A method for removing impurities from phosphogypsum

By using chlorine-containing oxidant heating reaction and ion ratio adjustment in phosphogypsum, combined with resin adsorption, the impurities in phosphogypsum were successfully removed, solving the problems of high energy consumption and low quality in phosphogypsum treatment, and achieving high purity and high whiteness. degree of gypsum preparation and efficient use of resources.

CN117125733BActive Publication Date: 2024-10-15YIDU XINGFA CHEMICAL CO LTD +1
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202310859597.4
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2023-07-13
Publication Date
2024-10-15
Estimated Expiration
2043-07-13

AI Technical Summary

Technical Problem

The existing technology has problems such as high energy consumption, complex processes, low quality and secondary pollution when processing phosphogypsum, which limits the effective utilization of phosphogypsum resources.

Method used

The chlorine-containing oxidant is used to heat the reaction, adjust the ion ratio and add crystal seeds for crystallization. Combined with resin adsorption, the impurities in the phosphogypsum are removed through physical and chemical methods to achieve whitening and purity of the phosphogypsum.

Benefits of technology

It achieves the preparation of high-purity, high-whiteness gypsum crystals, reduces energy consumption, simplifies the process, increases the gypsum recovery rate, and slows down the impact on the environment.

✦ Generated by Eureka AI based on patent content.
Patent Text Reader

Abstract

The invention provides a method for removing impurities from phosphogypsum. The main steps are: S1, placing phosphogypsum in a reaction container, adding a chlorine-containing oxidant for mixing, heating the reaction until the chloride ion content in the feed liquid is stable, filtering to obtain solid phase insolubles and a filtrate; S2, adjusting the ratio of alkali metal ions, aluminum ions and fluoride ions in the filtrate, adding seed crystals for crystallization, filtering to obtain fluoride and / or silicate precipitates, adding resin to the filtrate for mixing and adsorption, and separating to obtain a clear liquid; S3, adjusting the ratio of calcium ions and sulfate ions in the clear liquid, concentrating and then crystallizing, filtering, and obtaining crystals of calcium sulfate dihydrate.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of phosphogypsum processing, and particularly relates to a method for removing impurities from phosphogypsum. Background Art

[0002] Phosphogypsum is an industrial by-product gypsum containing a variety of impurities. Its main component is CaSO4 dihydrate, and it also contains a small amount of water-soluble phosphorus, fluorine compounds, metal oxides, organic matter and other impurities. It is strongly acidic and has a high water content. Among them, the impurity phosphorus, when used as a cement additive, will delay the coagulation and hardening of cement, reduce the early strength of cement and the strength of gypsum products. However, fluorine compounds make it unusable in building materials such as gypsum boards, and the presence of impurities such as metal oxides and organic matter makes it gray-black. In short, the presence of various impurities greatly limits its application and becomes a bottleneck restricting the healthy and sustainable development of the industry.

[0003] Patent application 201410135538.3 discloses a method for preparing calcium sulfate dihydrate whiskers from phosphogypsum, which is only applicable to the preparation of calcium sulfate dihydrate whiskers. The method also involves heating treatment, which has relatively high energy consumption and a complex process flow. Patent application 201710322103.3 discloses a method for preparing anhydrous calcium sulfate whiskers from industrial by-product phosphogypsum. The preparation of anhydrous phosphogypsum is achieved through the action of complex chemical reagents and the use of strong alkaline substances such as quicklime, but the purification process is not optimized.

[0004] The above scheme can consume and utilize the phosphogypsum inventory to a certain extent, but there are still many difficulties, such as large investment in treatment process, high energy consumption, small treatment volume, difficulty in solving secondary pollution, and the quality of the treated phosphogypsum is still low. Therefore, in order to solve the practical problem of phosphogypsum resource utilization, it is urgent to seek new methods in terms of technology, cost and product quality. Summary of the invention

[0005] The invention provides a method for removing impurities from phosphogypsum, which is simple to operate and can quickly remove impurities in the phosphogypsum and improve its quality.

