A photo-induced heating and temperature-sensitive elastic phase-change energy storage fiber and a preparation method thereof

By uniformly dispersing the thermal conductivity material in the phase-change energy storage fiber and loading it on porous polyurethane fibers, combined with the elastic coating, the balance of thermal conductivity and mechanical properties is solved, and efficient photothermal conversion and temperature sensing functions are achieved.

CN116590915BActive Publication Date: 2024-11-29SOUTH CHINA UNIV OF TECH

Patent Information

Application Number
CN202310385124.5
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2023-04-11
Publication Date
2024-11-29
Estimated Expiration
2043-04-11

AI Technical Summary

Technical Problem

While the existing thermal phase change energy storage fibers improve thermal conductivity and photothermal conversion efficiency, their mechanical properties have decreased, and the surface-coated thermal conductivity improvement of thermal conductivity is limited, and the fibers receive light is low.

Method used

By uniformly dispersing the thermally conductive material in the phase change material and vacuum drying, a highly thermally conductive composite phase change material is formed, loaded in porous elastic polyurethane fibers, and an elastic protective layer is applied to the fiber surface to form photoheating and temperature Inductive elastic phase change energy storage fiber.

Benefits of technology

The thermal conductivity and stability of phase change materials are improved, the mechanical properties and enthalpy of the fiber are enhanced, and the conductivity of the fiber changes with temperature, achieving efficient photothermal conversion and temperature sensing functions.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure HDA0004173644030000011
    Figure HDA0004173644030000011
Patent Text Reader

Abstract

The present invention belongs to the technical field of phase change fiber, and discloses an elastic phase change energy storage fiber with photo-induced heating and temperature sensing and a preparation method thereof. Method: 1) polyurethane is dissolved in an organic solvent to obtain a spinning solution; the spinning solution is subjected to wet spinning, freezing, and drying to obtain a porous polyurethane fiber; 2) a thermal conductive material is evenly dispersed in the phase change material, vacuum treated, and a thermal conductive composite phase change material is obtained; 3) the composite phase change material is loaded on the pore structure and fiber surface of the porous polyurethane fiber by a vacuum impregnation method to obtain a thermal conductive phase change fiber; 4) a coating is applied on the surface of the thermal conductive phase change fiber, and dried to obtain an elastic phase change energy storage fiber with photo-induced heating and temperature sensing. The fiber of the present invention can load a large amount of thermal conductive phase change material, has the functions of photo-induced heating and temperature sensing, and the electrical conductivity of the fiber will change with the change of the external temperature.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention belongs to the technical field of smart materials, and in particular relates to a photo-induced heating and temperature-sensitive elastic phase-change energy storage fiber and a preparation method thereof. Background Art

[0002] Phase change energy storage fiber can change phase when the external environment temperature changes drastically, absorbing / releasing heat in the process, which can effectively buffer the impact of temperature changes on the human microclimate environment and achieve personalized thermal regulation effect. With the development of smart wearable products, phase change energy storage fiber needs to be given more functions.

[0003] Since phase change energy storage materials can absorb / release latent heat during the phase change process and the temperature of this process remains constant, they are widely used in fields such as construction and clothing. According to the phase transition mode, phase change energy storage materials are divided into solid-liquid phase change materials, solid-gas phase change materials and liquid-gas phase change materials. Among them, the volume of solid-liquid phase change materials does not change much before and after the phase change, and it is easier to encapsulate in a carrier, so it is widely used.

[0004] Pure phase change materials have low thermal conductivity and low heat storage efficiency, which limits their application in the fields of heat transfer and photothermal heating. The use of thermal conductive materials and phase change materials in combination can give the phase change material excellent thermal conductivity, improve its heat transfer rate and photothermal conversion efficiency. Existing thermally conductive phase change energy storage fibers use a thermally conductive carrier bracket or add thermally conductive components to the carrier bracket to increase the thermal conductivity of the phase change energy storage material, absorb solar energy to generate heat, and extend the thermal insulation effect of the phase change material. However, a thermally conductive carrier bracket or the addition of thermally conductive components to the carrier bracket will lead to a decrease in the mechanical properties of the fiber and poor elasticity.

[0005] Polyurethane, also known as polyurethane, contains repeating carbamate groups on the main chain. Due to the structure of soft and hard segments embedded in its chain segments, polyurethane fibers have excellent elasticity and an elongation at break of up to 700%. It has excellent elastic recovery rate and fatigue resistance and has been widely used in the clothing field.

