A solid carbon dioxide adsorbent and preparation method thereof

The preparation of carbon dioxide adsorbents with porous structures through industrial waste such as fly ash and steel slag has solved the problems of low adsorption amount and high preparation cost, and achieved efficient carbon dioxide adsorption and waste utilization.

CN118122286BActive Publication Date: 2024-11-22SHANXI LUAN ENVIRONMENTAL ENERGY DEV CO LTD
View PDF 0 Cites 5 Cited by

Patent Information

Application Number
CN202410450493.2
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-04-15
Publication Date
2024-11-22
Estimated Expiration
2044-04-15

AI Technical Summary

Technical Problem

The existing carbon dioxide adsorbent has low adsorption amount, complex preparation process and high cost, which limits its large-scale industrial production and fails to effectively utilize industrial waste fly ash and steel slag.

Method used

Solid carbon dioxide adsorbent composed of fly ash, steel slag, coke powder, zinc oxide, acrylic acid, surfactant and organic amine are used to form a porous structure through high-temperature calcination and oxidation reaction, combining the synergistic effect of surfactant and organic amine. Improve adsorption performance.

Benefits of technology

It significantly improves the adsorption amount and circulation stability of carbon dioxide adsorbent, reduces the preparation cost, realizes waste treatment, and alleviates the pressure of industrial waste treatment.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118122286B_ABST
    Figure CN118122286B_ABST
Patent Text Reader

Abstract

The invention discloses a solid carbon dioxide adsorbent and a preparation method thereof, belonging to the technical field of adsorption and separation. The invention firstly calcines fly ash and steel slag at high temperature to generate micropores, then mixes coke powder, zinc oxide and acrylic acid for shaping, and calcines at high temperature in the absence of oxygen to form partial mesopores and more micropores, then introduces oxygen after a period of time to continue calcining to form more mesopores, and finally sprays a mixture of surfactant and organic amine on the surface thereof, the two have a synergistic effect, and can improve carbon dioxide adsorption and cyclic stability performance; the obtained carbon dioxide adsorbent has good adsorption performance, and solves the problems of complex process, high cost, low yield and the like of the existing carbon dioxide adsorbent preparation method and the low adsorption amount of the existing carbon dioxide adsorbent.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention belongs to the technical field of adsorption separation, and relates to a carbon dioxide adsorbent, specifically a carbon dioxide adsorbent based on fly ash, steel slag and coke powder, and a preparation method thereof. Background Art

[0002] Carbon dioxide emissions from fossil fuel combustion account for about 78% of greenhouse gas emissions, and about a quarter of carbon dioxide emissions come from large energy facilities such as power plants. Therefore, capturing carbon dioxide produced by power plants is the top priority for reducing carbon dioxide emissions. For existing power plants, post-combustion carbon capture technology is the most suitable because the capture device can be retrofitted in low-investment power plants. Although liquid ammonia technology has been used in industry, its main problem is the high regeneration cost. In addition, liquid ammonia is highly volatile and has defects such as corrosion of equipment, reagent degradation, and odor.

[0003] In order to avoid the above problems, solid carbon dioxide adsorbents came into being. Solid carbon dioxide adsorbents do not need to evaporate a large amount of water in the solvent, thereby reducing corrosion and volatilization problems. In addition, solid carbon dioxide adsorbents have the advantages of low regeneration energy consumption, good carbon dioxide adsorption performance, and high selectivity. However, the synthesis of most solid carbon dioxide adsorbents usually requires the use of multiple templates. These preparation methods make the synthesis process of solid carbon dioxide adsorbents complicated, costly, and low in output, thus limiting their large-scale industrial production.

[0004] About 750 million tons of fly ash are produced globally each year, of which 60% are not effectively utilized; the global production of steel slag is about 180-270 million tons, and most of the steel slag is not effectively treated; fly ash and steel slag that are not effectively utilized are disposed of by landfill and dumping into the sea, which not only wastes resources, but also causes environmental pollution and harms human health. If these industrial wastes can be used in the preparation of carbon dioxide adsorbents, it can not only achieve waste treatment with waste, but also relieve the pressure of industrial waste treatment.

[0005] At present, the adsorbents for preparing carbon dioxide using fly ash have the problem of low adsorption capacity, especially the adsorbents based on physical adsorption. For example, patent CN114904479A uses fly ash as raw material to prepare carbon dioxide adsorbent, and its adsorption capacity is 2.02mmol / g. In order to create a good pore structure in the adsorbent and increase the adsorption capacity in the prior art, templates, pore expanders, etc. are used, which invisibly increases the preparation cost of the adsorbent, such as patent CN114272892A. In addition, the preparation cycle of some adsorbents is very long, which is not conducive to large-scale production of adsorbents, such as patent CN105817197A. Summary of the invention

[0006] The present invention overcomes the shortcomings of the prior art, provides a solid carbon dioxide adsorbent and a preparation method thereof, and solves the problem of low adsorption capacity of the prior carbon dioxide adsorbent.

