A kind of MFI nano zeolite without structural defects and preparation method thereof

Through microwave heating and dialysis purification combined with fluorine ion assisted method, the synthesis of MFI nanozeolites without structural defects in a strong acid environment has solved the problem of difficulty in synthesizing small-particle nanozeolites under a strong acid environment in the prior art, and improved the problem of Catalytic activity and mass transfer efficiency and reduce production costs.

CN116395712BActive Publication Date: 2024-11-19FUDAN UNIVERSITY
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202310581800.6
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2023-05-23
Publication Date
2024-11-19
Estimated Expiration
2043-05-23

AI Technical Summary

Technical Problem

The prior art is difficult to synthesize small particle size, structurally defectless MFI nanozeolites under strong acidic environments, resulting in low catalytic activity and mass transfer efficiency. The ZSM-5 zeolites with structural defects in conventional methods in high alkaline environments are limited. Its application.

Method used

Using microwave heating-assisted synthesis method, microwave heat treatment and dialysis purification are carried out by mixing the aqueous solution of silicon source, aluminum source and template agent, combined with fluorine ion assisted synthesis of MFI nanozeolites in a strong acidic environment, adjust the pH value to 2 for hydrothermal treatment. Structural defect-free ZSM-5 and Silicalite-1 nanozeolites were obtained.

Benefits of technology

The synthesis of MFI nanozeolites without structural defects, small particle size and uniform morphology under a strong acid environment is achieved, which improves catalytic activity and mass transfer efficiency, reduces production costs, and is suitable for industrial production.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN116395712B_ABST
    Figure CN116395712B_ABST
Patent Text Reader

Abstract

The present invention provides a kind of MFI nano zeolite without structural defects and its preparation method, belonging to the technical field of molecular sieves. The present invention adopts tetrapropylammonium hydroxide as a template agent, adopts a method of microwave heating assisted synthesis, can simply, quickly and efficiently obtain ZSM-5 zeolite crystals with uniform structure, obtain a high-purity ZSM-5 zeolite crystallite aqueous solution through dialysis purification, ZSM-5 zeolite crystallite has extremely high growth activity, can be oriented and aggregated and crystallized under strong acidic conditions by hydrothermal treatment with the assistance of fluoride ions, obtain MFI nano zeolite crystals without structural defects with small particle size, good uniformity, large specific surface, stable morphology, high crystal face selectivity, and the b-axis direction of the ZSM-5 molecular sieve crystal has a short and regular straight channel, which can provide a shorter diffusion path and more active sites, effectively improving the mass transfer efficiency and catalytic activity of the molecular sieve.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of molecular sieves, and in particular to an MFI nano zeolite without structural defects and a preparation method thereof. Background Art

[0002] At present, the preparation methods of ZSM-5 zeolite mainly include sol-gel method, organic solvent method, hydrothermal method, etc. Among them, the hydrothermal method has the advantages of convenience, high cost-effectiveness, and easy to scale up, and is the most widely used. The preparation of ZSM-5 zeolite is usually synthesized in a relatively high alkaline environment (pH>9). However, the nano zeolite obtained in the alkaline medium contains a large number of strong hydrophilic groups - terminal silanol groups. The presence of terminal silanol groups will produce some structural defects in the zeolite, which will limit the application of zeolite catalysts and reduce their lifespan.

[0003] Chinese patent CN114380301A discloses a method for preparing a nano-flaky MFI molecular sieve, comprising the following steps: mixing a silicon source, tetrapropylammonium hydroxide and water, performing microwave heat treatment and then dialysis purification to obtain an MFI crystallite solution; adjusting the pH value of the MFI crystallite solution to 5.7-12.7, performing hydrothermal treatment, and obtaining a nano-flaky MFI molecular sieve. However, the above preparation method cannot achieve the synthesis of MFI molecular sieves with small particle size and no structural defects (silanol defects) in a strongly acidic environment. In a strongly acidic environment, a mineralizer (such as fluoride ions) is usually required to synthesize ZSM-5 zeolite. However, due to the low nucleation rate of ZSM-5 zeolite in a strongly acidic environment, a large amount of silicon source can only grow on a limited crystal nucleus, resulting in the synthesized ZSM-5 zeolite size generally being tens of microns or even hundreds of microns, and the large size of the zeolite leads to its small specific surface area and low mass transfer efficiency, which limits its practical applications such as catalysis. Summary of the invention

[0004] In view of this, the purpose of the present invention is to provide a MFI nano zeolite without structural defects and a preparation method thereof. The MFI nano zeolite prepared by the preparation method provided by the present invention in a strong acidic environment has no structural defects, small particle size, good morphology uniformity, large specific surface area, high mass transfer efficiency and catalytic activity.

[0005] In order to achieve the above-mentioned object of the invention, the present invention provides the following technical solutions:

[0006] The present invention provides a method for preparing MFI nano zeolite without structural defects, comprising the following steps:

[0007] (1) first mixing an aqueous solution of a silicon source, an aluminum source and a template agent, and sequentially subjecting the obtained first mixed solution to a first microwave heat treatment and a first dialysis purification to obtain a ZSM-5 zeolite crystallite solution; the template agent includes tetrapropylammonium hydroxide;

[0008] (2) secondly mixing the aqueous solution of the silicon source and the template agent, and sequentially subjecting the obtained second mixed solution to a second microwave heat treatment and a second dialysis purification to obtain a Silicalite-1 zeolite crystallite solution; the template agent comprises tetrapropylammonium hydroxide;

[0009] (3) mixing the ZSM-5 zeolite crystallite solution and / or the Silicalite-1 zeolite crystallite solution with fluoride ions, adjusting the pH value of the resulting crystallite-fluoride ion mixed solution to 2, and performing hydrothermal treatment to obtain a MFI nano zeolite without structural defects;

[0010] There is no chronological order between step (1) and step (2).

[0011] Preferably, the molar ratio of silicon dioxide, aluminum oxide, template and water in the first mixed solution is 1: 0.0001-0.025: 0.1-0.45: 3-10.

[0012] Preferably, the molar ratio of silicon dioxide, template and water in the second mixed solution is 1:0.1-0.45:3-10.

[0013] Preferably, after the first mixing and the second mixing, the obtained mixture is aged, the aging temperature is 15 to 40° C., and the aging time is 4 to 48 hours.

