A method for preparing titanium niobium oxide by co-dissolution and co-precipitation
By reacting titanium dioxide and niobium pentoxide in KOH submolten salt, adjusting the pH value to co-precipitate titanium and niobium and calcining it, the problem of complex and high cost preparation process of titanium niobium oxide is solved, and low cost, high yield and high cost are achieved. Preparation of titanium niobium oxide with excellent electrochemical properties, suitable for use as anode material for lithium-ion batteries.
Patent Information
- Application Number
- CN202311397513.6
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2023-10-25
- Publication Date
- 2024-10-29
- Estimated Expiration
- 2043-10-25
AI Technical Summary
Existing preparation methods for titanium niobium oxide (TNO) have problems such as complex processes, high costs, and difficulty in large-scale production. In particular, the solvothermal/hydrothermal method has low yield, and the electrospinning method uses toxic solvents and has complicated processes. .
The co-solution and co-precipitation method is used to react titanium dioxide and niobium pentoxide in KOH sub-molten salt, adjust the pH value to co-precipitate titanium and niobium, and then calcine to obtain titanium niobium oxide. This method uses traditional oxide raw materials, which are easily available and cheap, and the process conditions are mild, making it suitable for large-scale production.
The preparation of titanium niobium oxide with low cost and high yield has been achieved. The product particles have been refined and have excellent electrochemical properties. They are suitable for use as negative electrode materials for lithium-ion batteries.
Smart Images

Figure CN117566795B_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of batteries, and in particular to a method for preparing titanium niobium oxide by co-dissolution and co-precipitation. Background Art
[0002] As a negative electrode material for lithium-ion batteries, titanium niobium oxide (TNO) has the advantages of high safety and high capacity. However, the current preparation methods of TNO have more or less some problems. The solid phase method usually uses traditional ball milling mixing, which has high yield, but the particle size of the synthesized product is large, the uniformity is poor, and the electrochemical performance lacks commercial competitiveness; the biggest problem with the solvothermal / hydrothermal method for synthesizing TNO is that its yield is low and it is difficult to apply to actual industrial production; the sol-gel method usually uses niobium chloride or niobium ethanol as the niobium source, titanium isopropoxide or tetrabutyl titanate as the titanium source, the raw material price is relatively expensive, the chemical properties are unstable, and the preparation cost is high; the electrospinning method often requires the use of toxic solvents, and its process is relatively complicated, making it difficult to use for large-scale production. Summary of the invention
[0003] The purpose of the present invention is to provide a method for preparing titanium niobium oxide by co-dissolution and co-precipitation, so as to solve the technical problems in the prior art that the preparation process of titanium niobium oxide (TNO) is complicated, the preparation cost is high, and it is difficult to be used for large-scale production.
[0004] The present invention discloses a method for preparing titanium niobium oxide by co-dissolution and co-precipitation, comprising the following steps:
[0005] S1, adding titanium dioxide and niobium pentoxide into KOH sub-molten salt for reaction;
[0006] S2, washing the product obtained in step S1, and centrifuging to obtain a solid phase byproduct and a washing liquid;
[0007] S3, adding acid to the washing liquid obtained in step S2 to co-precipitate titanium and niobium to obtain a precipitate, separating the precipitate from the solid and liquid, and drying to obtain a solid powder;
[0008] S4, calcining the solid powder obtained in step S3 to obtain titanium niobium oxide.
[0009] Furthermore, in step S1, the molar ratio of titanium dioxide to niobium pentoxide is 1:12 to 1:1.
[0010] Furthermore, in step S1, the alkali-ore ratio is 1:5 to 20:1, and the alkali-ore ratio is the mass ratio of KOH plus the sum of the masses of titanium dioxide and niobium pentoxide.
[0011] Furthermore, the initial KOH mass percentage (the mass ratio of KOH to the sum of the mass of KOH and the mass of water) of the KOH sub-molten salt is 40-90%.
[0012] Furthermore, in step S1, the reaction temperature is 100-350° C., and the reaction time is 1-10 h.
[0013] Furthermore, in step S2, the pH of the washing solution is >13.
