A method for improving the electrical conductivity of amorphous oxide on the surface of pure iron sheet and its application

By applying weak magnetic field and magnet slip technology on the surface of pure iron sheets, the conductivity of amorphous oxide films is improved, and the problem of low heavy metal removal efficiency in traditional technology is solved, achieving a more efficient heavy metal removal effect.

CN118028807BActive Publication Date: 2024-11-22TIANHE COLLEGE GUANGDONG POLYTECHNIC NORMAL UNIV
View PDF 4 Cites 0 Cited by

Patent Information

Application Number
CN202311855370.9
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2023-12-29
Publication Date
2024-11-22
Estimated Expiration
2043-12-29

AI Technical Summary

Technical Problem

In traditional large-size zero-valent iron treatment technology, the low conductivity of the amorphous oxide film hinders electron transport, resulting in the heavy metal removal efficiency and cycling performance not meeting the speed and cost requirements of industrial applications.

Method used

By applying a weak magnetic field of appropriate strength to the surface of the pure iron sheet, negative magnetoresistance effect is triggered, the conductivity of the amorphous inorganic film is improved, and combined with stirring technology, the magnetization strength of the magnetization is enhanced, so that it slides along the surface of the iron sheet to improve Conductivity.

Benefits of technology

The rate of zero-valent iron sheets to remove heavy metals in wastewater has been significantly improved, the reaction rate and removal efficiency have been improved, and the requirements of industrial applications have been met.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118028807B_ABST
    Figure CN118028807B_ABST
Patent Text Reader

Abstract

The present invention is a method for improving the conductivity of an amorphous oxide film on the surface of a pure iron sheet and its application. 1) Cut the iron sheet (1) into a rectangular shape, with the short side of the iron sheet being an integral multiple of the width of a magnet (2) and equal to or lower than the depth of the liquid level of a cylindrical waste liquid container; 2) Divide the iron sheet (1) into a plurality of regions, with the width of each region being the same as the width of the magnet (2); 3) Use the magnet (2) to slide along the surface of the iron sheet (1) and each region, and the sliding direction of the magnet (2) is parallel to the long side of the iron sheet (1), and the sliding rate and number of times of the magnet (2) on the surface of each region of the iron sheet (1) are the same, and the sliding direction is also the same. After the present invention is treated in this way, the conductivity of the amorphous inorganic film on the surface of the iron sheet can be improved. If the treated iron sheet surface is placed vertically in heavy metal wastewater close to the container wall, and the long side of the iron sheet is parallel to the liquid plane, the rate of removing heavy metals from the wastewater by the zero-valent iron sheet can be improved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to a method for improving the electrical conductivity of amorphous oxides and its application, in particular to a method for improving the electrical conductivity of amorphous oxides on the surface of pure iron sheets and its application, belonging to an innovative technology for improving the electrical conductivity of amorphous oxides on the surface of pure iron sheets and its application. Background Art

[0002] At present, with the development of industrial production, more and more heavy metal wastewater needs to be treated. Traditional technology has high treatment costs, complex processes and low treatment efficiency. This seriously hinders the development of industrial production. Large-scale zero-valent iron treatment technology is the most promising technology to solve this problem, but there is still a final bottleneck. Figure 1 As shown, the reason is that there is an amorphous mixed film on the surface of zero-valent iron that is oxidized by air and precipitated during the treatment process. This film prevents electrons from being transferred from the core to the surface to undergo redox reactions with heavy metals in the solution, resulting in the removal efficiency and cycle performance failing to meet the rate and operating cost requirements required for large-scale applications. Therefore, the key to the technical application of large-size iron sheets to remove heavy metals from wastewater is to increase the conductivity of the amorphous mixed film on its surface. The higher the conductivity of this film, the more electrons that reach the surface from the inside of the iron sheet to participate in the reaction per unit time, and the greater the reaction rate. Summary of the invention

[0003] The purpose of the present invention is to provide a method for improving the conductivity of amorphous oxide on the surface of pure iron sheet in consideration of the above problems. The present invention uses a weak magnetic field within a suitable intensity range to act on the amorphous film to cause a negative magnetoresistance effect, thereby improving the conductivity of the amorphous inorganic film, thereby improving the rate of removing heavy metals from wastewater by zero-valent iron sheet.