[0014] Preferably, the first microwave heat treatment and the second microwave heat treatment both comprise low-temperature microwave heat treatment and high-temperature microwave heat treatment in sequence; the temperature of the low-temperature microwave heat treatment is independently 70 to 100°C, and the time is independently 60 to 150 min; the temperature of the high-temperature microwave heat treatment is independently 120 to 180°C, and the time is independently 10 to 90 min.

[0015] Preferably, the molecular weight cut-offs of the first dialysis purification and the second dialysis purification are independently 1.5 to 6 kDa;

[0016] The first dialysis purification and the second dialysis purification both comprise dialysis with a tetrapropylammonium hydroxide aqueous solution and dialysis with water in sequence, and the concentration of the tetrapropylammonium hydroxide aqueous solution is independently 2 to 16 mmol / L.

[0017] Preferably, the molar amount of the fluoride ions is 1 to 18% of the molar amount of silicon dioxide in the crystallite-fluoride ion mixed solution.

[0018] Preferably, the pH value is adjusted using an acid, which includes one or more of hydrochloric acid, sulfuric acid and nitric acid.

[0019] Preferably, the temperature of the hydrothermal treatment is 60 to 180° C., the time is 3 to 30 days, and the hydrothermal treatment is a static hydrothermal treatment.

[0020] The present invention also provides a structural defect-free MFI nano zeolite prepared by the preparation method described in the above technical scheme, wherein the structural defect-free MFI nano zeolite includes a structural defect-free ZSM-5 nano zeolite and / or a structural defect-free Silicalite-1 nano zeolite; the structural defect-free Silicalite-1 nano zeolite has a length of 200 to 400 nm, a width of 200 to 400 nm, and a thickness of 30 to 60 nm; the structural defect-free ZSM-5 nano zeolite has a length of 500 to 800 nm, a width of 200 to 400 nm, and a thickness of 30 to 60 nm.

[0021] The present invention uses tetrapropylammonium hydroxide as a template agent and a microwave heating-assisted synthesis method, which has the advantages of simple operation, good repeatability, and fast preparation of MFI crystals (ZSM-5 zeolite crystals and / or Silicalite-1 zeolite crystals). It can efficiently synthesize MFI zeolite crystals with uniform structure, high growth activity, and high porosity. By using a dialysis treatment method, it has the advantages of accurate particle screening and retaining more effective components. After dialysis purification, the excess raw materials (such as free silicon) are removed to obtain a high-purity MFI crystallite aqueous solution, which provides high-quality raw materials for further synthesis of MFI nano-zeolites without structural defects. By using fluoride ion-assisted crystallization, Silicalite-1 zeolite crystals and ZSM-5 zeolite crystals can both aggregate and crystallize in a strongly acidic environment of pH=2.0. Under acidic conditions, the growth rate of zeolite is very slow, and there is enough time to integrate skeleton defects; in OH - The MFI zeolite is synthesized in the system, and the silanol group acts as a charge compensator to balance the charge of the MFI zeolite framework. - MFI zeolite was synthesized in the system of - It plays the role of charge compensator, solves the problem of structural defects, and each crystallite is equivalent to a crystal nucleus, so that the size of MFI zeolite can be reduced, and then the sheet-like MFI nano zeolite crystals with small particle size, good uniformity, large specific surface, stable morphology, and high crystal face selectivity without structural defects in the short b-axis direction are obtained. The sheet-like MFI nano zeolite crystals prepared by the present invention are small in size, rich in pores, and large in specific surface area. The short b-axis allows the material to have a shorter diffusion path, which greatly improves the mass transfer efficiency of the material; and the characteristic of no structural defects makes the zeolite have a longer life and higher catalytic efficiency, and has a good application prospect as a catalyst. Moreover, the preparation method provided by the present invention has a simple process, cheap and easy-to-obtain raw materials, low energy consumption, low production cost, and is suitable for industrial production.

[0022] Furthermore, the present invention is beneficial to improve the yield of MFI zeolite crystals by controlling the molar ratio of silicon dioxide, aluminum isopropoxide, template and water in the silicon source, or controlling the molar ratio of silicon dioxide, template and water.

[0023] Furthermore, the present invention first promotes the formation of a large number of ZSM-5 zeolite crystals in a mixed solution of a silicon source, an aqueous template solution and an aluminum source through low-temperature microwave heat treatment, and then makes the structure of the ZSM-5 zeolite crystals develop towards order through high-temperature microwave heat treatment. By controlling the temperature and time of the high-temperature microwave heat treatment, the structure of the ZSM-5 zeolite crystals is highly ordered and has extremely high growth activity, which helps to subsequently synthesize high-quality MFI nano-zeolite without structural defects in a strongly acidic environment.

[0024] Furthermore, the present invention is beneficial to improving the yield of ZSM-5 zeolite crystals by controlling the concentration of the tetrapropylammonium hydroxide aqueous solution for dialysis.

[0025] The present invention provides a structurally defect-free MFI nano zeolite obtained by the preparation method described in the above technical solution, wherein the structurally defect-free MFI nano zeolite includes a structurally defect-free ZSM-5 nano zeolite and / or a structurally defect-free Silicalite-1 nano zeolite; the structurally defect-free Silicalite-1 nano zeolite has a length of 200 to 400 nm, a width of 200 to 400 nm, and a thickness of 30 to 60 nm; the structurally defect-free ZSM-5 nano zeolite has a length of 500 to 800 nm, a width of 200 to 400 nm, and a thickness of 30 to 60 nm. The structurally defect-free MFI nano zeolite provided by the present invention has a small particle size, good morphology uniformity, a large specific surface area, and a high degree of crystal face selectivity. It has short and regular straight channels in the b-axis direction, can provide a shorter diffusion path and more active sites, can effectively improve the mass transfer efficiency and catalytic activity of the molecular sieve, and has a good application prospect as a catalyst. BRIEF DESCRIPTION OF THE DRAWINGS

[0026] Figure 1 TEM image of the Silicalite-1 nanozeolite without structural defects prepared in Example 1;

[0027] Figure 2 The X-ray diffraction spectrum of the Silicalite-1 nano zeolite without structural defects prepared in Example 1;

[0028] Figure 3 The infrared spectra of the hydroxyl region of the Silicalite-1 nano zeolite (S-1-F) without structural defects prepared in Example 1 and the Silicalite-1 nano zeolite (S-1) prepared in a conventional manner in Comparative Example 1;

