The inorganic nanowire winding structure and spectral selectivity were prepared by secondary hydrothermal method, combined with silane hydrophobic modifiers, and the problem of single color and insufficient self-cleaning performance of radiation refrigeration film materials was solved, and the colored bird's nest-like superhydrophobic radiation refrigeration was realized The high-efficiency radiation refrigeration and self-cleaning properties of membrane materials extend the service life.

CN116656207BActive Publication Date: 2024-11-22SOUTHEAST UNIV
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202310591025.2
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2023-05-24
Publication Date
2024-11-22
Estimated Expiration
2043-05-24

AI Technical Summary

Technical Problem

While improving the refrigeration effect, the existing radiation refrigeration film materials have single colors and limited applications, and the reflectivity in the sunlight area is high, which affects actual application; the self-cleaning performance of traditional materials is insufficient, resulting in a short outdoor service life.

Method used

The bird's nest-like structure formed by inorganic nanowire wrapping is prepared by secondary hydrothermal method, combining the spectral selectivity of various materials, enhancing infrared emission ability, and modifying it through silane hydrophobic modifiers to form colored bird's nest-like superhydrophobic radiation refrigeration The film material achieves selective absorption and radiation and has self-cleaning properties.

Benefits of technology

It realizes the ability to absorb in the narrow band of the sunlight zone, reduce reflectivity, enhance radiant heat, combines diverse colors and self-cleaning properties, and extends the outdoor service life of the material.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN116656207B_ABST
    Figure CN116656207B_ABST
Patent Text Reader

Abstract

The present invention discloses a colorful bird's nest-shaped super-hydrophobic radiation refrigeration film material and a preparation method thereof. The invention belongs to the technical field of radiation refrigeration materials. The material is prepared by applying colorful bird's nest-shaped powder and organic binder solution to the surface of a substrate after ultrasonic dispersion and curing at room temperature. The colorful bird's nest-shaped powder is obtained by a secondary hydrothermal method, so that inorganic nanowires are subjected to shear stress during the growth process, and the vertical growth is changed to curved growth, so that they are intertwined and stacked to form a unique bird's nest-shaped structure, which is beneficial to enhancing the material's scattering ability to sunlight. The reflectivity of the material in the sunlight area is 89% to 93%, the emissivity in the atmospheric window is 92% to 94%, and the solar irradiance is 800 to 1200W / m 2 The present invention solves the problems that the design only considers the optical properties of the material itself, but does not pay attention to the structure of the material, and the performance gap between the colored radiation cooling coating and the white radiation cooling coating is too large. It is expected to be applied to the fields of building energy saving, intelligent equipment, human thermal management, etc. in the future.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of radiation refrigeration materials and relates to a colorful bird's nest-shaped super-hydrophobic radiation refrigeration film material and a preparation method thereof. Background Art

[0002] With the national "carbon peak" and "carbon neutrality" goals, for buildings, achieving energy conservation and emission reduction while meeting indoor comfort is now the goal pursued by people. Traditional refrigeration methods based on vapor compression technology consume a lot of energy, causing a sharp increase in daily carbon emissions from buildings, which invisibly aggravates the greenhouse effect. Passive radiation cooling materials have attracted widespread attention from researchers because of their ability to achieve cooling under high irradiance without energy input, and are expected to be applied to architectural skills, photovoltaics, chip manufacturing and other fields.

[0003] Most of the radiation cooling film materials reported so far are based on the optical properties of the material itself, using its internal chemical bonds to improve the material's ability to radiate heat outward; at the same time, in order to ensure the material's high reflectivity to sunlight, the material is usually designed to be white, but pure white will greatly limit its practical application. Therefore, designing a radiation cooling film material with a special structure and a variety of colors is of great significance for future practical applications.

[0004] Patent CN113861771A discloses a radiation cooling coating with self-cleaning function and its preparation method and application. The material is made by coating a self-cleaning coating containing specific components on the surface of the cooling material layer, so that the material has excellent self-cleaning performance while having cooling effect. However, the material only relies on the characteristic absorption and color of its internal functional groups to achieve good optical properties, and the cooling effect is limited. The key to solving this problem lies in the unique structure of the material and the intrinsic absorption of the internal functional groups to enhance the cooling effect of the material.

