Polyurea antistatic wear-resistant antiskid floor coating, preparation method and application

By adding a combination of conjugated π-bonded polymer conductive polymer and polypyrrole/polythiophene to polyurea floor coating, combined with nonionic surfactant pretreatment, the problem of insufficient anti-static performance of polyurea floor coating is solved. It achieves efficient anti-static effect, good wear resistance and chemical stability.

CN118085704BActive Publication Date: 2024-11-19深圳市朗迈新材料科技有限公司
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202410313376.1
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-03-19
Publication Date
2024-11-19
Estimated Expiration
2044-03-19

AI Technical Summary

Technical Problem

Polyurea floor coatings have shortcomings in anti-static properties. The addition of conductive fillers will affect their mechanical properties and chemical resistance, and the poor dispersion of conductive fillers leads to uneven anti-static effects.

Method used

The conductive network is formed to improve antistatic properties by adding polymer conductive polymers with conjugated π bonds to the polyurea coating formulation and improve conductivity by combining polypyrrole and polythiophene and nonionic surfactant pretreatment. Dispersibility of polymers.

Benefits of technology

It significantly improves the anti-static properties of the coating, maintains good wear resistance and chemical stability, and ensures the safety and service life of the floor.

✦ Generated by Eureka AI based on patent content.
Patent Text Reader

Abstract

The present invention discloses a polyurea antistatic wear-resistant antiskid floor coating, a preparation method and an application. The polyurea antistatic wear-resistant antiskid floor coating is characterized in that it comprises component A and component B: component A comprises isophorone diisocyanate, polyethylene terephthalate and a conductive polymer; component B comprises polyethylene terephthalate, terminal amino polyether, silicone compound, diamine chain extender, conductive polymer and catalyst. The mass ratio of component A to component B is 1:(0.5-1.5), and the conductive polymer is a conjugated π-bond polymer with conductive function. The polyurea antistatic wear-resistant antiskid floor coating of the present invention integrates multiple excellent properties such as antistatic, wear resistance, antiskid, impact resistance and chemical corrosion resistance, which not only ensures the safety of the working environment, but also improves work efficiency and reduces maintenance costs. It is an ideal ground treatment material.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to a polyurea antistatic wear-resistant antiskid floor coating, a preparation method and application thereof. Background Art

[0002] In modern industrial environments, the selection of floor materials is becoming more and more important, because different industries and environments have special requirements for floor materials. These requirements have gradually upgraded from the original basic protection needs, such as moisture and dust, to requirements for strength, wear resistance and chemical stability. This is because there are a lot of physical impacts, chemical corrosion, mechanical wear and other harsh factors in the industrial environment, which pose challenges to the durability and stability of floor materials. At the same time, with the advancement of science and technology, static electricity has brought serious safety problems to some specific environments, such as microelectronics manufacturing, pharmaceuticals, chemicals, petroleum and dust environments. Static electricity may damage electronic equipment, cause data loss, and even cause fires and explosions. Therefore, in addition to having good physical and chemical properties, floor materials must also have excellent anti-static properties to ensure the safety and stability of industrial production.

[0003] In order to meet this demand, scientists and researchers are committed to developing new floor coatings. Polyurea floor coatings have become an ideal choice due to their outstanding performance characteristics. Polyurea is a polymer material with excellent wear resistance and chemical corrosion resistance, which enables it to maintain stability in various harsh industrial environments. In addition, polyurea materials have good elasticity and excellent impact resistance, which can effectively resist the impact force from industrial equipment and protect the ground from damage. Therefore, polyurea floor coatings are widely used in industrial environments.

[0004] However, although polyurea floor coatings show excellent performance in many aspects, their anti-static performance is somewhat insufficient. This is mainly because the resistivity of the polyurea material itself is high, making it difficult to achieve an anti-static effect. In order to solve this problem, people have tried to add some conductive fillers to polyurea coatings to enhance their anti-static performance. These conductive fillers include metal powder, carbon black, graphite, conductive fibers and conductive pigments. By adding these conductive fillers, the resistivity of the coating can be reduced, thereby achieving the purpose of anti-static. However, although this method solves the anti-static problem of polyurea floor coatings to a certain extent, it also brings some new problems.