[0029] Figure 4 Solid silicon nuclear magnetic spectra of the Silicalite-1 nano zeolite (S-1-F) without structural defects prepared in Example 1 and the Silicalite-1 nano zeolite (S-1) prepared in a conventional manner in Comparative Example 1;

[0030] Figure 5 TEM image of the ZSM-5 nano zeolite without structural defects prepared in Example 2;

[0031] Figure 6 The X-ray diffraction spectrum of the ZSM-5 nano zeolite without structural defects prepared in Example 2;

[0032] Figure 7 The infrared spectra of the hydroxyl region of the ZSM-5 nano zeolite (ZSM-5-F) without structural defects prepared in Example 2 and the ZSM-5 nano zeolite (ZSM-5) prepared in a conventional manner in Comparative Example 2;

[0033] Figure 8 Solid silicon nuclear magnetic spectra of the ZSM-5 nano zeolite (ZSM-5-F) without structural defects prepared in Example 2 and the ZSM-5 nano zeolite (ZSM-5) prepared in a conventional manner in Comparative Example 2;

[0034] Fig. 9 TEM image of Silicalite-1 nanozeolite prepared in Comparative Example 3;

[0035] Fig.10 TEM image of ZSM-5 nano zeolite prepared in Comparative Example 4;

[0036] Fig.11 TEM image of Silicalite-1 nano zeolite prepared in Comparative Example 5;

[0037] Fig.12 TEM image of ZSM-5 nano zeolite prepared in Comparative Example 6;

[0038] Fig.13 TEM image of Silicalite-1 nanozeolite prepared in Example 3;

[0039] Fig.14 TEM image of the ZSM-5 nano zeolite prepared in Example 4;

[0040] Fig.15 TEM image of ZSM-5 nano zeolite prepared in Comparative Example 7;

[0041] Fig.16 This is the TEM image of the ZSM-5 nano zeolite prepared in Comparative Example 8. DETAILED DESCRIPTION

[0042] The present invention provides a method for preparing MFI nano zeolite without structural defects, comprising the following steps:

[0043] (1) first mixing an aqueous solution of a silicon source, an aluminum source and a template agent, and sequentially subjecting the obtained first mixed solution to a first microwave heat treatment and a first dialysis purification to obtain a ZSM-5 zeolite crystallite solution; the template agent includes tetrapropylammonium hydroxide;

[0044] (2) secondly mixing the aqueous solution of the silicon source and the template agent, and sequentially subjecting the obtained second mixed solution to a second microwave heat treatment and a second dialysis purification to obtain a Silicalite-1 zeolite crystallite solution; the template agent comprises tetrapropylammonium hydroxide;

[0045] (3) mixing the ZSM-5 zeolite crystallite solution and / or the Silicalite-1 zeolite crystallite solution with ammonium fluoride, adjusting the pH value of the resulting crystallite-fluoride ion mixed solution to 2, and performing hydrothermal treatment to obtain an MFI nano zeolite without structural defects;

[0046] There is no chronological order between step (1) and step (2).

[0047] Unless otherwise specified, the raw materials used in the present invention are all commercially available products.

[0048] The invention mixes the aqueous solution of silicon source, aluminum source and template agent, and sequentially performs the first microwave heat treatment and the first dialysis purification on the obtained first mixed solution to obtain ZSM-5 zeolite crystallite solution.

[0049] In the present invention, the silicon source preferably includes one or more of white carbon black, silica sol, silica gel powder, tetraethyl orthosilicate and sodium silicate, and more preferably tetraethyl orthosilicate (TEOS). In the present invention, the aluminum source preferably includes one or more of aluminum isopropoxide, aluminum nitrate and aluminum chloride, and more preferably aluminum isopropoxide. In the present invention, the template includes tetrapropylammonium hydroxide (TPAOH). The present invention uses tetrapropylammonium hydroxide as a template to obtain ZSM-5 zeolite crystals with uniform structure. When tetraethyl orthosilicate and TPAOH are used as raw materials, the raw material source is wide and the cost is lower.

[0050] In the present invention, the molar ratio of silicon dioxide, aluminum oxide, template and water in the first mixed solution is preferably 1: 0.0001-0.025: 0.1-0.45: 3-10, more preferably 1: 0.005-0.01: 0.2-0.3: 5-8, and further preferably 1: 0.0068: 0.21: 6.958. The present invention controls the usage ratio of silicon source, aluminum source, template and water within the above range, which is conducive to obtaining MFI crystals with good quality, high growth activity and high porosity.

[0051] The present invention has no special limitation on the first mixing, and the raw materials can be mixed uniformly, such as stirring and mixing, and the stirring and mixing speed is preferably 100-400rpm, more preferably 200-300rpm; the temperature of the first mixing is preferably room temperature. In the present invention, the order of the first mixing is preferably to add the aqueous solution of the aluminum source, the silicon source and the template agent in sequence, and the concentration of the template agent in the aqueous solution of the template agent is preferably 25wt%.

[0052] After the first mixing is completed, the present invention preferably further comprises aging the obtained mixture, the aging temperature is preferably 15 to 40°C, more preferably room temperature; the aging time is preferably 4 to 48 hours, more preferably 20 to 24 hours; the aging is preferably carried out under stirring conditions, and the stirring speed is preferably 100 to 400 rpm, more preferably 200 to 300 rpm. The present invention performs aging under the above conditions, so that the silicon source and the aluminum source can be fully hydrolyzed in the first mixed solution, so as to facilitate the subsequent nucleation and growth of the ZSM-5 zeolite.