[0005] Patent CN224345367A discloses a color radiation cooling film and its preparation method, which is prepared by laminating a radiation cooling film layer with a structural color forming layer formed by self-assembly of polystyrene microspheres. The film does not absorb sunlight and has a cooling effect and beautiful structural color. However, the self-assembly process of polystyrene microspheres is easily disturbed during its preparation, and the brightness and saturation of the structural color are far less than those of pigments, which limits its practical application. The key to solving this problem is to develop a color radiation cooling material that can achieve narrow-band absorption in the sunlight zone, thereby reducing the impact on the reflectivity of the material in the sunlight zone. Summary of the invention

[0006] Purpose of the invention: The purpose of the present invention is to provide a colorful bird's nest-shaped super-hydrophobic radiation cooling film material and its preparation method, which uses a bird's nest structure formed by the entanglement of inorganic nanowires prepared by a secondary hydrothermal method, so that the diameter of the circular hole in the center of the structure is perfectly matched with the wavelength of sunlight, thereby enhancing the internal dissipation of sunlight and reducing the absorption of sunlight energy; utilizing the spectral selectivity of a variety of materials to construct a wide-spectrum infrared emission and enhance the material's ability to radiate heat. In addition, the radiation cooling film material prepared by the present invention has a variety of colors, achieves selective absorption in the visible light band, reduces the influence of visible light absorption on cooling performance; has self-cleaning ability, and extends outdoor service life.

[0007] Technical solution: A colorful bird's nest-shaped super-hydrophobic radiation refrigeration film material according to the present invention; the material is prepared by coating a colorful bird's nest-shaped viscous emulsion on the surface of a substrate and curing at room temperature, and the average film thickness of the material is 100 μm to 200 μm;

[0008] Wherein, the colored bird's nest-shaped viscous emulsion is prepared by ultrasonically dispersing hydrophobic colored bird's nest-shaped powder into an organic binder solution;

[0009] The hydrophobic colored bird's nest-shaped powder is prepared by grafting a silane hydrophobic modifier on the surface of the colored bird's nest-shaped powder;

[0010] The colorful bird's nest-shaped powder is prepared by a hydrothermal method at a stirring rate of 200 to 300 r / min from inorganic nanowires, nitrates, and nitrogen-containing catalysts;

[0011] The inorganic nanowires are prepared from metal oxides by a hydrothermal method under alkaline conditions and a stirring rate of 300 to 600 r / min;

[0012] There is a circular cavity in the center of the bird's nest structure of the colored bird's nest powder, and the average diameter of the cavity opening is 0.5 μm to 3 μm.

[0013] Furthermore, the preparation method of the colorful bird's nest-shaped super-hydrophobic radiation refrigeration film material has the following specific preparation steps:

[0014] Step (1), at room temperature, add 1 part by weight of a metal oxide, 8 parts by weight of an inorganic base, and 50 to 200 parts by weight of water into a reaction kettle, so that the pH value of the reaction system is 10 to 12, stir for 1 to 2 hours, heat to 100° C. to 200° C., stir at 300 to 600 r / min for 12 to 28 hours, cool to room temperature, filter, wash the filter cake alternately with deionized water and ethanol until the filtrate is neutral, and vacuum dry at 40° C. to 100° C. for 3 to 6 hours to obtain inorganic nanowires;

[0015] Step (2), at room temperature, add 1 part by weight of the inorganic nanowires prepared in step (1), 2 to 6 parts by weight of nitrate, 1 part by weight of a nitrogen-containing catalyst, and 50 to 100 parts by weight of water into a reaction kettle, stir for 2 to 3 hours, heat to 150° C. to 250° C., stir at 200 to 300 r / min for 6 to 18 hours, cool to room temperature, filter, wash the filter cake alternately with deionized water and ethanol until the filtrate is neutral, protect under argon atmosphere, and dry at 200° C. to 300° C. for 4 to 5 hours to obtain a colored bird's nest-shaped powder;

[0016] Step (3), at room temperature, add 8 parts by weight of the colored bird's nest-shaped powder prepared in step (2), 100 to 200 parts by weight of ethanol, and 1 part by weight of ammonia water into a reaction kettle, wherein the concentration of ammonia water is 25% to 35%, and stir for 0.5 to 1.5 hours, then add 2 parts by weight of a silane hydrophobic modifier, heat to 40° C. to 60° C., stir for 1 to 3 hours, filter, wash 1 part by weight of the filter cake with 2 to 2.5 parts by weight of ethanol 2 to 3 times, and dry at 60° C. to 80° C. for 3 to 6 hours to obtain a hydrophobic colored bird's nest-shaped powder;