[0007] In order to achieve the above object, the present invention is achieved through the following technical solutions:

[0008] A solid carbon dioxide adsorbent, comprising fly ash, steel slag, coke powder, zinc oxide, acrylic acid, a surfactant and an organic amine; the fly ash contains 4-15wt.% carbon, the steel slag contains 10-30wt.% ferrosoferric oxide; the mass ratio of fly ash to steel slag is 1:3-9.

[0009] Preferably, the mass ratio of zinc oxide to coke powder is 2:1.

[0010] Preferably, the surfactant is 2-ethylhexyl phosphate, and the organic amine is polyethyleneimine.

[0011] More preferably, the mass ratio of 2-ethylhexyl phosphate to polyethyleneimine is 1:1.

[0012] Preferably, the particle size of the fly ash and steel slag after mixing is less than 100 mesh.

[0013] The method for preparing a solid carbon dioxide adsorbent comprises the following steps:

[0014] 1) fully mixing and grinding fly ash and steel slag to obtain a first mixture; calcining the first mixture at 700-950° C. for 5-10 hours in an aerobic environment to obtain a second mixture;

[0015] 2) the second mixture, coke powder, zinc oxide and acrylic acid are fully mixed and shaped, and then isolated from air and calcined at 920-1200° C. to obtain a third mixture;

[0016] 3) calcining the third mixture at 650-800° C. for 5-8 hours in an aerobic environment, and then cooling the mixture to obtain a fourth mixture; spraying a mixed solution of a surfactant and an organic amine onto the fourth mixture, and drying the mixture to obtain a carbon dioxide adsorbent.

[0017] Preferably, the heating rates of calcination in step 1), step 2), and step 3) are all 2-10°C / min.

[0018] Preferably, the mass ratio of the second mixture to the coke powder is 3:1-2.5, and the mass ratio of acrylic acid to the second mixture is 4:1.2-2.4.

[0019] Preferably, the micropore volume of the obtained second mixture is 0.15-0.55 cm 3 / g; the mesopore diameter of the fourth mixture obtained is 8.5-10.7nm.

[0020] Preferably, the mass ratio of the surfactant to the fourth mixture is 0.01-0.1:1.

[0021] The beneficial effects of the present invention compared with the prior art are as follows:

[0022] The present invention uses fly ash, steel slag and coke powder, which are industrial wastes, as raw materials, and constructs disordered porous carrier materials from the wastes to load surfactants and organic amines to form an adsorbent with good carbon dioxide adsorption performance.

[0023] First, under the combined effects of high temperature and oxygen in the high-temperature furnace, the carbon in the fly ash reacts chemically with the ferroferric oxide in the steel slag:

[0024] Fe3O4+4C→3Fe+4CO, in which carbon volatilizes in the form of gas CO, forming gas channels inside the solid, which is the source of micropore volume.

[0025] Afterwards, the present invention fully mixes the calcined mixture with coke powder, zinc oxide and acrylic acid, and forms a macroscopic fixed structure under the bonding effect of acrylic acid and the effect of the mold. Under the high temperature effect of the high temperature furnace and the condition of air isolation, the zinc oxide reacts chemically with the carbon in the coke powder:

[0026] C+2ZnO→2Zn+CO2, where zinc evaporates in the form of steam and C evaporates in the form of CO2 gas, forming certain micropores and mesopores inside the solid.

[0027] Next, oxygen is introduced into the mixture under high temperature in a high temperature furnace. Acrylic acid will be pyrolyzed under high temperature and oxygen-rich conditions to generate CO2 gas and water vapor. The mixture is placed in dry ice or liquid nitrogen, where water vapor forms ice crystals in the sample. The ice crystals expand during the freezing process and form a porous structure. Therefore, there are a large number of irregular mesopores with a pore size of 8.5 to 10.7 nm in the mixture.

[0028] Finally, the mixture of the surfactant 2-ethylhexyl phosphate and polyethyleneimine sprayed by the present invention has a synergistic effect. The presence of 2-ethylhexyl phosphate enhances the diffusion of CO2. It also improves the dispersion of polyethyleneimine in the carrier pores, so that more active amine sites are exposed at the gas-solid interface, reducing the diffusion resistance of CO2. In addition, the adsorbent modified by 2-ethylhexyl phosphate has higher thermal stability, which is beneficial to the adsorption cycle performance to a certain extent. The organic amine and CO2 can undergo the following reversible chemical reaction:

[0029] . BRIEF DESCRIPTION OF THE DRAWINGS

[0030] Figure 1 This is a scanning electron microscope image of the carbon dioxide adsorbent S1 prepared when the mass of the steel slag is 270g;