[0006] The existing elastic thermally conductive phase change fabric uses a method of coating the surface of the phase change fabric with a thermally conductive material, so that the phase change energy storage fabric generates light-induced heat during use to extend the thermal insulation effect of the phase change composite material; at the same time, the volume change of the phase change material causes the conductivity of the conductive layer on the surface to change, so that the thermally conductive phase change fabric has a temperature sensing function. However, the thermally conductive material coated on the surface does not improve the thermal conductivity of the phase change fiber much, and the fiber has a low light receiving power. Summary of the invention

[0007] In view of the shortcomings and deficiencies of the above prior art, the purpose of the present invention is to provide a photo-induced heating and temperature-sensitive elastic phase change energy storage fiber and a preparation method thereof. The thermally conductive phase change fiber of the present invention has excellent thermal conductivity and elasticity, and responds quickly to temperature changes.

[0008] The present invention obtains a high thermal conductivity phase change material by uniformly dispersing the thermal conductive material in the phase change material, and then vacuum drying it, and then loading it into a porous elastic polyurethane fiber, and then coating a layer of elastic protective layer on the fiber surface to obtain a photo-induced heating and temperature-sensitive elastic phase change energy storage fiber. Since the thermal conductive material and the phase change material are composited to produce physical adsorption force, covalent bonds and intermolecular forces, the thermal conductivity and stability of the phase change material will be greatly improved, and the thermal conductive phase change fiber is endowed with the function of photothermal conversion; the porous polyurethane elastic fiber with high porosity can load a large amount of thermal conductive composite phase change material, and at the same time provides excellent mechanical properties; the multi-level pore structure and the thermal conductive composite phase change material generate capillary force, which improves the enthalpy value and thermal stability of the phase change fiber; at the same time, most thermal conductive materials are conductive, and the volume of the phase change material inside the fiber will expand or shrink during the phase change process, so that the conductive network in the thermal conductive composite phase change material is formed or destroyed, so the conductivity of the fiber will change with the change of the external temperature.

[0009] To achieve the purpose of the present invention, the technical solution of the present invention is as follows:

[0010] A photo-induced heating and temperature-sensitive elastic phase-change energy storage fiber comprises an elastic polyurethane fiber, a thermally conductive composite phase-change material and an elastic coating, wherein the elastic polyurethane fiber has a three-dimensional porous network structure; the internal pore structure and the external pore structure in the elastic polyurethane fiber are connected, that is, the internal pores are connected with the pores on the fiber surface; the thermally conductive composite phase-change material is filled in the three-dimensional porous network structure of the elastic polyurethane fiber; the thermally conductive composite phase-change material is composed of a thermally conductive material and a phase-change material; the elastic coating is water-based polyurethane, prepared from water-based acrylate or silicone emulsion; the elastic coating gives the fiber surface an elastic protective layer to achieve the stability of the loaded phase-change material, and its elasticity can provide space for the volume change of the phase-change material during temperature sensing.

[0011] The elastic polyurethane fiber has a three-dimensional porous network structure, with small pores less than 5 μm, accounting for 10-20%; medium pores 5-50 μm, accounting for 30-40%; and large pores greater than 50 μm, accounting for 50-60%.

[0012] The method for preparing the photo-induced heating and temperature-sensitive elastic phase-change energy storage fiber comprises the following steps:

[0013] 1) dissolving polyurethane in an organic solvent to obtain a spinning solution; preparing polyurethane fibers from the spinning solution through a wet spinning process, and then freeze-drying the solution to obtain porous polyurethane fibers;

[0014] 2) The thermal conductive material is evenly dispersed in the phase change material, and then vacuum dried to obtain a thermal conductive composite phase change material; the vacuum drying process helps the thermal conductive material and the phase change material to be fully mixed to generate physical adsorption force, covalent bond and intermolecular force;

[0015] 3) using a vacuum impregnation method to load the thermally conductive composite phase change material into the pore structure of the porous polyurethane fiber to obtain a thermally conductive phase change fiber containing the thermally conductive composite phase change material;

[0016] 4) A water-soluble elastic polymer coating is coated on the surface of the thermally conductive phase change fiber, and the coating is dried to form a film, thereby obtaining a photo-induced heating and temperature-sensitive elastic phase change energy storage fiber.

[0017] The polyurethane in step 1) comprises a polyether type and / or polyester type thermoplastic polyurethane having a weight average relative molecular weight of 1000 to 6000 g / mol. The polyurethane is a linear polyurethane; preferably a thermoplastic polyurethane;

[0018] The organic solvent in step 1) is one or more of N,N-dimethylformamide, dimethylacetamide, methylpyrrolidone, ethylene dichloride, butanone, acetone and toluene.

[0019] In step 1), the concentration of the polyurethane in the spinning solution is 1 to 50 wt%, preferably 10 to 30 wt%.