[0005] First, adding these conductive fillers will change the original properties of the coating. Although conductive fillers can improve the antistatic properties of the coating, they may also affect the mechanical properties, wear resistance and chemical resistance of the coating. This is because the parameters of the conductive fillers, such as hardness, strength, and chemical stability, are very different from those of the coating itself, which may lead to a decrease in the overall performance of the coating. For example, adding metal powders may increase the weight and hardness of the coating, but it may also reduce the elasticity and impact resistance of the coating. Adding carbon black or graphite may improve the antistatic properties of the coating, but it may also reduce the chemical resistance of the coating.

[0006] Secondly, the poor dispersion of conductive fillers in the coating may lead to unstable antistatic effect of the coating. Since the coating is affected by various forces during the coating process, the conductive fillers may aggregate or precipitate in the coating, resulting in uneven antistatic performance of the coating. This situation may cause some safety issues, such as static electricity accumulation, electric sparks, etc.

[0007] Therefore, how to improve the antistatic performance of polyurea floor coatings while maintaining their original excellent performance has become an important topic of current research. Summary of the invention

[0008] In view of the deficiencies in the prior art, the technical problem to be solved by the present invention is to provide a polyurea antistatic wear-resistant and antiskid floor coating, a preparation method and an application thereof.

[0009] The inventive concept of the present invention is: starting from the perspective of microscopic molecular structure, drawing on the characteristics of high molecular conductive polymers, by adding high molecular conductive polymers with conjugated π bonds to the polyurea coating formula, the antistatic performance of the coating is improved. Due to its special electronic structure, the high molecular conductive polymer with conjugated π bonds can migrate freely on the molecular chain, which enables the coating to effectively conduct current when an electric field is applied, thereby achieving an antistatic effect.

[0010] Specifically, the technical solution of the present invention is as follows:

[0011] A polyurea antistatic wear-resistant antiskid floor coating, comprising component A and component B:

[0012] The component A comprises isophorone diisocyanate, polyethylene terephthalate and a conductive polymer;

[0013] The B component comprises polyethylene terephthalate, terminal amino polyether, silicone compound, diamine chain extender, conductive polymer and catalyst.

[0014] Preferably, the mass ratio of component A to component B is 1:(0.5-1.5).

[0015] Preferably, the conductive polymer is a conjugated π-bond high molecular polymer with conductive function.

[0016] Preferably, the conductive polymer is at least one of polyparaphenylene, polyaniline, polyacetylene, polypyrrole and polythiophene.

[0017] Preferably, the component A comprises the following raw materials in parts by weight: 40-80 parts of isophorone diisocyanate, 25-45 parts of polyethylene terephthalate and 2-8 parts of conductive polymer.

[0018] Preferably, the B component comprises the following raw materials in parts by weight: 20-40 parts of polyethylene terephthalate, 20-30 parts of terminal amino polyether, 15-25 parts of silicone compound, 10-20 parts of diamine chain extender, 5-15 parts of conductive polymer, and 0.1-1.0 parts of catalyst.

[0019] Furthermore, the inventors discovered through experiments that the antistatic properties of the coating can be further improved by using two conductive polymers, polypyrrole and polythiophene, in combination.

[0020] Therefore, preferably, the conductive polymer is composed of polypyrrole and polythiophene. Further preferably, the conductive polymer is composed of polypyrrole and polythiophene in a mass ratio of (10-30): (10-30).

[0021] The silicone compound is selected from at least one of aminopropyl-terminated polydimethylsiloxane, polymethylsiloxane, monovinyl-terminated dimethyl (siloxane and polysiloxane), and hydroxyl-terminated polydimethylsiloxane.

[0022] The present invention also provides a method for preparing a polyurea antistatic wear-resistant antiskid floor coating, comprising the following steps:

[0023] (1) Preparation of component A:

[0024] Mix isophorone diisocyanate, polyethylene terephthalate and conductive polymer; keep at 70-85°C for 4-6 hours;

[0025] (2) Preparation of component B:

[0026] Mix polyethylene terephthalate, terminal amino polyether, silicone compound, diamine chain extender, conductive polymer and catalyst; keep at 100-110°C for 3-5 hours;

[0027] (3) Mixing:

[0028] Spray components A and B.

[0029] The invention also provides an application of a polyurea antistatic, wear-resistant and antiskid floor coating in antistatic, wear-resistant and antiskid flooring.

[0030] The polyurea antistatic wear-resistant antiskid floor coating of the present invention has significant beneficial effects, which are discussed in detail below:

[0031] Excellent antistatic performance: By adding conductive polymers to the coating, the present invention significantly improves the antistatic performance of the coating. The conductive polymer has good dispersibility in the coating and can form a uniform conductive network, thereby effectively reducing the resistivity of the coating film and improving its antistatic performance.

