High performance concrete for ultra-thin composite floor slab and preparation method thereof

Through the composite of high-performance concrete, the problems of low strength and construction difficulties of ultra-thin overlapping floor slabs have been solved, early strength development and construction efficiency have been achieved, and the construction needs of prefabricated buildings have been met.

CN118221401BActive Publication Date: 2024-11-22XI'AN UNIVERSITY OF ARCHITECTURE AND TECHNOLOGY
View PDF 0 Cites 1 Cited by

Patent Information

Application Number
CN202410220206.9
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-02-28
Publication Date
2024-11-22
Estimated Expiration
2044-02-28

AI Technical Summary

Technical Problem

The existing ultra-thin overlapping floor slabs have low strength, poor toughness and difficult construction. Especially in prefabricated buildings, ordinary reinforced truss floor bearing plates and PC overlapping boards have problems such as transportation damage, high self-weight and high construction costs.

Method used

A high-performance concrete preparation method is adopted, including cement, modified ore powder, magnesium oxide fume, activation enhancer, water reducing agent, defoaming agent, quartz sand, modified resin liquid, curing agent and fiber, through The raw materials are used to meet the mechanical properties of self-leveling, improve early strength and reduce construction support needs, and use modified ore powder and modified resin liquid to form a multi-layer core-shell structure and dynamic cross-linked grid to improve the mechanical strength and toughness of concrete.

Benefits of technology

The mechanical properties of high-performance concrete have been optimized, and the early strength has developed rapidly, reducing construction support and lifting costs, speeding up construction progress, and improving the installation efficiency and safety of floor slabs.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0004717922280000141
    Figure BDA0004717922280000141
Patent Text Reader

Abstract

The invention discloses a high-performance concrete for ultra-thin laminated floor slabs and a preparation method thereof. The concrete comprises the following raw materials in parts by weight: 700-900 parts, 100-200 parts of modified mineral powder, 10-100 parts of magnesium oxide silica fume, 8-10 parts of activation enhancer, 1-5 parts of water reducer, 1-3 parts of defoamer, 1000-1500 parts of quartz sand, 300-500 parts of modified resin liquid, 150-250 parts of curing agent, 200-300 parts of water and 30-100 parts of fiber; the modified resin molecule is a hyperbranched structure and contains elastic segments and dynamically cross-linked grids, and can form a continuous three-dimensional elastic network structure in fillers such as cement, and the fillers can also pass through the pores of the modified resin grids to form a staggered continuous grid structure, thereby increasing the adaptability between the fillers and thus improving the mechanical strength of the concrete.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of lightweight building materials, and in particular to high-performance concrete for ultra-thin composite floor slabs and a preparation method thereof. Background Art

[0002] The advantages of prefabricated buildings, coupled with the support and development requirements of national policies, have prompted the reform and upgrading of the construction industry. However, the prefabricated construction scheme that only uses prefabricated stairs and prefabricated walls can no longer meet the requirements of the current prefabricated construction industry, so different forms of prefabricated floor slabs are often used in the market to achieve the goal of increasing the assembly rate. In existing engineering construction, ordinary steel truss floor slabs are mostly suitable for steel structure projects, and wooden and aluminum formwork floor slabs need to be dismantled after construction, which does not meet the development requirements of prefabricated building construction.

[0003] Although ordinary PC composite panels are suitable for most projects, they also have many problems. First, they have low strength and slow strength development. They not only require steam curing and molding, but also have a high damage rate during transportation. Secondly, PC composite panels need to be prefabricated in the factory with 60mm thick prefabricated components. Due to their heavy weight, this type of composite panel requires lifting equipment to participate in the construction during transportation and construction site. In addition, due to their low strength and poor toughness, a lot of support is required during the construction process. After the construction is completed, due to the accuracy and force requirements, post-casting strips need to be laid at the board joints. Its production and construction methods not only extend the construction time but also increase the construction cost. Summary of the invention

[0004] The purpose of the present invention is to provide a high-performance concrete for ultra-thin composite floor slabs and a preparation method thereof, so as to solve the problems of low strength, poor toughness and difficult construction of ultra-thin composite floor slabs at the current stage.

[0005] The purpose of the present invention can be achieved through the following technical solutions:

[0006] A method for preparing high-performance concrete for ultra-thin composite floor slabs, comprising the following steps:

[0007] Weigh the following raw materials in parts by weight: 700-900 parts of cement, 100-200 parts of modified mineral powder, 10-100 parts of magnesium oxide silica fume, 8-10 parts of activation enhancer, 1-5 parts of water reducer, 1-3 parts of defoamer, 1000-1500 parts of quartz sand, 300-500 parts of modified resin liquid, 150-250 parts of curing agent, 200-300 parts of water and 30-100 parts of fiber, mix the raw materials evenly to obtain concrete.