[0017] Step (4), mixing 1 part by weight of an organic binder with 20 to 30 parts by weight of an organic solvent, adding 10 to 15 parts by weight of the hydrophobic colored bird's nest-shaped powder prepared in step c, ultrasonically dispersing for 1 to 1.5 hours to obtain a colored bird's nest-shaped viscous emulsion, and then spraying it onto the surface of the substrate, controlling the average thickness of the film material to be 100 μm to 200 μm, and curing at room temperature for 24 hours to obtain a colored bird's nest-shaped super-hydrophobic radiation refrigeration film material.

[0018] Furthermore, in step (1), the metal oxide is one of TiO2, Ta2O5, and Y2O3;

[0019] The inorganic base is one of NaOH, Na2CO3, and NaHCO3.

[0020] Furthermore, in step (2), the nitrate is one of Co(NO3)2·6H2O, Ni(NO3)2·6H2O, and Ce(NO3)3·6H2O;

[0021] The nitrogen-containing catalyst is one of thiourea and triethanolamine.

[0022] Furthermore, in step (3), the silane hydrophobic modifier is one of hexadecyltrimethoxysilane, triethyltrifluoromethylsilane, and 1H,1H,2H,2H-perfluorooctyltrichlorosilane;

[0023] Furthermore, in step (4), the organic binder is one of polymethyl methacrylate, epoxy resin, and polydimethylsiloxane;

[0024] The organic solvent is one of acetone, toluene and ethanol;

[0025] The substrate is one of a quartz glass sheet, a PET film, and a copper sheet, and more preferably one of a quartz glass sheet and a PET film.

[0026] Furthermore, in steps (1)-(4), the room temperature is between 20-25°C.

[0027] Beneficial effects: Compared with the prior art, the present invention has the following characteristics: 1. Compared with the traditional static hydrothermal method, the advantages of the stirring hydrothermal method used in the present invention are: the interference of external force breaks the dissolution-crystallization process of the inorganic nanowires growing in the static process, and accelerates the dissolution of metal oxides under unsaturated conditions; the transport rate of the precursor formed after the metal oxide is dissolved in the solution increases with the increase of the stirring rate, so that it can grow into nanowires in the radial and axial directions; under the action of the stirring field force, the nanowires change from vertical growth to curved growth, making it easier for the nanowires to be entangled into a bird's nest structure; stirring can make the solution evenly mixed and prevent precipitation, so as to ensure the occurrence of uniform hydrothermal reaction;

[0028] 2. The secondary hydrothermal method adopted in the present invention needs to control the appropriate stirring rate to ensure the bending growth of the nanowires and the formation of the bird's nest structure; in the first hydrothermal process, the rotation speed is controlled to be 300-600r / min. On the one hand, the transmission rate of the precursor formed after the dissolution of the metal oxide in the solution is controlled to control the growth rate of the inorganic nanowires. On the other hand, the inorganic nanowires are subjected to appropriate shear stress during the growth process to obtain an appropriate degree of bending, avoiding the breakage of the inorganic nanowires caused by too fast a rotation speed or the insufficient bending degree of the inorganic nanowires caused by too slow a rotation speed; in the second hydrothermal process, the rotation speed is controlled to be 200-300r / min. On the one hand, under the action of the nitrogen-containing catalyst, nitrates are deposited on the surface of the nanowires, so that the inorganic nanowires increase their relative diameters during the secondary growth. On the other hand, the appropriate rotation speed controls the relative diameter of the inorganic nanowires during the secondary growth. The diameter is regulated so that the average diameter of the cavity of the bird's nest structure is 0.5μm-3μm;

[0029] 3. The diameter of the hole openings of the bird's nest-like structure is concentrated in the range of 0.5μm to 3μm. The perfect match between the hole opening size and the wavelength of the sunlight band causes surface electron oscillation and stimulates the plasmon effect, which not only enhances the structure's backscattering ability for sunlight, but also helps to improve the coating's reflectivity in the sunlight area and reduce the absorption of sunlight energy. It also helps to reduce the absorption of energy in the near-infrared band, enabling the material to achieve selective emission, solving the shortcoming of traditional radiation cooling coating materials that only rely on the optical properties of the material to improve the reflectivity in the sunlight area;