[0004] Another object of the present invention is to provide an application in the treatment of heavy metal wastewater. The present invention utilizes a magnetic field combined with stirring to increase the conductivity of the amorphous inorganic film, thereby increasing the rate at which the zero-valent iron sheet removes heavy metals from wastewater.

[0005] The technical solution of the present invention is: the method of improving the conductivity of amorphous oxide on the surface of pure iron sheet of the present invention comprises the following steps:

[0006] 1) Cut the iron sheet into a rectangular shape, with the short side of the iron sheet being an integer multiple of the magnet width;

[0007] 2) Divide the iron sheet into several areas, and the width of each area is the same as the width of the magnet;

[0008] 3) Use a magnet to slide along the surface and various areas of the iron sheet, and the sliding direction of the magnet is parallel to the long side of the iron sheet. The speed and number of times the magnet slides on the surface of each area of ​​the iron sheet are the same, and the sliding direction is also the same.

[0009] The method for improving the conductivity of amorphous oxide on the surface of pure iron sheet of the present invention is used for treating heavy metal waste liquid.

[0010] The above heavy metal waste liquid is the following single or multiple heavy metal ions: Ni 2+ 、Co 2+ 、Zn 2+ 、Cd 3+ , Pb 2+ , Cu 2+ , Mn 2+ Sn 2+ .

[0011] The present invention is used for treating heavy metal waste liquid, and the treatment process is as follows:

[0012] The process used for heavy metal waste treatment is as follows:

[0013] 1) Cut the iron sheet into a rectangular shape, with the long side of the iron sheet being an integer multiple of the width of the magnet;

[0014] 2) Divide the iron sheet into several areas, and the width of each area is the same as the width of the magnet;

[0015] 3) Use a magnet to slide along the surface and various areas of the iron sheet, and the sliding direction of the magnet is the same as the long side direction of the iron sheet. The magnet slides on the surface of each area of ​​the iron sheet at the same speed and number of times, and in the same direction;

[0016] The average magnetic induction intensity of the iron sheet is magnetized to the range of 35-354mT. The average magnetic induction intensity is measured by using a Gauss meter close to the surface of the iron sheet to measure at several points and then take the average value;

[0017] 4) Bend the long side of the iron sheet into the shape of the inner wall of a cylindrical container and place the iron sheet vertically into the heavy metal waste close to the container wall, with the long side of the iron sheet parallel to the liquid plane;

[0018] 5) Stir the waste liquid until the heavy metal content in the waste liquid no longer changes.

[0019] The present invention cuts the iron sheet into a suitable size: cuts out a rectangular shape, the short side of the iron sheet is an integer multiple of the width of the magnet as the short side size of the iron sheet, and then divides the iron sheet into several areas, the width of each area is the same as the width of the magnet, and the magnet is used to slide along the surface of the iron sheet and the drawn area, and the sliding direction of the magnet is parallel to the long side direction of the iron sheet. The rate and number of surface sliding of the magnet in each area of ​​the iron sheet are the same, that is, the number of regional slip magnetizations is the same, and the iron sheet is magnetized to an average magnetic induction intensity of 100mT to 500mT. The average magnetic induction intensity is measured by using a Gauss meter close to the surface of the iron sheet at several points and then taking the average value. After such treatment, the conductivity of the amorphous inorganic film on the surface of the iron sheet can be improved, and the rate of removing heavy metals from wastewater by the zero-valent iron sheet can be improved. The present invention is a convenient and practical method for improving the conductivity of amorphous oxides on the surface of pure iron sheets. BRIEF DESCRIPTION OF THE DRAWINGS

