A method for preparing a sample target plate for mass spectrometry detection

By plasma processing of mass spectrometry detection target plate, cutting point circle grooves and engraving barcodes, and applying hydrophobic coatings on the surface, the problems of residual and cross-infection of the agent in the prior art are solved, and higher detection accuracy and reliability.

CN118443404BActive Publication Date: 2024-11-29KANGLIDA AUTO PARTS (SUZHOU) CO LTD
View PDF 4 Cites 0 Cited by

Patent Information

Application Number
CN202410556914.X
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-05-07
Publication Date
2024-11-29
Estimated Expiration
2044-05-07

AI Technical Summary

Technical Problem

The existing mass spectrometry detection target plates have complex processing processes, and there are prone to drug residues between layers, resulting in cross-infection and low reliability.

Method used

The target plate substrate is treated with plasma, the processing point circle grooves are cut, the bar code is engraved, and the surface of the target plate is coated with hydrophobic coating. After curing, it forms a hydrophobic coating to restrain the agent.

Benefits of technology

Effectively constrain the agent in the dot circle groove, reduce agent residue, improve detection accuracy, reduce the risk of cross-infection, simplify the process and improve the reliability of the target plate.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0004826316450000091
    Figure BDA0004826316450000091
Patent Text Reader

Abstract

The present application relates to a method for preparing a sample target plate for mass spectrometry detection, which includes the following preparation methods: (1) subjecting a stainless steel target plate substrate to surface plasma treatment; (2) cutting treatment to obtain point ring grooves; (3) engraving a barcode to obtain a processed target plate; (4) coating the surface of the processed target plate except the point ring grooves with a hydrophobic coating; (5) high-temperature curing of the processed target plate coated with the hydrophobic coating to form a hydrophobic coating on the surface of the processed target plate to obtain a sample target plate. The present application has the effect of enhancing the constraint effect on the position of drug detection.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present application relates to the field of mass spectrometry medical equipment detection, and in particular to a method for preparing a sample target plate for mass spectrometry detection. Background Art

[0002] A mass spectrometer is a scientific instrument that uses electromagnetics to separate ions based on their mass-to-charge ratios, and then measures the mass and content of a substance. Usually, the sample is first fixed on a target point on a target plate, and then analyzed and identified using a mass spectrometer.

[0003] The target plate is a carrier for the sample and the matrix for crystallization. The points on the target plate can carry the test samples. In order to constrain the samples at the target plate points, the target plate can use the layered adhesion barrier principle to limit the position of the agent. However, the processing process of this target plate is complicated, and it is easy for agents to remain between the layers, resulting in cross-infection and low reliability, so it needs to be improved. Summary of the invention

[0004] In order to solve the above technical problems, the present application provides a method for preparing a sample target plate for mass spectrometry detection.

[0005] The present application provides a method for preparing a sample target plate for mass spectrometry detection using the following technical solution:

[0006] A method for preparing a sample target plate for mass spectrometry detection includes the following preparation methods:

[0007] (1) subjecting the target plate substrate to surface plasma treatment;

[0008] (2) cutting and processing to obtain point grooves;

[0009] (3) Carving a barcode to obtain a processed target plate;

[0010] (4) The surface of the processed target plate is coated with a hydrophobic coating except for the point grooves;

[0011] (5) The processed target plate coated with the hydrophobic coating is cured at high temperature, so that a hydrophobic coating is formed on the surface of the processed target plate, thereby obtaining a sample target plate.

[0012] By adopting the above technical scheme, a hydrophobic coating is coated on the surface of the target plate to form a layer of hydrophobic coating, which can effectively restrain the detection agent so that the agent stays in the point circle groove. The coating process is used to coat the processed target plate with the hydrophobic coating to reduce the complexity of the processing technology; after the surface of the target plate substrate is plasma treated, the roughness of the target plate surface is improved, and the surface energy is increased, which is conducive to the adhesion effect of the hydrophobic material on the target plate surface; the thickness difference between the cut point circle groove and the hydrophobic coating can further restrain the agent and effectively reduce the agent residue.

[0013] Preferably, the hydrophobic coating comprises fluorine-modified silica, siloxane organic matter and epoxy resin.