[0014] Furthermore, in step S3, the acid is hydrochloric acid, nitric acid or sulfuric acid.
[0015] Furthermore, in step S3, the washing liquid is adjusted to pH=1-6.
[0016] Furthermore, in step S4, the calcination conditions are calcination in an air atmosphere, the calcination temperature is 700-1500° C., preferably the calcination temperature is 600-900° C., the calcination time is 1-24 hours, preferably the calcination time is 1-12 hours.
[0017] Furthermore, after calcining in air atmosphere, sintering is performed in protective atmosphere, the sintering temperature is 700-1400° C., and the time is 1-48 hours; the protective atmosphere is argon, nitrogen or hydrogen in argon.
[0018] Furthermore, in the step S4, the calcination is followed by crushing.
[0019] Furthermore, the crushing process includes one or more of ball milling, air flow milling and sand milling.
[0020] A titanium niobium oxide is prepared by using the above method.
[0021] An application of titanium niobium oxide for preparing lithium-ion batteries.
[0022] Furthermore, it is used to prepare negative electrode materials for lithium-ion batteries.
[0023] Compared with the prior art, the present invention has the following beneficial effects:
[0024] 1. The method for preparing titanium niobium oxide by co-dissolution and co-precipitation of the present invention uses traditional titanium and niobium oxides, and the raw materials are easily available and cheap, which is a low-cost synthesis method. The preparation process has low equipment requirements, mild reaction conditions, good repeatability, and can ensure a high yield;
[0025] 2. The method for preparing titanium niobium oxide by co-dissolution and co-precipitation of the present invention utilizes the high activity of sub-molten salt to achieve co-dissolution of titanium oxide and niobium oxide, adjusts the pH to achieve co-precipitation, and achieves the effect of molecular-level homogeneous mixing and refined particles. The final calcined product has good performance consistency and is expected to obtain relatively excellent electrochemical properties. BRIEF DESCRIPTION OF THE DRAWINGS
[0026] In order to more clearly illustrate the technical solutions of the embodiments of the present invention, the drawings required for use in the embodiments are briefly introduced below. It should be understood that the following drawings only represent some embodiments of the present invention and therefore should not be regarded as limiting the scope. For ordinary technicians in this field, other related drawings can be obtained based on these drawings without creative work.
[0027] Figure 1 These are the XRD test results of the titanium-niobium ratios of 1:2, 1:6 and 1:12 in Example 1 of the present invention.
[0028] Figure 2 These are the XRD test results of the alkali-ore ratio of 3:1 and the alkali-ore ratio of 1:1 in Example 2 of the present invention.
[0029] Figure 3 This is the SEM test result of the alkali-ore ratio of 1:1 in Example 2 of the present invention.
[0030] Figure 4 This is the EDS test result of the alkali-ore ratio of 1:1 in Example 2 of the present invention.
[0031] Figure 5 This is the TG-DSC test result of the alkali-ore ratio of 1:1 in Example 2 of the present invention.
[0032] Figure 6 These are the XRD test results of by-product-220, by-product-200, and by-product-180 in Example 3 of the present invention.
[0033] Figure 7 These are the XRD test results of TNO-900, TNO-800 and TNO-700 in Example 4 of the present invention.
[0034] Figure 8 This is the SEM test result of TNO-800 in Example 4 of the present invention.
[0035] Fig. 9 This is the SEM test result of TNO-900 in Example 4 of the present invention.
[0036] Fig.10 These are the rate performance test results of TNO-900 and TNO-800 in Example 4 of the present invention.
[0037] Fig.11 These are the SEM and XRD test results of TNO-1h, TNO-3h and TNO-5h in Example 5 of the present invention.
[0038] Fig.12 These are the rate performance test results of TNO-1h, TNO-3h and TNO-5h in Example 5 of the present invention.
[0039] Fig.13 This is the SEM test result of A-TNO in Example 6 of the present invention.
[0040] Fig.14 This is the SEM test result of B-TNO in Example 6 of the present invention.