[0053] In the present invention, the first microwave heat treatment preferably includes low-temperature microwave heat treatment and high-temperature microwave heat treatment in sequence; the first microwave heat treatment is preferably carried out in a microwave reactor, and the microwave reactor is preferably an AntonPaar Monowave 400 microwave reactor. In the present invention, the temperature of the low-temperature microwave heat treatment is preferably 70 to 100°C, more preferably 80 to 90°C; the time of the low-temperature microwave heat treatment is preferably 60 to 150 minutes, more preferably 80 to 100 minutes. In the present invention, the temperature of the high-temperature microwave heat treatment is preferably 120 to 180°C, more preferably 140 to 160°C; the time of the high-temperature microwave heat treatment is preferably 10 to 90 minutes, more preferably 30 to 50 minutes. The present invention adopts a microwave heating-assisted synthesis method, which has the advantages of simple operation and fast preparation speed of ZSM-5 zeolite crystals, and can efficiently synthesize ZSM-5 zeolite crystals with uniform structure. Specifically, the present invention first promotes the silicon source, the template agent and the aluminum source to form a large amount of ZSM-5 zeolite crystals in a first mixed solution through low-temperature microwave heat treatment, and then uses high-temperature microwave heat treatment to make the structure of the ZSM-5 zeolite crystals develop towards order. By controlling the temperature and time of the high-temperature microwave heat treatment, the structure of the ZSM-5 zeolite crystals is highly ordered and has extremely high growth activity, which helps to subsequently synthesize high-quality, structurally defect-free, small-sized and uniform ZSM-5 nano-zeolites under strong acidic conditions.

[0054] In the present invention, the dialysis membrane used for the first dialysis purification is preferably a cellulose semipermeable membrane, and the molecular weight cutoff of the first dialysis purification is preferably 1.5 to 6 kDa, more preferably 3.5 to 4 kDa. The present invention uses the above dialysis membrane to remove particles with a size of less than 2.5 nm. In the present invention, the temperature of the first dialysis purification is preferably room temperature; the first dialysis purification is preferably carried out under low-speed stirring conditions, and the speed of the low-speed stirring is preferably 10 to 100 rpm, more preferably 30 to 40 rpm. In the present invention, the first dialysis purification preferably includes sequentially performing dialysis with tetrapropylammonium hydroxide aqueous solution and dialysis with water. In the present invention, the concentration of the tetrapropylammonium hydroxide aqueous solution is preferably 2-16 mmol / L, more preferably 5-12 mmol / L, and further preferably 6-8 mmol / L; in the present invention, too high a concentration of the TPAOH aqueous solution will dissolve the ZSM-5 zeolite crystallites, thereby affecting the yield of the ZSM-5 zeolite crystallites, and will also affect the subsequent growth quality of the MFI nano zeolite without structural defects. The present invention can remove free silicon and excess TPAOH and improve the yield of ZSM-5 zeolite crystallites by controlling the concentration of the TPAOH aqueous solution; the dialysis time of the tetrapropylammonium hydroxide aqueous solution is preferably 8-72 hours, more preferably 15-24 hours. In the present invention, the water used for the water dialysis is preferably pure water, more preferably Watsons distilled water; the water is preferably replaced during the water dialysis process, and the interval time for replacing the water is preferably 3-24 hours, more preferably 8-10 hours; the present invention has no special limitation on the number of water dialysis, and the water can be dialyzed until the pH value of the dialyzate external fluid is 7-8. In a specific embodiment of the present invention, the interval time of water replacement is 8h, and the water dialysis time is 24h. The present invention adopts the first dialysis purification method, which can achieve the advantages of accurate screening of particles and retaining more effective components, and can obtain a high-purity ZSM-5 zeolite crystallite aqueous solution, and the obtained ZSM-5 zeolite crystallite has high purity, uniform structure, high growth activity, and high porosity, which provides raw materials for further synthesizing high-quality, structurally defect-free, small-particle-size and uniform ZSM-5 zeolite in a strongly acidic environment.

[0055] The present invention secondly mixes the aqueous solutions of the silicon source and the template, and sequentially performs a second microwave heat treatment and a second dialysis purification on the obtained second mixed solution to obtain a Silicalite-1 zeolite crystallite solution; the template includes tetrapropylammonium hydroxide. In the present invention, the molar ratio of silicon dioxide, template and water in the second mixed solution is preferably 1:0.1-0.45:3-10, more preferably 1:0.2-0.3:5-8, and further preferably 1:0.21:6.958. In the present invention, the other preparation conditions of the Silicalite-1 zeolite crystallite solution are the same as those of the ZSM-5 zeolite crystallite solution, which will not be described one by one here.

[0056] After obtaining the ZSM-5 zeolite crystallite solution and the Silicalite-1 zeolite crystallite solution, the present invention mixes the ZSM-5 zeolite crystallite solution and / or the Silicalite-1 zeolite crystallite solution with fluoride ions, adjusts the pH value of the obtained crystallite-fluoride ion mixed solution to 2, and performs hydrothermal treatment to obtain MFI nano zeolite without structural defects.

[0057] In the present invention, the fluoride ions are preferably provided by ammonium fluoride and / or hydrofluoric acid, more preferably ammonium fluoride; the molar amount of the fluoride ions is preferably 1-18% of the molar amount of silicon dioxide in the crystallite-fluoride ion mixed solution, more preferably 5-15%, and further preferably 10%. In the present invention, the fluoride ion solution is preferably used in the form of a fluoride ion aqueous solution, and the concentration of the fluoride ion aqueous solution is preferably 0.5-10 mol / L, more preferably 1-2 mol / L.

[0058] In the present invention, the pH value is adjusted by acid; the acid preferably includes one or more of hydrochloric acid, sulfuric acid and nitric acid, more preferably hydrochloric acid, and the concentration of the acid is preferably 0.1-3 mol / L, more preferably 1-2 mol / L; the present invention has no special limitation on the amount of the acid, as long as the pH value can be adjusted to 2.

[0059] In the present invention, the temperature of the hydrothermal treatment is preferably 60 to 180°C, more preferably 60 to 120°C, and further preferably 80 to 100°C; the time of the hydrothermal treatment is preferably 3 to 30 days, more preferably 5 to 25 days, and more preferably 7 to 21 days; the hydrothermal treatment is preferably static hydrothermal treatment. In the present invention, the hydrothermal treatment is preferably: placing the pH-adjusted crystallized solution in a thick-walled reaction tube, and then sealing the thick-walled reaction tube and placing it in a static constant temperature oven for static hydrothermal treatment.