[0008] The cement is a mixture of one or more of silicate cement, sulphoaluminate cement and aluminate cement in any proportion; the silicon dioxide content in magnesium oxide silica fume is 90%; the activation enhancer is a mixture of one or two of nano alumina, nano magnesium oxide, hydrated calcium silicate and quicklime in any proportion; the water reducer is a powdered polycarboxylic acid water reducer with a water reduction rate greater than 30%; the defoamer is a mixture of one or two of powdered organic silicon, polyether modified silicone oil and tributyl phosphate in any proportion; the fiber is a mixture of two or more of steel fiber, polypropylene fiber, polyethylene fiber, basalt fiber and rubber fiber in any proportion; and the curing agent is one of T31 curing agent, 590 curing agent and H113 curing agent.

[0009] Furthermore, the modified mineral powder is prepared by the following steps:

[0010] Step A1: Disperse the mineral powder in ethanol, add KH550 and deionized water, react for 2-3 hours at a speed of 150-200 r / min and a temperature of 40-50° C. to obtain a pretreated mineral powder, mix epichlorohydrin and tetrabutylammonium hydrogen sulfate, add polyvinyl alcohol and sodium hydroxide solution at a speed of 150-200 r / min and a temperature of 0-3° C., heat to 15-20° C., and react for 3-4 hours to obtain a treatment agent;

[0011] Step A2: The pretreated mineral powder, the treatment agent and DMF are mixed evenly, and reacted for 3-5 hours at a speed of 120-150 r / min, a temperature of 30-40°C and a pH value of 11-12, and then 2-aminobenzimidazole is added, and the reaction is continued for 2-3 hours to obtain a precursor, and the precursor is dispersed in DMF, sodium bicarbonate is added, and copper acetate is added at a speed of 60-80 r / min and a temperature of 50-60°C, and stirred for 20-25 hours to obtain a modified mineral powder.

[0012] Furthermore, the amount of KH550 described in step A1 is 1-1.5 of the mass of the mineral powder, the amount ratio of epichlorohydrin, tetrabutylammonium hydrogen sulfate, polyvinyl alcohol and sodium hydroxide solution is 1 mol:8.5mmol:0.2mol:160mL, the mass fraction of the sodium hydroxide solution is 35%, and the molecular weight of polypropylene alcohol is 1000.

[0013] Furthermore, the molar ratio of the amino groups on the surface of the pretreated mineral powder in step A2, the epoxy groups on the treating agent and 2-aminobenzimidazole is 1:3:2.2, and the mass ratio of the precursor, sodium bicarbonate and copper acetate is 1:4:10.

[0014] Further, the modified resin solution is prepared by the following steps:

[0015] Step B1: 4-formylphenylboronic acid and tetrahydrofuran are mixed, nitrogen is introduced for protection, and the reaction is carried out for 3-5 hours at a speed of 150-200 r / min and a temperature of 50-60° C., and then ethanolamine is added and the reaction is continued for 6-8 hours to obtain a chain extender. Polytetrahydrofuran ether diol, isophorone diisocyanate and DMF are mixed, nitrogen is introduced for protection, and the reaction is carried out for 1-2 hours at a speed of 120-150 r / min and a temperature of 70-75° C. to obtain a prepolymer;

[0016] Step B2: The prepolymer, chain extender and DMF are mixed evenly, nitrogen protection is introduced, and the reaction is carried out for 5-7 hours at a speed of 60-80 r / min and a temperature of 75-80° C., and (3-aminopropyl) dimethylethoxysilane is added, and the reaction is continued for 2-4 hours to obtain an elastic monomer, and the elastic monomer, diphenyldichlorosilane and deionized water are mixed, and the stirring is carried out for 10-15 minutes at a speed of 200-300 r / min and a temperature of 60-70° C., and concentrated sulfuric acid and 1,1,3,3-tetramethyldisiloxane are added, and the reaction is carried out for 4-6 hours, and the pH is adjusted to neutral to obtain a hydrogen-terminated polysiloxane;

[0017] Step B3: Evenly mix the hydrogen-terminated polysiloxane, p-hydroxystyrene and DMF, stir and add chloroplatinic acid at a speed of 150-200 r / min and a temperature of 50-60°C, and react for 10-15 hours to obtain intermediate 1; evenly mix intermediate 1, epichlorohydrin and DMF, add sodium hydroxide solution, and react for 2-3 hours at a speed of 120-150 r / min and a temperature of 80-85°C, then distill off DMF, and add the substrate into ethyl acetate to obtain a modified resin liquid.

[0018] Furthermore, the molar ratio of 4-formylphenylboronic acid and ethanolamine in step B1 is 1:1, the molar ratio of polytetramethylene ether diol and isophorone diisocyanate is 2:5, and the molecular weight of polytetramethylene ether diol is 2000.

[0019] Furthermore, the mass ratio of the prepolymer, chain extender and (3-aminopropyl)dimethylethoxysilane described in step B2 is 12:3:1, the amount ratio of the elastic monomer, diphenyldichlorosilane and deionized water and 1,1,3,3-tetramethyldisiloxane is 47g:8g:100mL:5.6g, and the amount of concentrated sulfuric acid is 3% of the mass of diphenyldichlorosilane.