[0041] Fig.15 These are the rate performance test results of A-TNO and B-TNO in Example 6 of the present invention. DETAILED DESCRIPTION
[0042] In order to make the purpose, technical solutions and advantages of the embodiments of the present invention clearer, the technical solutions in the embodiments of the present invention are clearly and completely described below. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments.
[0043] Example 1
[0044] KOH Sub-molten Salt Reactions of Titanium Dioxide and Niobium Pentoxide with Different Titanium-Nibium Ratios
[0045] 12g potassium hydroxide and 3ml deionized water were placed in a polytetrafluoroethylene liner, and then 0.5545g titanium dioxide and 1.8455g niobium pentoxide were added. The oil bath was heated to 220°C, and magnetic stirring was turned on at 800rpm, and the temperature was kept for 2h. The reaction product was washed with deionized water, and the solid phase by-product and washing liquid were obtained by centrifugation. The solid phase by-product was dried at 75°C for 12h. Nitric acid was added to the washing liquid under stirring until the pH was <4, the precipitate was centrifuged, and the precipitate was washed with deionized water and anhydrous ethanol to obtain a solid phase product. The solid phase product was dried at 75°C for 12h to obtain a calcined precursor, and then calcined at 900°C for 3h to obtain titanium niobium oxide. The number is titanium niobium ratio 1:2.
[0046] 12g potassium hydroxide and 3ml deionized water were placed in a polytetrafluoroethylene liner, and then 0.2185g titanium dioxide and 2.1815g niobium pentoxide were added. The oil bath was heated to 220°C, and magnetic stirring was turned on at 800rpm, and the temperature was kept for 2h. The reaction product was washed with deionized water, and the solid phase by-product and washing liquid were obtained by centrifugation. The solid phase by-product was dried at 75°C for 12h. Nitric acid was added to the washing liquid under stirring until the pH was <4, the precipitate was centrifuged, and the precipitate was washed with deionized water and anhydrous ethanol to obtain a solid phase product. The solid phase product was dried at 75°C for 12h to obtain a calcined precursor, and then calcined at 900°C for 3h to obtain titanium niobium oxide. The number is titanium niobium ratio 1:6.
[0047] 12g potassium hydroxide and 3ml deionized water were placed in a polytetrafluoroethylene liner, and then 0.1093g titanium dioxide and 2.1815g niobium pentoxide were added. The oil bath was heated to 220°C, and magnetic stirring was turned on at 800rpm, and the temperature was kept for 2h. The reaction product was washed with deionized water, and the solid phase by-product and washing liquid were obtained by centrifugation. The solid phase by-product was dried at 75°C for 12h. Nitric acid was added to the washing liquid under stirring until the pH was <4, the precipitate was centrifuged, and the precipitate was washed with deionized water and anhydrous ethanol to obtain a solid phase product. The solid phase product was dried at 75°C for 12h to obtain a calcined precursor, and then calcined at 900°C for 3h to obtain titanium niobium oxide. The number is titanium niobium ratio 1:12.
[0048] The XRD test results of the titanium-niobium ratio of 1:2, titanium-niobium ratio of 1:6 and titanium-niobium ratio of 1:12 in Example 1 are as follows: Figure 1 As shown, titanium dioxide is both a reactant and a catalyst in the process (see Comparative Example 1). As the ratio of titanium to niobium in the initial raw material decreases, niobium will generate a large amount of insoluble byproducts, and the soluble matter of niobium will decrease, resulting in a low yield of the final product and a low niobium content in the product, and lattice distortion. Among them, when the ratio of titanium to niobium in the initial raw material is 1:2, the target product closest to the diffraction peak of pure phase TiNb2O7 (PDF#70-2009) can be obtained, and the yield is relatively high.
