A synthesis method and application of high-performance moisture-curing silicone resin

By introducing silicone and modified epoxy resin into polyurethane materials, high-performance wet curing silicone resin is prepared and combined with modified fillers, the insufficient performance of polyurethane materials in specific fields is solved, and mechanical properties and stability are improved meets the needs of the coatings industry.

CN118325034BActive Publication Date: 2024-11-29GUANGDONG JIMEIBANG NEW MATERIAL CO LTD
View PDF 3 Cites 0 Cited by

Patent Information

Application Number
CN202410604623.3
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-05-15
Publication Date
2024-11-29
Estimated Expiration
2044-05-15

AI Technical Summary

Technical Problem

Existing polyurethane materials have problems in specific fields such as insufficient heat resistance, water resistance and dielectricity, and bubbles and holes are generated during the curing process, which affects performance; at the same time, the mechanical properties of the modified resin materials are degraded and cannot meet the coating industry. need.

Method used

Using silicone, polyether polyol, diisocyanate, silane coupling agent and modified epoxy resin, high-performance wet curing silicone resin is prepared through moisture curing reaction, and combined with modified fillers to enhance the mechanics of the material. Performance and stability to avoid gas production.

Benefits of technology

It has achieved high mechanical properties, stability and adhesion of the materials, overcomes the performance shortcomings of traditional polyurethane materials, meets the needs of the coating industry, and provides better application prospects.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0004841594350000051
    Figure BDA0004841594350000051
  • Figure BDA0004841594350000052
    Figure BDA0004841594350000052
  • Figure BDA0004841594350000061
    Figure BDA0004841594350000061
Patent Text Reader

Abstract

The present invention relates to a method for synthesizing a high-performance moisture-curing silicone resin and its application, comprising the following steps: S1, mixing silicone, polyether polyol and diisocyanate, heating reaction under inert gas protection to obtain a prepolymer, then adding a silane coupling agent, and continuing the reaction to obtain an intermediate product; S2, mixing a bisphenol compound with triglycidyl isocyanurate, adding a catalyst, heating reaction, and obtaining a modified epoxy resin; S3, mixing the intermediate product, the modified epoxy resin and a chain extender, heating and stirring, and then adding a catalyst to obtain a product. The present invention uses silicone, polyether polyol, diisocyanate and modified epoxy resin as raw materials to prepare a resin material, and compounding it with a modified filler for application in a coating, effectively improving multiple performances of the product, overcoming the problem that the current polyurethane coating has insufficient mechanical properties, stability and other capabilities and cannot meet actual use requirements.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of coatings, and in particular to a synthesis method of a high-performance moisture-curing organic silicon resin and application thereof. Background Art

[0002] Polyurethane (PU, polyurethane) is a polymer material obtained by polycondensation of polyols and isocyanates, and its structure contains repeated carbamate groups. This type of material has strong mechanical properties, good fatigue resistance and wear resistance, and has been widely used in a variety of light and heavy industries. However, existing traditional polyurethane materials have problems such as insufficient heat resistance, water resistance, and dielectric properties, which limit their application in specific fields; at the same time, the curing process of polyurethane materials will produce carbon dioxide gas, resulting in bubbles and holes in the material, which has a negative impact on product performance.

[0003] Silicone material is an organic polymer synthetic material containing silicon atoms in its molecular structure. It can remain stable within a large temperature and humidity range. It also has excellent dielectric properties, heat resistance, weather resistance and water resistance, as well as good biocompatibility. It is a widely used material.

[0004] In recent years, the use of silicone-modified polyurethane materials has received much attention. By adjusting the chemical structure and composition of the two components of polyurethane and silicone, the stability and dielectric properties of polyurethane materials have been improved. However, the modified resin materials also have the problems of decreased original mechanical properties and insufficient improvement of specific functions. In addition, the existing technology lacks research and reports on high-performance moisture-curing silicone resin materials, which can hardly meet the needs of the coatings industry.

[0005] In summary, it is urgent to develop a new technical solution to solve the problems existing in the prior art. Summary of the invention

[0006] Based on this, the present invention provides a method for synthesizing a high-performance moisture-curing silicone resin and its application. The present invention uses silicone, polyether polyol, diisocyanate, silane coupling agent and modified epoxy resin as raw materials to prepare a resin material, and mixes it with a modified filler and applies it to a coating, effectively improving multiple properties of the product, overcoming the problem that the current polyurethane coating has insufficient mechanical properties, stability and other capabilities and cannot meet actual use requirements.

