A method for preparing low-sodium light-burned alpha-alumina
By using specific alkali agents and emulsifiers in the alumina preparation process to form polymer aluminum chloride, combined with low-temperature calcination technology, the problem of difficulty in reducing sodium oxide content is solved, the preparation of low-sodium alumina is achieved, and the purity and performance of the product are improved. , while reducing energy consumption and harmful emissions.
Patent Information
- Application Number
- CN202311156483.X
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2023-09-08
- Publication Date
- 2024-11-22
- Estimated Expiration
- 2043-09-08
Smart Images

Figure 4GOTBPIOG7AEDVZVCGTUUN7NSEUDSQYGTQL8ZPYB 
Figure SMPM3OELUTG5NMNTNZ7VV6PD1AMLDQM7EAA37BDQ
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of alumina preparation, and in particular to a method for preparing low-sodium light-burned alpha-alumina. Background Art
[0002] Low-sodium α-alumina powder is mainly used in aluminum-containing special glass such as TFT-LCD (thin-film transistor liquid crystal display) cover glass and solar photovoltaic glass. Domestic special alumina powder materials for such high-end applications have long been mainly dependent on imports, and are in urgent need of domestic research and development and industrialization to complete import substitution and fill industry gaps.
[0003] Sodium oxide is the main impurity in alumina, followed by trace impurities SiO 2 , Fe 2 O 3 When preparing alumina by the Bayer process, it is inevitable to use excessive sodium hydroxide as a solvent in the process of removing iron oxide and silicon dioxide, so Na 2 O impurities, the content of which may be as high as 0.5% or more.
[0004] With the development of industry, higher requirements are put forward for the content of sodium oxide at this stage. For example, for white corundum, sodium oxide will directly affect the performance of white corundum abrasives. If the sodium oxide content in white corundum abrasives is too high, more β-alumina will be generated, which will reduce the crystal hardness of white corundum, reduce the cutting ability, and make it easy to pulverize and break, and have low thermal stability. For electronic ceramic powder, the sodium oxide content is generally required to be less than 0.1%, because β-alumina has a certain conductivity, which affects its electrical properties. In addition, in the fields of medicine, chemical industry, catalyst, ceramics, etc., it is often necessary to control the sodium oxide content to a certain extent.
[0005] At present, the method for preparing high-purity alumina for special glass is mainly through high-temperature calcination, adding a large amount of mineralizers such as boric acid, ammonium chloride, aluminum fluoride, ammonium fluoride, etc. to remove sodium. However, this process is not completely de-sodiumed due to uneven mixing of mineralizers and fluctuations in process conditions, and the product fluctuates greatly. In addition, because the additives contain toxic fluorides, it is harmful to occupational health. At the same time, due to uneven mixing of mineralizers or uneven temperatures during calcination, the composition and crystallization of the product have large deviations, resulting in fluctuations in indicators and uneven product performance. In order to ensure the de-sodium effect, the existing process technology has a high calcination temperature (above 1350℃), a long insulation time, high energy consumption, and a large amount of harmful gas emissions. Summary of the invention
[0006] The purpose of the present invention is to solve the above-mentioned technical problems and provide a method for preparing low-sodium light-burned α-alumina. The present invention adopts specific types of alkali agents and emulsifiers and combines the timing of adding the alkali agents and emulsifiers to prepare alumina products with a sodium content lower than the existing technical level. The method has many beneficial effects such as low sintering temperature, low sodium content, and low energy consumption.
[0007] A method for preparing low-sodium light-burned α-alumina of the present invention comprises the following steps:
[0008] S1: Take industrial-grade alumina products, add de-sodium agent and emulsifier, and dissolve for a period of time;
[0009] S2: After the dissolution in step S1 is completed, an alkali agent is added into the system, and the filtrate and filter are obtained by aging and filtering;
[0010] S3: calcining the filter cake obtained in step S2 and cooling it;
[0011] S4: Grind and sieve to obtain a low-sodium light-burned α-alumina.
[0012] Furthermore, the sodium removal agent is preferably hydrochloric acid, and the amount of hydrochloric acid used is 5%-12% of the mass of alumina. The dissolution time is: 3-6h.
[0013] The present invention adopts hydrochloric acid as the sodium removal agent, which can more fully dissolve the sodium oxide in the alumina after a long period of pre-dissolution. At the same time, the dispersing effect of the emulsifier can further promote the sodium removal agent to enter the alumina lattice and increase the dissolution rate of the intercrystalline alkali.