[0020] The wet spinning process in step 1) refers to the spinning solution passing through the spinning device to form a spinning solution stream, and the spinning solution stream enters the coagulation bath and stays in the coagulation bath to be formed to obtain polyurethane fibers.

[0021] The inner diameter of the spinning device is 1 to 1000 μm.

[0022] The residence time of the spinning solution thin stream in the coagulation bath is 1 to 20 minutes; the flow rate of the spinning solution is 0.01 to 100 m / min.

[0023] The coagulation bath is water or a mixture of an organic solvent and water, the organic solvent is one or more of N,N-dimethylformamide, cyclohexanone, butanone, acetone, ethyl acetate and toluene, preferably N,N-dimethylformamide; the mass concentration of the organic solvent in the mixture is 0 to 70 wt%.

[0024] The freezing temperature of the freezing in step 1) is -10 to -200°C, and the freezing time is 15 minutes to 16 hours; the absolute pressure of the drying is 1 to 100 Pa, and the drying time is 6 to 48 hours.

[0025] The phase change material in step 2) is one or more of alkanes, polyethylene glycol, higher fatty acids, higher fatty alcohols and ionic liquids with a phase change temperature of 20 to 150° C. The alkanes are alkanes with 15 to 35 carbon atoms, the weight average relative molecular weight of polyethylene glycol is 600 to 20,000 g / mol, the higher fatty acids are higher fatty acids with 15 to 30 carbon atoms, and the higher fatty alcohols are higher fatty alcohols with 15 to 30 carbon atoms. The ionic liquid is one or more of 1-ethyl-3-methylimidazolium tetrafluoroborate, 1-ethyl-3-methylimidazolium chloride, 1-ethyl-3-methylimidazolium nitrate, 1-ethyl-3-methylimidazolium tetrachloroaluminate, 1-butyl-3-methylimidazolium chloride, 1-butyl-3-methylimidazolium hexafluorophosphate, 1-decyl-3-methylimidazolium bromide, 1-hexadecyl-3-methylimidazolium laurate, 1-tetradecyl-3-methylimidazolium laurate, and 1-dodecyl-3-methylimidazolium laurate.

[0026] The thermally conductive material in step 2) is graphene, multi-walled carbon nanotubes, expanded graphite, carbon black, nanosilver wires, nanosilver rods, nanocopper wires, boron nitride, nickel foam, Ti3C2T x , MXenes, MOFs and carbon fibers.

[0027] The phase change material in step 2) is in liquid state before vacuum drying, for example, it is molten by heating; the heating temperature is 60-160° C., and the heating time is 10-40 min.

[0028] Dispersing the thermal conductive material uniformly in the phase change material means dispersing the thermal conductive material in water, then mixing it with the liquid phase change material, and then vacuum drying it.

[0029] The mixing conditions are as follows: heating ultrasonic dispersion is adopted, the ultrasonic dispersion temperature is 60 to 160° C., and the ultrasonic dispersion time is 10 to 30 minutes.

[0030] The vacuum drying conditions in step 2) are as follows: in a vacuum environment, the vacuum drying temperature is 60 to 160° C., and the vacuum drying time is 0.5 to 12 h.

[0031] The mass ratio of the thermally conductive material in the thermally conductive composite phase change material to the volume ratio of the phase change material in step 2) is 1-20 g:100 mL, preferably 3-10 g:100 mL.

[0032] The thermally conductive composite phase change material in step 3) is in liquid state before vacuum impregnation, for example, it is molten by heating; the heating treatment temperature is 60-160° C., and the heating treatment time is 20-60 min.

[0033] The conditions of the vacuum impregnation in step 3) are as follows: in a vacuum environment, the vacuum impregnation temperature is 60 to 160° C., and the vacuum impregnation time is 3 to 24 hours.

[0034] After the vacuum impregnation in step 3), the phase change material on the surface of the thermal conductive phase change fiber is removed, and the fiber is placed in an air environment at 60-160° C. for 3-8 hours.

[0035] The water-soluble elastic polymer in step 4) is one or more of water-based polyurethane, water-based acrylate and silicone emulsion.

[0036] The aqueous polymer coating refers to a polymer solution, wherein the concentration of the polymer in the solution is 0.1-10 wt %.

[0037] The coating in step 4) includes spraying and / or soaking, the spraying distance is 5 to 10 cm, and the number of spraying is 1 to 100 times. Soaking means soaking the fiber in the elastic polymer solution for 0.5 to 1.5 minutes.

[0038] In step 4), the drying is ventilation drying, the drying temperature is 20-25° C., and the drying time is 5-20 min.