[0007] An object of the present invention is to provide a method for synthesizing a high-performance moisture-curable silicone resin, the method comprising the following steps:

[0008] S1, mixing organosilicon, polyether polyol and diisocyanate, heating and reacting under the protection of inert gas to obtain a prepolymer, and then adding a silane coupling agent and continuing the reaction to obtain an intermediate product;

[0009] S2, mixing the bisphenol compound with triglycidyl isocyanurate, adding a catalyst under the protection of an inert gas, and heating the mixture to react to obtain a modified epoxy resin;

[0010] S3, mixing the intermediate product, modified epoxy resin and chain extender, heating and stirring, adding a catalyst, stirring and degassing to obtain a product.

[0011] Furthermore, the organosilicon is hydroxy-terminated polysiloxane.

[0012] Furthermore, the polyether polyol is selected from one or more of polyoxypropylene diol, polyoxypropylene triol and polytetramethylene ether diol.

[0013] Furthermore, the silane coupling agent is selected from one or more of 3-isocyanate propyl triethoxy silane, 3-isocyanate propyl trimethoxy silane, 3-aminopropyl trimethoxy silane, 3-aminopropyl triethoxy silane, and 3-(3-trimethoxysilylpropyl) isocyanurate.

[0014] Furthermore, in step S1, the temperature of the heating reaction is 60-90°C and the time is 2-4h; the temperature of the continued reaction is 20-40°C and the time is 2-5h.

[0015] Furthermore, in step S2, the heating reaction temperature is 60-70°C and the time is 40-50h.

[0016] Furthermore, in step S3, the heating temperature is 50-70° C. and the heating time is 0.5-2 h.

[0017] Furthermore, the bisphenol compound is selected from one or more of bisphenol A, bisphenol F, bisphenol S, tetramethyl bisphenol A, and tetramethyl bisphenol F.

[0018] Furthermore, the mass ratio of the organosilicon, polyether polyol and diisocyanate is (1-5):(10-15):(1-10).

[0019] Furthermore, the molar ratio of NCO groups to silane coupling agents in the prepolymer is 1:(0.8-1).

[0020] Furthermore, the mass ratio of the bisphenol compound to triglycidyl isocyanurate is (0.5-1.5):1.

[0021] Another object of the present invention is to provide the use of the synthesis method of the high-performance moisture-curable silicone resin in a coating, wherein the coating comprises the following components in parts by weight:

[0022] High performance moisture curing silicone resin 80-100 parts

[0023] Modified filler 1-20 parts

[0024] 1-10 parts of additives;

[0025] in,

[0026] The modified filler is a polyether polyol or a fatty acid modified filler.

[0027] Furthermore, the preparation method of the modified filler comprises the following steps:

[0028] The polyether polyol, fatty acid and acid catalyst are mixed, heated for reaction, purified, mixed with filler, and subjected to ultrasonic heating reaction to obtain a modified filler;

[0029] The filler is pre-treated by surface hydroxylation.

[0030] Furthermore, the temperature of the heating reaction is 80-120°C, and the temperature of the ultrasonic heating reaction is 30-60°C.

[0031] Furthermore, the auxiliary agent is selected from one or more of a leveling agent, a defoaming agent, an emulsifier, a diluent, and a desiccant.

[0032] Furthermore, the filler is selected from one or more of silicon dioxide, silicon carbide, boron nitride, and metal oxides.

[0033] The present invention has the following beneficial effects:

[0034] 1. In the synthesis method of the high-performance moisture-curable silicone resin of the present invention, firstly, a prepolymer is prepared with silicone, polyether polyol and diisocyanate as raw materials, and then further reacted with a silane coupling agent to obtain a silane-terminated intermediate product. In the resin, silicone and polyether polyol provide soft segments, and isocyanate provides hard segments, thereby ensuring the mechanical strength of the resin while making the material have stronger hydrophobicity and stability. After silane end-capping, the silane alkoxy group can react with water in the air to achieve moisture curing, which not only avoids the generation of gas, enhances the mechanical properties, but also helps to improve the adhesion. The present invention also obtains a modified epoxy resin with a branched structure by reacting triglycidyl isocyanurate and a bisphenol compound. By introducing the modified epoxy resin, the material has a higher cross-linking density, and the structure is more three-dimensional and stable, thereby further improving the mechanical properties such as toughness, as well as adhesion and stability.