[0031] Figure 2 This is a scanning electron microscope image of the carbon dioxide adsorbent S2 prepared when the mass of the coke powder is 15 g;

[0032] Figure 3 This is a test result diagram of carbon dioxide circulation of carbon dioxide adsorbent S3 in Example 3;

[0033] Figure 4 This is a test result diagram of the carbon dioxide cycle of the carbon dioxide adsorbent S4 in Example 3;

[0034] Figure 5 This is a test result diagram of the carbon dioxide cycle of the carbon dioxide adsorbent S5 in Example 3. DETAILED DESCRIPTION

[0035] In order to make the technical problems, technical solutions and beneficial effects to be solved by the present invention clearer, the present invention is further described in detail in conjunction with the embodiments and the accompanying drawings. It should be understood that the specific embodiments described herein are only used to explain the present invention and are not intended to limit the present invention. The technical solutions of the present invention are described in detail below in conjunction with the embodiments and the accompanying drawings, but the scope of protection is not limited thereto.

[0036] Example 1

[0037] A method for preparing a carbon dioxide adsorbent based on fly ash, steel slag and coke powder comprises the following steps:

[0038] 1. Grind and mix 30g of fly ash and a certain amount of steel slag. The particle size of the mixed fly ash and steel slag is 80 mesh to obtain a first mixture. The carbon content of the fly ash in the first mixture is 10wt.%, and the amount of ferroferric oxide in the steel slag is 10wt.%. Put the first mixture into a high-temperature furnace, introduce oxygen, and calcine at 850℃ for 8h. The heating rate of the high-temperature furnace is 10℃ / min to obtain a second mixture.

[0039] 2. Fully mix 18 g of the second mixture, 6 g of coke powder, 12 g of zinc oxide and 60 g of acrylic acid, and then put them into a 1 cubic centimeter cube particle mold. After shaping, put them into a high-temperature furnace isolated from air and calcine at 920°C for 6 hours. The heating rate of the high-temperature furnace is 10°C / min to obtain a third mixture.

[0040] 3. The third mixture was continued to be calcined at 650°C in a high temperature furnace with oxygen introduced therein, and the heating rate of the high temperature furnace was 10°C / min. After 6 hours, the sample was quickly placed in dry ice to cool down, and a fourth mixture was obtained. 0.5 g of 2-ethylhexyl phosphate and 0.5 g of polyethyleneimine were sprayed into the fourth mixture to obtain a carbon dioxide adsorbent S1.

[0041] 4. Test on the adsorption capacity of carbon dioxide adsorbent S1:

[0042] The carbon dioxide adsorption amount of the carbon dioxide adsorbent S1 was analyzed using a fixed bed reactor, and the adsorption temperature was 70°C. First, 1g of carbon dioxide adsorbent S1 was filled in the fixed bed, and then nitrogen was introduced at a gas flow rate of 80ml / min, and the temperature was raised to 100°C and maintained at 100°C for 1.5h. Then the temperature was lowered to 70°C, and the nitrogen was switched to a mixture of carbon dioxide and nitrogen, in which the volume concentration of carbon dioxide was 15%; the gas flow rate of the mixed gas was 60ml / min. At the same time, the concentration of the mixed gas was analyzed using a carbon dioxide analyzer, and the test results are listed in Table 1.

[0043]

[0044] It can be seen from Table 1 that as the amount of steel slag increases, the amount of carbon dioxide adsorbed increases. This is because the presence of steel slag is indeed conducive to pore formation, which in turn is conducive to the dispersion of polyethyleneimine and 2-ethylhexyl phosphate, and further conducive to the increase in carbon dioxide adsorption. When the amount of steel slag is 270g, the maximum carbon dioxide adsorption is 4.0mmol / g.

[0045] Example 2

[0046] A method for preparing a carbon dioxide adsorbent based on fly ash, steel slag and coke powder comprises the following steps:

[0047] 1. Grind and mix 30g of fly ash and 270g of steel slag. The particle size of the mixed fly ash and steel slag is 80 mesh to obtain a first mixture, wherein the fly ash contains 10wt.% carbon and the steel slag contains 10wt.% ferroferric oxide. Put the first mixture into a high-temperature furnace, introduce oxygen, and calcine at 850°C for 8h. The heating rate of the high-temperature furnace is 10°C / min to obtain a second mixture.

[0048] 2. Fully mix 18 g of the second mixture, a certain mass of coke powder, zinc oxide twice the mass of the coke powder, and 60 g of acrylic acid, and then put them into a 1 cubic centimeter cube particle mold. After shaping, put them into a high-temperature furnace isolated from air, and calcine at 920°C for 6 hours with a heating rate of 10°C / min to obtain a third mixture.