[0030] 4. The metal oxides deposited on the surface of the inorganic nanowires by the three nitrates used in the present invention, on the one hand, make the inorganic nanowires grow again and have different colors, and on the other hand, have a narrow absorption peak in the wave number range corresponding to the visible light region. Taking the nitrate Co(NO3)2·6H2O as an example, the Co(NO3)2 deposited on the surface of the inorganic nanowires gives the inorganic nanowires red color, and Co(NO3)2 has a narrow band absorption in the range of 650nm to 750nm, which reduces the influence on the reflectivity of the sunlight area and the emissivity of the atmospheric window, ensures the excellent radiation cooling performance of the coating, and solves the problem that the performance of the original colored radiation cooling coating is too far behind that of the white radiation cooling coating;

[0031] 5. The hydroxyl groups on the surface of the nanowires react with the -OR (R represents an alkyl) group at one end of the silane hydrophobic modifier to form a homogeneous system, which not only removes moisture from the surface of the inorganic nanowires, but also forms a covalent bond with the oxygen atom in the -OR group of the silane hydrophobic modifier, so that the polymer functional group carried by the other end of the silane hydrophobic modifier is firmly combined with the inorganic nanowires to produce a coating film, thereby reducing the surface energy of the inorganic nanowires; at the same time, the micro-nano structure formed by the mutual entanglement of the nanowires is conducive to enhancing the surface roughness of the coating, so that the water droplets and the coating surface form an air film, which can avoid being attached by water while also taking away the dust on the coating surface, maintaining the radiation cooling performance of the coating material, and solving the problem of poor cooling effect caused by dust accumulation when traditional radiation cooling coating materials are used outdoors. BRIEF DESCRIPTION OF THE DRAWINGS

[0032] Figure 1 It is a preparation flow chart of the present invention;

[0033] Figure 2 This is a microscopic morphology image (SEM) of the colorful bird's nest-shaped radiation cooling film material in Example 1 of the present invention;

[0034] Figure 3 is an actual temperature drop curve diagram of the red bird's nest-shaped radiation refrigeration film material in Example 1 of the present invention;

[0035] Figure 4 This is a static contact angle diagram of the red bird's nest-shaped radiation cooling film material in Example 1 of the present invention. DETAILED DESCRIPTION

[0036] In order to more clearly illustrate the technical solution of the present invention, the technical solution of the present invention is further described in detail below with reference to the accompanying drawings;

[0037] Embodiment 1:

[0038] Step (1), at room temperature, add 1 part of Ta2O5, 8 parts of NaOH and 70 parts of water into a reaction kettle, make the pH value of the reaction system 10, stir for 1.5 hours, heat to 120°C, stir at 400r / min for 24 hours, cool to room temperature, filter, wash the filter cake with deionized water and ethanol alternately until the filtrate is neutral, and dry under vacuum at 50°C for 4 hours to obtain inorganic nanowires;

[0039] Step (2), at room temperature, add 1 part of inorganic nanowires prepared in step (1), 3 parts of Co(NO3)2·6H2O, 1 part of triethanolamine, and 60 parts of water into a reaction kettle, stir for 2 hours, heat to 180°C, stir at 200r / min for 8 hours, cool to room temperature, filter, wash the filter cake with deionized water and ethanol alternately until the filtrate is neutral, protect with argon atmosphere, and dry at 200°C for 4 hours to obtain a red bird's nest-like powder, such as Figure 2 As shown;

[0040] Step (3), add 8 parts of the red bird's nest-like powder obtained in step (2), 120 parts of ethanol, and 1 part of 25% ammonia water into a reactor, stir for 1 hour, then add 2 parts of a silane hydrophobic modifier, heat to 40°C, stir for 3 hours, filter, wash 1 part of the filter cake with 2 parts of ethanol 2 to 3 times, and dry at 60°C for 6 hours to obtain a hydrophobic red bird's nest-like powder;

[0041] Step (4), mix 1 part of epoxy resin with 20 parts of ethanol, add 12 parts of the hydrophobic red bird's nest powder prepared in step (3), ultrasonically disperse for 1 hour to obtain a red bird's nest viscous emulsion, spray it onto the surface of the quartz glass sheet, control the average thickness of the film material to 120 μm, and cure it at room temperature for 24 hours to obtain a red bird's nest super hydrophobic radiation refrigeration film material.