[0049] Example 2
[0050] KOH Sub-molten Salt Reaction with Different Alkali-Ore Ratios
[0051] 6g potassium hydroxide and 1.5ml deionized water were placed in a polytetrafluoroethylene liner, and then 0.4621g titanium dioxide and 1.5379g niobium pentoxide were added. The oil bath was heated to 220°C, and magnetic stirring was turned on at 800rpm, and the temperature was kept for 2h. The reaction product was washed with deionized water, and the solid phase by-product and washing liquid were obtained by centrifugation. The solid phase by-product was dried at 75°C for 12h. Nitric acid was added to the washing liquid while stirring until the pH was <4, the precipitate was centrifuged, and the precipitate was washed with deionized water and anhydrous ethanol to obtain a solid phase product. The solid phase product was dried at 75°C for 12h to obtain a calcined precursor. The number is alkali-ore ratio 3:1.
[0052] 2g potassium hydroxide and 0.5ml deionized water were placed in a polytetrafluoroethylene liner, and then 0.4621g titanium dioxide and 1.5379g niobium pentoxide were added, and the oil bath was heated to 220°C, and the magnetic stirring was turned on at 800rpm, and the temperature was kept for 2h. The reaction product was washed with deionized water, and the solid phase by-product and washing liquid were obtained by centrifugation. The solid phase by-product was dried at 75°C for 12h. Nitric acid was added to the washing liquid while stirring until the pH was <4, the precipitate was centrifuged, and the precipitate was washed with deionized water and anhydrous ethanol to obtain a solid phase product, and the solid phase product was dried at 75°C for 12h to obtain a calcined precursor. The number is 1:1 for the alkali-ore ratio.
[0053] The XRD test results of the calcined precursors obtained with different alkali-ore ratios are shown in Figure 2 As shown, they all correspond to the amorphous state. Precursor morphology ( Figure 3 ) is mainly composed of irregular particles with a primary particle size of <100nm. Compared with the initial raw material, the particle size is significantly refined; compared with simple ball milling, the co-dissolution and co-precipitation method has an outstanding effect on the homogeneous mixing of elements.
[0054] Example 3
[0055] Different sub-molten salt reaction temperatures
[0056] 2g potassium hydroxide and 0.5ml deionized water were placed in a polytetrafluoroethylene liner, and then 0.4621g titanium dioxide and 1.5379g niobium pentoxide were added, and the oil bath was heated to 220°C, and the magnetic stirring was turned on at 800rpm, and the temperature was kept for 2h. The reaction product was washed with deionized water and centrifuged to obtain a solid by-product and a washing liquid. The solid by-product was dried at 75°C for 12h and numbered as by-product-220. Nitric acid was added to the washing liquid while stirring until the pH was <4, the precipitate was centrifuged, and the precipitate was washed with deionized water and anhydrous ethanol to obtain a solid product, and the solid product was dried at 75°C for 12h to obtain a calcined precursor.
[0057] 2g potassium hydroxide and 0.5ml deionized water were placed in a polytetrafluoroethylene liner, and then 0.4621g titanium dioxide and 1.5379g niobium pentoxide were added, and the oil bath was heated to 200°C, and the magnetic stirring was turned on at 800rpm, and the temperature was kept for 2h. The reaction product was washed with deionized water and centrifuged to obtain a solid by-product and a washing liquid. The solid by-product was dried at 75°C for 12h and numbered as by-product-200. Nitric acid was added to the washing liquid while stirring until the pH was <4, the precipitate was centrifuged, and the precipitate was washed with deionized water and anhydrous ethanol to obtain a solid product, and the solid product was dried at 75°C for 12h to obtain a calcined precursor.
[0058] 2g potassium hydroxide and 0.5ml deionized water were placed in a polytetrafluoroethylene liner, and then 0.4621g titanium dioxide and 1.5379g niobium pentoxide were added, and the oil bath was heated to 180°C, and the magnetic stirring was turned on at 800rpm, and the temperature was kept for 2h. The reaction product was washed with deionized water and centrifuged to obtain a solid by-product and a washing liquid. The solid by-product was dried at 75°C for 12h and numbered as by-product-180. Nitric acid was added to the washing liquid while stirring until the pH was <4, the precipitate was centrifuged, and the precipitate was washed with deionized water and anhydrous ethanol to obtain a solid product, and the solid product was dried at 75°C for 12h to obtain a calcined precursor.