[0035] 2. The present invention also compounds high-performance moisture-curable silicone resin with modified fillers and applies them to coating products. The modified filler is first subjected to surface hydroxylation treatment, and dibasic fatty acids and polyethylene glycol are reacted to obtain an amphiphilic polyester with long alkyl and ethoxy segments, and then the active hydroxyl groups on the filler surface are adsorbed and cross-linked with the hydrophilic ethoxy segments by electrostatic force and intermolecular force, thereby obtaining the modified filler. The modified filler has better compatibility with the organic resin, the introduced long alkyl segments are conducive to improving dispersibility, and can cause entanglement and cross-linking between components to form a network structure, thereby improving the mechanical properties of the coating, and the alkoxy segments can also generate hydrogen bonds with the oxygen-containing active groups in the resin, further enhancing the product stability and strength, and having good application prospects. DETAILED DESCRIPTION

[0036] In order to more clearly illustrate the technical solution of the present invention, the following examples are listed. Unless otherwise stated, the raw materials, reactions and post-treatment methods shown in the examples are common raw materials on the market and technical methods well known to those skilled in the art.

[0037] The words "preferred", "preferably", "more preferably", etc. in the present invention refer to embodiments of the present invention that can provide certain beneficial effects in certain circumstances. However, other embodiments may also be preferred under the same circumstances or other circumstances. In addition, the description of one or more preferred embodiments does not imply that other embodiments are not applicable, nor is it intended to exclude other embodiments from the scope of the present invention.

[0038] It should be understood that, except in any operating examples, or where otherwise indicated, all numbers indicating, for example, the amounts of ingredients used in the specification and claims should be understood to be modified in all cases by the term "about". Therefore, unless indicated to the contrary, the numerical parameters set forth in the following specification and the appended claims are approximate values ​​that vary depending on the desired properties to be obtained by the present invention.

[0039] The hydroxy-terminated polydimethylsiloxane in the embodiment of the present invention was purchased from Jining Zhongjian Chemical Co., Ltd. n =1000.

[0040] The polytetrahydrofuran ether glycol in the embodiment of the present invention is Mitsubishi PTMG1000.

[0041] The co-solvent in the embodiment of the present invention is No. 120 solvent oil.

[0042] The chain extender in the embodiment of the present invention is ethylenediamine.

[0043] The catalyst in the embodiment of the present invention is dibutyltin dilaurate.

[0044] The leveling agent in the application example of the present invention is CAB381-20.

[0045] The defoamer in the application example of the present invention is BYK-141.

[0046] The hydroxy-terminated polydimethylsiloxane and polytetramethylene ether glycol in the embodiments of the present invention are subjected to vacuum dehydration treatment before use.

[0047] The preparation method of the modified filler in the application example of the present invention comprises the following steps:

[0048] The silicon dioxide was immersed in a mixture of concentrated sulfuric acid and hydrogen peroxide (hydrogen peroxide concentration 30 wt%) in a volume ratio of 7:3, heated at 70° C. for 1 h, and washed and dried to obtain a hydroxylated filler;

[0049] Under nitrogen protection, polyethylene glycol (PEG-600) and lauric acid in a mass ratio of 1:1 were mixed with toluene as solvent, concentrated sulfuric acid (1wt% of the reaction system) was added with stirring, and the mixture was refluxed at 120°C for 12 hours. After cooling, a saturated NaOH solution was added with stirring until the pH was neutral, the solid product was removed by centrifugation, and then the toluene was removed by reduced pressure distillation to obtain an intermediate product.

[0050] The intermediate product and the hydroxylated filler in a mass ratio of 3:1 were blended, subjected to ultrasonic reaction at 50° C. for 2 h, and the modified filler was obtained after filtering and drying.

[0051] The "parts" in the embodiments of the present invention refer to parts by mass.