[0039] The photo-induced heating and temperature-sensitive elastic phase-change energy storage fiber is prepared by the above method. The photo-induced heating and temperature-sensitive elastic phase-change energy storage fiber includes a porous elastic polyurethane fiber, a thermally conductive composite phase-change material and an elastic coating. The elastic polyurethane fiber is prepared by a wet spinning process and a freeze-drying process. The interior is a porous structure, and the pores are connected and can achieve pore size control and quantity distribution. The internal pore support is elastic; the composite phase-change material is composed of a thermally conductive material and a phase-change material; the thermally conductive composite phase-change material is loaded in a porous elastic polyurethane fiber; the elastic coating is a water-based polyurethane, a water-based acrylate and / or a silicone emulsion, which is uniformly coated on the surface of the fiber and closely fits the fiber surface.

[0040] The size of the fiber internal pores is 0.5 to 100 μm, the fiber diameter is 1 to 5000 μm, and the specific surface area is 1 to 700 m 2 / g; the thermal enthalpy value of the fiber is 50-350 J / g, the elongation at break is 50-500%, it has good thermal conductivity, and has the functions of light-heat conversion, phase change energy storage and temperature sensing.

[0041] The present invention obtains a high thermal conductivity phase change material by compounding a thermal conductive material with a phase change material, loading it into a porous elastic polyurethane fiber, and then coating a layer of elastic protective layer on the fiber surface to obtain an elastic phase change energy storage fiber that can be photoinduced to generate heat and temperature sensing. Since the compound of the thermal conductive material and the phase change material will produce physical adsorption force, covalent bonds and intermolecular forces, the thermal conductivity and stability of the phase change material will be greatly improved, giving the thermal conductive phase change fiber the function of photothermal conversion; the porous polyurethane elastic fiber with high porosity can load a large amount of thermal conductive composite phase change material, while providing excellent mechanical properties; the multi-level pore structure and the thermal conductive composite phase change material generate capillary force, which improves the enthalpy value and thermal stability of the phase change fiber; at the same time, most thermal conductive materials are conductive, and the volume of the phase change material inside the fiber will expand or shrink during the phase change process, so that the conductive network in the thermal conductive composite phase change material is formed or destroyed, so the conductivity of the fiber will change with the change of the external temperature.

[0042] Compared with the prior art, the present invention has the following advantages:

[0043] (1) The thermally conductive composite phase change material prepared by uniform blending and vacuum drying has high thermal conductivity and high photothermal conversion efficiency; the porous polyurethane fiber prepared by wet spinning and freeze drying has a high internal porosity and can encapsulate a large amount of thermally conductive composite phase change material, so that the thermally conductive phase change fiber has a high phase change enthalpy. At the same time, since the porous polyurethane fiber and the surface coating have excellent elasticity, the thermally conductive phase change material inside the fiber changes in volume during the solid-liquid phase transformation, so that the conductive network inside the fiber is formed or destroyed, so the conductivity of the fiber will change with the change of external temperature.

[0044] (2) The elastic phase-change energy storage fiber capable of photoinduced heating and temperature sensing provided by the present invention has a simple preparation process and mild preparation conditions and is suitable for large-scale production.

[0045] (3) The elastic phase change energy storage fiber capable of photo-induced heating and temperature sensing provided by the present invention can be used in photothermal conversion, phase change energy storage, electrothermal conversion, intelligent sensing and flexible wearable devices. BRIEF DESCRIPTION OF THE DRAWINGS

[0046] Figure 1 Schematic diagram of the structure of elastic phase change energy storage fiber. DETAILED DESCRIPTION

[0047] The present invention is further described in detail below in conjunction with specific examples, but the embodiments of the present invention are not limited thereto. Figure 1As shown, it includes elastic polyurethane fiber (i.e. porous polyurethane), thermally conductive composite phase change material and elastic coating, wherein the elastic polyurethane fiber has a three-dimensional porous network structure; the thermally conductive composite phase change material is filled inside the three-dimensional porous network structure of the elastic polyurethane fiber and adsorbed on the fiber surface; the elastic coating covers the surface of the thermally conductive phase change fiber; the thermally conductive composite phase change material is composed of a thermally conductive material and a phase change material; the elastic coating is water-based polyurethane, water-based acrylate and / or silicone emulsion;

[0048] The internal pore structure of the elastic polyurethane fiber is connected to the external pore structure, that is, the internal pores are connected to the pores on the fiber surface.

[0049] The elastic polyurethane fiber has a three-dimensional porous network structure, with small pores less than 5 μm, accounting for 10-20%; medium pores 5-50 μm, accounting for 30-40%; and large pores greater than 50 μm, accounting for 50-60%.