[0042] Embodiment 2:

[0043] Step (1), at room temperature, add 1 part of TiO2, 8 parts of NaHCO3, and 150 parts of water into a reaction kettle, make the pH value of the reaction system 12, stir for 1 hour, heat to 160°C, stir at 450r / min for 18 hours, cool to room temperature, filter, wash the filter cake with deionized water and ethanol alternately until the filtrate is neutral, and vacuum dry at 80°C for 3 hours to obtain inorganic nanowires;

[0044] Step (2), at room temperature, add 1 part of inorganic nanowires prepared in step (1), 2 parts of Ni(NO3)2·6H2O, 1 part of thiourea, and 80 parts of water into a reactor, stir for 3 hours, heat to 200°C, stir at 250r / min for 12 hours, cool to room temperature, filter, wash the filter cake with deionized water and ethanol alternately until the filtrate is neutral, protect with argon atmosphere, and dry at 240°C for 5 hours to obtain a green bird's nest-like powder;

[0045] Step (3), add 8 parts of the green bird's nest-shaped powder obtained in step (2), 140 parts of ethanol, and 1 part of 30% ammonia water into a reactor, stir for 0.5 h, then add 2 parts of a silane hydrophobic modifier, heat to 60° C., stir for 1 h, filter, wash 1 part of the filter cake with 2.5 parts of ethanol 2 to 3 times, and dry at 70° C. for 4 h to obtain a hydrophobic green bird's nest-shaped powder;

[0046] Step (4), mix 1 part of polymethyl methacrylate with 25 parts of acetone, then add 10 parts of the hydrophobic green bird's nest powder prepared in step (3), ultrasonically disperse for 1 hour to obtain a green bird's nest-like viscous emulsion, and then spray it onto the surface of the PET film, control the average thickness of the film material to 150 μm, and cure it at room temperature for 24 hours to obtain a green bird's nest-like super hydrophobic radiation refrigeration film material.

[0047] Embodiment 3:

[0048] Step (1), at room temperature, add 1 part of Y2O3, 8 parts of Na2CO3, and 100 parts of water into a reaction kettle, make the pH value of the reaction system 11, stir for 2 hours, heat to 180°C, stir at 550r / min for 26 hours, cool to room temperature, filter, wash the filter cake alternately with deionized water and ethanol until the filtrate is neutral, and vacuum dry at 50°C for 5 hours to obtain inorganic nanowires;

[0049] Step (2), at room temperature, add 1 part of inorganic nanowires prepared in step (1), 2 parts of Ce(NO3)3·6H2O, 1 part of triethanolamine, and 100 parts of water into a reaction kettle, stir for 2 hours, heat to 240°C, stir at 300r / min for 18 hours, cool to room temperature, filter, wash the filter cake with deionized water and ethanol alternately until the filtrate is neutral, protect with argon atmosphere, and dry at 280°C for 4 hours to obtain a yellow bird's nest-like powder;

[0050] Step (3), add 8 parts of the yellow bird's nest-like powder prepared in step (2), 170 parts of ethanol, and 1 part of 35% ammonia water into a reactor, stir for 0.5 h, then add 2 parts of a silane hydrophobic modifier, heat to 50° C., stir for 2 h, filter, wash 1 part of the filter cake with 2.5 parts of ethanol 2 to 3 times, and dry at 80° C. for 3 h to obtain a hydrophobic yellow bird's nest-like powder;

[0051] Step (4), mix 1 part of polydimethylsiloxane with 30 parts of toluene, then add 15 parts of the hydrophobic yellow bird's nest powder prepared in step (3), ultrasonically disperse for 1 hour to obtain a yellow bird's nest viscous emulsion, and then spray it onto the surface of the copper sheet, control the average thickness of the film material to 180 μm, and cure it at room temperature for 24 hours to obtain a yellow bird's nest super hydrophobic radiation refrigeration film material.