[0006] The technical solution of the present invention is a method for removing impurities from phosphogypsum, comprising the following steps:

[0007] S1, placing phosphogypsum in a reaction container, adding a chlorine-containing oxidant to mix, heating to react for a certain period of time, and filtering to obtain a solid phase insoluble matter and a filtrate 1;

[0008] S2, adjusting the ratio of alkali metal ions, aluminum ions and fluoride ions in the filtrate, adding seed crystals for crystallization, filtering to obtain fluoride and / or silicate precipitates, adding resin to the filtrate for mixing and adsorption, and separating to obtain a clear liquid;

[0009] S3. Adjust the ratio of calcium ions to sulfate ions in the clear solution, concentrate and crystallize it, filter it, and obtain the crystals of calcium sulfate dihydrate.

[0010] Furthermore, the chlorine-containing oxidant is chlorine water, hypochlorous acid, hypochlorite, or a mixture of hydrochloric acid and hypochlorous acid; and its added amount is 0.5 to 1.0 times the mass of gypsum.

[0011] Furthermore, in S1, the reaction time is 1-2 hours after the addition of the chlorine-containing oxidant, and the reaction temperature is controlled at 70°C to 80°C.

[0012] Furthermore, the reaction container in S1 is a light-transmitting container, and illumination is performed during the reaction, with the illumination intensity being 500 lux to 1000 lux.

[0013] Furthermore, the molar ratio of alkali metal ions, aluminum ions and fluoride ions in S2 is 1-3:1:4-6.

[0014] Furthermore, the seed crystal in S2 is fluorite, potassium feldspar, sodium feldspar or aluminum fluoride.

[0015] Furthermore, the resin in S2 is a cation exchange resin or a chelating resin or a mixture of the two in any ratio.

[0016] Furthermore, the molar ratio of calcium ions to sulfate ions in S3 is 1:1.1-1.5.

[0017] Further, S3 is evaporated and crystallized under vacuum conditions, with a specific vacuum degree of -50 kPa to -70 kPa.

[0018] Furthermore, the evaporation temperature of S3 is 80-85°C.

[0019] The present invention utilizes chemical and physical methods to remove the main ionic impurities in phosphogypsum and realize whitening of phosphogypsum. Through the oxidation and bleaching effect of a chlorine-containing oxidant such as chlorine water or hypochlorous acid, part of the black matter (mainly organic impurities) in the phosphogypsum can be removed, and the phosphogypsum can be dissolved by converting it into hydrochloric acid through light. The reaction principle is as follows: (1). By adjusting the molar ratio between the ions, a composite precipitate can be formed between the alkali metal ions, the aluminum ions and the fluoride ions. The reaction principle is as follows: (2) (3). The system is preliminarily purified. The resin can adsorb all the iron ions and a small amount of residual aluminum ions, and the solution is basically colorless. Finally, gypsum crystals with less impurity content and high whiteness are obtained by evaporation and cooling.

[0020] CaSO4·2H2O+HCl→Ca 2+ +Cl - +SO4 2- +2H2O (1)

[0021] Al 3+ +3F - →AlF3↓ (2)

[0022] 3Na + +Al 3+ +6F - →Na3AlF6↓ (3)

[0023] The present invention has the following beneficial effects:

[0024] The present invention adopts a method combining physics and chemistry to prepare high-purity and high-whiteness gypsum crystals, with a high gypsum recovery rate, simple process operation, no need for high-pressure and high-temperature reaction equipment, and low energy consumption. The solid generated in the process can be used for phosphate fertilizer production, and the liquid can be recycled as a reactant, which greatly reduces the impact of phosphogypsum on the environment. DETAILED DESCRIPTION

[0025] The embodiments of the present invention will be described in detail below with reference to examples, but those skilled in the art will appreciate that the following examples are only used to illustrate the present invention and should not be construed as limiting the scope of the present invention.

[0026] Example 1 Take 1000g of phosphogypsum in a sealed light-transmitting container, add 1000g of hypochlorous acid solution (5wt%), keep the container in a sealed state, light intensity of 800 lux, react for 1 hour and filter, obtain silicon-containing solid phase insoluble matter and sodium, aluminum, fluoride ion A solution. Adjust the molar ratio of alkali metal ions, aluminum ions and fluoride ions in solution A to 3:1:6, add fluorine aluminum sodium magnesium ore, slowly stir and react at 60°C for 2h and then filter, obtain fluorine aluminum precipitate and low sodium, aluminum, fluoride ion B solution. Mix solution B with D001 type cation exchange resin, stir and contact at 50°C for 3h, separate and obtain clear solution C containing calcium, chloride ions and sulfate. The molar ratio of sulfate to calcium ion in solution C was adjusted to 1.4:1, and the solution was evaporated and crystallized under vacuum conditions. After crystals appeared, the evaporation was stopped and the temperature was slowly lowered to 25°C. The precipitated crystals were calcium sulfate dihydrate with low impurities. The purity was determined to be 98%, the blue light whiteness was 69, and the yield was 95%.