[0020] Figure 1 It is a schematic diagram of the composition and phase structure of the iron sheet;

[0021] Figure 2 A schematic diagram of the operation method of magnetizing an iron sheet according to the present invention;

[0022] Figure 3 It is a schematic diagram of the present invention using a magnet to magnetize an iron sheet and using a Gaussmeter to measure the average magnetic induction intensity of the iron sheet after magnetization, and measuring a total of five points A, B, C, D, and O;

[0023] Figure 4 This is a rendering of the treatment of heavy metal waste liquid in Example 1 of the present invention;

[0024] Figure 5 This is a rendering of the treatment of heavy metal waste liquid in Example 2 of the present invention;

[0025] Figure 6 This is a rendering of the treatment of heavy metal waste liquid by Example 3 of the present invention;

[0026] Figure 7 This is a diagram showing the effect of treating heavy metal waste liquid in Example 4 of the present invention. DETAILED DESCRIPTION

[0027] Embodiment 1:

[0028] The method for improving the electrical conductivity of amorphous oxide on the surface of a pure iron sheet of the present invention comprises the following steps:

[0029] 1) Cut the iron sheet 1 into a rectangular shape, with the short side of the iron sheet being an integer multiple of the width of the magnet 2;

[0030] 2) Divide the iron sheet 1 into several regions, and the width of each region is the same as the width of the magnet 2;

[0031] 3) Use magnet 2 to slide along the surface and various areas of iron sheet 1, and the sliding direction of magnet 2 is parallel to the long side of iron sheet 1. The speed and number of times that magnet 2 slides on the surface of various areas of iron sheet 1 are the same, and the sliding direction is also the same.

[0032] The iron sheet 1 has a circumference of a cylindrical container containing waste liquid as the long side dimension of the iron sheet.

[0033] The iron sheet 1 is magnetized to an average magnetic induction intensity of 35 mT to 354 mT.

[0034] Furthermore, the iron sheet 1 is magnetized to an average magnetic induction intensity of 200 mT to 300 mT.

[0035] The iron sheet 1 is magnetized to an average magnetic flux density, and the average magnetic flux density is obtained by measuring the average magnetic flux density at several points close to the surface of the iron sheet using a Gauss meter. The several points can be evenly distributed on the surface of the iron sheet 1 .

[0036] The long side of the iron sheet is bent into the shape of the inner wall of a cylindrical container, and the iron sheet is placed vertically into the heavy metal wastewater close to the container wall, with the long side of the iron sheet parallel to the liquid plane.

[0037] The method for improving the conductivity of amorphous oxide on the surface of pure iron sheet is applied to the treatment of heavy metal waste liquid.

[0038] The above heavy metal waste liquid is a mixed waste liquid containing a single or multiple heavy metal ions: Cu 2+ 、Se 4+ 、Te 4+ 、Bi 3 + , Pb 2+ 、As 3+ .

[0039] The process of the present invention for treating heavy metal waste liquid is as follows:

[0040] 1) Cut the iron sheet into a rectangular shape, with the long side of the iron sheet being an integer multiple of the width of the magnet;

[0041] 2) Divide the iron sheet 1 into a plurality of regions, the width of each region being the same as the width of the magnet (2);

[0042] 3) Use the magnet 2 to slide along the surface and various regions of the iron sheet 1, and the sliding direction of the magnet 2 is the same as the long side direction of the iron sheet 1. The magnet 2 slides on the surface of various regions of the iron sheet 1 at the same speed and number of times, and in the same direction;

[0043] The average magnetic induction intensity of the iron sheet is magnetized to the range of 35-354mT. The average magnetic induction intensity is measured by using a Gauss meter close to the surface of the iron sheet to measure at several points and then take the average value;

[0044] 4) Bend the long side of the iron sheet into the shape of the inner wall of a cylindrical container and place the iron sheet vertically into the heavy metal waste close to the container wall, with the long side of the iron sheet parallel to the liquid plane;

[0045] 5) Stir the waste liquid until the heavy metal content in the waste liquid no longer changes.