[0032] Excellent wear resistance: The coating of the present invention contains a large amount of polyurea components, which have extremely high wear resistance and can effectively resist various mechanical wear. In addition, the present invention also adds silicone compounds to the coating, which have excellent wear resistance and heat resistance, and can further improve the wear resistance of the coating film.

[0033] Strong weather resistance and chemical stability: Both polyurea and silicone compounds have good weather resistance and chemical stability, and can resist the erosion of various harsh climatic conditions and chemicals, greatly extending the service life of the coating.

[0034] Elasticity and impact resistance: Polyurea coatings have good elasticity and impact resistance, which can resist heavy impact and mechanical vibration and protect the ground from damage. At the same time, the elasticity of the coating can also provide good anti-slip performance and improve the safety of workers.

[0035] In summary, the polyurea antistatic wear-resistant and anti-skid floor coating of the present invention integrates multiple excellent properties such as antistatic, wear resistance, anti-skid, impact resistance and chemical corrosion resistance, which not only ensures the safety of the working environment, but also improves work efficiency and reduces maintenance costs. It is an ideal ground treatment material. DETAILED DESCRIPTION

[0036] Isophorone diisocyanate, Isophorone diisocyanate; 3-Isocyanatomethyl-3,5,5-trime, molecular formula: C 12 H 18 N2O2. Capable of forming urea bonds and urea bonds during the polymerization process, the formation of these bonds can provide good physical properties such as wear resistance and heat resistance.

[0037] Polyethylene terephthalate, Poly(ethylene terephthalate); PET; Polyethyleneglycol tereph. PET's high strength and wear resistance provide a tough foundation for coatings. This strength and wear resistance make the coatings more durable and have a longer service life. PET has good adhesion, which helps the coatings adhere tightly to the floor and prevents peeling and cracking of the coating layer. The physical and chemical properties of PET itself also help to improve the overall performance of the coating. For example, PET's chemical resistance and heat resistance can improve the environmental stability of the coating, allowing the coating to maintain its performance and stability under various adverse conditions.

[0038] Terminal amino polyether, preferably Jeffamine D-2000. It is a multifunctional amine that can react with isophorone diisocyanate to form a urea link. Its main function in the formulation is to adjust the hardness and flexibility of the coating, and also provides a part of the film-forming properties.

[0039] Silicone compounds are a class of polymers containing siloxane structures. In the present invention, the main function is to improve the weather resistance and chemical corrosion resistance of the coating. Silicone compounds can undergo a cleavage reaction of silicon-hydrogen bonds under the action of a catalyst to form a cross-linked network. This cross-linked network can improve the wear resistance, weather resistance and other properties of the coating.

[0040] Preferably, the silicone compound is selected from at least one of aminopropyl-terminated polydimethylsiloxane, polymethylsiloxane, monovinyl-terminated dimethyl (siloxane and polysiloxane), and hydroxy-terminated polydimethylsiloxane.

[0041] The diamine chain extender is preferably at least one of 3,3-dichloro-4,4-diaminodiphenylmethane, 3,5-diamino-4-chlorobenzoic acid isobutyl ester, diethyltoluenediamine (DETDA) and isophoronediamine (IPDA).

[0042] The catalyst is an organic tin catalyst or an organic bismuth catalyst. Preferably, the tin catalyst is at least one of dibutyltin dilaurate, stannous octoate, bismuth isooctanoate, BCAT-20C organic bismuth catalyst and BCAT-30C organic bismuth catalyst. The catalyst can accelerate the reaction of isophorone diisocyanate with other substances and improve the efficiency of the coating preparation process.

[0043] The conductive polymer selected by the present invention is a conjugated π-bond high molecular polymer with excellent conductive properties. Specifically, we prefer to use at least one conductive high molecular polymer such as polyparaphenylene, polyaniline, polyacetylene, polypyrrole and polythiophene. These polymers with a large number of π-conjugated systems can provide a continuous electronic conductor network. When the coating is electrostatically charged, the network path formed by these conductive polymers can promote the flow of electrons, thereby effectively eliminating static electricity and improving the antistatic properties of the coating. The conjugated π-bond high molecular polymer not only enhances the antistatic property of the coating, but also further enhances the durability and stability of the coating due to its chemical stability and excellent mechanical properties.