[0060] After the hydrothermal treatment, the present invention preferably further comprises cooling the system obtained after the hydrothermal treatment to room temperature and then performing solid-liquid separation, washing the obtained solid material with water and then drying it to obtain MFI nano zeolite without structural defects. The present invention has no special limitation on the cooling method, and a cooling method well known in the art can be used, such as natural cooling. The present invention has no special limitation on the solid-liquid separation method, and a solid-liquid separation method well known in the art can be used, such as filtration, suction filtration or centrifugal separation; the rotation speed of the centrifugal separation is preferably 8000-15000rpm, more preferably 10000-12000rpm, and the time of the centrifugal separation is preferably 3-10min, more preferably 5-8min. In the present invention, the water washing is preferably centrifugal water washing, and the temperature of the centrifugal water washing is preferably room temperature; the speed of the centrifugal water washing is preferably 8000-15000rpm, more preferably 10000-12000rpm; the number of water washings is preferably 1-6 times, more preferably 2-3 times; the time of a single water washing is preferably 1-60min, more preferably 10-30min; during the centrifugal water washing process, after adding water to the solid material, it is preferably first ultrasonically treated and then centrifuged, and the ultrasonic treatment is preferably carried out in an ultrasonic cleaning machine, and the purpose of the ultrasonic treatment is to redisperse the solid material to ensure that the water washing is clean. In the present invention, the drying temperature is preferably 25-140°C, more preferably 50-80°C; the drying time is preferably 1-48h, more preferably 5-12h.

[0061] The present invention provides a MFI nano zeolite without structural defects prepared by the preparation method described in the above technical solution, wherein the MFI nano zeolite without structural defects includes a ZSM-5 nano zeolite without structural defects and / or a Silicalite-1 nano zeolite without structural defects. In the present invention, the length of the Silicalite-1 nano zeolite without structural defects is 200 to 400 nm, preferably 200 to 250 nm; the width of the Silicalite-1 nano zeolite without structural defects is 200 to 400 nm, preferably 200 to 250 nm; the thickness of the Silicalite-1 nano zeolite without structural defects is 30 to 60 nm, preferably 30 to 50 nm. In the present invention, the length of the ZSM-5 nano zeolite without structural defects is 500 to 800 nm, preferably 500 to 700 nm; the width of the ZSM-5 nano zeolite without structural defects is 200 to 400 nm, preferably 200 to 250 nm; the thickness of the ZSM-5 nano zeolite without structural defects is 30 to 60 nm, preferably 30 to 50 nm.

[0062] The MFI nano zeolite without structural defects prepared by the present invention has the characteristics of no structural defects, small particle size, large specific surface area, uniform structure, high porosity, multiple effective components, high growth activity and high mass transfer efficiency, and has good application prospects as a catalyst.

[0063] The technical solutions in the present invention will be described clearly and completely below in conjunction with the embodiments of the present invention. Obviously, the described embodiments are only a part of the embodiments of the present invention, not all of them. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0064] Example 1

[0065] TEOS and TPAOH aqueous solutions (mass concentration of 25wt%) were mixed, and the obtained second mixed solution was mixed and aged for 24h at room temperature and 300rpm magnetic stirring conditions, and then transferred to Anton Paar Monowave 400 microwave instrument. First, low-temperature microwave heat treatment was carried out at 90℃ for 90min, and then high-temperature microwave heat treatment was carried out at 140℃ for 50min, and then transferred to a dialysis membrane with a molecular weight cutoff of 3.5kDa, and then immersed in 1L TPAOH aqueous solution with a concentration of 6mmol / L, dialyzed for 24h at room temperature and 40rpm magnetic stirring conditions, and then placed in Watsons distilled water for dialysis treatment, and the distilled water was replaced every 8h until the pH of the dialyzed external solution was between 7 and 8, and a Silicalite-1 crystallite solution was obtained. Among them, the molar ratio of silica: template: water in the second mixed solution is 1:0.21:6.958.

[0066] The Silicalite-1 crystallite solution was mixed with a 1 mol / L ammonium fluoride aqueous solution, and the pH was adjusted to 2.0 using a 1 mol / L hydrochloric acid aqueous solution, and then placed in a preheated 80°C constant temperature oven for hydrothermal treatment for 7 days, the thick-walled reaction tube was taken out and cooled to room temperature, transferred to a centrifuge tube, and the centrifuge tube was placed in a centrifuge. Centrifugation was performed at room temperature and 10,000 rpm, and after the centrifugation, the supernatant was poured out, deionized water was added, and the solution was ultrasonically dispersed evenly in an ultrasonic cleaning machine before the next centrifugation. The ultrasonic dispersion-centrifugal washing times were 3 times, and the single centrifugation time was 5 minutes, and then dried in an oven at 65°C for 12 hours to obtain a powdered Silicalite-1 nanozeolite without structural defects; wherein the molar ratio of ammonium fluoride: silica in the Silicalite-1 crystallite-fluoride ion mixed solution × 100% = 10%.

[0067] Figure 1This is a TEM image of the Silicalite-1 nanozeolite without structural defects prepared in Example 1. Figure 1 It can be seen that the defect-free Silicalite-1 nano zeolite prepared in Example 1 has a length×width×thickness=200nm×200nm×40nm, and is a defect-free Silicalite-1 sheet nano zeolite in the short b-axis direction with high crystal face selectivity and good size uniformity.

[0068] Figure 2 This is the X-ray diffraction spectrum of the Silicalite-1 nano zeolite without structural defects prepared in Example 1. Figure 2 It can be seen that the nano zeolite without structural defects prepared in Example 1 has a highly crystalline MFI topological structure.

[0069] Comparative Example 1

[0070] TEOS and TPAOH aqueous solutions (mass concentration of 25wt%) were mixed, and the obtained second mixed solution was mixed and aged for 24h at room temperature and 300rpm magnetic stirring conditions, and then transferred to Anton Paar Monowave 400 microwave instrument. First, low-temperature microwave heat treatment was carried out at 90℃ for 90min, and then high-temperature microwave heat treatment was carried out at 140℃ for 50min, and then transferred to a dialysis membrane with a molecular weight cutoff of 3.5kDa, and then immersed in 1L TPAOH aqueous solution with a concentration of 6mmol / L, dialyzed for 24h at room temperature and 40rpm magnetic stirring conditions, and then placed in Watsons distilled water for dialysis treatment, and the distilled water was replaced every 8h until the pH of the dialyzed external solution was between 7 and 8, and a Silicalite-1 crystallite solution was obtained. Wherein, the molar ratio of silica: template: water in the second mixed solution is 1:0.21:6.958.