[0052] Performance Testing:

[0053] The reflectivity and emissivity of the colored bird's nest-shaped radiation cooling film materials of Examples 1-3 are shown in Table 1. The real-time temperature curve of the red bird's nest-shaped super-hydrophobic radiation cooling film material of Example 1 and the sub-environment is shown in Table 1. Figure 3 As shown, the contact angle between the red bird's nest-shaped super-hydrophobic radiation cooling film material and water in Example 1 is as follows: Figure 4 As shown:

[0054] As can be seen from Table 1, by adjusting the ratio of metal oxide to metal nitrate, the influence of the color of the coating material on the reflectivity in the visible light region is reduced. The reflectivity of the red bird's nest-shaped super hydrophobic radiation refrigeration film material in Example 1 is 90.12% in the visible light band, and the reflectivity of the sunlight band is 96.65%; the reflectivity of the green bird's nest-shaped super hydrophobic radiation refrigeration film material in Example 2 is 93.18% in the visible light band, and the reflectivity of the sunlight band is 96.32%; the reflectivity of the yellow bird's nest-shaped super hydrophobic radiation refrigeration film material in Example 3 is 92.36% in the visible light band, and the reflectivity of the sunlight band is 98.54%;

[0055] In addition, the emissivity of the colorful bird's nest-shaped super-hydrophobic radiation cooling film materials prepared in Examples 1-3 is all above 92%; the atmospheric window emissivity of the red bird's nest-shaped super-hydrophobic radiation cooling film material in Example 1 is 92.68%, the atmospheric window emissivity of the green bird's nest-shaped super-hydrophobic radiation cooling film material in Example 2 is 94.13%, and the atmospheric window emissivity of the yellow bird's nest-shaped super-hydrophobic radiation cooling film material in Example 3 is 94.52%; therefore, the colorful bird's nest-shaped super-hydrophobic radiation cooling film material of the present invention can reflect most of the sunlight and dissipate the absorbed heat into outer space through the atmospheric window.

[0056] Depend on Figure 3 It can be seen that the red bird's nest-shaped super-hydrophobic radiation cooling film material of Example 1 has a daytime solar irradiance of 800 W / m 2 A 5℃ cooling effect can be achieved under Figure 4 It can be seen that the static contact angle between the red bird's nest-shaped super-hydrophobic radiative cooling film material of Example 1 and water is above 150°, which can achieve self-cleaning properties and extend the outdoor service life.

[0057] In summary, the colorful bird's nest-shaped super-hydrophobic radiation cooling film material of the present invention is prepared by compounding a bird's nest-shaped structure formed by the entanglement and accumulation of curved inorganic nanowires and an organic binder. By adjusting the proportion of raw materials, the influence of color on the reflectivity in the sunlight area is reduced, thereby taking into account both the radiation cooling performance and aesthetic characteristics of the coating material. At the same time, the coating material also has self-cleaning properties, which can effectively avoid the accumulation of pollutants such as dust and extend the outdoor service life.

[0058] The above embodiments are preferred implementations of the present invention, but the implementations of the present invention are not limited to the above embodiments, and other equivalent replacement methods are all included in the protection scope of the present invention.

[0059] Table 1 Reflectivity and emissivity values ​​of colored radiation bird's nest-shaped super-hydrophobic radiation cooling coating materials

[0060]

[0061] The above are only preferred embodiments of the present invention, and the protection scope of the present invention is not limited to the above embodiments. All technical solutions under the concept of the present invention belong to the protection scope of the present invention. It should be pointed out that for ordinary technicians in this technical field, some improvements and modifications without departing from the principle of the present invention should be regarded as the protection scope of the present invention.

Claims

1. A colorful bird's nest-shaped super-hydrophobic radiation refrigeration film material, characterized in that: The material is made by coating a colorful bird's nest-shaped viscous emulsion on the surface of a substrate and curing it at room temperature; The average film thickness of the prepared material is 100 μm to 200 μm; The colorful bird's nest-shaped viscous emulsion is prepared by ultrasonically dispersing hydrophobic colorful bird's nest-shaped powder into an organic binder solution; The hydrophobic colored bird's nest-shaped powder is prepared by grafting a silane hydrophobic modifier on the surface of the colored bird's nest-shaped powder; The colorful bird's nest-shaped powder is prepared by a hydrothermal method at a stirring rate of 200-300 r / min from inorganic nanowires, nitrates, and nitrogen-containing catalysts; The inorganic nanowires are prepared from metal oxides by a hydrothermal method under alkaline conditions and a stirring rate of 300-600 r / min; Wherein, the nitrate is one of Co(NO3)2·6H2O, Ni(NO3)2·6H2O, and Ce(NO3)3·6H2O; The nitrogen-containing catalyst is one of thiourea and triethanolamine.