[0050] Example 1

[0051] 10g of BASF model 1185A thermoplastic polyurethane was dissolved in 30ml of butanone as the spinning solution; deionized water was used as the coagulation bath, wet spinning was performed at 25°C, the curing time was 10min, the fiber was frozen at -40°C for 8h, and then dried in a freeze drying device at 30°C for 16h to obtain porous polyurethane fiber; 0.3g of carboxyl carbon nanotubes was dispersed in 30ml of deionized water, added to 10ml of eicosane liquid, ultrasonically dispersed at 60°C for 10min, and then vacuum dried at 80°C for 8h to obtain carbon nanotubes. The porous polyurethane fiber is completely immersed in the molten carbon nanotube-eicosane composite phase change material, and vacuum treated at 60°C for 5 hours. The fiber is taken out and placed on filter paper and allowed to stand at 60°C for 3 hours to remove excess phase change material. 2 g of an aqueous polyurethane emulsion with a polymer mass fraction of 60% is dispersed in 30 mL of deionized water, and the mixture is mixed evenly to obtain an emulsion. The prepared emulsion is sprayed on the fiber surface and dried at room temperature. The spray drying process is repeated 5 times to obtain an elastic phase change energy storage fiber that can generate light and heat and sense temperature.

[0052] The thermal enthalpy of the thermally conductive phase change material obtained in this embodiment is 241.6 J / g, and the phase change temperature is 40°C. The thermal enthalpy of the elastic phase change energy storage fiber capable of photoinduced heating and temperature sensing is 177.2 J / g, and the phase change temperature is 42.6°C. The thermal conductivity of the thermally conductive phase change material obtained in this embodiment is 0.342 W·m -1 ·K -1Compared with the eicosane phase change fiber (the above-mentioned carbon nanotube-eicosane composite phase change material is replaced with eicosane phase change material, and other conditions are the same), the thermal conductivity of the obtained fiber is increased by 1.46 times, and the received light power is increased by 62.9%; when the temperature of the thermal conductive phase change fiber increases, the resistance of the fiber increases sharply by 7 times.

[0053] Example 2

[0054] 8 g of BASF model 685A thermoplastic polyurethane was dissolved in a mixture of 30 ml of toluene and 0.01 g of 1-ethyl-3-methylimidazolium tetrafluoroborate to obtain a spinning solution; deionized water was used as a coagulation bath, wet spinning was performed at 25°C, the curing time was 5 min, the fiber was frozen at -20°C for 12 h, freeze-dried in a freeze dryer for 24 h, and porous polyurethane fibers were obtained; 0.3 g of carbon nanotubes was dispersed in 30 ml of deionized water and added to 10 ml of l palmitic acid liquid, ultrasonically dispersed at 80℃ for 10min, and then vacuum dried at 100℃ for 8h to obtain carbon nanotube-palmitic acid composite phase change material; the porous polyurethane fiber was completely immersed in the molten carbon nanotube-palmitic acid, vacuum treated at 100℃ for 3h, the fiber was taken out and placed on filter paper and stood at 100℃ for 5h to remove excess palmitic acid; 2g of aqueous polyurethane emulsion with a polymer mass fraction of 60% was dispersed in 30mL of deionized water, and mixed evenly to obtain an emulsion. After taking it out, it was dried at room temperature, and the soaking and drying process was repeated 10 times to obtain an elastic phase change energy storage fiber that can generate light-induced heat and temperature sensing.

[0055] The thermal enthalpy of the thermally conductive phase change material obtained in this embodiment is 209.5 J / g, and the phase change temperature is 66.4°C; the enthalpy of the obtained elastic phase change energy storage fiber capable of photoinduced heating and temperature sensing is 187 J / g, and the phase change temperature is 73.5°C; the thermal conductivity of the thermally conductive phase change material obtained in this embodiment is 0.547 W·m -1 ·K -1 Compared with the palmitic acid phase change fiber (the above-mentioned carbon nanotube-palmitic acid composite phase change material is replaced with palmitic acid phase change material, and other conditions are the same), the thermal conductivity of the obtained fiber is increased by 2.06 times, and the received light power is increased by 146.03%; when the temperature of the thermal conductive phase change fiber increases, the resistance of the fiber increases sharply by 7 times.