[0020] Furthermore, the molar ratio of SiH on the hydrogen-terminated polysiloxane and p-hydroxystyrene in step B3 is 1:1, the amount of chloroplatinic acid used is 1‰ of the mass of p-hydroxystyrene, the amount ratio of intermediate 1, epichlorohydrin and sodium hydroxide solution is 1g:2g:10mL, the mass fraction of sodium hydroxide solution is 30%, and the amount of substrate and ethyl acetate used is 1g:10mL.

[0021] Beneficial effects of the present invention: The high-performance concrete for ultra-thin composite floor slabs disclosed in the present application includes the following raw materials: cement, modified mineral powder, magnesium oxide silica fume, activation enhancer, water reducer, defoamer, quartz sand, modified resin liquid, curing agent, water and fiber. The raw materials are compounded to achieve optimal mechanical properties under the premise of self-leveling, and the early strength develops rapidly. During the factory production process, the requirement of rapid demolding can be achieved without steaming. The high-performance concrete is modified by adding fibers and activation enhancer components to improve mechanical strength, enhance rigidity and toughness. When the floor slab is in use, on-site support is reduced and it can be installed in place only by manual labor, saving hoisting costs and speeding up construction progress. The modified mineral powder is treated with KH550 with mineral powder as raw material so that active amino groups are grafted on the surface to obtain pretreated mineral powder. Epichlorohydrin and polyvinyl alcohol are reacted to graft epoxy groups on the polyethylene molecular chain to obtain a treatment agent. The pretreated mineral powder and the treatment agent are reacted so that the amino groups on the surface of the pretreated mineral powder react with part of the epoxy groups on the treatment agent to form a structure in which the treatment agent molecules encapsulate the pretreated mineral powder. 2-aminobenzimidazole is then added so that the remaining epoxy groups react with the amino groups on the 2-aminobenzimidazole to obtain a precursor. The precursor is blended with copper acetate so that the imidazole on the surface of the precursor cooperates with copper ions to form a further coating. The modified mineral powder is a multi-layer core-shell structure, which can be formed through the molecular movement between different shell layers. The toughness of concrete is improved. The modified resin liquid uses 4-formylphenylboronic acid as a raw material. The boric acid groups on the 4-formylphenylboronic acid react to form a BO six-membered ring dynamic cross-linked network structure. Ethanolamine is then added to react the amino groups on the ethanolamine with the aldehyde groups to obtain a chain extender. Polytetramethyleneimine ether diol and isophorone diisocyanate are reacted to obtain a prepolymer. The prepolymer and the chain extender are reacted and then end-capped with (3-aminopropyl) dimethylethoxysilane to obtain an elastic monomer. The elastic monomer and diphenyldichlorosilane are hydrolyzed and then polymerized with 1,1,3,3-tetramethyldisiloxane to form a terminal hydrogen polysiloxane. The terminal hydrogen polysiloxane and p-hydroxystyrene are reacted under the action of chloroplatinic acid to make the S on the terminal hydrogen polysiloxane. The iH bond reacts with the double bond on p-hydroxystyrene to obtain an intermediate 1, and the intermediate 1 is reacted with epichlorohydrin and then blended with ethyl acetate to obtain a modified resin liquid. The modified resin molecule is a hyperbranched structure and contains elastic segments and dynamic cross-linked grids, which can form a continuous three-dimensional elastic network structure in fillers such as cement. At the same time, the filler can also pass through the pores of the modified resin grid to form an interlaced continuous grid structure, thereby increasing the adaptability between the fillers and thereby improving the mechanical strength of the concrete. DETAILED DESCRIPTION

[0022] The technical solutions in the embodiments of the present invention are described clearly and completely below. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of them. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0023] Example 1

[0024] A method for preparing high-performance concrete for ultra-thin composite floor slabs, comprising the following steps:

[0025] Weigh the following raw materials in parts by weight: 700 parts of cement, 100 parts of modified mineral powder, 10 parts of magnesium oxide silica fume, 8 parts of activation enhancer, 1 part of water reducer, 1 part of defoamer, 1000 parts of quartz sand, 300 parts of modified resin liquid, 150 parts of curing agent, 200 parts of water and 30 parts of fiber, mix the raw materials evenly, and prepare concrete.

[0026] The cement is silicate cement P.O42.5, the silicon dioxide content in magnesium oxide silica fume is 90%, the activation enhancer is nano alumina, the water reducer is water reducer CSP-13, the defoamer is AFE-1410, the particle size of quartz sand is 1 mm, the fiber is a mixture of steel fiber and polypropylene fiber in a mass ratio of 1:1, the length of the steel fiber is 30 mm, the diameter is 0.2 mm, the length of the polypropylene fiber is 6 mm, the diameter is 0.5 mm, the molecular weight is 80000, and the curing agent is T31 curing agent.