[0052] Example 1

[0053] A method for synthesizing a high-performance moisture-curable silicone resin comprises the following steps:

[0054] S1, 10 parts of hydroxy-terminated polydimethylsiloxane, 50 parts of polytetramethylene ether glycol and 5 parts of cosolvent were mixed, 20 parts of toluene diisocyanate were added under nitrogen protection, and the mixture was reacted at 80° C. for 2 h to obtain a prepolymer;

[0055] Add KH550 to the prepolymer (the molar ratio of NCO group to KH550 in the prepolymer is 1:0.9), stir and react at 30° C. for 3 h to obtain an intermediate product;

[0056] S2, using tetrahydrofuran as solvent, 10 parts of bisphenol A and 9 parts of triglycidyl isocyanurate were mixed, and under nitrogen protection, 0.8wt% of tetrabutylammonium bromide was added to the reaction system, and the mixture was reacted at 65°C for 50h. After cooling, cyclohexane was added for precipitation, and the modified epoxy resin was obtained after washing and drying;

[0057] S3, 50 parts of the intermediate product, 5 parts of modified epoxy resin and 0.5 parts of chain extender were mixed, stirred at 70°C for 3 hours, 0.5 parts of catalyst were added, and the mixture was stirred and degassed at -0.095 MPa for 0.5 hours to obtain the product.

[0058] Example 2

[0059] A method for synthesizing a high-performance moisture-curable silicone resin comprises the following steps:

[0060] S1, 15 parts of hydroxy-terminated polydimethylsiloxane, 45 parts of polytetramethylene ether glycol and 5 parts of cosolvent were mixed, 20 parts of toluene diisocyanate were added under nitrogen protection, and the mixture was reacted at 85° C. for 2 h to obtain a prepolymer;

[0061] Add KH550 to the prepolymer (the molar ratio of NCO group to KH550 in the prepolymer is 1:0.9), stir and react at 30° C. for 3 h to obtain an intermediate product;

[0062] S2, using tetrahydrofuran as solvent, 10 parts of bisphenol A and 8 parts of triglycidyl isocyanurate were mixed, and under nitrogen protection, 0.8wt% of tetrabutylammonium bromide was added to the reaction system, and the mixture was reacted at 65°C for 50h. After cooling, cyclohexane was added for precipitation, and the modified epoxy resin was obtained after washing and drying;

[0063] S3, 50 parts of the intermediate product, 5 parts of modified epoxy resin and 0.5 parts of chain extender were mixed, stirred at 60°C for 3 hours, 0.5 parts of catalyst were added, and the mixture was stirred and degassed at -0.095 MPa for 0.5 hours to obtain the product.

[0064] Application Example 1

[0065] A coating comprising the following components in parts by weight:

[0066]

[0067] in,

[0068] The high performance moisture-curable silicone resin is prepared according to Example 1.

[0069] Application Example 2

[0070] A coating comprising the following components in parts by weight:

[0071]

[0072] in,

[0073] The high performance moisture-curable silicone resin is prepared according to Example 2.

[0074] Comparative Example 1

[0075] A coating, the difference between this comparative example and application example 1 is that the prepolymer (50 parts) of step S1 in embodiment 1 is directly mixed with a curing agent (2-isopropyl-3-hydroxyethyl-1,3-oxazolidine, 3 parts) and a catalyst (dibutyltin dilaurate, 0.5 parts), and a silicone resin is obtained after vacuum degassing. The other ingredients and preparation method are the same as those in application example 1.

[0076] Comparative Example 2

[0077] A coating, the difference between this comparative example and application example 1 is that the modified filler and other qualities are replaced by unmodified silica, and the other components and preparation method are the same as those of application example 1.

[0078] Test Case

[0079] The coatings prepared according to the examples and comparative examples were subjected to performance tests.

[0080] Test method: Refer to GB / T16777-2008 standard for tensile strength, elongation at break, water impermeability, acid and alkali resistance and other tests.

[0081] The test results are shown in Table 1.