[0027] Example 2 1000g of phosphogypsum was placed in a sealed light-transmitting container, and 1000g of hypochlorous acid solution (5wt%) was added. The container was kept sealed, and the light intensity was 500 lux. The reaction was carried out for 1 hour and filtered to obtain a solid phase insoluble matter containing silicon and a solution A containing sodium, aluminum and fluoride ions. The molar ratio of alkali metal ions, aluminum ions and fluoride ions in the solution A was adjusted to 3:1:6, and fluoroaluminum sodium magnesium ore was added. The reaction was slowly stirred at 60°C for 2h and then filtered to obtain a precipitate containing fluorine and aluminum and a solution B containing relatively low sodium, aluminum and fluoride ions. The solution B was mixed with D001 cation exchange resin, stirred and contacted at 50°C for 3h, and a clear solution C containing calcium, chloride ions and sulfate was separated. The molar ratio of sulfate to calcium ion in solution C was adjusted to 1.4:1, and the solution was evaporated and crystallized under vacuum conditions. After crystals appeared, the evaporation was stopped and the temperature was slowly lowered to 25°C. The precipitated crystals were low-impurity calcium sulfate dihydrate, which was measured to have a purity of 97%, a blue light whiteness of 67, and a yield of 90%.

[0028] Example 3 1000g of phosphogypsum was placed in a sealed light-transmitting container, and 1000g of hypochlorous acid solution (5wt%) was added. The container was kept sealed, and the light intensity was 500 lux. The reaction was carried out for 1 hour and filtered to obtain a solid phase insoluble matter containing silicon and a solution A containing sodium, aluminum and fluoride ions. The molar ratio of alkali metal ions, aluminum ions and fluoride ions in the solution A was adjusted to 1:1:4, and fluoroaluminum sodium magnesium ore was added. The reaction was slowly stirred at 60°C for 2h and then filtered to obtain a precipitate containing fluorine and aluminum and a solution B containing relatively low sodium, aluminum and fluoride ions. The solution B was mixed with D001 cation exchange resin, stirred and contacted at 50°C for 3h, and a clear solution C containing calcium, chloride ions and sulfate was separated. The molar ratio of sulfate to calcium ion in solution C was adjusted to 1.4:1, and the solution was evaporated and crystallized under vacuum conditions. After crystals appeared, the evaporation was stopped and the temperature was slowly lowered to 25°C. The precipitated crystals were calcium sulfate dihydrate with low impurities. The purity was determined to be 90%, the blue light whiteness was 65, and the yield was 93%.

[0029] Example 4 1000g of phosphogypsum was placed in a sealed light-transmitting container, and 1000g of hypochlorous acid solution (5wt%) was added. The container was kept sealed, and the light intensity was 1000 lux. The reaction was carried out for 1 hour and filtered to obtain a solid phase insoluble matter containing silicon and a solution A containing sodium, aluminum and fluoride ions. The molar ratio of alkali metal ions, aluminum ions and fluoride ions in the solution A was adjusted to 1:1:6, aluminum fluoride was added, and the reaction was slowly stirred at 60°C for 2h and then filtered to obtain a precipitate containing aluminum fluoride and a solution B containing relatively low sodium, aluminum and fluoride ions. The solution B was mixed with D001 cation exchange resin, and stirred and contacted at 50°C for 3h to separate and obtain a clear solution C containing calcium, chloride ions and sulfate. The molar ratio of sulfate to calcium ion in solution C was adjusted to 1.4:1, and the solution was evaporated and crystallized under vacuum conditions. After crystals appeared, the evaporation was stopped and the temperature was slowly lowered to 25°C. The precipitated crystals were low-impurity calcium sulfate dihydrate, which was measured to have a purity of 96%, a blue light whiteness of 68, and a yield of 92%.