[0027] The modified mineral powder is prepared by the following steps:

[0028] Step A1: disperse the mineral powder in ethanol, add KH550 and deionized water, react for 2 hours at a speed of 150 r / min and a temperature of 40°C to obtain a pretreated mineral powder, mix epichlorohydrin and tetrabutylammonium hydrogen sulfate, add polyvinyl alcohol and sodium hydroxide solution at a speed of 150 r / min and a temperature of 0°C, heat to 15°C, and react for 3 hours to obtain a treatment agent;

[0029] Step A2: The pretreated mineral powder, the treatment agent and DMF are mixed evenly, and reacted for 3 hours at a speed of 120 r / min, a temperature of 30°C and a pH value of 11, and then 2-aminobenzimidazole is added, and the reaction is continued for 2 hours to obtain a precursor, and the precursor is dispersed in DMF, sodium bicarbonate is added, and copper acetate is added at a speed of 60 r / min and a temperature of 50°C, and stirred for 20 hours to obtain a modified mineral powder.

[0030] The dosage of KH550 described in step A1 is 1% of the mass of the mineral powder, the mineral powder is S95, the dosage ratio of epichlorohydrin, tetrabutylammonium hydrogen sulfate, polyvinyl alcohol and sodium hydroxide solution is 1 mol:8.5 mmol:0.2 mol:160 mL, the mass fraction of the sodium hydroxide solution is 35%, and the molecular weight of polypropylene alcohol is 1000.

[0031] The molar ratio of the amino groups on the surface of the pretreated mineral powder, the epoxy groups on the treating agent and 2-aminobenzimidazole in step A2 is 1:3:2.2, and the mass ratio of the precursor, sodium bicarbonate and copper acetate is 1:4:10.

[0032] The modified resin solution is prepared by the following steps:

[0033] Step B1: 4-formylphenylboronic acid and tetrahydrofuran are mixed, nitrogen is introduced for protection, and the reaction is carried out for 3 hours at a speed of 150 r / min and a temperature of 50° C., and then ethanolamine is added and the reaction is continued for 6 hours. Polytetrahydrofuran ether diol, isophorone diisocyanate and DMF are mixed, nitrogen is introduced for protection, and the reaction is carried out for 1 hour at a speed of 120 r / min and a temperature of 70° C. to obtain a prepolymer;

[0034] Step B2: The prepolymer, chain extender and DMF are mixed evenly, nitrogen protection is introduced, and the reaction is carried out at a speed of 60 r / min and a temperature of 75° C. for 5 hours, and (3-aminopropyl) dimethylethoxysilane is added, and the reaction is continued for 2 hours to obtain an elastic monomer, and the elastic monomer, diphenyldichlorosilane and deionized water are mixed, and the reaction is carried out at a speed of 200 r / min and a temperature of 60° C. After stirring for 10 minutes, concentrated sulfuric acid and 1,1,3,3-tetramethyldisiloxane are added, and the reaction is carried out for 4 hours, and the pH is adjusted to neutral to obtain a hydrogen-terminated polysiloxane;

[0035] Step B3: Mix the hydrogen-terminated polysiloxane, p-hydroxystyrene and DMF evenly, stir and add chloroplatinic acid at a speed of 150 r / min and a temperature of 50°C, and react for 10 hours to obtain intermediate 1. Mix the intermediate 1, epichlorohydrin and DMF evenly, add sodium hydroxide solution, and react for 2 hours at a speed of 120 r / min and a temperature of 80°C. After that, distill off DMF, add the substrate into ethyl acetate to obtain a modified resin liquid.

[0036] The molar ratio of 4-formylphenylboronic acid and ethanolamine in step B1 is 1:1, the molar ratio of polytetramethylene ether diol and isophorone diisocyanate is 2:5, and the molecular weight of polytetramethylene ether diol is 2000.

[0037] The mass ratio of the prepolymer, chain extender and (3-aminopropyl)dimethylethoxysilane described in step B2 is 12:3:1, the amount ratio of the elastic monomer, diphenyldichlorosilane and deionized water and 1,1,3,3-tetramethyldisiloxane is 47g:8g:100mL:5.6g, and the amount of concentrated sulfuric acid is 3% of the mass of diphenyldichlorosilane.

[0038] The molar ratio of Si-H on the hydrogen-terminated polysiloxane and p-hydroxystyrene in step B3 is 1:1, the amount of chloroplatinic acid used is 1‰ of the mass of p-hydroxystyrene, the amount ratio of intermediate 1, epichlorohydrin and sodium hydroxide solution is 1g:2g:10mL, the mass fraction of sodium hydroxide solution is 30%, and the amount of substrate and ethyl acetate used is 1g:10mL.

[0039] Example 2

[0040] A method for preparing high-performance concrete for ultra-thin composite floor slabs, comprising the following steps:

[0041] Weigh the following raw materials in parts by weight: 750 parts of cement, 150 parts of modified mineral powder, 50 parts of magnesium oxide silica fume, 8 parts of activation enhancer, 4.5 parts of water reducer, 3 parts of defoamer, 1000 parts of quartz sand, 300 parts of modified resin liquid, 180 parts of curing agent, 230 parts of water and 90 parts of fiber, mix the raw materials evenly, and prepare concrete.

