of the mineral processing tailings, the fine powder part after screening with a specific particle size is used as raw material, and the cementitious material is prepared by active activation. The cementitious material is used to replace cement to prepare mortar. It only requires simple screening and reasonable activation, and the cost is low.
[0026] 2) It does not use high-priced raw materials such as blast furnace slag and cement clinker. It uses solid waste raw materials as the main active material and activator, which simplifies the production process and reduces costs.
[0027] 3) The relatively coarse particles screened out from the ore dressing tailings and the crushed waste rock are used as aggregates, and the fine particles screened out from the tailings are used as raw materials for cementitious materials, which has a high utilization rate of solid waste and avoids environmental pollution due to storage.
[0028] 4) The ore dressing tailings have certain fine particles and potential activity. After screening during the utilization process, they do not need secondary grinding and can be used directly. Not only does it have a wide source of raw materials and a simple production process, but it also has better mortar performance and lower cost.
[0029] 5) Compared with using steel slag as aggregate, in the present application, the steel slag is used as both an active material and an activator for the activity of tailings micropowder, so that the activity of the steel slag is fully utilized.
[0030] 6) This application achieves the full solid waste preparation of spray mortar that meets performance requirements by optimizing the types and contents of solid waste and rationally mixing and matching them according to particle grading. In addition, the sources of various raw materials are wide, the number of components is reasonable, the preparation process is simple, and the production cost is low, thus realizing resource utilization and large-scale utilization. BRIEF DESCRIPTION OF THE DRAWINGS
[0031] Figure 1 It is a schematic flow chart of a method for preparing all-solid waste spraying mortar in one embodiment of the present invention. DETAILED DESCRIPTION
[0032] The technical solution of the present invention will be clearly and completely described below in conjunction with the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, rather than all of the embodiments. The following description of at least one exemplary embodiment is actually only illustrative and is by no means intended to limit the present invention and its application or use. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0033] The all-solid waste spraying mortar provided in the present application is composed of fly ash, industrial by-product gypsum, steel slag powder and tailings powder in mineral processing tailings to form cementitious materials, and the other parts of the mineral processing tailings and crushed waste rock are used as aggregates, thereby realizing the all-solid waste preparation of spraying mortar that meets the performance requirements; and the raw materials are widely available, the number of components is reasonable, the preparation process is simple, the production cost is low, and resource utilization and large-scale utilization are realized.
[0034] Figure 1 The following schematically shows a process flow for preparing all-solid waste spray mortar provided in a preferred embodiment. Figure 1 As shown, the beneficiation tailings are first screened, and the ultrafine particles with a particle size of ≤20μm are used as tailings powder, which is used as the raw material of the spray mortar cementitious material, and the tailings with a particle size of >20μm are used as mortar fine aggregate; then the tailings powder, fly ash, and a composite activator prepared by steel slag and gypsum are activated to prepare cementitious materials; the coarser particles screened from the beneficiation tailings and the crushed waste rock (≤16mm) are used as mortar aggregates, and water reducers, accelerators, and thickeners are added, and mixed evenly with the cementitious materials, and water is added and stirred evenly to obtain the spray mortar. In the cementitious material system composed of fly ash, industrial by-product gypsum, steel slag powder and tailings powder in the beneficiation tailings, the tailings powder is used as an active material, the fly ash is used as the tailings powder as a modifying material to improve and supplement the activity of the tailings powder, the desulfurized gypsum is used as a sulfate activator, and the steel slag powder is used as both an alkaline activator and a tailings powder as a modifying material, thereby replacing conventional cementitious materials such as cement. In addition, by screening the mineral processing tailings at 20μm, it is ensured that the particles under the screen are ultrafine particles, which are more conducive to the activation of activity when used as active materials.
[0035] The proportion of tailings powder in the beneficiation tailings must be greater than 30%, which can be about 320 to 450 parts by weight. The inventors of the present application have found that when the beneficiation tailings that meet the above-mentioned proportion requirements are used as the raw material of the cementitious material and the cementitious material is activated, the activity and micro-aggregate effect of the tailings powder can be fully exerted, and the strength and fluidity of the sprayed mortar obtained based on the cooperation of other components are better; if the proportion is less than 30%, it will lead to problems such as discontinuous tailings grading and insufficient active materials.
[0036] In this embodiment, the raw materials of the all-solid waste spraying mortar include, by weight, 820 to 1100 parts of ore dressing tailings; 920 to 960 parts of crushed waste rock; 90 to 140 parts of fly ash; 6 to 10 parts of industrial by-product gypsum; 4 to 10 parts of steel slag powder; 3 to 6 parts of water reducer; 6 to 12 parts of accelerator; 10 to 20 parts of thickener; and 160 to 240 parts of water. By using fly ash, industrial by-product gypsum, steel slag powder and tailings fine powder in ore dressing tailings to form a cementitious material, using the other parts of the ore dressing tailings and crushed waste rock as aggregates, adding a binder, an accelerator and a thickener, and optimizing the ratio of each raw material, the all-solid waste preparation of the spraying mortar is achieved.