[0044] The preparation method of the polyurea antistatic wear-resistant antiskid floor coating comprises the following steps:

[0045] (1) Preparation of component A:

[0046] Mix isophorone diisocyanate, polyethylene terephthalate and conductive polymer; keep at 70-85°C for 4-6 hours;

[0047] (2) Preparation of component B:

[0048] Mix polyethylene terephthalate, terminal amino polyether, silicone compound, diamine chain extender, conductive polymer and catalyst; keep at 100-110°C for 3-5 hours;

[0049] (3) Mixing:

[0050] Spray components A and B.

[0051] Through further experimental research, the inventors found that the combination of polypyrrole and polythiophene, two conductive polymers, can more effectively enhance the antistatic ability of the coating. Therefore, a more ideal choice is to use a conductive polymer composed of polypyrrole and polythiophene. For further optimization, we recommend that the conductive polymer be composed of polypyrrole and polythiophene in a mass ratio of (10-30): (10-30), and such a ratio can achieve the best antistatic effect.

[0052] After rigorous experimental verification, the inventors found that the compound use of polypyrrole and polythiophene can significantly enhance the antistatic properties of the coating and has a synergistic effect. The deep-seated reasons can be explained from the following aspects:

[0053] First, when polypyrrole and polythiophene are mixed together, they can form a composite, continuous conductive network at the microscopic scale. This conductive network is composed of the π-conjugated systems of the two polymers interwoven together, which can provide an effective charge conduction channel and enhance the continuity of the conductive path inside the coating, thereby improving the charge conduction ability of the coating. By improving the charge conduction ability of the coating, the accumulation of static electricity can be more effectively prevented, thereby improving the antistatic performance of the coating.

[0054] Secondly, although both polypyrrole and polythiophene contain π-conjugated systems, their electronic energy levels are different due to their slightly different molecular structures and electronic layouts. This difference in electronic energy levels can produce very favorable effects in the conductive network after compounding. In this mixed conductive network, electrons can transition between different energy levels, which greatly improves the conduction efficiency of electrons. This mechanism of transition between electronic energy levels enables the compounding of polypyrrole and polythiophene to produce significant synergistic effects on the antistatic properties of coatings.

[0055] Finally, when polypyrrole and polythiophene are compounded, some interfacial effects or microscopic mutual penetration may occur between them. Such interfacial effects or microscopic mutual penetration can further improve the continuity and stability of the conductive path, provide a more stable channel for charge conduction, and improve the antistatic performance of the coating, thereby designing the polyurea antistatic coating with excellent performance of the present invention.

[0056] Furthermore, the inventors found that the addition of powdered conductive polymers such as polypyrrole and polythiophene may cause uneven dispersion due to the adsorption and electrostatic forces between particles, forming particle aggregation, thereby affecting the performance of the coating. In order to improve the dispersion performance, the inventors further added non-ionic surfactants to the formula to improve its dispersion performance and further enhance the antistatic performance.

[0057] The inventors first mixed a nonionic surfactant with a conductive polymer and then added it to the coating formula. The nonionic surfactant can reduce the surface tension between liquids, increase the compatibility of liquids and solids, and enable the liquid to better wet the solids. Therefore, adding a nonionic surfactant can improve the dispersibility of the conductive polymer in the coating matrix and avoid aggregation between polymer particles. By premixing the nonionic surfactant with the conductive polymer, the nonionic surfactant can be more fully coated on the surface of the conductive polymer to form a hydrophilic shell, so that the conductive polymer can be more evenly dispersed in the coating matrix. This can not only improve the performance of the coating, but also improve the stability of the coating.

[0058] It should also be noted that nonionic surfactants themselves have an antistatic effect. The polar part of nonionic surfactants can form hydrogen bonds or electrostatic attraction in water or other polar solvents, so that the charges inside the film layer formed by the coating can be quickly conducted and dispersed. At the same time, their non-polar parts can be well dispersed and compatible in the organic matrix of the coating, so that the formed conductive channels can be evenly distributed in the coating film layer.

[0059] Therefore, nonionic surfactants can not only improve the dispersibility of conductive polymers such as polypyrrole and polythiophene, but also enhance the antistatic properties of coatings through their own conductive properties.

[0060] Preferably, in components A and B, the mass ratio of the nonionic surfactant to the conductive polymer is 1:(2-6).