[0056] Example 3

[0057] 10 g of BASF model 685A thermoplastic polyurethane was dissolved in 30 ml of N, N-dimethylformamide to prepare a spinning solution; 5% N, N-dimethylformamide aqueous solution was used as a coagulation bath, wet spinning was performed at 40°C, the curing time was 15 min, the fiber was frozen with liquid nitrogen for 15 min (-196°C), and freeze-dried in a freeze dryer for 18 h to obtain porous polyurethane fiber; 0.6 g of graphene was dispersed in 30 ml of deionized water, added to 10 ml of tetradecanol liquid, ultrasonically dispersed at 60°C for 10 min, and then vacuum dried at 80°C for 8 h to obtain A graphene-tetradecanol composite phase change material is obtained; a porous polyurethane fiber is completely immersed in a molten graphene-tetradecanol mixed solution, vacuum treated at 90°C for 5 hours, the fiber is taken out and placed on filter paper and allowed to stand at 90°C for 7 hours to remove excess tetradecanol; 0.4g of an aqueous polyurethane emulsion with a polymer mass fraction of 38% and a model number of 1526 of Yoshida Chemical is dispersed in 50mL of deionized water to obtain an emulsion, the fiber is placed in the emulsion and immersed for 1 minute, taken out and dried at room temperature, the immersion and drying process is repeated 100 times, and an elastic phase change energy storage fiber capable of photoinduced heating and temperature sensing is obtained.

[0058] The thermal enthalpy of the thermally conductive phase change material obtained in this embodiment is 228.2 J / g, and the phase change temperature is 40.5°C; the enthalpy of the elastic phase change energy storage fiber capable of photoinduced heating and temperature sensing is 193.2 J / g, and the phase change temperature is 46°C; the thermal conductivity of the thermally conductive phase change material obtained in this embodiment is 0.974 W·m -1 ·K -1 Compared with the tetradecanol phase change fiber (the graphene-tetradecanol composite phase change material is replaced with the tetradecanol phase change material, and other conditions are the same), the thermal conductivity of the obtained fiber is increased by 2.65 times, and the light receiving power is increased by 211%; when the temperature of the thermal conductive phase change fiber increases, the resistance of the fiber increases sharply by 10 times.

[0059] Example 4 (Reducing the content of heat-conducting components in heat-conducting phase change materials)

[0060] 12 g of BASF B95A thermoplastic polyurethane was dissolved in 30 ml of N, N-dimethylformamide to obtain a spinning solution. A 10% N, N-dimethylformamide aqueous solution was used as a coagulation bath, and wet spinning was performed at 40° C. The solidification time was 10 min. The fiber was frozen with liquid nitrogen for 15 min (-196° C.), and freeze-dried in a freeze dryer for 18 h to obtain a porous polyurethane fiber. 0.1 g of carboxyl carbon nanotubes was dispersed in 30 ml of deionized water, added to 10 ml of tetradecanol liquid, ultrasonically dispersed at 60° C. for 10 min, and then vacuum impregnated at 80° C. for 8 h. h, obtaining a carbon nanotube-tetradecanol composite phase change material; completely immersing the porous polyurethane fiber in the molten carbon nanotube-tetradecanol mixed solution, vacuum treating it at 90°C for 5h, taking out the fiber and placing it on filter paper and standing it at 90°C for 7h to remove excess tetradecanol; taking 2g of an aqueous polyurethane emulsion with a polymer mass fraction of 38% and a model number of 1526 of Yoshida Chemical, dispersed in 50mL of deionized water to obtain an emulsion, soaking the fiber in the emulsion for 1min, taking it out and drying it at room temperature, repeating the soaking and drying process 10 times, and obtaining an elastic phase change energy storage fiber that can generate light-induced heat and temperature sensitivity.

[0061] The thermal enthalpy of the thermally conductive phase change material obtained in this embodiment is 234 J / g, and the phase change temperature is 41.2°C; the enthalpy of the photoinduced heating and temperature-sensitive elastic phase change energy storage fiber obtained is 208.8 J / g, and the phase change temperature is 41.1°C; the thermal conductivity of the thermally conductive phase change material obtained in this embodiment is 0.501 W·m -1 ·K -1 The obtained fiber is compared with the tetradecanol phase change fiber (the carbon nanotube-tetradecanol composite phase change material is replaced with the tetradecanol phase change material, and other conditions are the same). The thermal conductivity of the fiber is increased by 1.14 times, and the light receiving power is increased by 45% (due to the low content of the thermal conductive component in the thermal conductive phase change material, the thermal expansion and contraction of the phase change material can still cause the material resistance to change). When the temperature rises from 25℃ to 50℃, the resistance increases to 1.45 times the original.