[0049] 3. The third mixture was continued to be calcined at 650°C in a high temperature furnace with oxygen introduced therein, and the heating rate of the high temperature furnace was 10°C / min. After 6 hours, the sample was quickly placed in dry ice to cool down, and a fourth mixture was obtained. 0.5 g of 2-ethylhexyl phosphate and 0.5 g of polyethyleneimine were sprayed into the fourth mixture to obtain a carbon dioxide adsorbent S2.

[0050] 4. Test on the adsorption capacity of carbon dioxide adsorbent S2:

[0051] The carbon dioxide adsorption amount of the carbon dioxide adsorbent S2 was analyzed using a fixed bed reactor, and the adsorption temperature was 70°C. First, 1g of carbon dioxide adsorbent S2 was filled in the fixed bed, and then nitrogen was introduced at a gas flow rate of 80ml / min, and the temperature was raised to 100°C and maintained at 100°C for 1.5h. Then the temperature was lowered to 70°C, and the nitrogen was switched to a mixture of carbon dioxide and nitrogen, where the volume concentration of carbon dioxide was 15% and the gas flow rate of the mixed gas was 60ml / min. At the same time, the concentration was analyzed using a carbon dioxide analyzer, and the test results are listed in Table 2.

[0052]

[0053] It can be seen from Table 2 that within the specified range, the more coke powder is added, the higher the adsorption of carbon dioxide adsorbent S2 is, and the adsorption value reaches 4.6mmol / g. This is because the carbon in the coke powder reacts with zinc oxide to generate new pores, which is beneficial to the subsequent loading and dispersion of 2-ethylhexyl phosphate as a surfactant and organic amines such as polyethyleneimine.

[0054] Example 3

[0055] A method for preparing a carbon dioxide adsorbent based on fly ash, steel slag and coke powder comprises the following steps:

[0056] 1. Grind and mix 30g of fly ash and 270g of steel slag to obtain a first mixture, wherein the particle size of the fly ash and steel slag after mixing is 80 mesh, wherein the carbon content of the fly ash is 10wt.%, and the iron oxide content of the steel slag is 10wt.%. Put the first mixture into a high-temperature furnace, introduce oxygen, and calcine at 850°C for 8h. The heating rate of the high-temperature furnace is 10°C / min to obtain a second mixture.

[0057] 2. Take 18g of the second mixture, 15g of coke powder, 30g of zinc oxide and 60g of acrylic acid, mix them thoroughly, and then put them into a 1 cubic centimeter cube particle mold. After shaping, put them into a high-temperature furnace, isolate them from air and calcine at 920°C for 6h. The heating rate of the high-temperature furnace is 10°C / min to obtain a third mixture.

[0058] 3. The third mixture was continued to be calcined at 650°C in a high temperature furnace with oxygen introduced therein, and the heating rate of the high temperature furnace was 10°C / min. After 6 hours, the sample was quickly placed in dry ice to cool down, and a fourth mixture was obtained. The mesopore diameter of the fourth mixture was 9.5 nm. 0.5 g of 2-ethylhexyl phosphate and 0.5 g of polyethyleneimine were sprayed into the fourth mixture to obtain a carbon dioxide adsorbent S3.

[0059] The other steps were the same, except that in the third step, only 0.5 g of polyethyleneimine was sprayed into the fourth mixture to obtain the carbon dioxide adsorbent S4.

[0060] The other steps were the same, except that in the third step, only 0.5 g of 2-ethylhexyl phosphate was sprayed into the fourth mixture to obtain the carbon dioxide absorbent S5.

[0061] 4. Test on the adsorption capacity of carbon dioxide adsorbents S3, S4 and S5:

[0062] The carbon dioxide adsorption cycle stability of the carbon dioxide adsorbent S3 obtained above was analyzed using a fixed bed reactor.

[0063] First, 1g of carbon dioxide adsorbent S3 was filled in the fixed bed, and then nitrogen was introduced at a gas flow rate of 80ml / min, and the temperature was raised to 100℃ and maintained at 100℃ for 1.5h. Then the temperature was lowered to 70℃ and the nitrogen was switched to a mixture of carbon dioxide and nitrogen, where the volume concentration of carbon dioxide was 15%; the gas flow rate of the mixture was 60ml / min, and the experiment was repeated ten times. At the same time, the concentration of the mixed gas was analyzed by a carbon dioxide analyzer. The test methods for carbon dioxide adsorbents S4 and S5 were the same as those for carbon dioxide adsorbent S3, and the test results are listed in Figure 3-Figure 5 middle.

[0064] pass Figure 3-Figure 5 It can be seen that only by adding 2-ethylhexyl phosphate and organic amines such as polyethyleneimine as surfactants at the same time can the cyclic stability of the adsorbent be improved, and adding only one of them will reduce its stability or adsorption capacity. When both exist at the same time, after 10 cycles of carbon dioxide adsorption and desorption experiments, the adsorption capacity can still be maintained at 4.4mmol / g.