[0061] Furthermore, the preparation method of the polyurea antistatic wear-resistant antiskid floor coating comprises the following steps:

[0062] (1) Preparation of component A:

[0063] First, a nonionic surfactant and a conductive polymer are mixed, and then isophorone diisocyanate and polyethylene terephthalate are added and mixed; the mixture is kept at 70-85° C. for 4-6 hours;

[0064] (2) Preparation of component B:

[0065] Firstly, a nonionic surfactant and a conductive polymer are mixed, and then polyethylene terephthalate, terminal amino polyether, silicone compound, diamine chain extender and catalyst are added and mixed; the mixture is kept at 100-110° C. for 3-5 hours;

[0066] (3) Mixing:

[0067] Spray components A and B.

[0068] In the embodiment:

[0069] Polyethylene terephthalate, specifically PET RE5264 NC010 provided by DuPont Company of the United States, item number AL-642177004679.

[0070] Polypyrrole, product number: 482552, brand: Aldrich, provided by Sigma-Aldrich (Shanghai) Trading Co., Ltd.

[0071] Polythiophene, product abbreviation PBDB-T (PCE12) | PBDTBDD, solid powder or granules, provided by Angxing New Carbon Materials Changzhou Co., Ltd.

[0072] The terminal amino polyether is Jeffamine D-2000, which is the Jeffamine D2000 epoxy curing agent provided by Huntsman Corporation of the United States.

[0073] Silicone compounds, monovinyl-terminated dimethyl (siloxane and polysiloxane), CAS No.: 68083-19-2, provided by Guangzhou Shanghe Chemical Technology Co., Ltd.

[0074] The diamine chain extender is 3,3-dichloro-4,4-diaminodiphenylmethane (CAS No.: 101-14-4), MOCA.

[0075] The catalyst is bismuth isooctanoate, also known as bismuth 2-ethylhexanoate.

[0076] The non-ionic surfactant used is Tween-80, item number 777777 Warner brand food grade Tween 80, provided by Henan Bondeli Biotechnology Co., Ltd.

[0077] Example 1

[0078] A polyurea antistatic wear-resistant antiskid floor coating, comprising component A and component B:

[0079] The component A comprises the following raw materials in parts by weight: 60 parts of isophorone diisocyanate, 36 parts of polyethylene terephthalate and 4 parts of conductive polymer polypyrrole;

[0080] The B component includes the following raw materials in parts by weight: 32 parts of polyethylene terephthalate, 25 parts of Jeffamine D-2000 terminal amino polyether, 20 parts of silicone compound monovinyl-terminated dimethyl (siloxane and polysiloxane), 15 parts of diamine chain extender 3,3-dichloro-4,4-diaminodiphenylmethane, 8 parts of conductive polymer polypyrrole, and 0.3 parts of catalyst bismuth isooctanoate;

[0081] The mass ratio of the A component to the B component is 1:1.

[0082] Preparation method of the above-mentioned polyurea antistatic wear-resistant antiskid floor coating:

[0083] (1) Preparation of component A (calculated by weight)

[0084] a. Take 60 parts of isophorone diisocyanate, add 36 parts of polyethylene terephthalate and 4 parts of a conductive polymer polypyrrole, and stir at room temperature for 10 minutes;

[0085] b. The mixture was then heated to 80 ° C and maintained at this temperature for 5 hours;

[0086] c. The mixture was cooled to 50°C to obtain component A;

[0087] (2) Preparation of component B (calculated by weight)

[0088] d. Take 32 parts of polyethylene terephthalate, 25 parts of Jeffamine D-2000 amino polyether, 20 parts of silicone compounds monovinyl-terminated dimethyl (siloxane and polysiloxane), 15 parts of diamine chain extender 3,3-dichloro-4,4-diaminodiphenylmethane, 8 parts of conductive polymer polypyrrole and 0.3 parts of catalyst bismuth isooctanoate, keep stirring at room temperature for 10 minutes;

[0089] e. The mixture was heated to 105°C, vacuum-dehydrated, and then kept at a constant temperature of 105°C for 4 hours;

[0090] f. After cooling to 50°C, component B is obtained;

[0091] (3) Coating test

[0092] g. Using spray equipment, set the reaction temperature of components A and B to 70°C and the working pressure to 2200psi.

[0093] h. Spray equal amounts of components A and B on the substrate to obtain a single-layer polyurea coating of 3.5 mm;

[0094] i. Place the coating in a constant temperature box at 25°C and perform performance test after 1 week.