[0062] Comparative Example 1 (no thermal conductive material added)

[0063] 10g of BASF B95A thermoplastic polyurethane was dissolved in 30ml of N,N-dimethylformamide to prepare a spinning solution; 5% N,N-dimethylformamide aqueous solution was used as a coagulation bath, wet spinning was carried out at room temperature, the solidification time was 8min, the fiber was frozen at -60°C for 4h, and freeze-dried in a freeze dryer for 18h to obtain a porous polyurethane fiber; the porous polyurethane fiber was completely immersed in molten tetradecanol, vacuum treated at 100°C for 3h, the fiber was taken out and placed on filter paper and stood at 100°C for 5h to remove excess tetradecanol; 0.4g of a water-based polyurethane emulsion with a polymer mass fraction of 38% and a Yoshida Chemical model of 1526 was dispersed in 50mL of deionized water to prepare an emulsion; the porous polyurethane fiber was immersed in the emulsion for 1min, taken out and dried at room temperature, and the soaking and drying process was repeated 10 times.

[0064] The thermal conductivity of the phase change material in this embodiment is 0.406 W·m -1 ·K -1 The phase change enthalpy of the phase change fiber obtained is 187.5J / g, and the phase change temperature is 45.4℃; when the temperature increases from 25℃ to 50℃, the resistance does not change.

[0065] Comparative Example 2

[0066] 10g of BASF model 685A thermoplastic polyurethane is dissolved in a mixed solution of 30ml of toluene and 0.01g of 1-ethyl-3-methylimidazole tetrafluoroborate as a spinning solution; deionized water is used as a coagulation bath, wet spinning is carried out at 25°C, the curing time is 5min, the fiber is placed at -20°C for freezing for 12h, and then freeze-dried in a freeze dryer for 24h to obtain porous polyurethane fiber; the porous polyurethane fiber is completely immersed in molten palmitic acid, vacuum treated at 100°C for 3h, the fiber is taken out and placed on filter paper and allowed to stand at 100°C for 5h to remove excess palmitic acid; 2g of an aqueous polyurethane emulsion with a polymer mass fraction of 60% and 0.5g of carbon nanotubes are dispersed in 30mL of deionized water, mixed evenly to obtain a conductive liquid, the prepared conductive liquid is sprayed on the fiber surface, dried at room temperature, and the spray drying process is repeated 25 times to obtain an elastic phase change energy storage fiber that can generate light and heat and sense temperature.

[0067] The thermal enthalpy value of the elastic phase change energy storage fiber capable of photoinduced heating and temperature sensing obtained in this comparative example is 169.5 J / g, and the phase change temperature is 68.2°C. Compared with the palmitic acid phase change fiber, the thermal conductivity of the obtained fiber is increased by 0.82 times, and the light receiving power is increased by 30.5%; as the temperature of the phase change fiber increases, the fiber resistance slowly increases to 1.35 times of the original value.

[0068] The above embodiments are only some better implementation methods of the present invention, but the implementation methods of the present invention are not limited to the above embodiments. Any equivalent replacement, deformation and modification of some technical features within the creative concept and principle of the present invention should be included in the protection scope of the present invention.