[0059] The XRD test results of byproducts at different sub-molten salt reaction temperatures are as follows: Figure 6As shown, the by-product XRD diffraction peak obtained at 180°C mainly corresponds to the diffraction peak of the raw material niobium pentoxide, and the by-product yield is as high as 42.9% (calculated as niobium). The by-product XRD diffraction peak obtained at 220°C mainly corresponds to the diffraction peak of the insoluble potassium metaniobate. Temperature affects the reaction rate. As the temperature increases, the reaction rate accelerates. When reacting at 200°C for 2h, more soluble niobate can be generated, but it does not have time to be converted into potassium metaniobate. The by-product yield is the lowest (2.0%, calculated as niobium).
[0060] Example 4
[0061] TNO prepared at different calcination temperatures
[0062] 2g potassium hydroxide and 0.5ml deionized water were placed in a polytetrafluoroethylene liner, and then 0.4621g titanium dioxide and 1.5379g niobium pentoxide were added. The oil bath was heated to 200°C, and the magnetic stirring was turned on at 800rpm, and the temperature was kept for 2h. The reaction product was washed with deionized water, and the solid phase byproduct and washing liquid were obtained by centrifugation. The solid phase byproduct was dried at 75°C for 12h. Nitric acid was added to the washing liquid under stirring until the pH was <4, the precipitate was centrifuged, and the precipitate was washed with deionized water and anhydrous ethanol to obtain a solid phase product. The solid phase product was dried at 75°C for 12h to obtain a calcined precursor. The precursor was calcined at 900°C for 3h to obtain titanium niobium oxide, numbered TNO-900; the precursor was calcined at 800°C for 3h to obtain titanium niobium oxide, numbered TNO-800; the precursor was calcined at 700°C for 3h to obtain titanium niobium oxide, numbered TNO-700.
[0063] The XRD test results of titanium niobium oxides obtained at different calcination temperatures are as follows: Figure 7 As shown in the figure, the crystallinity of the calcined product improves with increasing temperature. As the temperature increases, the grains grow ( Figure 8 , Fig. 9 ), calcined at 900℃ for 3h, can ensure good crystallinity while having smaller grains, in the shape of short rods of 100-300nm ( Fig. 9 ). Compared with the calcination temperature (generally greater than 1000°C) and calcination time (generally greater than 12h) of traditional solid phase reactions, the gain is obvious.
[0064] The performance of the obtained titanium niobium oxide was tested by mixing the obtained TNO-800 or TNO-900 with conductive carbon black and PVDF, adding NMP as a solvent and coating it on copper foil to make an electrode sheet, and then assembling a half-cell with a lithium sheet as a counter electrode to measure its capacity and rate performance. The current density is defined as 1C = 300mA / g. The rate performance is as follows Fig.10 shown.
[0065] The test results of Example 4 are compared. Fig.10As shown, the results show that the rate performance of TNO-900 is significantly higher than that of TNO-800.
[0066] Example 5
[0067] TNO prepared with different calcination times
[0068] The precursor obtained in Example 4 was calcined at 900°C for 1 hour to obtain titanium niobium oxide, numbered TNO-1h; the precursor was calcined at 900°C for 3 hours to obtain titanium niobium oxide, numbered TNO-3h; the precursor was calcined at 900°C for 5 hours to obtain titanium niobium oxide, numbered TNO-5h. According to the test method of Example 4, the rate performance of titanium niobium oxide prepared with different calcination times was tested. The test results are shown in FIG. Fig.12 shown.
[0069] Comparison of the rate performance test results of Example 5 Fig.12 As shown, the results show that calcination at 900℃ for 3h has better rate performance.