[0065] Example 4

[0066] The pore structures of carbon dioxide adsorbent S1 and carbon dioxide adsorbent S2 were tested, and the test results are shown in Table 3. The pore structure parameters of each adsorbent were measured by a BSD-660 adsorption instrument, the specific surface area was measured by the BET method, the micropore volume was measured by the t-Plot method, and the average pore size was measured by the BJH method.

[0067]

[0068] Example 5

[0069] A method for preparing a carbon dioxide adsorbent based on fly ash, steel slag and coke powder comprises the following steps:

[0070] 1. Grind and mix 30g of fly ash and 270g of steel slag to obtain a first mixture. The particle size of the mixed fly ash and steel slag is 80 mesh, wherein the carbon content of the fly ash is 10wt.%, and the iron oxide content of the steel slag is 10wt.%. Put the first mixture into a high-temperature furnace, introduce oxygen, calcine at a certain temperature for 8h, and the heating rate is 10℃ / min to obtain a second mixture.

[0071] 2. Take 18g of the second mixture, 15g of coke powder, 30g of zinc oxide and 60g of acrylic acid, mix them thoroughly, and then put them into a 1 cubic centimeter cube particle mold. After shaping, put them into a high-temperature furnace, isolate them from air and calcine at 920°C for 6h. The heating rate of the high-temperature furnace is 10°C / min to obtain a third mixture.

[0072] 3. The third mixture was continued to be calcined at 650°C in a high temperature furnace with oxygen introduced therein, and the temperature rise rate of the high temperature furnace was 10°C / min. After 6 hours, the sample was quickly placed in dry ice to cool down, and a fourth mixture was obtained. The mesopore diameter of the fourth mixture was 8.9 nm. 0.5 g of 2-ethylhexyl phosphate and 0.5 g of polyethyleneimine were sprayed into the fourth mixture to obtain carbon dioxide adsorbent S6.

[0073] 4. Test on the adsorption capacity of carbon dioxide adsorbent S6:

[0074] The carbon dioxide adsorption capacity of the carbon dioxide adsorbent S6 was analyzed using a fixed bed reactor, and its carbon dioxide adsorption capacity at 70°C was tested.

[0075] First, 1g of carbon dioxide adsorbent S6 was filled in the fixed bed, and then nitrogen was introduced at a gas flow rate of 80ml / min, and the temperature was raised to 100℃ and maintained at 100℃ for 1.5h. Then the temperature was lowered to 70℃, and the nitrogen was switched to a mixture of carbon dioxide and nitrogen, where the volume concentration of carbon dioxide was 15%; the gas flow rate of the mixed gas was 60ml / min. At the same time, the concentration of the mixed gas was analyzed by a carbon dioxide analyzer, and the test results are listed in Table 4.

[0076]

[0077] It can be seen from Table 4 that the adsorption amount of carbon dioxide adsorbent S6 reaches the highest when the first calcination temperature is 950° C., which is 4.7 mmol / g. It can be seen that the pore structure can only reach the best within the temperature range set by the present invention.

[0078] Example 6

[0079] A method for preparing a carbon dioxide adsorbent based on fly ash, steel slag and coke powder comprises the following steps:

[0080] 1. Grind and mix 30g of fly ash and 270g of steel slag to obtain a first mixture, wherein the particle size of the fly ash and steel slag after mixing is 80 mesh, wherein the carbon content of the fly ash is 4-15wt.%, and the amount of ferroferric oxide in the steel slag is 10wt.%. Put the first mixture into a high-temperature furnace, introduce oxygen, and calcine at 950℃ for 8h. The heating rate of the high-temperature furnace is 10℃ / min to obtain a second mixture.

[0081] 2. Take 18g of the second mixture, 15g of coke powder, 30g of zinc oxide, and 60g of acrylic acid, mix them thoroughly, and then put them into a 1 cubic centimeter cube particle mold. After shaping, put them into a high-temperature furnace isolated from air and calcine at 1000°C for 6h. The heating rate of the high-temperature furnace is 10°C / min to obtain a third mixture.

[0082] 3. The third mixture was continued to be calcined at 700°C in a high temperature furnace with oxygen introduced therein, and the temperature rise rate of the high temperature furnace was 10°C / min. After 6 hours, the sample was quickly placed in dry ice to cool down, and a fourth mixture was obtained. The mesopore diameter of the fourth mixture was 9.4 nm. 0.5 g of 2-ethylhexyl phosphate and 0.5 g of polyethyleneimine were sprayed into the fourth mixture to obtain carbon dioxide adsorbent S7.

[0083] 4. Test on the adsorption capacity of carbon dioxide adsorbent S7:

[0084] The carbon dioxide adsorption capacity of the carbon dioxide adsorbent S7 was analyzed using a fixed bed reactor, and its carbon dioxide adsorption capacity at 80°C was tested.