[0071] The obtained Silicalite-1 crystallite solution was placed in an oven at 80°C for 3 days. The solution was transferred to a centrifuge tube and placed in a centrifuge. The solution was centrifuged at room temperature and 10,000 rpm. After centrifugation, the supernatant was poured out, deionized water was added, and the solution was ultrasonically dispersed in an ultrasonic cleaning machine for uniformity before the next centrifugation. The number of ultrasonic dispersion-centrifugal washing was 3 times, and the time for a single centrifugation was 5 minutes. The solution was then dried in an oven at 65°C for 12 hours to obtain powdered Silicalite-1 nanozeolite.

[0072] Figure 3 The infrared spectra of the hydroxyl region of the Silicalite-1 nano zeolite (S-1-F) without structural defects prepared in Example 1 and the Silicalite-1 nano zeolite (S-1) prepared in a conventional manner in Comparative Example 1 are shown in FIG. Figure 3It can be seen that the nano zeolite prepared in Example 1 has a low content of silanol and very few structural defects.

[0073] Figure 4 Solid silicon nuclear magnetic resonance spectra of the Silicalite-1 nano zeolite (S-1-F) without structural defects prepared in Example 1 and the Silicalite-1 nano zeolite (S-1) prepared in a conventional manner in Comparative Example 1. Figure 4 It can be seen that the Silicalite-1 nano zeolite prepared in Example 1 has very few structural defects.

[0074] Example 2

[0075] Aluminum isopropoxide, TEOS and TPAOH aqueous solution (mass concentration of 25wt%) were mixed, and the obtained first mixed solution was mixed and aged for 24h at room temperature and 300rpm magnetic stirring conditions, and then transferred to Anton Paar Monowave 400 microwave instrument, firstly subjected to low temperature microwave heat treatment at 90℃ for 90min, and then subjected to high temperature microwave heat treatment at 150℃ for 30min, and then transferred to a dialysis membrane with a molecular weight cutoff of 3.5kDa, and then immersed in 1L TPAOH aqueous solution with a concentration of 6mmol / L, dialyzed for 24h at room temperature and 40rpm magnetic stirring conditions, and then placed in Watsons distilled water for dialysis treatment, and the distilled water was replaced every 8h until the pH of the dialyzed external solution was between 7.0 and 8.0, and a ZSM-5 crystallite solution was obtained. Wherein, the molar ratio of silica:alumina:template:water in the first mixed solution is 1:0.0068:0.21:6.958.

[0076] The ZSM-5 crystallite solution was mixed with a 1mol / L ammonium fluoride aqueous solution, and the pH was adjusted to 2.0 using a 1mol / L hydrochloric acid aqueous solution, and the solution was placed in a preheated 80°C constant temperature oven for hydrothermal treatment for 21 days, and the thick-walled reaction tube was taken out, and the milky white solution obtained after cooling was transferred to a centrifuge tube, and the centrifuge tube was placed in a centrifuge, and centrifuged at room temperature and 10000rpm. After the centrifugation, the supernatant was poured out. Deionized water was added, and the solution was evenly dispersed ultrasonically in an ultrasonic cleaning machine and then centrifuged again. The number of ultrasonic dispersion-centrifugal washing was 3 times, and the time of a single centrifugation was 5 minutes, and then dried in a 65°C oven for 12 hours to obtain a powdery ZSM-5 sheet-like nano zeolite without structural defects (silicon-aluminum ratio of 73); wherein the molar ratio of ammonium fluoride: silicon dioxide in the ZSM-5 crystallite-fluoride ion mixed solution × 100% = 10%.

[0077] Figure 5 TEM image of the ZSM-5 nano zeolite without structural defects prepared in Example 2. Figure 5It can be seen that the length×width×thickness of the ZSM-5 nano zeolite crystals without structural defects obtained in Example 2 is 670nm×240nm×50nm, which is a ZSM-5 nano zeolite crystal without structural defects in the short b-axis direction with high crystal face selectivity and good size uniformity.

[0078] Figure 6 This is the X-ray diffraction spectrum of the ZSM-5 nano zeolite without structural defects prepared in Example 2. Figure 6 It can be seen that the nano zeolite prepared in Example 2 has a highly crystalline MFI topological structure.

[0079] Comparative Example 2

[0080] Aluminum isopropoxide, TEOS and TPAOH aqueous solution (mass concentration of 25wt%) were mixed, and the obtained first mixed solution was mixed and aged for 24h at room temperature and 300rpm magnetic stirring conditions, and then transferred to Anton Paar Monowave 400 microwave instrument, firstly subjected to low temperature microwave heat treatment at 90℃ for 90min, and then subjected to high temperature microwave heat treatment at 150℃ for 30min, and then transferred to a dialysis membrane with a molecular weight cutoff of 3.5kDa, and then immersed in 1L TPAOH aqueous solution with a concentration of 6mmol / L, dialyzed for 24h at room temperature and 40rpm magnetic stirring conditions, and then placed in Watsons distilled water for dialysis treatment, and the distilled water was replaced every 8h until the pH of the dialyzed external solution was between 7.0 and 8.0, and a ZSM-5 crystallite solution was obtained. Wherein, the molar ratio of silica:alumina:template:water in the first mixed solution is 1:0.0068:0.21:6.957

[0081] The obtained ZSM-5 crystallite solution was placed in an oven at 80°C for 3 days. The solution was transferred to a centrifuge tube and placed in a centrifuge. The solution was centrifuged at room temperature and 10,000 rpm. After centrifugation, the supernatant was poured out, deionized water was added, and the solution was ultrasonically dispersed in an ultrasonic cleaning machine for uniformity before the next centrifugation. The number of ultrasonic dispersion-centrifugal washing was 3 times, and the single centrifugation time was 5 minutes. The solution was then dried in an oven at 65°C for 12 hours to obtain a powdered ZSM-5 nano-zeolite.

[0082] Figure 7 The infrared spectra of the hydroxyl region of the ZSM-5 nano-zeolite (ZSM-5-F) without structural defects prepared in Example 2 and the ZSM-5 nano-zeolite (ZSM-5) prepared in a conventional manner in Comparative Example 2 are shown in FIG. Figure 7 It can be seen that the nano zeolite prepared in Example 2 has fewer silanol groups and very few structural defects.

[0083] Figure 8The solid silicon nuclear magnetic resonance spectra of the ZSM-5 nano zeolite (ZSM-5-F) without structural defects prepared in this example and the ZSM-5 nano zeolite (ZSM-5) prepared in a conventional manner in comparative example 2 are shown in FIG. Figure 8 It can be seen that the ZSM-5 nano zeolite prepared in Example 2 has very few structural defects.