[0042] The cement is sulphoaluminate cement, the silicon dioxide content in magnesium oxide silica fume is 90%, the activation enhancer is nano magnesium oxide, the water reducer is water reducer FDN-F1, the defoamer is OFX-0400, the particle size of quartz sand is 1 mm, the fiber is a mixture of polypropylene fiber and polyethylene fiber in a mass ratio of 1:1, the length of the polypropylene fiber and the polyethylene fiber is 6 mm, the diameter is 0.5 mm, the molecular weight is 80000, and the curing agent is T31 curing agent, 590 curing agent and H113 curing agent.

[0043] The modified mineral powder is prepared by the following steps:

[0044] Step A1: disperse the mineral powder in ethanol, add KH550 and deionized water, react for 2.5 hours at a speed of 150 r / min and a temperature of 45°C to obtain a pretreated mineral powder, mix epichlorohydrin and tetrabutylammonium hydrogen sulfate, add polyvinyl alcohol and sodium hydroxide solution at a speed of 150 r / min and a temperature of 3°C, heat to 18°C, and react for 3.5 hours to obtain a treatment agent;

[0045] Step A2: The pretreated mineral powder, the treatment agent and DMF are mixed evenly, and reacted for 4 hours at a speed of 120 r / min, a temperature of 35°C and a pH value of 12. Then, 2-aminobenzimidazole is added and the reaction is continued for 2.5 hours to obtain a precursor. The precursor is dispersed in DMF, sodium bicarbonate is added, and copper acetate is added at a speed of 60 r / min and a temperature of 55°C. The mixture is stirred and copper acetate is added and stirred for 25 hours to obtain a modified mineral powder.

[0046] The dosage of KH550 described in step A1 is 1-1.5% of the mass of the mineral powder, the mineral powder is S95, the dosage ratio of epichlorohydrin, tetrabutylammonium hydrogen sulfate, polyvinyl alcohol and sodium hydroxide solution is 1 mol:8.5 mmol:0.2 mol:160 mL, the mass fraction of the sodium hydroxide solution is 35%, and the molecular weight of polypropylene alcohol is 1000.

[0047] The molar ratio of the amino groups on the surface of the pretreated mineral powder, the epoxy groups on the treating agent and 2-aminobenzimidazole in step A2 is 1:3:2.2, and the mass ratio of the precursor, sodium bicarbonate and copper acetate is 1:4:10.

[0048] The modified resin solution is prepared by the following steps:

[0049] Step B1: 4-formylphenylboronic acid and tetrahydrofuran were mixed, nitrogen was introduced for protection, and the reaction was carried out for 4 hours at a speed of 150 r / min and a temperature of 55° C., and then ethanolamine was added and the reaction was continued for 7 hours. Polytetrahydrofuran ether diol, isophorone diisocyanate and DMF were mixed, nitrogen was introduced for protection, and the reaction was carried out for 1.5 hours at a speed of 120 r / min and a temperature of 73° C. to obtain a prepolymer;

[0050] Step B2: The prepolymer, chain extender and DMF are mixed evenly, nitrogen protection is introduced, and the reaction is carried out at a speed of 60 r / min and a temperature of 78° C. for 6 hours, and (3-aminopropyl) dimethylethoxysilane is added, and the reaction is continued for 3 hours to obtain an elastic monomer, and the elastic monomer, diphenyldichlorosilane and deionized water are mixed, and the stirring is carried out at a speed of 200 r / min and a temperature of 65° C. for 15 minutes, and concentrated sulfuric acid and 1,1,3,3-tetramethyldisiloxane are added. After reacting for 5 hours, the pH is adjusted to neutral to obtain a hydrogen-terminated polysiloxane;

[0051] Step B3: Mix the hydrogen-terminated polysiloxane, p-hydroxystyrene and DMF evenly, stir and add chloroplatinic acid at a speed of 150 r / min and a temperature of 55°C, and react for 13 hours to obtain intermediate 1. Mix the intermediate 1, epichlorohydrin and DMF evenly, add sodium hydroxide solution, and react for 3 hours at a speed of 120 r / min and a temperature of 83°C. After that, distill off DMF, add the substrate into ethyl acetate to obtain a modified resin liquid.

[0052] The molar ratio of 4-formylphenylboronic acid and ethanolamine in step B1 is 1:1, the molar ratio of polytetramethylene ether diol and isophorone diisocyanate is 2:5, and the molecular weight of polytetramethylene ether diol is 2000.

[0053] The mass ratio of the prepolymer, chain extender and (3-aminopropyl)dimethylethoxysilane described in step B2 is 12:3:1, the amount ratio of the elastic monomer, diphenyldichlorosilane and deionized water and 1,1,3,3-tetramethyldisiloxane is 47g:8g:100mL:5.6g, and the amount of concentrated sulfuric acid is 3% of the mass of diphenyldichlorosilane.