[0014] By adopting the above technical scheme, the epoxy resin has excellent chemical resistance and good adhesion, which can make the hydrophobic coating more stably adhere to the surface of the processed target plate, thereby improving the overall stability of the hydrophobic coating after curing. Fluorine-modified silica has good light transmittance and hydrophobicity, which can restrain the mass spectrometry detection agents, thereby improving the detection accuracy. After adding siloxane organic matter, the wear resistance of the hydrophobic coating after curing can be improved, and the hydrophobic durability of the hydrophobic coating is also improved, further improving the overall hydrophobic performance of the hydrophobic coating.

[0015] Preferably, the mass ratio of the fluorine-modified silica, the siloxane organic matter and the epoxy resin is 1:(2.1-2.3):10.4.

[0016] By adopting the above technical solution, the mass ratio of fluorine-modified silica, siloxane organic matter and epoxy resin is preferably within the above range, which can improve the overall hydrophobic effect of the hydrophobic coating.

[0017] Preferably, the fluorine-modified silica is prepared by the following method:

[0018] Ethyl orthosilicate, an alkaline catalyst, anhydrous ethanol and deionized water are mixed and stirred to obtain a silica particle mixed solution, and ethanol and perfluorodecyltrimethylsilane are added to the silica particle mixed solution and stirred to obtain fluorine-modified silica.

[0019] By adopting the above technical scheme, the prepared silica sol is fluorinated with perfluorodecyltrimethylsilane, so that the surface energy of the silica sol is reduced, so as to further improve the overall hydrophobic properties of the hydrophobic coating and enhance the restraining effect on mass spectrometry detection agents.

[0020] Preferably, the mass ratio of the tetraethyl orthosilicate to perfluorodecyltrimethylsilane is (2.9-3.1):1.

[0021] By adopting the above technical solution, preferably the mass ratio between ethyl orthosilicate and perfluorodecyltrimethylsilane is within the above range, the hydrophobicity and stability of the prepared fluorine-modified silica can be improved.

[0022] Preferably, the alkaline catalyst comprises aqueous ammonia.

[0023] By adopting the above technical scheme, ethyl orthosilicate is hydrolyzed under the catalysis of ammonia water, and spherical silica sol particles are obtained after condensation, and the particle size of the sol particles can be adjusted to obtain fluorine-modified silica with better hydrophobic properties.

[0024] Preferably, the amount of ammonia water added is 2.5-0.3% of the total fluorine-modified silica.

[0025] By adopting the above technical solution and controlling the amount of ammonia water added within the above range, the transmittance and hydrophobic performance of the prepared hydrophobic coating can be improved.

[0026] Preferably, the fluorine-modified silica is further added with nano-silica particles, and the particle size of the nano-silica particles is 105-115 nm.

[0027] By adopting the above technical solution, nano-silica particles are added to fluorine-modified silica, and after being compounded with colloidal silica, the hydrophobic properties of the hydrophobic nano-coating can be better improved, and the wear resistance and mechanical properties of the granular nano-silica are further improved, thereby improving the stability of the prepared hydrophobic coating.

[0028] Preferably, the siloxane organic compound is prepared by the following method:

[0029] Anhydrous ethanol, acetic acid, triethoxymethylsilane, ethyl orthosilicate and deionized water are mixed and stirred to obtain a siloxane condensate, and water ethanol is continuously added to the siloxane condensate and stirred to obtain a siloxane organic matter.

[0030] By adopting the above technical scheme, a variety of silanes are hydrolyzed and condensed to obtain a polymer with a low molecular weight having properties such as high viscosity and high cross-linking. After hydrolysis, the various silanes can cross-link with each other to form a network structure and form a film, so that the cured hydrophobic coating has good corrosion resistance, mechanical properties and light transmittance, and improves the adhesion and wear resistance of the hydrophobic coating, so that the prepared sample target plate still has good hydrophobic properties after long-term use.

[0031] Preferably, the hydrophobic coating is prepared by the following method:

[0032] The epoxy resin is mixed with the acetone solution, and then fluorine-modified silica and siloxane organic matter are added, and 3-aminopropyltrimethoxysilane is added after dispersion, and after stirring, a hydrophobic coating is obtained.

[0033] By adopting the above technical solution, the hydrophobic coating to which 3-aminopropyltrimethoxysilane is added can further improve the hydrophobic properties of the hydrophobic coating.