[0084] Comparative Example 3

[0085] TEOS and TPAOH aqueous solutions (mass concentration of 25wt%) were mixed, and the resulting second mixed solution was mixed and aged for 24h at room temperature and 300rpm magnetic stirring conditions, and then transferred to an Anton Paar Monowave 400 microwave instrument. First, low-temperature microwave heat treatment was performed at 90°C for 90min, and then high-temperature microwave heat treatment was performed at 140°C for 50min to obtain a Silicalite-1 crystallite stock solution. The molar ratio of silica: template: water in the second mixed solution is 1:0.21:6.958.

[0086] The Silicalite-1 crystallite stock solution was mixed with a 1mol / L ammonium fluoride aqueous solution, and the pH was adjusted to 2.0 using a 1mol / L hydrochloric acid aqueous solution, and then placed in a preheated 80°C constant temperature oven for hydrothermal treatment for 14 days, the thick-walled reaction tube was taken out and cooled to room temperature, transferred to a centrifuge tube, and the centrifuge tube was placed in a centrifuge. Centrifugation was performed at room temperature and 10,000 rpm, and after the centrifugation, the supernatant was poured out, deionized water was added, and the next centrifugation was performed in an ultrasonic cleaning machine. The ultrasonic dispersion-centrifugal water washing number was 3 times, and the single centrifugation time was 5 minutes, and then dried in an oven at 65°C for 12 hours to obtain a powdered Silicalite-1 nanozeolite; wherein the molar ratio of ammonium fluoride: silica in the Silicalite-1 crystallite-fluoride ion mixed solution × 100% = 10%.

[0087] Fig. 9 TEM image of the structural defect-free Silicalite-1 nanozeolite prepared in Comparative Example 3. Fig. 9 It can be seen that the length of the structural defect-free Silicalite-1 nano-zeolite prepared from the Silicalite-1 crystallite stock solution without dialysis is 400-600 nm, the width is 300-500 nm, and the thickness is 30-80 nm, and the size of the zeolite is large.

[0088] Comparative Example 4

[0089] Aluminum isopropoxide, tetraethyl orthosilicate, TPAOH and water were mixed evenly at room temperature and 300 rpm stirring conditions, and the obtained first mixed solution was aged at room temperature for 24 hours, then transferred to a microwave reactor, first subjected to low-temperature microwave heat treatment at 90°C for 90 minutes, then subjected to high-temperature microwave heat treatment at 140°C for 20 minutes, transferred to a cellulose semipermeable membrane with a molecular weight cutoff of 3.5 kDa, and then immersed in 1L of a 6 mmol / L TPAOH aqueous solution, dialyzed and purified for 24 hours at room temperature and 40 rpm, and then placed in Watsons distilled water for dialyzation and purification, and the distilled water was replaced every 8 hours until the pH of the dialyzed external solution was between 7 and 8, thereby obtaining a ZSM-5 crystallite solution. Wherein, the molar ratio of silica:alumina:template:water in the first mixed solution is 1:0.0025:0.39:19.5.

[0090] The ZSM-5 crystallite solution was mixed with a 1mol / L ammonium fluoride aqueous solution, and the pH was adjusted to 2.0 using a 1mol / L hydrochloric acid aqueous solution, and then placed in a preheated 80°C constant temperature oven for hydrothermal treatment for 7 days, the thick-walled reaction tube was taken out and cooled to room temperature, transferred to a centrifuge tube, and the centrifuge tube was placed in a centrifuge. Centrifugation was performed at room temperature and 10,000 rpm, and after the centrifugation, the supernatant was poured out, deionized water was added, and the next centrifugation was performed in an ultrasonic cleaning machine. The ultrasonic dispersion-centrifugal washing number was 3 times, and the single centrifugation time was 5 minutes, and then dried in a 65°C oven for 12 hours to obtain a powdered ZSM-5 nano zeolite without structural defects (silicon-aluminum ratio of 200); wherein the molar ratio of silicon dioxide in the ammonium fluoride:silicalite-1 crystallite-fluoride ion mixed solution × 100% = 10%.

[0091] Fig.10 TEM image of ZSM-5 zeolite prepared in Comparative Example 4, Fig.10 It can be seen that the aluminum content of the ZSM-5 zeolite prepared in Comparative Example 4 is very low, resulting in its morphology being similar to that of the Silicalite-1 nano zeolite prepared in Example 1.

[0092] Comparative Example 5

[0093] Silicalite-1 nano zeolite was prepared according to the method of Example 1, the only difference from Example 1 being that the pH value of the Silicalite-1 crystal solution was adjusted to 3.0, 5.0 and 7.0 respectively.

[0094] Fig.11 TEM image of Silicalite-1 sheet-like nano zeolite with few structural defects prepared in Comparative Example 5. Fig.11 It can be seen that the acidity of the crystallization environment affects the morphology and size of zeolite.

[0095] Comparative Example 6

[0096] ZSM-5 nano zeolite was prepared according to the method of Comparative Example 4, the only difference from Comparative Example 4 being that the pH value of the ZSM-5 crystallization solution was adjusted to 3.0, 5.0 and 7.0, respectively, to obtain ZSM-5 flaky nano zeolite with few structural defects (silicon-aluminum ratio of 200).

[0097] Fig.12 TEM image of the ZSM-5 flaky nano zeolite with few structural defects prepared in Comparative Example 6. Fig.12 It can be seen that the acidity of the crystallization environment affects the morphology and size of zeolite.

[0098] Example 3

[0099] Silicalite-1 nano zeolite was prepared according to the method of Example 1, the only difference from Example 1 being that the temperature of the hydrothermal treatment was 160°C.

[0100] Fig.13 TEM image of Silicalite-1 nano zeolite prepared in Example 3, Fig.13 It can be seen that the temperature of hydrothermal treatment affects the morphology and size of Silicalite-1 nanozeolite.

[0101] Example 4

[0102] The ZSM-5 nano zeolite was prepared according to the method of Example 2, the only difference from Example 2 being that the temperature of the hydrothermal treatment was 160°C.

[0103] Fig.14 TEM image of ZSM-5 nano zeolite prepared in Example 4. Fig.14 It can be seen that the temperature of hydrothermal treatment affects the morphology and size of ZSM-5 nanozeolite.