[0085] First, 2g of carbon dioxide adsorbent S7 was filled in the fixed bed, and then nitrogen was introduced at a gas flow rate of 80ml / min, and the temperature was raised to 100℃ and maintained at 100℃ for 1.5h. Then the temperature was lowered to the required test temperature, and the nitrogen was switched to a mixture of carbon dioxide and nitrogen, where the volume concentration of carbon dioxide was 12% and the gas flow rate of the mixed gas was 60ml / min. At the same time, the concentration of the mixed gas was analyzed by a carbon dioxide analyzer, and the test results are listed in Table 5.

[0086]

[0087] It can be seen from Table 5 that when the carbon content in fly ash is high, its adsorption capacity is higher, and the maximum adsorption capacity is 4.7mmol / g. This is because the carbon in fly ash reacts with ferroferric oxide in steel slag to form microporous voids. The higher the carbon content, the larger the pore volume of the micropores, which is more conducive to the diffusion of carbon dioxide molecules.

[0088] Example 7

[0089] A method for preparing a carbon dioxide adsorbent based on fly ash, steel slag and coke powder comprises the following steps:

[0090] 1. Grind and mix 30g of fly ash and 270g of steel slag to obtain a first mixture, wherein the particle size of the fly ash and steel slag after mixing is 80 mesh, wherein the carbon content of the fly ash is 15wt.%, and the amount of ferroferric oxide in the steel slag is 10wt.%. Put the first mixture into a high-temperature furnace, introduce oxygen, and calcine at 950℃ for 8h. The heating rate of the high-temperature furnace is 10℃ / min to obtain a second mixture.

[0091] 2. Take 18g of the second mixture, 15g of coke powder, 30g of zinc oxide and 60g of acrylic acid, mix them thoroughly, and then put them into a 1 cubic centimeter cube particle mold. After shaping, put them into a high-temperature furnace isolated from air and calcine at 1200°C for 6h to obtain a third mixture.

[0092] 3. The third mixture was continued to be calcined at 800°C in a high temperature furnace with oxygen introduced therein, and the heating rate of the high temperature furnace was 10°C / min. After 6 hours, the sample was quickly placed in dry ice to cool down, and a fourth mixture was obtained. 0.5 g of 2-ethylhexyl phosphate and 0.5 g of polyethyleneimine were sprayed into the fourth mixture to obtain a carbon dioxide adsorbent S8.

[0093] 4. Test on the adsorption capacity of carbon dioxide adsorbent S8:

[0094] The carbon dioxide adsorption capacity of the carbon dioxide adsorbent S8 was analyzed using a fixed bed reactor, and its carbon dioxide adsorption capacity at 70°C was tested.

[0095] First, 1g of carbon dioxide adsorbent S8 was filled in a fixed bed, and then nitrogen was introduced at a gas flow rate of 80ml / min, and the temperature was raised to 100℃ and maintained at 100℃ for 1.5h. Then the temperature was lowered to the required test temperature, and the nitrogen was switched to a mixture of carbon dioxide and nitrogen, where the volume concentration of carbon dioxide was 15% and the gas flow rate of the mixture was 60ml / min. At the same time, the concentration was analyzed using a carbon dioxide analyzer, and the test results are listed in Table 6.

[0096]

[0097] It can be seen from Table 6 that the adsorption amount reaches the highest when the heating rate is 10℃ / min, and the adsorption amount of carbon dioxide adsorbent S8 is 4.7mmol / g. When the heating rate exceeds the specified range, the adsorption amount decreases instead. This is because the heating rate is too fast and the reaction between zinc oxide and coke powder is incomplete.

[0098] Example 8

[0099] A method for preparing a carbon dioxide adsorbent based on fly ash, steel slag and coke powder comprises the following steps:

[0100] 1. Grind and mix 30g of fly ash and 270g of steel slag to obtain a first mixture, wherein the particle size of the fly ash and steel slag after mixing is 80 mesh, wherein the carbon content of the fly ash is 10wt.%, and the iron oxide content of the steel slag is 10wt.%. Put the first mixture into a high-temperature furnace, introduce oxygen, and calcine at 950℃ for 8h. The heating rate of the high-temperature furnace is 10℃ / min to obtain a second mixture.

[0101] 2. Take 18g of the second mixture, 15g of coke powder, 30g of zinc oxide, and 60g of acrylic acid, mix them thoroughly, and then put them into a 1 cubic centimeter cube particle mold. After shaping, put them into a high-temperature furnace isolated from air and calcine at 1000°C for 6h. The heating rate of the high-temperature furnace is 8°C / min to obtain a third mixture.