[0054] The molar ratio of Si-H on the hydrogen-terminated polysiloxane and p-hydroxystyrene in step B3 is 1:1, the amount of chloroplatinic acid used is 1‰ of the mass of p-hydroxystyrene, the amount ratio of intermediate 1, epichlorohydrin and sodium hydroxide solution is 1g:2g:10mL, the mass fraction of sodium hydroxide solution is 30%, and the amount of substrate and ethyl acetate used is 1g:10mL.

[0055] Example 3

[0056] A method for preparing high-performance concrete for ultra-thin composite floor slabs, comprising the following steps:

[0057] Weigh the following raw materials in parts by weight: 800 parts of cement, 150 parts of modified mineral powder, 50 parts of magnesium oxide silica fume, 8 parts of activation enhancer, 4.5 parts of water reducer, 3 parts of defoamer, 1000 parts of quartz sand, 350 parts of modified resin liquid, 150 parts of curing agent, 230 parts of water and 90 parts of fiber, mix the raw materials evenly, and prepare concrete.

[0058] The cement is aluminate cement CA50, the silicon dioxide content in magnesium oxide silica fume is 90%, the activation enhancer is a mixture of hydrated calcium silicate and quicklime in a mass ratio of 1:1, the water reducer is FDN-F2, the defoamer is tributyl phosphate, the particle size of quartz sand is 1 mm, the fiber is a mixture of basalt fiber and rubber fiber in a mass ratio of 1:1, the length of the basalt fiber is 6 mm, the diameter is 9 μm, the rubber fiber is nylon 6 fiber, the length is 6 mm, the diameter is 0.5 mm, the molecular weight is 30000, and the curing agent is H113 curing agent.

[0059] The modified mineral powder is prepared by the following steps:

[0060] Step A1: disperse the mineral powder in ethanol, add KH550 and deionized water, react for 3 hours at a speed of 200 r / min and a temperature of 50°C to obtain a pretreated mineral powder, mix epichlorohydrin and tetrabutylammonium hydrogen sulfate, add polyvinyl alcohol and sodium hydroxide solution at a speed of 200 r / min and a temperature of 3°C, heat to 20°C, and react for 4 hours to obtain a treatment agent;

[0061] Step A2: The pretreated mineral powder, the treatment agent and DMF are mixed evenly, and reacted for 5 hours at a speed of 150 r / min, a temperature of 40°C and a pH value of 12, and then 2-aminobenzimidazole is added, and the reaction is continued for 3 hours to obtain a precursor, and the precursor is dispersed in DMF, sodium bicarbonate is added, and copper acetate is added at a speed of 80 r / min and a temperature of 60°C, and stirred for 25 hours to obtain a modified mineral powder.

[0062] The dosage of KH550 described in step A1 is 1.5% of the mass of the mineral powder, the mineral powder is S95, the dosage ratio of epichlorohydrin, tetrabutylammonium hydrogen sulfate, polyvinyl alcohol and sodium hydroxide solution is 1 mol:8.5 mmol:0.2 mol:160 mL, the mass fraction of the sodium hydroxide solution is 35%, and the molecular weight of polypropylene alcohol is 1000.

[0063] The molar ratio of the amino groups on the surface of the pretreated mineral powder, the epoxy groups on the treating agent and 2-aminobenzimidazole in step A2 is 1:3:2.2, and the mass ratio of the precursor, sodium bicarbonate and copper acetate is 1:4:10.

[0064] The modified resin solution is prepared by the following steps:

[0065] Step B1: 4-formylphenylboronic acid and tetrahydrofuran are mixed, nitrogen is introduced for protection, and the reaction is carried out for 5 hours at a speed of 200 r / min and a temperature of 60° C., and then ethanolamine is added and the reaction is continued for 8 hours. Polytetrahydrofuran ether diol, isophorone diisocyanate and DMF are mixed, nitrogen is introduced for protection, and the reaction is carried out for 2 hours at a speed of 150 r / min and a temperature of 75° C. to obtain a prepolymer;

[0066] Step B2: The prepolymer, chain extender and DMF are mixed evenly, nitrogen protection is introduced, and the reaction is carried out at a speed of 80 r / min and a temperature of 80° C. for 7 hours, and (3-aminopropyl) dimethylethoxysilane is added, and the reaction is continued for 4 hours to obtain an elastic monomer, and the elastic monomer, diphenyldichlorosilane and deionized water are mixed, and the reaction is carried out at a speed of 300 r / min and a temperature of 70° C. After stirring for 15 minutes, concentrated sulfuric acid and 1,1,3,3-tetramethyldisiloxane are added, and the reaction is carried out for 6 hours, and the pH is adjusted to neutral to obtain a hydrogen-terminated polysiloxane;

[0067] Step B3: Mix the hydrogen-terminated polysiloxane, p-hydroxystyrene and DMF evenly, stir and add chloroplatinic acid at a speed of 200 r / min and a temperature of 60°C, and react for 15 hours to obtain intermediate 1. Mix the intermediate 1, epichlorohydrin and DMF evenly, add sodium hydroxide solution, and react for 3 hours at a speed of 150 r / min and a temperature of 85°C. After that, distill off DMF, add the substrate into ethyl acetate to obtain a modified resin liquid.