[0104] Comparative Example 7

[0105] Aluminum isopropoxide, TEOS and TPAOH aqueous solution (mass concentration of 25wt%) were mixed, and the obtained first mixed solution was mixed and aged for 24h at room temperature and 300rpm magnetic stirring conditions, and then transferred to Anton Paar Monowave 400 microwave instrument, firstly subjected to low temperature microwave heat treatment at 90℃ for 90min, and then subjected to high temperature microwave heat treatment at 150℃ for 30min, and then transferred to a dialysis membrane with a molecular weight cutoff of 3.5kDa, and then immersed in 1L TPAOH aqueous solution with a concentration of 6mmol / L, dialyzed for 24h at room temperature and 40rpm magnetic stirring conditions, and then placed in Watsons distilled water for dialysis treatment, and the distilled water was replaced every 8h until the pH of the dialyzed external solution was between 7.0 and 8.0, and a ZSM-5 crystallite solution was obtained. Wherein, the molar ratio of silica:alumina:template:water in the first mixed solution is 1:0.0068:0.21:6.958.

[0106] The ZSM-5 crystallite solution was mixed with a 1mol / L ammonium fluoride aqueous solution, and the pH was adjusted to 2.0 using a 1mol / L hydrochloric acid aqueous solution, and the solution was placed in a preheated 80°C constant temperature oven for hydrothermal treatment for 21 days, and the thick-walled reaction tube was taken out, and the milky white solution obtained after cooling was transferred to a centrifuge tube, and the centrifuge tube was placed in a centrifuge, and centrifuged at room temperature and 10000rpm. After the centrifugation, the supernatant was poured out. Deionized water was added, and the solution was evenly dispersed ultrasonically in an ultrasonic cleaning machine and then centrifuged again. The number of ultrasonic dispersion-centrifugal washing was 3 times, and the time of a single centrifugation was 5min, and then dried in an oven at 65°C for 12h to obtain a powdery ZSM-5 sheet-like nano zeolite without structural defects; wherein the molar ratio of ammonium fluoride: silicon dioxide in the ZSM-5 crystallite-fluoride ion mixed solution × 100% = 20%.

[0107] Fig.15 The ZSM-5 nano zeolite without structural defects prepared in Comparative Example 7 is Fig.15 It can be seen that when the amount of fluoride ions is too much, the length of the prepared ZSM-5 nano zeolite is 500-700 nm, the width is 400-600 nm, and the thickness is 30-80 nm.

[0108] Comparative Example 8

[0109] According to the literature Expanding the Synthesis Field of High-Silica Zeolites [J]. Angewandte Chemie International Edition, 2020, 59 (44), ZSM-5 zeolite without structural defects was synthesized.

[0110] Fig.16The ZSM-5 zeolite without structural defects prepared in Comparative Example 8 is Fig.16 It can be seen that the particle size of the prepared ZSM-5 zeolite reaches several tens of microns, and the zeolite size is large.

[0111] The above is only a preferred embodiment of the present invention. It should be pointed out that for ordinary technicians in this technical field, several improvements and modifications can be made without departing from the principle of the present invention. These improvements and modifications should also be regarded as the scope of protection of the present invention.

Claims

1. A method for preparing MFI nano zeolite without structural defects, The following steps are involved: (1) first mixing an aqueous solution of a silicon source, an aluminum source and a template agent, and sequentially subjecting the obtained first mixed solution to a first microwave heat treatment and a first dialysis purification to obtain a ZSM-5 zeolite crystallite solution; the template agent includes tetrapropylammonium hydroxide; (2) secondly mixing the aqueous solution of the silicon source and the template agent, and sequentially subjecting the obtained second mixed solution to a second microwave heat treatment and a second dialysis purification to obtain a Silicalite-1 zeolite crystallite solution; the template agent comprises tetrapropylammonium hydroxide; (3) mixing the ZSM-5 zeolite crystallite solution and / or the Silicalite-1 zeolite crystallite solution with fluoride ions, adjusting the pH value of the resulting crystallite-fluoride ion mixed solution to 2, and performing hydrothermal treatment to obtain a MFI nano zeolite without structural defects; There is no chronological order between steps (1) and (2); The first microwave heat treatment and the second microwave heat treatment both include low-temperature microwave heat treatment and high-temperature microwave heat treatment in sequence; the temperature of the low-temperature microwave heat treatment is independently 70-100°C, and the time is independently 60-150min; the temperature of the high-temperature microwave heat treatment is independently 120-180°C, and the time is independently 10-90min.

2. The preparation method according to claim 1, It is characterized in that The molar ratio of silicon dioxide, aluminum oxide, template and water in the first mixed solution is 1: 0.0001-0.025: 0.1-0.45: 3-10.

3. The preparation method according to claim 1, It is characterized in that The molar ratio of silicon dioxide, template and water in the second mixed solution is 1:0.1-0.45:3-10.

4. The preparation method according to claim 1, 2 or 3, It is characterized in that After the first mixing and the second mixing, the obtained mixture is aged at a temperature of 15 to 40° C. for 4 to 48 hours.

5. The preparation method according to claim 1, It is characterized in that The molecular weight cut-offs of the first dialysis purification and the second dialysis purification are independently 1.5 to 6 kDa; The first dialysis purification and the second dialysis purification both comprise dialysis with a tetrapropylammonium hydroxide aqueous solution and dialysis with water in sequence, and the concentration of the tetrapropylammonium hydroxide aqueous solution is independently 2 to 16 mmol / L.

6. The preparation method according to claim 1, It is characterized in that The molar amount of the fluoride ions is 1 to 18% of the molar amount of silicon dioxide in the crystallite-fluoride ion mixed solution.

7. The preparation method according to claim 1, It is characterized in that The temperature of the hydrothermal treatment is 60 to 180° C., the time is 3 to 30 days, and the hydrothermal treatment is a static hydrothermal treatment.

8. The MFI nano zeolite without structural defects prepared by the preparation method according to any one of claims 1 to 7, wherein the MFI nano zeolite without structural defects comprises a ZSM-5 nano zeolite without structural defects and / or a Silicalite-1 nano zeolite without structural defects; the Silicalite-1 nano zeolite without structural defects has a length of 200 to 400 nm, a width of 200 to 400 nm, and a thickness of 30 to 60 nm; the ZSM-5 nano zeolite without structural defects has a length of 500 to 800 nm, a width of 200 to 400 nm, and a thickness of 30 to 60 nm.