Claims

1. A method for preparing a photothermal and temperature-sensitive elastic phase-change energy storage fiber. Features: The following steps are involved: 1) dissolving polyurethane in an organic solvent to obtain a spinning solution; preparing polyurethane fibers through a wet spinning process using the spinning solution, and then freeze-drying the spinning solution to obtain porous polyurethane fibers; the polyurethane in step 1) comprises polyether-type and / or polyester-type thermoplastic polyurethane with a weight-average relative molecular mass of 1000-6000 g / mol; the organic solvent in step 1) is one or more of N,N-dimethylformamide, dimethylacetamide, methylpyrrolidone, ethylene dichloride, butanone, acetone and toluene; the concentration of the polyurethane in the spinning solution in step 1) is 1-50wt%; 2) uniformly dispersing the thermal conductive material in the phase change material, and then vacuum drying to obtain a thermal conductive composite phase change material; the mass ratio of the thermal conductive material to the volume ratio of the phase change material in the thermal conductive composite phase change material is 3-10 g:100 mL; 3) The thermally conductive composite phase change material is loaded inside and on the surface of the porous structure of the porous polyurethane fiber by a vacuum impregnation method to obtain a thermally conductive phase change fiber containing the thermally conductive composite phase change material; 4) coating a water-soluble elastic polymer coating on the surface of the thermally conductive phase change fiber, drying it to form a film, and obtaining a photo-induced heating and temperature-sensitive elastic phase change energy storage fiber; The photo-induced heating and temperature-sensitive elastic phase-change energy storage fiber comprises a three-dimensional porous elastic polyurethane fiber, a thermally conductive composite phase-change material and an elastic coating; The thermally conductive composite phase change material is filled in the three-dimensional porous structure of the elastic polyurethane fiber; the elastic coating is coated on the surface of the elastic polyurethane fiber; The porous structure in the elastic polyurethane fiber is a composite pore structure composed of macropores, mesopores and small pores, the pore size of the macropores is greater than 50 μm, the pore size of the mesopores is 5-50 μm, and the pore size of the small pores is less than 5 μm; the small pores in the elastic polyurethane fiber are less than 5 μm, accounting for 10-20%; the mesopores are 5-50 μm, accounting for 30-40%; the macropores are greater than 50 μm, accounting for 50-60%; The internal pore structure and the external pore structure of the elastic polyurethane fiber are interconnected; The freezing temperature of the freezing in step 1) is -10~-200°C, and the freezing time is 15min~16h; the absolute pressure of the freeze drying is 1~100Pa, and the drying time is 6~48h; The wet spinning process in step 1) refers to the spinning solution passing through the spinning device to form a spinning solution stream, and the spinning solution stream enters the coagulation bath and stays in the coagulation bath to be formed to obtain polyurethane fibers; The vacuum drying conditions in step 2) are as follows: in a vacuum environment, the vacuum drying temperature is 60-160° C., and the vacuum drying time is 0.5-12 h; The phase change material in step 2) is one or more of alkanes, polyethylene glycol, higher fatty acids, and higher fatty alcohols with a phase change temperature of 20 to 150° C.; the alkane is an alkane with 15 to 35 carbon atoms, and the weight average relative molecular weight of the polyethylene glycol is 600 to 20,000 g / mol; The higher fatty acid is a higher fatty acid having 15 to 30 carbon atoms, and the higher fatty alcohol is tetradecanol; The thermal conductive material in step 2) is graphene, multi-walled carbon nanotubes, expanded graphite, carbon black, nano silver wires, nano silver rods, nano copper wires, boron nitride, nickel foam, Ti 3 C 2 T x , MXenes, MOFs and carbon fibers; The phase change material in step 2) is in liquid state before vacuum drying; dispersing the thermal conductive material uniformly in the phase change material means dispersing the thermal conductive material in water, then mixing it with the liquid phase change material, and then vacuum drying; The vacuum impregnation conditions in step 3) are as follows: in a vacuum environment, the vacuum impregnation temperature is 60-160° C., and the vacuum impregnation time is 3-24 hours; The water-soluble elastic polymer in step 4) is one or more of water-based polyurethane, water-based acrylate and silicone emulsion; The mass concentration of the elastic polymer in the coating in step 4) is 0.1-10%; the mass of the coating is the total mass of the elastic polymer and water.

2. The method for preparing the photothermal and temperature-sensitive elastic phase-change energy storage fiber according to claim 1, Features: The thermally conductive composite phase change material in step 3) is in liquid state before vacuum impregnation; After the vacuum impregnation in step 3), the phase change material on the surface of the thermal conductive phase change fiber is removed, and the fiber is placed in an air environment at 60-160° C. for 3-8 hours; In step 4), coating includes spraying and / or immersion, the spraying distance is 5 to 10 cm, and the number of spraying is 1 to 100 times; Soaking refers to soaking the fiber in the elastic polymer solution for 0.5 to 1.5 minutes; The drying process is ventilation drying, the drying temperature is 20~25℃, and the drying time is 5~20min.

3. The method for preparing the photothermal and temperature-sensitive elastic phase-change energy storage fiber according to claim 1, Features: The residence time of the spinning solution stream in the coagulation bath is 1 to 20 minutes; the flow rate of the spinning solution is 0.01 to 100 m / min; The coagulation bath is water or a mixture of an organic solvent and water, the organic solvent is one or more of N,N-dimethylformamide, cyclohexanone, butanone, acetone, ethyl acetate and toluene; the mass concentration of the organic solvent in the mixture is 0-70wt%.

4. A photo-induced heating and temperature-sensitive elastic phase-change energy storage fiber obtained by the preparation method according to any one of claims 1 to 3.

5. Application of the photo-induced heating and temperature-sensitive elastic phase-change energy storage fiber according to claim 4, Features: The photo-induced heating and temperature-sensitive elastic phase-change energy storage fiber is used in the fields of photothermal conversion, phase-change energy storage, electrothermal conversion, intelligent sensing and flexible wearable devices.

Citation Information

Patent Citations

  • Phase change thermo-regulation fiber containing ionic liquid and preparation method of phase change thermo-regulation fiber

    CN108360079A

  • Elastic phase change energy storage polyurethane fiber and preparation method thereof

    CN113235299A

Cited By

  • Preparation method of photo-thermal driven liquid metal microsphere-polymer shape memory fiber and infrared anti-counterfeiting application of photo-thermal driven liquid metal microsphere-polymer shape memory fiber

    CN120520084A