[0034] In summary, the present application includes at least one of the following beneficial technical effects:

[0035] 1. A hydrophobic coating is coated on the surface of the target plate. After curing, a layer of hydrophobic coating is formed on the surface of the target plate. There is a thickness difference between the hydrophobic coating and the point groove obtained by cutting. At the same time, the hydrophobic coating has good hydrophobic properties and can play a good restraining role on the mass spectrometry detection agent. Before the hydrophobic coating is coated on the surface of the target plate, the surface of the stainless steel target plate substrate is plasma-treated to improve the roughness of the target plate surface, so that the hydrophobic coating can better adhere to the surface of the target plate, thereby improving the stability of the hydrophobic coating obtained after curing, and the prepared sample target plate can restrain the agent in the point groove;

[0036] 2. The hydrophobic coating is composed of fluorine-modified silica, siloxane organic matter and epoxy resin. The epoxy resin has excellent chemical resistance and adhesion, and can effectively improve the overall stability of the hydrophobic coating after curing. The fluorine-modified silica has excellent light transmittance and hydrophobicity. The siloxane organic matter can improve the wear resistance of the hydrophobic coating after curing, thereby improving the stability and durability of the hydrophobic coating.

[0037] 3. Siloxane organic matter is obtained through the hydrolysis and condensation of multiple silanes, and can be cross-linked to obtain a network structure, thereby improving the mechanical properties of the hydrophobic coating, making the hydrophobic coating more stable, so as to enhance the binding effect on the detection agent. DETAILED DESCRIPTION

[0038] The present application is further described in detail below with reference to the embodiments:

[0039] Materials preparation:

[0040] The target plate substrate is made of 316 stainless steel; the curing agent is ethylenediamine (CAS No. 107-15-3), and the alkaline catalyst is ammonia water (CAS No. 1336-21-6).

[0041] The method for preparing a sample target plate for mass spectrometry detection is prepared by the following steps:

[0042] (1) Plasma treatment of target substrate surface:

[0043] Lay the target plate substrate flat in the reaction chamber of the plasma equipment, set the electrode spacing to 3 cm, turn on the vacuum pump, evacuate the chamber to 3-5 Pa, introduce argon gas, and the argon gas flow rate range is 50-100 mL / min. After the air pressure stabilizes, turn on the open power switch, the discharge power is 200-400w, the discharge time is 10-50s, and the power is turned off after the processing time is reached to obtain plasma-treated stainless steel.

[0044] (2) Cutting and processing of grooves:

[0045] According to the specifications of different mass spectrometer target carriers, the plasma-treated stainless steel is cut, and the cut stainless steel is processed using a micro-engraving tool to form 96-hole point grooves on the surface of the steel, with a depth of 2-3 μm.

[0046] (3) Engraving barcode:

[0047] A barcode is engraved on the surface of the steel plate by a laser engraving machine to obtain a processed target plate.

[0048] (4) Pour the hydrophobic coating into the spray gun, control the spray gun pressure to 4-5 Kpa, keep the nozzle 20-30 cm away from the base of the processing target plate, spray the water-transporting coating to the surface of the processing target plate except the point circle groove, so that the surface of the processing target plate except the point circle groove is adhered to the hydrophobic coating, and the thickness of the hydrophobic coating is 2-3 μm.

[0049] (5) Drying the processed target plate coated with the hydrophobic coating in an oven at a temperature of 90-110° C. for 1-2 h, so that the hydrophobic coating on the surface of the processed target plate is solidified into a hydrophobic coating attached to the surface of the processed target plate, thereby obtaining a sample target plate.

[0050] Example 1

[0051] Preparation of fluorine-modified silica:

[0052] 3.72 g of tetraethyl orthosilicate (CAS No.: 78-10-4), 1.2 g of alkaline catalyst ammonia water, 40 g of anhydrous ethanol and 3 g of deionized water were mixed, and stirred at 800 rpm for 6 hours at 50° C. to obtain a silica particle mixture. Ethanol was added to the silica particle mixture, and 1.28 g of perfluorodecyltrimethylsilane (CAS No.: 83048-65-1) was added. After stirring at 1200 rpm for 8 minutes, 0.5 g of nano-silica particles with a particle size of 105 nm (CAS No.: CAS: 60676-86-0) was added, and stirred at 2000 rpm for 12 minutes to obtain fluorine-modified silica.