[0014] Furthermore, the emulsifier in the present application is polyoxyethylene nonylphenol ether; the amount of the emulsifier added is 1-3% of the mass of the aluminum oxide.
[0015] Polyoxyethylene nonylphenol ether itself is an emulsifier. On the one hand, it can promote the diffusion of the de-sodium agent into the interior of alumina. On the other hand, after adding aluminum hydroxide, aluminum hydroxide combines with related substances in the system to form polyaluminum chloride. Polyoxyethylene nonylphenol ether further promotes the stability of the flocculant polyaluminum chloride, thereby promoting the flocculation and ion exchange of polyaluminum chloride on sodium ions.
[0016] In the further step S2, the alkaline agent is preferably aluminum hydroxide, and the molar ratio of hydrochloric acid to aluminum hydroxide is 1-4:1.
[0017] The present invention adds aluminum hydroxide to the system, which can form polyaluminum chloride with the sodium removal agent in the system. The polyaluminum chloride solution generates an inorganic polymer material with a large molecular weight and a high charge due to the bridging effect of hydroxide ions and the polymerization effect of multivalent anions. After aluminum oxide and the polyaluminum chloride solution are mixed, high-charge ions in the polyaluminum chloride replace sodium impurities in the aluminum oxide and enter the solution to form low-charge sodium ions, thereby further allowing sodium ions to enter the polyaluminum chloride system to obtain low-sodium aluminum oxide.
[0018] Furthermore, the aging temperature in step S2 is 50-100° C. and the aging time is 1-3 h.
[0019] Furthermore, in step S3, the calcination temperature is 1200-1300° C. and the calcination time is 3-7 hours.
[0020] Furthermore, the calcination equipment in step S3 is a tunnel kiln or a shuttle kiln.
[0021] Furthermore, the grinding conditions in step S4 are: α-Al 2 O 3 The raw powder is placed in a ball mill for grinding; the grinding balls and α-Al 2 O 3 The weight ratio of the original powder is 5:1, and the weight ratio of grinding balls with different diameters is: 40mm:30mm:20mm=3:5:1; the grinding time is 5 hours.
[0022] The beneficial effects of the present invention are:
[0023] The present invention adopts industrial alumina and additives to be mixed evenly and then placed in a tunnel kiln or a shuttle kiln for calcination; the calcination temperature is 1250±50°C and the calcination time is 3-7 hours; the calcined clinker is crushed and screened to obtain a light-burned α-alumina for low-sodium special glass of required particle size, and its performance index α-phase conversion rate is 96-98%; Na 2 O<0.02%; crystal 0.3-0.8μm.
[0024] The present invention first adds a de-sodium agent for pretreatment, and combines the dispersing effect of an emulsifier to increase the dissolution rate of intercrystalline alkali in alumina. After a period of dissolution, aluminum hydroxide is added to the system, and aluminum hydroxide can form polyaluminum chloride with the de-sodium agent. According to the flocculation and ion exchange of polyaluminum chloride, the dissolution of sodium ions in alumina is further promoted. In addition, the emulsifier used in the present application can delay or block the behavior of polymers with electron layers in the structure of polyaluminum chloride to attract each other, thereby preventing the polyaluminum chloride polymer from agglomerating through charge action; at the same time, it plays the role of re-dispersing the polyaluminum chloride that has been agglomerated, thereby effectively delaying or preventing the occurrence of gelation of the polyaluminum chloride solution, and then obtaining aluminum chloride with ultra-low sodium content. Compared with directly adding polyaluminum chloride in the system, the preparation method of the present invention can obtain a product with a lower sodium content, and the calcination temperature is low and the energy consumption is low.
[0025] Compared with the current similar production processes, the mineralizer used in the present invention is pollution-free, the product purity is high, no harmful gas and solid emissions are generated, and at the same time, the production cost is low, the product purity is high, and the particle size distribution is reasonable, which can increase the chemical stability of special glass. The original crystal particles are 0.3-0.8μm, and have the characteristics of good grindability, easy sintering, good electrical insulation performance, good original crystal sphericity, narrow particle size distribution, good fluidity, etc. DETAILED DESCRIPTION
[0026] The following embodiments of the present invention are described in detail. The following embodiments are exemplary and intended to be used to explain the present invention, but should not be construed as limiting the present invention.
[0027] It should be noted that the specific process parameters of industrial alumina used in the following examples of the present invention are shown in Table 1.