[0082] Table 1 Performance test results

[0083]

[0084] According to Table 1, it can be concluded that the high-performance moisture-curing silicone resin prepared by the present invention is applied to coatings, which has excellent mechanical properties and good stability, and can be used for a long time under various conditions. However, Comparative Example 1 does not use silane end-capping, but uses conventional moisture curing agents for curing, and deletes the modified epoxy resin, resulting in a significant decrease in the mechanical properties and weather resistance of the coating; Comparative Example 2 replaces the modified filler, resulting in reduced compatibility between the components, uneven distribution of the filler, affecting the strength and stability of the coating, and poor chemical resistance. In summary, the present invention overcomes the defects existing in the prior art and has good application prospects.

[0085] It will be apparent to those skilled in the art that the present invention is not limited to the details of the exemplary embodiments described above and that the present invention can be implemented in other specific forms without departing from the spirit or essential features of the present invention. Therefore, the embodiments should be considered exemplary and non-restrictive in all respects, and the scope of the present invention is defined by the appended claims rather than the above description, and it is intended that all changes falling within the meaning and scope of the equivalent elements of the claims be included in the present invention.

[0086] In addition, it should be understood that although the present specification is described according to implementation modes, not every implementation mode contains only one independent technical solution. This description of the specification is only for the sake of clarity. Those skilled in the art should regard the specification as a whole. The technical solutions in each embodiment may also be appropriately combined to form other implementation modes that can be understood by those skilled in the art.

Claims

1. A method for synthesizing a high-performance moisture-curing silicone resin and its application in coatings, characterized in that: The synthesis method of the high-performance moisture-curable silicone resin comprises the following steps: S1, mixing organosilicon, polyether polyol and diisocyanate, heating and reacting under the protection of inert gas to obtain a prepolymer, and then adding a silane coupling agent and continuing the reaction to obtain an intermediate product; S2, mixing the bisphenol compound with triglycidyl isocyanurate, adding a catalyst under the protection of an inert gas, and heating the mixture to react to obtain a modified epoxy resin; S3, mixing the intermediate product, modified epoxy resin and chain extender, heating and stirring, adding a catalyst, stirring and degassing to obtain a product; The coating comprises the following components in parts by weight: High performance moisture curing silicone resin 80-100 parts Modified filler 1-20 parts 1-10 parts of additives; in, The preparation method of the modified filler comprises the following steps: The polyethylene glycol, fatty acid and acid catalyst are mixed, heated for reaction, purified, mixed with filler, and subjected to ultrasonic heating for reaction to obtain a modified filler; The filler is pre-treated by surface hydroxylation; The organosilicon is hydroxyl-terminated polysiloxane; The molar ratio of NCO groups to silane coupling agents in the prepolymer is 1:(0.8-0.9).

2. The use of the synthesis method of high-performance moisture-curable silicone resin according to claim 1 in coatings, characterized in that: The polyether polyol is selected from one or more of polyoxypropylene diol, polyoxypropylene triol and polytetramethylene ether diol.

3. The use of the synthesis method of high-performance moisture-curable silicone resin according to claim 1 in coatings, characterized in that: The silane coupling agent is selected from one or more of 3-aminopropyltrimethoxysilane and 3-aminopropyltriethoxysilane.

4. The use of the synthesis method of high-performance moisture-curable silicone resin according to claim 1 in coatings, characterized in that: In step S1, the temperature of the heating reaction is 60-90°C and the time is 2-4 h; the temperature of the continued reaction is 20-40°C and the time is 2-5 h.

5. Application of the synthesis method of high-performance moisture-curable silicone resin according to claim 1 in coatings, characterized in that: In step S2, the heating reaction temperature is 60-70°C and the time is 40-50 h.

6. Application of the synthesis method of high-performance moisture-curable silicone resin according to claim 1 in coatings, characterized in that: In step S3, the heating temperature is 50-70° C. and the heating time is 0.5-2 h.

7. Application of the synthesis method of high-performance moisture-curable silicone resin according to claim 1 in coatings, characterized in that: In the preparation method of the modified filler, the temperature of the heating reaction is 80-120°C, and the temperature of the ultrasonic heating reaction is 30-60°C.

Citation Information

Patent Citations

  • Silane modified polyurethane sealant prepolymer and preparation method thereof and sealant

    CN106279614A

  • Silicon-containing polyurethane oligomer and preparation method thereof

    CN106750082A

  • High-performance moisture-curing polyurea resin and preparation method thereof

    CN117986524A