[0030] Example 5 1000g of phosphogypsum was placed in a sealed light-transmitting container, and 1000g of hypochlorous acid solution (5wt%) was added. The container was kept sealed, and the light intensity was 1000 lux. The reaction was carried out for 1 hour and filtered to obtain a solid phase insoluble matter containing silicon and a solution A containing sodium, aluminum, and fluoride ions. The molar ratio of alkali metal ions, aluminum ions, and fluoride ions in the solution A was adjusted to 2:1:5, and aluminum fluoride was added. The reaction was slowly stirred at 60°C for 2h and then filtered to obtain a precipitate containing aluminum fluoride and a solution B containing relatively low sodium, aluminum, and fluoride ions. The solution B was mixed with D001 cation exchange resin, stirred and contacted at 50°C for 3h, and a clear solution C containing calcium, chloride ions, and sulfate was separated. The molar ratio of sulfate to calcium ion in solution C was adjusted to 1.4:1, and the solution was evaporated and crystallized under vacuum conditions. After crystals appeared, the evaporation was stopped and the temperature was slowly lowered to 25°C. The precipitated crystals were low-impurity calcium sulfate dihydrate, which was measured to have a purity of 93%, a blue light whiteness of 65, and a yield of 93%.

[0031] Comparative Example 1: Based on Example 1, the difference is that the oxidant hydrogen peroxide is added, and the other conditions and steps remain unchanged. Finally, calcium sulfate dihydrate is obtained with a purity of 20%, a blue light whiteness of 63, and a yield of 1%.

[0032] Comparative Example 2: Based on Example 1, the difference is that the amount of hypochlorous acid solution added is 100g, and other conditions and steps remain unchanged. The purity is 93%, the blue light whiteness is 65, and the yield is 32%.

[0033] Comparative Example 3: Based on Example 1, the difference is that the molar ratio of alkali metal ions, aluminum ions and fluoride ions is 1:1:1, and other conditions and steps remain unchanged. The purity is 85%, the blue light whiteness is 60, and the yield is 93%.

[0034] Comparative Example 4: Based on Example 1, the difference is that no illumination condition is provided, and other conditions and steps remain unchanged. The purity is measured to be 93%, the blue light whiteness is 60, and the yield is 5%.

[0035] The above embodiments are only for illustrating the technical ideas and features of the present invention, and the contents are only preferred embodiments of the present invention, but the protection scope of the present invention is not limited thereto. Within the technical scope disclosed by the present invention, equivalent changes or improvements made according to the technical solution and inventive concept of the present invention should be included in the protection scope of the present invention.

Claims

1. A method for removing impurities from phosphogypsum, characterized in that: The following steps are involved: S1. Place phosphogypsum in a reaction container, add hypochlorous acid solution to mix, heat at 70°C to 80°C to react for 1-2 hours, use a light-transmitting container as the reaction container, illuminate during the reaction, and the illumination intensity is 500 lux to 1000 lux. After the reaction, filter to obtain the solid insoluble matter and filtrate 1; the amount of hypochlorous acid added is 0.5 to 1.0 times the mass of gypsum; S2, adjusting the molar ratio of alkali metal ions, aluminum ions and fluoride ions in the filtrate to 1-3:1:4-6, adding seed crystals for crystallization, filtering to obtain fluoride and / or silicate precipitates, adding resin to the filtrate for mixing and adsorption, and separating to obtain a clear liquid; S3. Adjust the ratio of calcium ions to sulfate ions in the clear solution, concentrate and crystallize it, filter it, and obtain the crystals of calcium sulfate dihydrate.

2. The method according to claim 1, characterized in that: The seed crystal in S2 is dawsonite or sodium fluoroaluminate or aluminum fluoride.

3. The method according to claim 1, characterized in that: The resin in S2 is a cation exchange resin or a chelating resin or a mixture of the two in any ratio.

4. The method according to claim 1, characterized in that: The molar ratio of calcium ions to sulfate ions in S3 is 1:1.1-1.

5.

5. The method according to claim 1, characterized in that: S3 is evaporated and crystallized under vacuum conditions, with a specific vacuum degree of -50 kpa to -70 kpa.

6. The method according to claim 1, characterized in that: S3 is evaporated and concentrated, and the evaporation temperature is 80-85℃.