[0028]
[0029] The following is a specific implementation of this application:
[0030] Example 1
[0031] S1: Take industrial-grade alumina product, add 5% hydrochloric acid by weight of alumina and 1% polyoxyethylene nonylphenol ether by weight of alumina, respectively, and dissolve for 3 hours;
[0032] S2: After the dissolution in step S1 is completed, a certain amount of aluminum hydroxide is added into the system, aged, and filtered to obtain a filtrate and a filter cake; the molar ratio of hydrochloric acid to aluminum hydroxide is 1:1;
[0033] S3: calcining the filter cake obtained in step S2 at 1200° C. for 3 hours in a tunnel kiln or shuttle kiln, and then cooling;
[0034] S4: α-Al 2 O3 The raw powder was placed in a ball mill for grinding to obtain α-Al 2 O 3 Micro powder. Grinding balls and α-Al in the mill 2 O 3 The weight ratio of the original powder is 5:1, the weight ratio of grinding balls with different diameters is: 40mm:30mm:20mm=3:5:1, the grinding time is 5 hours, and a low-sodium light-burned α-alumina is obtained by sieving.
[0035] Example 2
[0036] S1: Take industrial-grade alumina product, add 10% hydrochloric acid by weight of alumina and 2% polyoxyethylene nonylphenol ether by weight of alumina, respectively, and dissolve for 4 hours;
[0037] S2: After the dissolution in step S1 is completed, a certain amount of aluminum hydroxide is added into the system, aged, and filtered to obtain a filtrate and a filter cake; the molar ratio of hydrochloric acid to aluminum hydroxide is 3:1;
[0038] S3: calcining the filter cake obtained in step S2 in a tunnel kiln or shuttle kiln at 1300° C. for 5 hours and then cooling;
[0039] S4: α-Al 2 O 3 The raw powder was placed in a ball mill for grinding to obtain α-Al 2 O 3 Micro powder, grinding balls and α-Al in mill 2 O 3 The weight ratio of the original powder is 5:1, the weight ratio of grinding balls with different diameters is: 40mm:30mm:20mm=3:5:1, the grinding time is 5 hours, and a low-sodium light-burned α-alumina is obtained by sieving.
[0040] Example 3
[0041] S1: Take industrial-grade alumina product, add 12% hydrochloric acid by weight of alumina and 3% polyoxyethylene nonylphenol ether by weight of alumina, respectively, and dissolve for 6 hours;
[0042] S2: After the dissolution in step S1 is completed, a certain amount of aluminum hydroxide is added into the system, aged and filtered to obtain a filtrate and a filter cake; the molar ratio of hydrochloric acid to aluminum hydroxide is 4:1;
[0043] S3: calcining the filter cake obtained in step S2 at 1250° C. in a tunnel kiln or shuttle kiln for 7 hours and then cooling;
[0044] S4: α-Al 2 O 3 The raw powder was placed in a ball mill for grinding to obtain α-Al 2 O3 Micro powder, grinding balls and α-Al in mill 2 O 3 The weight ratio of the original powder is 5:1, the weight ratio of grinding balls with different diameters is: 40mm:30mm:20mm=3:5:1, the grinding time is 5 hours, and a low-sodium light-burned α-alumina is obtained by sieving.
[0045] Comparative Example 1
[0046] S1: Take an industrial-grade alumina product and prepare it into a slurry; according to the amount of polyaluminium chloride formed in Example 2, mix the alumina with the polyaluminium chloride solution to obtain a mixed solution;
[0047] S2: calcining the filter cake obtained in step S2 in a tunnel kiln or a shuttle kiln at 1300° C. for 5 hours and then cooling;
[0048] S3: α-Al 2 O 3 The raw powder was placed in a ball mill for grinding to obtain α-Al 2 O 3 Micro powder, grinding balls and α-Al in mill 2 O 3 The weight ratio of the original powder is 5:1, the weight ratio of grinding balls with different diameters is: 40mm:30mm:20mm=3:5:1, the grinding time is 5 hours, and a low-sodium light-burned α-alumina is obtained by sieving.