[0053] Preparation of siloxane organic matter:

[0054] Mix 10 g of anhydrous ethanol, 1 g of acetic acid, 4 g of triethoxymethylsilane (CAS No.: 1825-62-3), 4 g of ethyl orthosilicate and 1 g of deionized water, stir at 800 rpm for 4 hours at 25°C to obtain a siloxane condensate, then add 10 g of anhydrous ethanol to the siloxane condensate, and stir at 800 rpm for 30 minutes to obtain a siloxane organic matter.

[0055] Preparation of hydrophobic coating:

[0056] 38.53 g of epoxy resin and 15 g of curing agent were added to 10 mL of acetone solution, ultrasonicated at 2000 rpm for 30 min, then 3.7 g of fluorine-modified silica and 7.77 g of siloxane organic matter were added, stirred at 800 rpm for 3 min, 0.5 g of 3-aminopropyltrimethoxysilane and 0.5 g of perfluorodecyltrimethylsilane were added, and stirred at 1200 rpm for 5 min to obtain a hydrophobic coating.

[0057] Prepare sample target plate:

[0058] (1) Plasma treatment of target substrate surface:

[0059] The target plate substrate is laid flat in the reaction chamber of the plasma equipment, the electrode spacing is set to be fixed at 3 cm, the vacuum pump is turned on, the chamber is evacuated to 3 Pa, argon gas is introduced, and the argon gas flow range is 50 mL / min. After the air pressure stabilizes, the power switch is turned on, the discharge power is 200 W, the discharge time is 50 s, and the power is turned off after the processing time is reached to obtain plasma-treated stainless steel.

[0060] (2) Cutting and processing of grooves:

[0061] According to the specifications of different mass spectrometer target carriers, the plasma-treated stainless steel is cut, and the cut stainless steel is processed using a micro-engraving tool to form 96-hole point grooves on the surface of the steel, with a depth of 2 μm.

[0062] (3) Engraving barcode:

[0063] A barcode is engraved on the surface of the steel plate by a laser engraving machine to obtain a processed target plate.

[0064] (4) Pour the hydrophobic coating into the spray gun, control the spray gun pressure to 4 KPa, and keep the nozzle 30 cm away from the base of the processing target plate. Spray the water-transporting coating to the surface of the processing target plate except the point circle groove, so that the surface of the processing target plate except the point circle groove is adhered to the hydrophobic coating. The thickness of the hydrophobic coating is 3 μm.

[0065] (5) Drying the processed target plate coated with the hydrophobic coating in an oven at 90° C. for 2 h, so that the hydrophobic coating on the surface of the processed target plate is solidified into a hydrophobic coating attached to the surface of the processed target plate, thereby obtaining a sample target plate.

[0066] Example 2

[0067] Preparation of fluorine-modified silica:

[0068] 3.78 g of tetraethyl orthosilicate, 1.4 g of alkaline catalyst ammonia water, 40 g of anhydrous ethanol and 3 g of deionized water were mixed, and stirred at 800 rpm for 6 hours at 50°C to obtain a silica particle mixture. Ethanol was added to the silica particle mixture, and 1.22 g of perfluorodecyltrimethylsilane was added. After stirring at 1200 rpm for 8 minutes, 0.5 g of nano-silica particles with a particle size of 115 nm was added, and stirred at 2000 rpm for 12 minutes to obtain fluorine-modified silica.

[0069] Preparation of siloxane organic matter:

[0070] Mix 10 g of anhydrous ethanol, 1 g of acetic acid, 5 g of triethoxymethylsilane, 3 g of ethyl orthosilicate and 1 g of deionized water, stir at 800 rpm for 4 hours at 25°C to obtain a siloxane condensate, then add 10 g of anhydrous ethanol to the siloxane condensate, and stir at 800 rpm for 30 minutes to obtain a siloxane organic matter.

[0071] Preparation of hydrophobic coating:

[0072] 37.96 g of epoxy resin and 15 g of curing agent were added to 10 mL of acetone solution, ultrasonicated at 2000 rpm for 30 min, then 3.65 g of fluorine-modified silica and 8.39 g of siloxane organic matter were added, stirred at 800 rpm for 3 min, 0.5 g of 3-aminopropyltrimethoxysilane and 0.5 g of perfluorodecyltrimethylsilane were added, and stirred at 1200 rpm for 5 min to obtain a hydrophobic coating.