2. A colorful bird's nest-shaped super-hydrophobic radiation cooling film material according to claim 1, characterized in that: There is a circular cavity in the center of the bird's nest structure of the colored bird's nest powder, and the average diameter of the cavity opening is between 0.5 μm and 3 μm.

3. A method for preparing a colorful bird's nest-shaped super-hydrophobic radiation refrigeration film material according to any one of claims 1 to 2, characterized in that: The specific preparation steps are as follows: (1) At room temperature, 1 part by weight of the prepared metal oxide, 8 parts by weight of the inorganic base, and 50-200 parts by weight of water are added to a reaction kettle in proportion and stirred for 1-2 hours, then heated to 100°C-200°C, stirred at 300-600 r / min for 12-28 hours, cooled to room temperature, filtered, and the filter cake is washed alternately with deionized water and ethanol until the filtrate is neutral, and vacuum dried at 40°C-100°C for 3-6 hours to obtain inorganic nanowires; (2) At room temperature, 1 part by weight of the inorganic nanowires prepared in step (1), 2 to 6 parts by weight of nitrate, 1 part by weight of a nitrogen-containing catalyst, and 50 to 100 parts by weight of water are added to a reaction kettle in proportion, stirred for 2 to 3 hours, then heated to 150°C to 250°C, stirred at 200 to 300 r / min for 6 to 18 hours, cooled to room temperature, filtered, and the filter cake was washed alternately with deionized water and ethanol until the filtrate was neutral, and dried at 200°C to 300°C for 4 to 5 hours under argon atmosphere to obtain a colored bird's nest-shaped powder; (3) At room temperature, 8 parts by weight of the colored bird's nest-shaped powder prepared in step (2), 100-200 parts by weight of ethanol, and 1 part by weight of ammonia water are added to a reaction kettle in proportion and stirred for 0.5-1.5 hours, followed by adding 2 parts by weight of a silane hydrophobic modifier, and then the temperature is raised to 40°C-60°C, stirred for reaction for 1-3 hours, filtered, 1 part by weight of the filter cake is washed 2-3 times with 2-2.5 parts by weight of ethanol, and dried at 60°C-80°C for 3-6 hours to obtain a hydrophobic colored bird's nest-shaped powder; (4) Mix 1 part by weight of an organic binder with 20 to 30 parts by weight of an organic solvent, and then take 10 to 15 parts by weight of the hydrophobic colored bird's nest-like powder prepared in step (3), and ultrasonically disperse for 1 to 1.5 hours to prepare a colored bird's nest-like viscous emulsion; It is then coated on the surface of the substrate, the average thickness of the film material is controlled to be 100μm~200μm, and cured at room temperature for 24 hours to finally obtain a colorful bird's nest-shaped super-hydrophobic radiation refrigeration film material.

4. The method for preparing a colorful bird's nest-shaped super-hydrophobic radiation refrigeration film material according to claim 3, characterized in that: In step (1), the metal oxide is one of TiO2, Ta2O5, and Y2O3; The inorganic base is one of NaOH, Na2CO3, and NaHCO3.

5. The method for preparing a colorful bird's nest-shaped super-hydrophobic radiation refrigeration film material according to claim 3, characterized in that: In step (1), the pH value of the reaction system in the reactor is 10-12.

6. The method for preparing a colorful bird's nest-shaped super-hydrophobic radiation refrigeration film material according to claim 3, characterized in that: In step (3), the silane hydrophobic modifier is one of hexadecyltrimethoxysilane, triethyltrifluoromethylsilane, and 1H,1H,2H,2H-perfluorooctyltrichlorosilane.

7. The method for preparing a colorful bird's nest-shaped super-hydrophobic radiation cooling film material according to claim 3, characterized in that: In step (3), the concentration of the ammonia water is 25% to 35%.

8. The method for preparing a colorful bird's nest-shaped super-hydrophobic radiation cooling film material according to claim 3, characterized in that: In step (4), the organic binder is one of polymethyl methacrylate, epoxy resin, and polydimethylsiloxane; The organic solvent is one of acetone, toluene and ethanol; The substrate is one of a quartz glass sheet, a PET film and a copper sheet.