[0070] Example 6
[0071] Ball milling TNO
[0072] 2g potassium hydroxide and 0.5ml deionized water were placed in a polytetrafluoroethylene liner, and then 0.4621g titanium dioxide and 1.5379g niobium pentoxide were added, the oil bath was heated to 200°C, magnetic stirring was turned on at 800rpm, and the temperature was kept for 2h. The reaction product was washed with deionized water to obtain a washing liquid, nitric acid was added to the washing liquid under stirring until the pH was <4, the precipitate was centrifuged, and the precipitate was washed with deionized water and anhydrous ethanol to obtain a solid phase product, and the solid phase product was dried at 75°C for 12h to obtain a calcined precursor. The precursor was calcined at 900°C for 3h to obtain titanium niobium oxide, numbered A-TNO; titanium niobium oxide was moistened with ethanol according to a ball-to-material ratio of 4:1, and ball-milled for 4h at 700rpm by a planetary ball mill to obtain ball-milled titanium niobium oxide, numbered B-TNO. The rate test method is as in Example 4.
[0073] Fig.13 This is the SEM photo of A-TNO. Fig.14 The SEM photo of B-TNO shows that the primary particle size does not change significantly after ball milling, but the agglomeration is reduced and the uniformity is improved. Fig.15 As shown, the results show that the capacity of titanium niobium oxide after ball milling is improved at different rates, among which the improvement effect is most obvious at 1C-20C.
[0074] Comparative Example 1
[0075] Sub-molten salt reaction of niobium pentoxide
[0076] Place 12g potassium hydroxide and 3ml deionized water in a polytetrafluoroethylene liner, then add 1.8455g niobium pentoxide, heat to 220°C in an oil bath, turn on magnetic stirring at 800rpm, and keep warm for 2h. Wash the reaction product with deionized water, and centrifuge to obtain solid by-products and washing liquid. Dry the solid by-products at 75°C for 12h. Add nitric acid to the washing liquid while stirring until the pH is <4, and no precipitate is generated.
[0077] The difference between this comparative example and Example 1 is that no titanium dioxide raw material is added. In Comparative Example 1, niobium pentoxide mainly generates potassium metaniobate as a byproduct, and no soluble niobate is generated (or the amount generated is extremely low), resulting in no precipitation when the washing liquid is acidified.
[0078] Comparative Example 2
[0079] Alkali-ore ratio 0.6:1
[0080] Place 1.2g potassium hydroxide and 0.3ml deionized water in a polytetrafluoroethylene liner, then add 0.4621g titanium dioxide and 1.5379g niobium pentoxide, heat the oil bath to 220°C, turn on the magnetic stirring at 800rpm, and keep warm for 2h. Wash the reaction product with deionized water, and centrifuge to obtain solid by-products and washing liquid. The solid by-products are dried at 75°C for 12h. Add nitric acid to the washing liquid while stirring until the pH is <4, centrifuge the precipitate, wash the precipitate with deionized water and anhydrous ethanol to obtain a solid product, and dry the solid product at 75°C for 12h to obtain a calcined precursor.
[0081] Comparative Example 3
[0082] Alkali-ore ratio 5:1
[0083] Place 10g potassium hydroxide and 2.5ml deionized water in a polytetrafluoroethylene liner, then add 0.4621g titanium dioxide and 1.5379g niobium pentoxide, heat the oil bath to 220°C, turn on the magnetic stirring at 800rpm, and keep warm for 2h. Wash the reaction product with deionized water, and centrifuge to obtain solid by-products and washing liquid. The solid by-products are dried at 75°C for 12h. Add nitric acid to the washing liquid while stirring until the pH is <4, centrifuge the precipitate, wash the precipitate with deionized water and anhydrous ethanol to obtain a solid product, and dry the solid product at 75°C for 12h to obtain a calcined precursor.
[0084] The difference between Comparative Examples 2 and 3 and Example 2 is that the amount of KOH used is different. The by-product phase in Comparative Example 2 mainly corresponds to the diffraction peak of the raw material niobium pentoxide. The small amount of KOH used results in an insufficient sub-molten salt environment and a slow reaction rate. The by-product yield and precipitate yield of Comparative Example 3 are not much different from those of Example 2 in which the alkali-ore ratio is 3:1, but the amount of nitric acid used is more, indicating that most of the KOH is wasted. The alkali-ore ratio of 1:1 in Example 2 has the highest yield of the target product.