[0046] In the above step 5), the stirring rate is in the range of 100 rpm-500 rpm.

[0047] The effect of the method of the present invention is shown by comparing the removal of Cr by non-magnetized and magnetized iron sheets. 6+ Saturation removal rate in the wastewater removal rate versus time curve R e Size and time to reach saturation removal rate t e To evaluate the size. R e The larger it is, the better the removal effect is. The more electrons participate in the reaction per unit time during the removal process, the smaller the potential barrier of the amorphous layer is, and the greater the conductivity is. t e The shorter the Re is, the more electrons participate in the reaction per unit time, and the greater the conductivity of the amorphous layer. t e The magnitude of the magnetization intensity is measured by a magnetometer close to the surface of the iron sheet. Figure 3 The five points shown (A, B, C, D, O) are measured and the average value is taken.

[0048] The specific embodiments of the present invention are as follows:

[0049] Embodiment 1:

[0050] Cut the iron sheet 1 into a rectangular shape, and use an integer multiple of the width of the magnet 2 as the short side of the iron sheet, and the short side is equal to or less than the depth of the waste liquid in the container, and the circumference of the cylindrical container containing the waste liquid is the length. Divide the iron sheet 1 into several areas, and the width of each area is the same as the width of the magnet 2; use the magnet 2 to slide along the surface of the iron sheet 1 and the designated area, and the sliding direction of the magnet 2 is the same as the long side direction of the iron sheet 1. The rate and number of sliding of the magnet 2 on the surface of each area of ​​the iron sheet 1 are the same, and the sliding direction is also the same. Magnetize the average magnetic induction intensity of the iron sheet 1 to 100mT. The average magnetic induction intensity is measured by placing a gaussmeter close to the surface of the iron sheet as follows: Figure 3The five points A, B, C, D, and O shown in the figure are measured and the average value is taken. The long side of the iron sheet is bent into the shape of the inner wall of a cylindrical container and the iron sheet 1 is placed vertically into the heavy metal wastewater close to the container wall, and the long side of the iron sheet 1 is parallel to the liquid plane; the waste liquid is stirred at a rate of 350 rpm until the heavy metal content in the waste liquid no longer changes; the heavy metal ion concentration in the remaining waste liquid at different times is detected by ICP.

[0051] In this embodiment, the iron sheet 1 is used to treat As with a concentration of 1 mg / L. 3+ Simulated wastewater As 3+ 10 times the concentration of wastewater discharge standards). Figure 4 As shown, the iron sheet with a surface magnetization intensity of 100mT after magnetization and before magnetization is treated with the above As 3+ Simulated wastewater R e Both are 99.997%; t e The treatment time was reduced from 30 min to 26 min, and the treatment rate was 1.15 times higher than the original. 3+ Simulated wastewater (As 3+ The results show that increasing the magnetization of the iron sheet to 100mT can improve the conductivity of the amorphous film.

[0052] Embodiment 2:

[0053] Cut the iron sheet 1 into a rectangular shape, with the short side dimension of the iron sheet 1 being an integer multiple of the magnet width, and the short side being equal to or less than the depth of the waste liquid in the container, and the circumference of the cylindrical container containing the waste liquid being the long side dimension. Divide the iron sheet into several areas, with the width of each area being the same as the width of the magnet; slide the magnet 2 along the surface of the iron sheet 1 and the designated area, with the sliding direction of the magnet 2 being the same as the long side direction of the iron sheet 1. The rate and number of sliding of the magnet 2 on the surface of each area of ​​the iron sheet 1 are the same, and the sliding direction is also the same. Magnetize the iron sheet to an average magnetic induction intensity of 35mT. The average magnetic induction intensity is measured by placing a gaussmeter close to the surface of the iron sheet at a temperature of 100°. Figure 3 The five points A, B, C, D, and O shown in the figure are measured and the average value is taken. The long side of the iron sheet is bent into the shape of the inner wall of a cylindrical container and the iron sheet is placed vertically into the heavy metal wastewater close to the container wall, with the long side of the iron sheet parallel to the liquid plane. The waste liquid is stirred at a rate of 400 rpm until the heavy metal content in the waste liquid no longer changes. The heavy metal ion concentration in the remaining waste liquid at different times is detected by ICP.