[0073] Prepare sample target plate:

[0074] (1) Plasma treatment of target substrate surface:

[0075] The target plate substrate is laid flat in the reaction chamber of the plasma equipment, the electrode spacing is set to 3 cm, the vacuum pump is turned on, the chamber is evacuated to 5 Pa, argon gas is introduced, and the argon gas flow rate range is 100 mL / min. After the air pressure stabilizes, the power switch is turned on, the discharge power is 400 W, the discharge time is 10 s, and the power is turned off after the processing time is reached to obtain plasma-treated stainless steel.

[0076] (2) Cutting and processing of grooves:

[0077] According to the specifications of different mass spectrometer target carriers, the plasma-treated stainless steel is cut, and the cut stainless steel is processed using a micro-engraving tool to form 96-hole point grooves on the surface of the steel, with a depth of 3 μm.

[0078] (3) Engraving barcode:

[0079] A barcode is engraved on the surface of the steel plate by a laser engraving machine to obtain a processed target plate.

[0080] (4) Pour the hydrophobic coating into the spray gun, control the spray gun pressure to 5 Kpa, and keep the nozzle 30 cm away from the base of the processing target plate. Spray the water-transporting coating to the surface of the processing target plate except the point groove, so that the surface of the processing target plate except the point groove is adhered to the hydrophobic coating. The thickness of the hydrophobic coating is 2 μm.

[0081] (5) Drying the processed target plate coated with the hydrophobic coating in an oven at a temperature of 110° C. for 1 h, so that the hydrophobic coating on the surface of the processed target plate is solidified into a hydrophobic coating attached to the surface of the processed target plate, thereby obtaining a sample target plate.

[0082] Example 3

[0083] Preparation of fluorine-modified silica:

[0084] 3.75 g of tetraethyl orthosilicate, 1.3 g of alkaline catalyst ammonia water, 40 g of anhydrous ethanol and 3 g of deionized water were mixed, and stirred at 800 rpm for 6 hours at 50°C to obtain a silica particle mixture. Ethanol was added to the silica particle mixture, and 1.25 g of perfluorodecyltrimethylsilane was added. After stirring at 1200 rpm for 8 minutes, 0.5 g of nano-silica particles with a particle size of 110 nm were added, and stirred at 2000 rpm for 12 minutes to obtain fluorine-modified silica.

[0085] Preparation of siloxane organic matter:

[0086] Mix 10 g of anhydrous ethanol, 1 g of acetic acid, 6 g of triethoxymethylsilane, 2 g of ethyl orthosilicate and 1 g of deionized water, stir at 800 rpm for 4 hours at 25°C to obtain a siloxane condensate, then add 10 g of anhydrous ethanol to the siloxane condensate, and stir at 800 rpm for 30 minutes to obtain a siloxane organic matter.

[0087] Preparation of hydrophobic coating:

[0088] 38.97 g of epoxy resin and 15 g of curing agent were added to 10 mL of acetone solution, ultrasonicated at 2000 rpm for 30 min, then 3.68 g of fluorine-modified silica and 7.35 g of siloxane organic matter were added, stirred at 800 rpm for 3 min, 0.5 g of 3-aminopropyltrimethoxysilane and 0.5 g of perfluorodecyltrimethylsilane were added, and stirred at 1200 rpm for 5 min to obtain a hydrophobic coating.

[0089] Prepare sample target plate:

[0090] (1) Plasma treatment of target substrate surface:

[0091] The target plate substrate is laid flat in the reaction chamber of the plasma equipment, the electrode spacing is set to be fixed at 3 cm, the vacuum pump is turned on, the chamber is evacuated to 4 Pa, argon gas is introduced, and the argon gas flow rate range is 75 mL / min. After the air pressure stabilizes, the open power switch is turned on, the discharge power is 300 w, the discharge time is 30 s, and the power is turned off after the processing time is reached to obtain plasma-treated stainless steel.

[0092] (2) Cutting and processing of grooves:

[0093] According to the specifications of different mass spectrometer target carriers, the plasma-treated stainless steel is cut and processed with a micro-engraving tool to form 96-hole point grooves on the surface of the steel. The depth of the point grooves is 2.5 μm.

[0094] (3) Engraving barcode:

[0095] A barcode is engraved on the surface of the steel plate by a laser engraving machine to obtain a processed target plate.