[0037] In addition, the main chemical components of the beneficiation tailings include SiO2, Al2O3, CaO and MgO, and the contents are as follows: SiO2>55%; Al2O3 4%-12%; CaO 3%-7%; MgO<6%. Since different tailings have different chemical compositions, the content of Si, Al and Ca is designed to meet the requirements of tailings as both fine aggregate and active material, and the content of MgO is designed to meet the requirements of mortar stability.
[0038] In addition, in order to meet the requirements of continuous grading of shotcrete aggregate, the particle size gradation distribution of beneficiation tailings is designed by weight as follows: -20μm>30%; 20~30μm 10%~25%; 30~74μm 20%~31%; 74~150μm 5%~11%; +150μm 5%~15%.
[0039] This embodiment uses industrial by-product gypsum and steel slag powder to form a composite activator to activate the active material. Furthermore, the composite ratio of industrial by-product gypsum and steel slag powder is 1 to 2:1, so that the tailings powder in the ore dressing tailings can be efficiently activated. During configuration, the industrial by-product gypsum and steel slag powder can be sent to the ball mill in proportion to grind to a fineness of 10%, and then the composite activator is prepared after grinding and homogenization. Among them, the industrial by-product gypsum can be one or more of desulfurized gypsum, fluorinated gypsum, phosphogypsum, etc. The SO3 content of industrial by-product gypsum is greater than 30%; the fineness (45μm sieve residue) is less than 10%. The steel slag is converter slag, and after ball mill grinding, the fineness (45μm sieve residue) is less than 10%, and the CaO content is greater than 40%, and steel slag powder is obtained. Fly ash must meet the requirements of Class I or Class II fly ash specified in the national standard "Fly ash used in cement and concrete" GB / T 1596-2017.
[0040] When preparing cementitious materials, the ore dressing tailings with the above-mentioned specific chemical composition are used, and according to their own potential activity, they are screened with the above-mentioned specific screening particle size, and the micro-powder part of the screened ultrafine particles is used as the raw material of the cementitious material, and the activity is activated by a composite activator configured with industrial by-product gypsum and steel slag, and fly ash is added to prepare the cementitious material; then the cementitious material is combined with other mortar aggregate and other components, and the ratio of each raw material and the particle size gradation are optimized, so that the cementitious material can completely replace cement to prepare mortar, and only simple screening is required, and consolidation is achieved by stimulating the potential activity of the tailings micro-powder to obtain a spray mortar with good performance (slump, compressive strength, water bleeding rate, rebound rate and other properties that meet the application requirements), and no secondary grinding is required after screening, the raw materials are from a wide range of sources, and the preparation cost is low.
[0041] In addition, the crushed waste rock is a solid waste generated during the ore mining process. According to the requirements of the spray mortar, the present application uses a crusher to crush the waste rock into a particle size of no more than 16 mm as a coarse aggregate, and the mud content is no more than 3%, and the coarse aggregate is prepared by continuous particle size. Based on the fine particles screened out from the tailings as a cementitious material for active activation, the cementitious material prepared is realized by using the other coarser particles screened out from the ore dressing tailings and the above-mentioned crushed waste rock as the spray mortar aggregate, which realizes the replacement of conventional river sand, machine-made sand, and gravel aggregate. With the continuous improvement of environmental protection requirements, river sand, machine-made sand, and gravel are in short supply in many areas, and the price continues to rise. The present invention does not use traditional mortar aggregates such as river sand, machine-made sand, and gravel, but uses bulk solid wastes from mines such as tailings and crushed waste rock, which not only improves the utilization rate of solid waste, avoids environmental pollution caused by storage, is beneficial to environmental protection, but also reduces production costs.
[0042] In addition, the water reducer is preferably a polycarboxylic acid water reducer to improve the fluidity of the mortar; the quick-setting agent is preferably an inorganic salt quick-setting agent, such as one of Red Star Type I, Type 7II, Type 782, and Type 8604; the thickener is one or more of bentonite, attapulgite, aluminum silicate, etc. Based on the preparation of cementitious materials by using the fine powder part of the sieved ore dressing tailings as raw materials for active activation, and the preparation of spraying mortar using the relatively coarse particles sieved from the ore dressing tailings and crushed waste rocks as aggregates, the performance of the sandblasting mortar can be further improved by using the above-mentioned water reducer, quick-setting agent, and thickener, truly realizing the full solid waste preparation of the sandblasting mortar.