[0054] In this embodiment, the iron sheet 1 is used to treat Bi with a concentration of 1 mg / L. 3+ Simulated wastewater (Bi 3+ 10 times the concentration of wastewater discharge standards). Figure 5As shown, the iron sheet with a surface magnetization intensity of 35mT after magnetization and before magnetization is treated with the above Bi 3+ Simulated wastewater R e Both are 99.990%; t e The treatment time was reduced from 20 min to 6 min, and the treatment rate was 3.33 times higher than the original. 3+ Simulated wastewater (Bi 3+ The concentration of 10 times the wastewater discharge standard) proved that increasing the magnetization of the iron sheet to 35 mT can increase the conductivity of the amorphous film.

[0055] Embodiment 3:

[0056] Cut the iron sheet 1 into a rectangular shape, and use an integer multiple of the width of the magnet 2 as the short side of the iron sheet, and the short side is equal to or less than the depth of the waste liquid in the container, and the circumference of the cylindrical container containing the waste liquid is used as the long side. Divide the iron sheet into several areas, and the width of each area is the same as the width of the magnet 2; use the magnet 2 to slide along the surface of the iron sheet 1 and the designated area, and the sliding direction of the magnet 2 is the same as the long side direction of the iron sheet. The rate and number of sliding of the magnet 2 on the surface of each area of ​​the iron sheet 1 are the same, and the sliding direction is also the same. The average magnetic induction intensity of the iron sheet 1 is magnetized to 354mT. The average magnetic induction intensity is measured by placing a gaussmeter close to the surface of the iron sheet as shown in the following figure. Figure 3 The five points A, B, C, D, and O shown in the figure are measured and the average value is taken. The long side of the iron sheet 1 is bent into the shape of the inner wall of a cylindrical container and the iron sheet 1 is placed vertically into the heavy metal wastewater close to the container wall, and the long side of the iron sheet 1 is parallel to the liquid plane; the waste liquid is stirred at a rate of 450 rpm until the heavy metal content in the waste liquid no longer changes; the heavy metal ion concentration in the remaining waste liquid at different times is detected by ICP.

[0057] In this embodiment, the iron sheet 1 is used to treat a solution containing 1 mg / L of Pb 2+ Simulated wastewater (Pb 2+ 10 times the concentration of wastewater discharge standards). Figure 6 As shown, the iron sheet with a surface magnetization intensity of 354mT after magnetization and before magnetization is used to treat the above Pb 2+ Simulated wastewater R e Both are 99.995%; t e The treatment time was reduced from more than 65 min to 50 min, and the treatment rate was 1.3 times greater than the original. 2+ Simulated wastewater (Pb 2+ 10 times the concentration of wastewater discharge standards) proved that increasing the magnetization of the iron sheet to 354mT can increase the conductivity of the amorphous film.