[0102] 3. The third mixture was continued to be calcined at 800°C in a high temperature furnace with oxygen introduced therein, and the heating rate of the high temperature furnace was 10°C / min. After 6 hours, the sample was quickly placed in dry ice to cool down, and a fourth mixture was obtained. A certain amount of 2-ethylhexyl phosphate and polyethyleneimine were sprayed on the fourth mixture to obtain a carbon dioxide adsorbent S9. The added amounts of 2-ethylhexyl phosphate and polyethyleneimine were equal.

[0103] 4. Test on the adsorption capacity of carbon dioxide adsorbent S9:

[0104] The carbon dioxide adsorption capacity of the carbon dioxide adsorbent S9 was analyzed using a fixed bed reactor, and its carbon dioxide adsorption capacity at 70°C was tested.

[0105] First, 1g of carbon dioxide adsorbent S9 was filled in a fixed bed, and then nitrogen was introduced at a gas flow rate of 80ml / min, and the temperature was raised to 100℃ and maintained at 100℃ for 1.5h. Then the temperature was lowered to the required test temperature, and the nitrogen was switched to a mixture of carbon dioxide and nitrogen, where the volume concentration of carbon dioxide was 15% and the gas flow rate of the mixture was 60ml / min. At the same time, the concentration was analyzed using a carbon dioxide analyzer, and the test results are listed in Table 7.

[0106]

[0107] It can be seen from Table 7 that the addition of 2-ethylhexyl phosphate and polyethyleneimine is indeed beneficial to the improvement of adsorption performance. With the increase of surfactant mass, the adsorption performance is improved. When the addition amount of 2-ethylhexyl phosphate is 2g, the adsorption amount reaches the maximum of 4.8mmol / g.

[0108] Example 9

[0109] A method for preparing a carbon dioxide adsorbent based on fly ash, steel slag and coke powder comprises the following steps:

[0110] 1. Grind and mix 30g of fly ash and 270g of steel slag to obtain a first mixture, wherein the particle size of the fly ash and steel slag after mixing is 80 mesh, wherein the carbon content of the fly ash is 15wt.%, and the amount of ferroferric oxide in the steel slag is 10wt.%. Put the first mixture into a high-temperature furnace, introduce oxygen, and calcine at 950℃ for 8h. The heating rate of the high-temperature furnace is 10℃ / min to obtain a second mixture.

[0111] 2. Take 18g of the second mixture, 15g of coke powder, 30g of zinc oxide, and 60g of acrylic acid, mix them thoroughly, and then put them into a 1 cubic centimeter cube particle mold. After shaping, put them into a high-temperature furnace isolated from air and calcine at 1200°C for 6h. The heating rate of the high-temperature furnace is 10°C / min to obtain a third mixture.

[0112] 3. The third mixture was continued to be calcined at a certain temperature in a high temperature furnace with oxygen introduced therein, and the heating rate of the high temperature furnace was 10°C / min. After 6 hours, the sample was quickly placed in dry ice to cool down, and a fourth mixture was obtained. 2 g of 2-ethylhexyl phosphate and 2 g of polyethyleneimine were sprayed into the fourth mixture to obtain a carbon dioxide adsorbent S10.

[0113] 4. Test on the adsorption capacity of carbon dioxide adsorbent S10:

[0114] The carbon dioxide adsorption capacity of the carbon dioxide adsorbent S10 was analyzed using a fixed bed reactor, and its carbon dioxide adsorption capacity at 70°C was tested.

[0115] First, 1g of carbon dioxide adsorbent S10 was filled in a fixed bed, and then nitrogen was introduced at a gas flow rate of 80ml / min, and the temperature was raised to 100℃ and maintained at 100℃ for 1.5h. Then the temperature was lowered to 70℃, and the nitrogen was switched to a mixture of carbon dioxide and nitrogen, where the volume concentration of carbon dioxide was 15% and the gas flow rate of the mixture was 60ml / min. At the same time, the concentration was analyzed using a carbon dioxide analyzer, and the test results are listed in Table 8.

[0116]

[0117] It can be seen from Table 8 that the adsorption amount of carbon dioxide adsorbent S10 reaches a maximum of 4.6 mmol / g when the third calcination temperature is 800°C. It can be found that within this set temperature range, the adsorption amount increases with the increase of calcination temperature. However, below this temperature range, the reaction is incomplete, and above this temperature range, the pore structure of the adsorbent will be destroyed, so the adsorption amount decreases.

[0118] Example 10

[0119] A method for preparing a carbon dioxide adsorbent based on fly ash, steel slag and coke powder comprises the following steps:

[0120] 1. Grind and mix 30g of fly ash and 270g of steel slag to obtain a first mixture, wherein the particle size of the fly ash and steel slag after mixing is 80 mesh, wherein the carbon content of the fly ash is 15wt.%, and the amount of ferroferric oxide in the steel slag is 10-30wt.%. Put the first mixture into a high-temperature furnace, introduce oxygen, calcine at 950℃ for 8h, and the heating rate is 10℃ / min to obtain a second mixture.