[0085] Comparative Example 4
[0086] 170℃ sub-molten salt reaction temperature
[0087] Place 12g potassium hydroxide and 3ml deionized water in a polytetrafluoroethylene liner, then add 1.8455g niobium pentoxide, heat to 170°C in an oil bath, turn on magnetic stirring at 800rpm, and keep warm for 2h. Wash the reaction product with deionized water, and centrifuge to obtain solid by-products and washing liquid. Dry the solid by-products at 75°C for 12h. Add nitric acid to the washing liquid while stirring until the pH is <4, and no precipitate is generated.
[0088] The difference between this comparative example and comparative example 1 is that the sub-molten salt reaction temperature is lower. In comparative example 4, niobium pentoxide mainly generates potassium metaniobate (close to 100%) as a byproduct, and niobium pentoxide does not react at a sub-molten salt temperature of 170°C.
[0089] The above are the implementation methods listed in this embodiment, but this embodiment is not limited to the above optional implementation methods. Those skilled in the art can arbitrarily combine the above methods to obtain other various implementation methods. Anyone can derive other various forms of implementation methods under the inspiration of this embodiment. The above specific implementation methods should not be understood as limiting the scope of protection of this embodiment. The scope of protection of this embodiment shall be based on the definition in the claims, and the description can be used to interpret the claims.
Claims
1. A method for preparing titanium niobium oxide by co-dissolution and co-precipitation, characterized in that: The steps include: S1, adding titanium dioxide and niobium pentoxide into KOH molten salt respectively, heating and stirring, and then keeping the temperature; S2, washing the product obtained in step S1, and centrifuging to obtain a solid phase byproduct and a washing liquid; S3, adding acid to the washing liquid obtained in step S2 to co-precipitate titanium and niobium to obtain a precipitate, separating the precipitate from the solid and liquid, and drying to obtain a solid powder; S4, calcining the solid powder obtained in step S3 to obtain titanium niobium oxide; In step S1, the reaction temperature is 200-350°C.
2. The method for preparing titanium niobium oxide by co-dissolution and co-precipitation according to claim 1, characterized in that: In the step S1, the molar ratio of titanium dioxide to niobium pentoxide is 1:12 to 1:
1.
3. The method for preparing titanium niobium oxide by co-dissolution and co-precipitation according to claim 1, characterized in that: The initial KOH mass percentage of the KOH sub-molten salt is 40-90%.
4. The method for preparing titanium niobium oxide by co-dissolution and co-precipitation according to claim 1, characterized in that: In the step S1, the alkali-ore ratio is 1:5-20:1, and the alkali-ore ratio is the mass ratio of KOH plus the sum of the masses of titanium dioxide and niobium pentoxide.
5. The method for preparing titanium niobium oxide by co-dissolution and co-precipitation according to claim 1, characterized in that: In step S1, the reaction temperature is 200-220° C., and the reaction time is 1-10 h.
6. The method for preparing titanium niobium oxide by co-dissolution and co-precipitation according to claim 1, characterized in that: In the step S4, the calcination conditions are calcination in an air atmosphere, the calcination temperature is 700 to 1500° C., and the calcination time is 1 to 24 hours.
7. The method for preparing titanium niobium oxide by co-dissolution and co-precipitation according to claim 6, characterized in that: In the step S4, the calcination conditions are calcination in an air atmosphere, the calcination temperature is 700-900° C., and the calcination time is 1-12 hours.
8. The method for preparing titanium niobium oxide by co-dissolution and co-precipitation according to claim 6 or 7, characterized in that: After calcining in air atmosphere, sintering is performed in protective atmosphere, the sintering temperature is 700-1400° C., and the sintering time is 1-48 hours; the protective atmosphere is argon, nitrogen or hydrogen in argon.
9. The method for preparing titanium niobium oxide by co-dissolution and co-precipitation according to claim 1, characterized in that: In the step S4, the calcination is followed by crushing.
Citation Information
Patent Citations
Preparation method for nano titanium niobate
CN105470508A
Preparation method for nanometer niobium pentoxide powder for lithium ion battery cathode material
CN105712403A
Carbon-coated niobium-doped modified titanium niobate material and preparation method thereof
CN112736250A