[0095] Example 2

[0096] A polyurea antistatic wear-resistant antiskid floor coating, comprising component A and component B:

[0097] The component A comprises the following raw materials in parts by weight: 60 parts of isophorone diisocyanate, 36 parts of polyethylene terephthalate and 4 parts of conductive polymer polythiophene;

[0098] The B component includes the following raw materials in parts by weight: 32 parts of polyethylene terephthalate, 25 parts of Jeffamine D-2000 terminal amino polyether, 20 parts of silicone compound monovinyl-terminated dimethyl (siloxane and polysiloxane), 15 parts of diamine chain extender 3,3-dichloro-4,4-diaminodiphenylmethane, 8 parts of conductive polymer polythiophene, and 0.3 parts of catalyst bismuth isooctanoate;

[0099] The mass ratio of the A component to the B component is 1:1.

[0100] Preparation method of the above-mentioned polyurea antistatic wear-resistant antiskid floor coating:

[0101] (1) Preparation of component A (calculated by weight)

[0102] a. Take 60 parts of isophorone diisocyanate, add 36 parts of polyethylene terephthalate and 4 parts of a conductive polymer polythiophene, and stir at room temperature for 10 minutes;

[0103] b. The mixture was then heated to 80 ° C and maintained at this temperature for 5 hours;

[0104] c. The mixture was cooled to 50°C to obtain component A;

[0105] (2) Preparation of component B (calculated by weight)

[0106] d. Take 32 parts of polyethylene terephthalate, 25 parts of Jeffamine D-2000 amino-terminated polyether, 20 parts of silicone compounds monovinyl-terminated dimethyl (siloxane and polysiloxane), 15 parts of diamine chain extender 3,3-dichloro-4,4-diaminodiphenylmethane, 8 parts of conductive polymer polythiophene and 0.3 parts of catalyst bismuth isooctanoate, keep stirring at room temperature for 10 minutes;

[0107] e. The mixture was heated to 105°C, vacuum-dehydrated, and then kept at a constant temperature of 105°C for 4 hours;

[0108] f. After cooling to 50°C, component B is obtained;

[0109] (3) Coating test

[0110] g. Using spray equipment, set the reaction temperature of components A and B to 70°C and the working pressure to 2200psi.

[0111] h. Spray equal amounts of components A and B on the substrate to obtain a single-layer polyurea coating of 3.5 mm;

[0112] i. Place the coating in a constant temperature box at 25°C and perform performance test after 1 week.

[0113] Example 3

[0114] A polyurea antistatic wear-resistant antiskid floor coating, comprising component A and component B:

[0115] The component A comprises the following raw materials in parts by weight: 60 parts of isophorone diisocyanate, 36 parts of polyethylene terephthalate, 2 parts of conductive polymer polypyrrole and 2 parts of conductive polymer polythiophene;

[0116] The B component includes the following raw materials in parts by weight: 32 parts of polyethylene terephthalate, 25 parts of Jeffamine D-2000 terminal amino polyether, 20 parts of silicone compound monovinyl-terminated dimethyl (siloxane and polysiloxane), 15 parts of diamine chain extender 3,3-dichloro-4,4-diaminodiphenylmethane, 4 parts of conductive polymer polypyrrole, 4 parts of conductive polymer polythiophene, and 0.3 parts of catalyst bismuth isooctanoate;

[0117] The mass ratio of the A component to the B component is 1:1.

[0118] Preparation method of the above-mentioned polyurea antistatic wear-resistant antiskid floor coating:

[0119] (1) Preparation of component A (calculated by weight)

[0120] a. Take 60 parts of isophorone diisocyanate, add 36 parts of polyethylene terephthalate, 2 parts of a conductive polymer polypyrrole and 2 parts of a conductive polymer polythiophene, and stir at room temperature for 10 minutes;

[0121] b. The mixture was then heated to 80 ° C and maintained at this temperature for 5 hours;

[0122] c. The mixture was cooled to 50°C to obtain component A;

[0123] (2) Preparation of component B (calculated by weight)

[0124] d. Take 32 parts of polyethylene terephthalate, 25 parts of Jeffamine D-2000 amino polyether terminal, 20 parts of silicone compound monovinyl-terminated dimethyl (siloxane and polysiloxane), 15 parts of diamine chain extender 3,3-dichloro-4,4-diaminodiphenylmethane, 4 parts of conductive polymer polypyrrole, 4 parts of conductive polymer polythiophene and 0.3 parts of catalyst bismuth isooctanoate, keep stirring at room temperature for 10 minutes;

[0125] e. The mixture was heated to 105°C, vacuum-dehydrated, and then kept at a constant temperature of 105°C for 4 hours;

[0126] f. After cooling to 50°C, component B is obtained;

[0127] (3) Coating test

[0128] g. Using spray equipment, set the reaction temperature of components A and B to 70°C and the working pressure to 2200psi.