[0043] In this embodiment, fly ash, industrial by-product gypsum, steel slag powder and tailings powder in ore dressing tailings are used as cementitious materials, and other parts of ore dressing tailings and crushed waste rock are used as aggregates. At the same time, the types and contents of solid wastes are reasonably designed, the raw material ratio is optimized, and the effects of fine aggregates, activated tailings powder and composite activator of ore dressing tailings are fully utilized to achieve the full solid waste preparation of spray mortar. The prepared spray mortar meets the performance requirements, has a high 28d compressive strength, and has better construction performance. Among them, based on the good compatibility (binding ability) of activated tailings powder in ore dressing tailings with tailings aggregates, it is combined with various other solid waste powders, especially fly ash, so as to increase the viscosity of the mortar, reduce rebound during spraying, and reduce the rebound rate to below 10%, thereby avoiding the waste of spray mortar.
[0044] The specific implementation methods of this application are described in more detail below in conjunction with specific embodiments:
[0045] Embodiment 1:
[0046] The tailings from an open-pit mine in Liaoning were analyzed for particle size distribution and chemical composition. The specific results are shown in Tables 1 and 2.
[0047] Table 1 Particle size distribution of tailings from an open-pit mine in Liaoning
[0048]
[0049] Table 2 Chemical composition of tailings from an open-pit mine in Liaoning
[0050]
[0051] The spray mortar preparation process in this embodiment is as follows:
[0052] 1) The tailings are sent to a high-frequency screen for screening, and the tailings with a particle size of more than 20 μm are used as fine aggregate, and the tailings powder with a particle size of ≤20 μm is used as a raw material for preparing cementitious materials;
[0053] 2) Fly ash, desulfurized gypsum and steel slag are taken from power plants and smelters of mining enterprises respectively. The fly ash of power plants meets the requirements of Class II fly ash after physical and chemical property analysis and testing; the chemical composition analysis of desulfurized gypsum and steel slag is shown in Table 3, in which the SO3 content of desulfurized gypsum is 41.60% and the CaO content of steel slag is 41.81%.
[0054] Table 3 Chemical composition of steel slag and desulfurized gypsum from an open-pit mine in Liaoning
[0055]
[0056] 3) The dried desulfurized gypsum and steel slag are fed into a ball mill at a weight ratio of 2:1 and ground to a fineness of 10%, and then ground and homogenized to prepare a composite activator; 4) Tailings powder, fly ash and composite activator are prepared into a full-solid waste cementitious material at a weight ratio of 70:24:3; 5) The cementitious material is mixed with tailings aggregate, crushed waste rock, polycarboxylic acid water reducer, accelerator and thickener in weights of 485 parts, 520 parts, 940 parts, 4 parts, 7 parts and 12 parts to prepare mortar dry material; 6) 185 parts of water are added to the above-prepared mortar dry material, and the mixture is stirred to prepare spray mortar.
[0057] The slump and 28d compressive strength of mortar were measured according to relevant standards such as GB / T 50080-2016 "Standard for test methods of properties of ordinary concrete mixtures" and GB / T50086-2015 "Technical specification for rock and soil anchor and shotcrete support engineering". The rebound rate was determined according to the "quantitative percentage method". The specific proportions and results are shown in Table 4.
[0058] Comparative Example 1:
[0059] The mortar was prepared according to the same water-cement ratio and cement-sand ratio as in Example 1, and the mortar properties were measured according to the same method. The specific ratios and performance test results are shown in Table 4.
[0060] Table 4 Mortar mix ratio and performance of Example 1 and Comparative Example 1
[0061]
[0062] Embodiment 2:
[0063] The tailings from a molybdenum mine in Hebei were taken, and the particle size analysis and chemical composition are shown in Table 5 and Table 6 respectively.
[0064] Table 5 Particle size distribution of tailings from a molybdenum mine in Hebei
[0065]
[0066] Table 6 Chemical composition of tailings from a molybdenum mine in Hebei
[0067]
[0068] The mortar preparation process of this embodiment is as follows:
[0069] 1) The molybdenum tailings were sent to a high-frequency sieve for screening, and the particle size of >20μm was used as aggregate, and the tailings powder with a particle size ≤20μm was used as raw material for preparing cementitious materials; 2) Fly ash, desulfurized gypsum and steel slag powder were purchased from power plants, wherein the fly ash was Class I fly ash, the desulfurized gypsum had a fineness of 8.7%, and the measured SO3 content was 35.61%, the steel slag powder had a fineness of 9.4%, and the CaO content was 46.6%; 3) The purchased desulfurized gypsum and steel slag powder were mixed in a weight ratio of 4:3 to form a composite 4) preparing a cementitious material by weight ratio of 160:70:7 with tailings powder, fly ash and composite activator; 5) mixing the cementitious material with tailings aggregate, crushed waste rock, polycarboxylic acid water reducer, 8604 type quick-setting agent and thickener bentonite in 474 parts by weight, 600 parts by weight, 950 parts by weight, 5 parts by weight, 8 parts by weight and 15 parts by weight respectively to prepare a mortar dry material; 6) adding 190 parts by weight of water to the above-prepared mortar dry material and stirring to prepare a mortar.