[0058] Embodiment 4:

[0059] Cut the iron sheet 1 into a rectangular shape, and use an integer multiple of the width of the magnet 2 as the short side size of the iron sheet 1, and the short side is equal to or less than the depth of the waste liquid in the container, and the circumference of the cylindrical container containing the waste liquid is used as the length. Divide the iron sheet 1 into several areas, and the width of each area is the same as the width of the magnet 2; use the magnet 2 to slide along the surface of the iron sheet 1 and the designated area, and the sliding direction of the magnet is the same as the long side direction of the iron sheet. The rate and number of sliding of the magnet 2 on the surface of each area of ​​the iron sheet 1 are the same, and the sliding direction is also the same. The average magnetic induction intensity of the iron sheet 1 is magnetized to 300mT. The average magnetic induction intensity is measured by placing a gaussmeter close to the surface of the iron sheet 1 as follows: Figure 3 The five points A, B, C, D, and O shown in the figure are measured and the average value is taken. The long side of the iron sheet 1 is bent into the shape of the inner wall of a cylindrical container and the iron sheet 1 is placed vertically in the heavy metal wastewater close to the container wall, and the long side of the iron sheet 1 is parallel to the liquid plane; the waste liquid is stirred at a rate of 300 rpm until the heavy metal content in the waste liquid no longer changes; the heavy metal ion concentration in the remaining waste liquid at different times is detected by ICP.

[0060] In this embodiment, the iron sheet 1 is used to treat Se with a concentration of 0.1 mg / L. 4+ Simulated wastewater (Se 4+ 10 times the concentration of wastewater discharge standards). Figure 7 As shown, the iron sheet with a surface magnetization intensity of 300mT after magnetization and before magnetization is treated with the above Se 4+ Simulated wastewater R e Both are 99.996%; t e The treatment time was reduced from 30 min to 16 min, and the treatment rate was 1.88 times higher than the original. 4+ Simulated wastewater (Se 4+ The results show that increasing the magnetization of the iron sheet to 300mT can improve the conductivity of the amorphous film.

Claims

1. A method for removing heavy metal ions from waste liquid, characterized in that The steps include: 1) Cut the iron sheet (1) into a rectangular shape, with the short side of the iron sheet being an integer multiple of the width of the magnet (2); 2) dividing the iron sheet (1) into a plurality of regions, wherein the width of each region is the same as the width of the magnet (2); 3) using a magnet (2) to slide along various regions of the surface of the iron sheet (1), and the sliding direction of the magnet (2) is parallel to the long side of the iron sheet (1), and the speed and number of sliding of the magnet (2) on the surface of various regions of the iron sheet (1) are the same, and the sliding direction is also the same; Bend the long side of the iron sheet into the shape of the inner wall of a cylindrical container, and vertically place the iron sheet into the waste liquid close to the container wall, with the long side of the iron sheet parallel to the liquid plane; 4) Stirring the waste liquid; The iron sheet (1) has a circumference of a cylindrical container for the waste liquid as the long side dimension of the iron sheet; The iron sheet (1) is magnetized to an average magnetic induction intensity of 35 mT to 354 mT; The above waste liquid is the following waste liquid containing single or multiple heavy metal ions: Cu 2+ 、Se 4+ 、Te 4+ 、Bi 3+ , Pb 2+ 、As 3+ .

2. The method for removing heavy metal ions from waste liquid according to claim 1, characterized in that The iron sheet (1) is magnetized to an average magnetic flux density of 200 mT to 300 mT.

3. The method for removing heavy metal ions from waste liquid according to claim 1, characterized in that The above average magnetic induction intensity is obtained by measuring at several points with a Gauss meter close to the surface of the iron sheet and taking the average value to obtain the average magnetic induction intensity.

4. The method for removing heavy metal ions from waste liquid according to claim 1, characterized in that The waste liquid is stirred until the heavy metal content in the waste liquid no longer changes.

5. The method for removing heavy metal ions from waste liquid according to claim 4, characterized in that The above stirring rate is in the range of 100 rpm-500 rpm.

Citation Information

Patent Citations

  • Soil heavy metal remediation method based on modified zero-valent iron

    CN109570219A

  • Method for rapidly removing pollutants in water by simply activating zero-valent iron

    CN110655172A

  • Vulcanization modified micron zero-valent iron material as well as preparation method and application thereof

    CN115771941A

  • Method for increasing reaction speed of zero-valent iron particles and iron sheets with heavy metal ions

    CN116119851A