[0129] h. Spray equal amounts of components A and B on the substrate to obtain a single-layer polyurea coating of 3.5 mm;

[0130] i. Place the coating in a constant temperature box at 25°C and perform performance test after 1 week.

[0131] Example 4

[0132] A polyurea antistatic wear-resistant antiskid floor coating, comprising component A and component B:

[0133] The component A comprises the following raw materials in parts by weight: 60 parts of isophorone diisocyanate, 36 parts of polyethylene terephthalate, 1 part of Tween-80 nonionic surfactant, 2 parts of conductive polymer polypyrrole and 2 parts of conductive polymer polythiophene;

[0134] The B component includes the following raw materials in parts by weight: 32 parts of polyethylene terephthalate, 25 parts of Jeffamine D-2000 terminal amino polyether, 20 parts of silicone compound monovinyl-terminated dimethyl (siloxane and polysiloxane), 15 parts of diamine chain extender 3,3-dichloro-4,4-diaminodiphenylmethane, 2 parts of Tween-80 nonionic surfactant, 4 parts of conductive polymer polypyrrole, 4 parts of conductive polymer polythiophene, and 0.3 parts of catalyst bismuth isooctanoate;

[0135] The mass ratio of the A component to the B component is 1:1.

[0136] Preparation method of the above-mentioned polyurea antistatic wear-resistant antiskid floor coating:

[0137] (1) Preparation of component A (calculated by weight)

[0138] a. First, 1 part of Tween-80 nonionic surfactant, 2 parts of conductive polymer polypyrrole and 2 parts of conductive polymer polythiophene were mixed uniformly, and then 60 parts of isophorone diisocyanate and 36 parts of polyethylene terephthalate were added, and stirred at room temperature for 10 minutes;

[0139] b. The mixture was then heated to 80 ° C and maintained at this temperature for 5 hours;

[0140] c. The mixture was cooled to 50°C to obtain component A;

[0141] (2) Preparation of component B (calculated by weight)

[0142] d. First, 2 parts of Tween-80 nonionic surfactant, 4 parts of conductive polymer polypyrrole and 4 parts of conductive polymer polythiophene were mixed uniformly, and then 32 parts of polyethylene terephthalate, 25 parts of Jeffamine D-2000 terminal amino polyether, 20 parts of silicone compounds monovinyl-terminated dimethyl (siloxane and polysiloxane), 15 parts of diamine chain extender 3,3-dichloro-4,4-diaminodiphenylmethane and 0.3 parts of catalyst bismuth isooctanoate were added, and stirred at room temperature for 10 minutes;

[0143] e. The mixture was heated to 105°C, vacuum-dehydrated, and then kept at a constant temperature of 105°C for 4 hours;

[0144] f. After cooling to 50°C, component B is obtained;

[0145] (3) Coating test

[0146] g. Using spray equipment, set the reaction temperature of components A and B to 70°C and the working pressure to 2200psi.

[0147] h. Spray equal amounts of components A and B on the substrate to obtain a single-layer polyurea coating of 3.5 mm;

[0148] i. Place the coating in a constant temperature box at 25°C and perform performance test after 1 week.

[0149] Test Example 1:

[0150] The electrostatic conductivity of the coating is determined by a surface resistivity tester. A thickness gauge is selected to measure the coating surface thickness. Based on the determined coating thickness, the surface resistance of the coating is measured using a TERA Ohmmeter TOM 600 (Germany). Each sample is tested five times. The resistance is measured and the surface resistivity is calculated by the Tom 600 test.

[0151] Table 1 Surface resistivity test results

[0152] Surface resistivity, Ω·cm Example 1 <![CDATA[1.1×10 8 ]]> Example 2 <![CDATA[8.8×10 7 ]]> Example 3 <![CDATA[5.6×10 7 ]]> Example 4 <![CDATA[1.2×10 7 ]]>

[0153] Test Example 2:

[0154] The wear resistance was determined in accordance with GB / T 1689-2014 Determination of wear resistance of vulcanized rubber (using Akron abrasion testing machine).