[0070] The slump and 28d compressive strength of mortar were measured in accordance with relevant standards such as GB / T 50080-2016 "Standard for Test Methods for Performance of Ordinary Concrete Mixtures" and GB / T50086-2015 "Technical Specifications for Geotechnical Anchors and Shotcrete Support Engineering". The rebound rate was determined according to the "quantitative percentage method". The specific mix ratios and measurement results are shown in Table 7.
[0071] Comparative Example 2:
[0072] The mortar was prepared according to the same water-cement ratio and cement-sand ratio as in Example 2, and the mortar properties were measured according to the same method. The specific ratios and performance test results are shown in Table 7.
[0073] Table 7 Mortar mix ratio and performance of Example 2 and Comparative Example 2
[0074]
[0075]
[0076] The description of the present invention is given for the purpose of illustration and description, and is not intended to be exhaustive or to limit the invention to the disclosed form. Many modifications and variations will be apparent to those of ordinary skill in the art. The embodiments are selected and described in order to better illustrate the principles and practical applications of the present invention and to enable those of ordinary skill in the art to understand the present invention and thereby design various embodiments with various modifications suitable for particular uses.
Claims
1. A solid waste spraying mortar, characterized in that: The cementitious material is composed of fly ash, industrial by-product gypsum, steel slag powder and tailings powder in ore dressing tailings, and the other parts of the ore dressing tailings and crushed waste rock are used as aggregates; wherein the ultrafine particles with a particle size of ≤20μm in the ore dressing tailings are used as tailings powder, and this part accounts for more than 30% of the ore dressing tailings; the particle size of the crushed waste rock is ≤16mm; The raw materials, in parts by weight, include: Ore dressing tailings: 820-1100 parts; Crushed waste rock: 920-960 parts; Fly ash: 90-140 parts; Industrial gypsum: 6-10 parts; Steel slag powder: 4-10 parts; Water reducing agent: 3-6 parts; Accelerator: 6-12 parts; Thickener: 10-20 parts; Water: 160-240 parts; The industrial by-product gypsum and steel slag powder are mixed into a composite activator, and the weight ratio of the two is 1 to 2:1; The main chemical components of the beneficiation tailings include SiO2, Al2O3, CaO and MgO, and the contents are as follows by weight percentage: SiO2>55%; Al2O3 4%~12%; CaO 3%~7%; MgO<6%; The particle size distribution of the beneficiation tailings is as follows: -20μm > 30%; 20-30μm 10%-25%; 30-74μm 20%-31%; 74-150μm 5%-11%; +150μm 5%-15%; The industrial by-product gypsum is one or more of desulfurized gypsum, fluorinated gypsum, and phosphogypsum, and its SO3 content is greater than 30%, and its fineness is 45μm mesh residue less than 10%; The steel slag powder is converter slag powder, with a fineness of 45 μm sieve residue <10%, and a CaO content >40%; The fly ash is Class I or Class II fly ash.
2. The all-solid waste spraying mortar according to claim 1, characterized in that: The crushed waste rock is solid waste generated during ore mining and is crushed by a crusher, and its mud content is not more than 3%.
3. The all-solid waste spraying mortar according to claim 1, characterized in that: The water reducer is a polycarboxylic acid water reducer; The quick-setting agent is an inorganic salt quick-setting agent, and the inorganic salt quick-setting agent includes one of Red Star Type I, Type 7II, Type 782, and Type 8604; The thickener is one or more of bentonite, attapulgite and aluminum silicate.
4. A method for preparing all-solid waste spraying mortar according to any one of claims 1 to 3, characterized in that: include: Weigh the raw materials according to weight parts; Screening the ore dressing tailings, taking the ultrafine particles with a particle size of ≤20 μm as tailings powder, taking the particles with a particle size of >20 μm as mortar fine aggregate, and mixing the tailings powder, desulfurized gypsum, steel slag powder and fly ash to prepare a cementitious material; Using mortar fine aggregate and crushed waste stone as aggregate, and mixing them with the cementitious material, water reducing agent, quick-setting agent and thickener to prepare mortar dry material; Water is added to the mortar dry material, and the mixture is stirred evenly with a mixer to prepare spray mortar.
Citation Information
Cited By
Jet repairing mortar for repairing acid-corrosion-resistant structures and preparation method of jet repairing mortar
CN122036291A