[0049] Comparative Example 2
[0050] S1: Take industrial-grade alumina products and prepare them into slurry; add 2% polyoxyethylene nonylphenol ether into the system;
[0051] S2: According to the amount of polyaluminium chloride formed in Example 2, aluminium oxide is mixed with the polyaluminium chloride solution to obtain a mixed solution;
[0052] S3: calcining the filter cake obtained in step S2 in a tunnel kiln or shuttle kiln at 1300° C. for 5 hours and then cooling;
[0053] S3: α-Al 2 O 3 The raw powder was placed in a ball mill for grinding to obtain α-Al 2 O 3 Micro powder, grinding balls and α-Al in mill 2 O 3 The weight ratio of the original powder is 5:1, the weight ratio of grinding balls with different diameters is: 40mm:30mm:20mm=3:5:1, the grinding time is 5 hours, and a low-sodium light-burned α-alumina is obtained by sieving.
[0054] The relevant parameters of the low-sodium light-burned α-alumina prepared in Examples 1-3 of the present invention and Comparative Examples 1-2 were tested using a D / MAX-ULTIMA IV X-ray diffractometer. 2 O 3 The content of Na 2 O content was analyzed, and the results are shown in Table 2:
[0055]
[0056] It can be seen that the present invention first adds a de-sodium agent for pretreatment, and combines the dispersing effect of an emulsifier to increase the dissolution rate of intercrystalline alkali in alumina. After a certain period of dissolution, aluminum hydroxide is added to the system. Aluminum hydroxide can form polyaluminum chloride with the de-sodium agent. According to the flocculation and ion exchange effect of polyaluminum chloride, the dissolution of sodium ions in alumina is further promoted. In addition, the emulsifier used in the present application can delay or block the mutual attraction of polymers with electron layers in the structure of polyaluminum chloride, thereby preventing the polyaluminum chloride polymer from agglomerating through charge action; at the same time, it plays a role in re-dispersing the polyaluminum chloride that has been agglomerated, thereby effectively delaying or preventing the occurrence of gelation of the polyaluminum chloride solution, and then obtaining aluminum chloride with ultra-low sodium content. Compared with directly adding polyaluminum chloride to the system, the preparation method of the present invention can obtain a product with a lower sodium content.
[0057] Compared with the current similar production processes, the mineralizer used in the present invention is pollution-free, the product purity is high, no harmful gas and solid emissions are generated, the production cost is low, the product purity is high, the particle size distribution is reasonable, and the chemical stability of special glass can be increased. It has the characteristics of good grindability, easy sintering, good electrical insulation performance, good original crystal sphericity, narrow particle size distribution, good fluidity, etc.
[0058] It will be apparent to those skilled in the art that the present invention is not limited to the details of the exemplary embodiments described above and that the present invention can be implemented in other specific forms without departing from the spirit or essential features of the present invention. Therefore, the embodiments should be considered exemplary and non-restrictive in all respects, and the scope of the present invention is defined by the appended claims rather than the above description, and it is intended that all changes falling within the meaning and scope of the equivalent elements of the claims be included in the present invention.
Claims
1. A method for preparing low-sodium light-burned α-alumina, characterized in that: The steps include: S1: Take industrial-grade alumina products, add de-sodium agent and emulsifier, and dissolve for a period of time; the de-sodium agent is hydrochloric acid, and the amount of hydrochloric acid is 5%-12% of the mass of alumina; the emulsifier is polyoxyethylene nonylphenol ether; S2: After the dissolution in step S1 is completed, an alkali agent is added into the system, and the filtrate and filter cake are obtained by aging and filtering; the alkali agent is aluminum hydroxide, and the molar ratio of hydrochloric acid to aluminum hydroxide is 1-4:1; S3: calcining the filter cake obtained in step S2 and cooling it; S4: grinding and sieving to obtain a low-sodium light-burned α-alumina; The calcination temperature in step S3 is 1200-1300°C.
2. The method for preparing low-sodium light-burned α-alumina according to claim 1, characterized in that: The dissolution time in step S1 is: 3-6h.
3. The method for preparing low-sodium light-burned α-alumina according to claim 1, characterized in that: In step S1, the amount of polyoxyethylene nonylphenol ether added is 1-3% of the mass of aluminum oxide.
4. The method for preparing low-sodium light-burned α-alumina according to claim 1, characterized in that: The aging temperature in step S2 is 50-100° C. and the aging time is 1-3 hours.
5. The method for preparing low-sodium light-burned α-alumina according to claim 1, characterized in that: The calcination time in step S3 is 3-7h.
6. The method for preparing low-sodium light-burned α-alumina according to claim 1, characterized in that: The calcining equipment in step S3 is a tunnel kiln or a shuttle kiln.