[0155] Table 2 Wear resistance test results

[0156] Sample wear index A, % Example 1 0.28 Example 2 0.23 Example 3 0.25 Example 4 0.24

[0157] Test Example 3:

[0158] Example 3 was subjected to conventional performance tests, and the data were as follows: tensile strength 17.8 MPa, elongation at break 520%, tear strength 80 kN / m, and surface hardness 88 Shore A.

[0159] Example 4 was subjected to conventional performance tests, and the data were as follows: tensile strength 19.2 MPa, elongation at break 590%, tear strength 84 kN / m, and surface hardness 88 Shore A.

[0160] Specific analysis example:

[0161] Example 3: Both polypyrrole and polythiophene are used. The antistatic performance of Example 3 is further improved, which may be due to the synergistic effect of polypyrrole and polythiophene in the coating. Although the antistatic performance of Example 3 is improved, due to the lack of pretreatment, the dispersibility of polypyrrole and polythiophene in the coating is still insufficient, and the antistatic performance still has room for improvement.

[0162] Example 4: Based on Example 3, polypyrrole and polythiophene were pre-wrapped with a nonionic surfactant. This step significantly improved the dispersibility of polypyrrole and polythiophene in the coating, thereby significantly improving the antistatic performance of the coating. Example 4 has the lowest surface resistivity and the best antistatic performance. In addition, the wear resistance and mechanical properties of Example 4 are also guaranteed, because the use of nonionic surfactants can not only improve the dispersibility of polypyrrole and polythiophene, but also will not significantly affect other properties of the coating.

[0163] In general, the polyurea antistatic wear-resistant and antiskid floor coating of Example 4 most successfully balances various performance requirements. By combining polypyrrole and polythiophene and pre-treating with a nonionic surfactant, the floor coating of Example 4 not only has excellent antistatic performance, but also has good wear resistance and mechanical properties.

[0164] Especially in terms of antistatic performance, the surface resistivity of the coating of Example 4 was significantly reduced to 1.2×10 7 Ω·cm, much lower than 1.1×10 8 Ω·cm. This shows that after adding polypyrrole and polythiophene and pre-wrapping with non-ionic surfactant, the antistatic performance of the coating is significantly improved, showing a strong antistatic effect.

[0165] In the wear resistance test of GB / T 1689-2014, the wear index A of the samples of all embodiments is between 0.23 and 0.28, indicating that the wear resistance of all embodiments is relatively excellent, and the introduction of the conductive polymer does not have a negative impact on the wear resistance of the coating.

[0166] The above-mentioned embodiments are only preferred embodiments of the present invention and cannot be used to limit the scope of protection of the present invention. Any non-substantial changes and substitutions made by technicians in this field on the basis of the present invention shall fall within the scope of protection required by the present invention.

Claims

1. A polyurea antistatic wear-resistant antiskid floor coating, characterized in that: Including component A and component B: The component A comprises the following raw materials in parts by weight: 40-80 parts of isophorone diisocyanate, 25-45 parts of polyethylene terephthalate and 2-8 parts of conductive polymer; The B component includes the following raw materials in parts by weight: 20-40 parts of polyethylene terephthalate, 20-30 parts of terminal amino polyether, 15-25 parts of silicone compound, 10-20 parts of diamine chain extender, 5-15 parts of conductive polymer, and 0.1-1.0 parts of catalyst; The mass ratio of component A to component B is 1:(0.5-1.5); The conductive polymer is composed of polypyrrole and polythiophene in a mass ratio of (10-30): (10-30).

2. The polyurea antistatic wear-resistant antiskid floor coating according to claim 1, characterized in that: The silicone compound is selected from at least one of aminopropyl-terminated polydimethylsiloxane, monovinyl-terminated dimethylpolysiloxane and hydroxyl-terminated polydimethylsiloxane.

3. The method for preparing the polyurea antistatic wear-resistant antiskid floor coating according to claim 1 or 2 comprises the following steps: (1) Preparation of component A: Mix isophorone diisocyanate, polyethylene terephthalate and conductive polymer; keep at 70-85°C for 4-6 hours; (2) Preparation of component B: Mix polyethylene terephthalate, terminal amino polyether, silicone compound, diamine chain extender, conductive polymer and catalyst; keep at 100-110°C for 3-5 hours; (3) Mixing: Spray components A and B.

4. Application of the polyurea antistatic, wear-resistant and anti-skid floor coating according to claim 1 or 2 in antistatic, wear-resistant and anti-skid flooring.