[0068] The molar ratio of 4-formylphenylboronic acid and ethanolamine in step B1 is 1:1, the molar ratio of polytetramethylene ether diol and isophorone diisocyanate is 2:5, and the molecular weight of polytetramethylene ether diol is 2000.

[0069] The mass ratio of the prepolymer, chain extender and (3-aminopropyl)dimethylethoxysilane described in step B2 is 12:3:1, the amount ratio of the elastic monomer, diphenyldichlorosilane and deionized water and 1,1,3,3-tetramethyldisiloxane is 47g:8g:100mL:5.6g, and the amount of concentrated sulfuric acid is 3% of the mass of diphenyldichlorosilane.

[0070] The molar ratio of SiH on the hydrogen-terminated polysiloxane and p-hydroxystyrene in step B3 is 1:1, the amount of chloroplatinic acid used is 1‰ of the mass of p-hydroxystyrene, the amount ratio of intermediate 1, epichlorohydrin and sodium hydroxide solution is 1g:2g:10mL, the mass fraction of sodium hydroxide solution is 30%, and the amount of substrate and ethyl acetate used is 1g:10mL.

[0071] Example 4

[0072] A method for preparing high-performance concrete for ultra-thin composite floor slabs, comprising the following steps:

[0073] Weigh the following raw materials in parts by weight: 800 parts of cement, 150 parts of modified mineral powder, 60 parts of magnesium oxide silica fume, 8 parts of activation enhancer, 3.5 parts of water reducer, 3 parts of defoamer, 1000 parts of quartz sand, 400 parts of modified resin liquid, 200 parts of curing agent, 230 parts of water and 60 parts of fiber, mix the raw materials evenly, and prepare concrete.

[0074] The rest is the same as Example 1.

[0075] Example 5

[0076] A method for preparing high-performance concrete for ultra-thin composite floor slabs, comprising the following steps:

[0077] Weigh the following raw materials in parts by weight: 800 parts of cement, 150 parts of modified mineral powder, 60 parts of magnesium oxide silica fume, 8 parts of activation enhancer, 3.5 parts of water reducer, 3 parts of defoamer, 1000 parts of quartz sand, 400 parts of modified resin liquid, 200 parts of curing agent, 230 parts of water and 30 parts of fiber, mix the raw materials evenly to obtain concrete.

[0078] The rest is the same as Example 1.

[0079] Example 6

[0080] A method for preparing high-performance concrete for ultra-thin composite floor slabs, comprising the following steps:

[0081] Weigh the following raw materials in parts by weight: 900 parts of cement, 200 parts of modified mineral powder, 100 parts of magnesium oxide silica fume, 10 parts of activation enhancer, 5 parts of water reducer, 3 parts of defoamer, 1500 parts of quartz sand, 500 parts of modified resin liquid, 250 parts of curing agent, 300 parts of water and 100 parts of fiber, mix the raw materials evenly to obtain concrete.

[0082] The rest is the same as Example 1.

[0083] Comparative Example 1

[0084] Compared with Example 1, this comparative example uses mineral powder S95 instead of modified mineral powder, and the other steps are the same.

[0085] Comparative Example 2

[0086] Compared with Example 1, the modified resin liquid and curing agent were not added in this comparative example, and the remaining steps were the same.

[0087] Comparative Example 3

[0088] Compared with Example 1, no chain extender was added in this comparative example, and the remaining steps were the same.

[0089] Comparative Example 4

[0090] Compared with Example 1, no elastic monomer was added in this comparative example, and the remaining steps were the same.

[0091] The concrete obtained in Examples 1-6 and Comparative Examples 1-4 was tested using a truncated cone mold with a height of 60 mm, an upper diameter of 70 mm, and a lower diameter of 100. When testing the fluidity, place the truncated cone mold flat on a smooth and flat glass plate, wet the inner surface of the truncated cone mold and the surface of the glass plate at the same time, then load the freshly mixed high-performance concrete slurry into the mold, scrape the surface flat and remove the excess, gently lift the mold, and after 15 seconds, use a steel ruler to measure the expansion scale of the mixture in the maximum direction, read the scale value of the steel ruler in the vertical direction, and then take the average value as the truncated cone fluidity. In accordance with the "Technical Code for the Application of Steel Truss Floor Decking" (T / CECS1069-2022), the loads in the construction stage include permanent loads and variable loads. Permanent loads include steel truss floor decking, steel bars and concrete deadweight; variable loads are construction loads, which should be based on the actual construction loads. When the actual construction variable load cannot be measured or the actual construction variable load is less than 1.5kN / m 2 When the construction variable load is 1.5kN / m 2 The composite slab is supported at both ends (one of which is a sliding hinge support), and three dial indicators are arranged at the mid-span and 1 / 4 span to measure the deflection. A specimen with a side length of 150 mm is made in accordance with the GB / T50081-2019 standard. The compressive strength is tested under an acceleration of 15 kN / s. The test results are shown in the following table.