[0121] 2. Take 18g of the second mixture, 15g of coke powder, 30g of zinc oxide and 60g of acrylic acid, mix them thoroughly, and then put them into a 1 cubic centimeter cube particle mold. After shaping, put them into a high-temperature furnace isolated from air and calcine at 1000℃ for 6h. The heating rate of the high-temperature furnace is 10℃ / min to obtain a third mixture.

[0122] 3. The third mixture was continued to be calcined at 700°C in a high temperature furnace with oxygen introduced therein, and the heating rate of the high temperature furnace was 10°C / min. After 6 hours, the sample was quickly placed in dry ice to cool down, and a fourth mixture was obtained. 2 g of 2-ethylhexyl phosphate and 2 g of polyethyleneimine were sprayed into the fourth mixture to obtain a carbon dioxide adsorbent S11.

[0123] 4. Test on the adsorption capacity of carbon dioxide adsorbent S11:

[0124] The carbon dioxide adsorption capacity of the carbon dioxide adsorbent S11 was analyzed using a fixed bed reactor, and its carbon dioxide adsorption capacity at 70°C was tested.

[0125] First, 2g of carbon dioxide adsorbent S11 was filled in a fixed bed, and then nitrogen was introduced at a gas flow rate of 80ml / min, and the temperature was raised to 100℃ and maintained at 100℃ for 1.5h. Then the temperature was lowered to the required test temperature, and the nitrogen was switched to a mixture of carbon dioxide and nitrogen, where the volume concentration of carbon dioxide was 15% and the gas flow rate of the mixture was 60ml / min. At the same time, the concentration was analyzed using a carbon dioxide analyzer, and the test results are listed in Table 9.

[0126]

[0127] It can be seen from Table 9 that when the content of ferroferric oxide in steel slag is higher, the adsorption amount of carbon dioxide adsorbent S11 is higher, and the maximum adsorption amount is 4.8mmol / g. This is because the carbon in fly ash reacts with ferroferric oxide in steel slag to form microporous voids. The higher the content of ferroferric oxide, the larger the pore volume of micropores, which is more conducive to the diffusion of carbon dioxide molecules.

[0128] The above content is a further detailed description of the present invention in combination with a specific preferred embodiment. It cannot be determined that the specific embodiments of the present invention are limited to this. For ordinary technicians in the technical field to which the present invention belongs, several simple deductions or substitutions can be made without departing from the present invention, which should be regarded as belonging to the present invention and the scope of patent protection determined by the submitted claims.

Claims

1. A solid carbon dioxide adsorbent, characterized in that: The ingredients include fly ash, steel slag, coke powder, zinc oxide, acrylic acid, surfactant and organic amine; the fly ash contains 4-15wt.% carbon, and the steel slag contains 10-30wt.% ferroferric oxide; the mass ratio of fly ash to steel slag is 1:3-9; the mass ratio of zinc oxide to coke powder is 2:1; The surfactant is 2-ethylhexyl phosphate, and the organic amine is polyethyleneimine; the mass ratio of 2-ethylhexyl phosphate to polyethyleneimine is 1:1; The particle size of the mixed fly ash and steel slag is <100 mesh.

2. The method for preparing a solid carbon dioxide adsorbent according to claim 1, characterized in that: The following steps are involved: 1) fully mixing and grinding fly ash and steel slag to obtain a first mixture; calcining the first mixture at 700-950° C. for 5-10 hours in an aerobic environment to obtain a second mixture; 2) the second mixture, coke powder, zinc oxide and acrylic acid are fully mixed and shaped, and then isolated from air and calcined at 920-1200° C. to obtain a third mixture; 3) calcining the third mixture at 650-800° C. for 5-8 hours in an aerobic environment, and then cooling the mixture to obtain a fourth mixture; spraying a mixed solution of a surfactant and an organic amine onto the fourth mixture, and drying the mixture to obtain a carbon dioxide adsorbent; The heating rate of calcination in step 1), step 2), and step 3) is 2-10°C / min; The mass ratio of the second mixture to the coke powder is 3:1-2.5, and the mass ratio of acrylic acid to the second mixture is 4:1.2-2.4; The micropore volume of the obtained second mixture was 0.15-0.55 cm 3 / g; the mesopore diameter of the fourth mixture obtained is 8.5-10.7nm; The mass ratio of the surfactant to the fourth mixture is 0.01-0.1:1.

Citation Information

Cited By

  • Carbon dioxide adsorption carbon material as well as preparation method and application thereof

    CN121755163A

  • Carbon dioxide adsorbing carbon material, method for producing the same, and use thereof

    CN121755163B

  • Solid waste source solid amine adsorbent and preparation method thereof

    CN121847073A

  • Solid waste source solid amine adsorbent and preparation method thereof

    CN121847073B

  • Batch synthesis method of CO2 charged adsorbent

    CN122273490A