[0092]

[0093] It can be seen from the above table that the present application has the advantages of high late strength and high toughness.

[0094] The above contents are merely examples and explanations of the concept of the present invention. Those skilled in the art may make various modifications or additions to the specific embodiments described or replace them in a similar manner. As long as they do not deviate from the concept of the invention or exceed the scope defined by the claims, they shall all fall within the protection scope of the present invention.

Claims

1. A method for preparing high performance concrete for ultra-thin composite floor slabs, characterized in that: The specific steps include: Weigh the following raw materials in parts by weight: 700-900 parts of cement, 100-200 parts of modified mineral powder, 10-100 parts of magnesium oxide silica fume, 8-10 parts of activation enhancer, 1-5 parts of water reducer, 1-3 parts of defoamer, 1000-1500 parts of quartz sand, 300-500 parts of modified resin liquid, 150-250 parts of curing agent, 200-300 parts of water and 30-100 parts of fiber, mix the raw materials evenly to prepare concrete; The modified mineral powder is prepared by the following steps: Step A1: dispersing the mineral powder in ethanol, adding KH550 and deionized water, reacting to obtain pretreated mineral powder, mixing epichlorohydrin and tetrabutylammonium hydrogen sulfate, adding polyvinyl alcohol and sodium hydroxide solution, heating to react, and obtaining a treatment agent; Step A2: After the pretreated mineral powder, the treatment agent and DMF are mixed and reacted, 2-aminobenzimidazole is added, and the reaction is continued to obtain a precursor, the precursor is dispersed in DMF, sodium bicarbonate is added, and copper acetate is added and stirred to obtain a modified mineral powder; The modified resin solution is prepared by the following steps: Step B1: 4-formylphenylboronic acid and tetrahydrofuran are mixed, nitrogen is introduced for protection, and after reaction, ethanolamine is added and the reaction is continued to obtain a chain extender; polytetrahydrofuran ether diol, isophorone diisocyanate and DMF are mixed, nitrogen is introduced for protection, and the reaction is carried out to obtain a prepolymer; Step B2: After the prepolymer, chain extender and DMF are mixed and reacted, (3-aminopropyl) dimethylethoxysilane is added and the reaction is continued to obtain an elastic monomer, and after the elastic monomer, diphenyldichlorosilane and deionized water are mixed and stirred, concentrated sulfuric acid and 1,1,3,3-tetramethyldisiloxane are added to react, and the pH is adjusted to neutral to obtain a hydrogen-terminated polysiloxane; Step B3: The hydrogen-terminated polysiloxane, p-hydroxystyrene and DMF are mixed and stirred, and chloroplatinic acid is added to react to obtain intermediate 1. The intermediate 1, epichlorohydrin and DMF are evenly mixed, and sodium hydroxide solution is added to react for 2-3 hours, and then DMF is distilled off, and the substrate is added to ethyl acetate to obtain a modified resin liquid.

2. The method for preparing high performance concrete for ultra-thin composite floor slabs according to claim 1, characterized in that: The amount of KH550 used in step A1 is 1-1.5% of the mass of the mineral powder, and the amount ratio of epichlorohydrin, tetrabutylammonium hydrogen sulfate, polyvinyl alcohol and sodium hydroxide solution is 1 mol:8.5 mmol:0.2 mol:160 mL.

3. The method for preparing high performance concrete for ultra-thin composite floor slabs according to claim 1, characterized in that: The molar ratio of the amino groups on the surface of the pretreated mineral powder, the epoxy groups on the treating agent and 2-aminobenzimidazole in step A2 is 1:3:2.2, and the mass ratio of the precursor, sodium bicarbonate and copper acetate is 1:4:

10.

4. The method for preparing high performance concrete for ultra-thin composite floor slabs according to claim 1, characterized in that: The molar ratio of 4-formylphenylboronic acid and ethanolamine in step B1 is 1:1, and the molar ratio of polytetramethylene ether diol and isophorone diisocyanate is 2:

5.

5. The method for preparing high performance concrete for ultra-thin composite floor slabs according to claim 1, characterized in that: The mass ratio of the prepolymer, chain extender and (3-aminopropyl)dimethylethoxysilane described in step B2 is 12:3:1, and the amount ratio of the elastic monomer, diphenyldichlorosilane, deionized water and 1,1,3,3-tetramethyldisiloxane is 47g:8g:100mL:5.6g.

6. The method for preparing high performance concrete for ultra-thin composite floor slabs according to claim 1, characterized in that: The molar ratio of Si-H on the hydrogen-terminated polysiloxane and p-hydroxystyrene in step B3 is 1:1, the amount ratio of intermediate 1, epichlorohydrin and sodium hydroxide solution is 1g:2g:10mL, and the amount of substrate and ethyl acetate is 1g:10mL.

7. A high performance concrete for ultra-thin composite floor slabs, characterized in that: Prepared according to any one of claims 1 to 6.

Citation Information

Cited By

  • Impermeable coating based on modified quartz and calcite and application thereof