[0096] (4) Pour the hydrophobic coating into the spray gun, control the spray gun pressure to 4.5 Kpa, and keep the nozzle 25 cm away from the base of the processing target plate. Spray the water-transporting coating to the surface of the processing target plate except the point groove, so that the surface of the processing target plate except the point groove is adhered to the hydrophobic coating. The thickness of the hydrophobic coating is 2.5 μm.

[0097] (5) Drying the processed target plate coated with the hydrophobic coating in an oven at a temperature of 100° C. for 1.5 h, so that the hydrophobic coating on the surface of the processed target plate is solidified into a hydrophobic coating attached to the surface of the processed target plate, thereby obtaining a sample target plate.

[0098] Example 4

[0099] Example 4 is based on Example 3. When preparing fluorine-modified silica in Example 4, 3.57 g of ethyl orthosilicate and 1.43 g of perfluorodecyltrimethylsilane are used.

[0100] Example 5

[0101] Example 5 is based on Example 3. When preparing fluorine-modified silica in Example 5, 3.89 g of ethyl orthosilicate and 1.11 g of perfluorodecyltrimethylsilane are used.

[0102] Example 6

[0103] Example 6 is based on Example 3. When preparing fluorine-modified silica in Example 6, 1 g of ammonia water is added.

[0104] Example 7

[0105] Example 7 is based on Example 3. When preparing fluorine-modified silica in Example 7, 1.5 g of ammonia water is added.

[0106] Example 8

[0107] Example 8 is based on Example 3. When preparing fluorine-modified silica in Example 8, the particle size of the added nano-silica particles is 90 nm.

[0108] Example 9

[0109] Example 9 is based on Example 3. When preparing fluorine-modified silica in Example 9, the particle size of the added nano-silica particles is 120 nm.

[0110] Example 10

[0111] Example 10 is based on Example 3, and in Example 10, no nano-silica particles are added to the fluorine-modified silica.

[0112] Embodiment 11

[0113] Example 11 is based on Example 3. When preparing the siloxane organic matter in Example 11, the amount of triethoxymethylsilane added is 8g.

[0114] Example 12

[0115] Example 12 is based on Example 3. When preparing the hydrophobic coating in Example 12, 3.82 g of fluorine-modified silica, 6.49 g of siloxane organic matter and 39.69 g of epoxy resin are added.

[0116] Example 13

[0117] Example 13 is based on Example 3. When preparing the hydrophobic coating in Example 13, 3.55 g of fluorine-modified silica, 9.57 g of siloxane organic matter and 36.88 g of epoxy resin are added.

[0118] Embodiment 14

[0119] Example 14 is based on Example 3. When preparing the hydrophobic coating in Example 14, the fluorine-modified silica is replaced with ordinary silica dispersion. The preparation method of the silica dispersion is as follows: 7.35 g of nano-silica with a particle size of 110 nm is mixed with 40 mL of ethanol, and then dispersed at a rotation speed of 2000 rpm for 10 minutes to obtain a silica dispersion.

[0120] Comparative Example 1

[0121] Comparative Example 1 is based on Example 3, and in Comparative Example 1, the surface of the target plate substrate is not subjected to plasma treatment.

[0122] Performance testing

[0123] Examples 1-14 and Comparative Example 1 were sampled and the following performance tests were performed:

[0124] (1) Hydrophobic performance test

[0125] For the sample target plate prepared by coating, contact angle tests were performed at three random locations where a hydrophobic coating was formed, and the test results were averaged and entered into Table 1.

[0126] (2) Wear resistance test

[0127] After sampling the sample, place 800-mesh 3M sandpaper on the side of the sample target plate with the hydrophobic coating attached, and place a weight of 100 g on the sandpaper. Wear on the sandpaper for 15 cm is considered as one wear. After the sample is worn 5 times, measure the contact angle of the friction part of the hydrophobic coating. Each sample is tested three times, and the test results are filled in Table 1.

[0128] (3) Test of light transmittance of hydrophobic coating

[0129] Observe the clarity of the barcode engraved on the coating surface and fill in the observation results in Table 1.

[0130] (4) Coating stability performance test

[0131] Add the blue ink-dyed aqueous solution to the dotted grooves, let it stand for 12 hours to observe whether there is ink uniformity in the non-dotted grooves. Test each sample 3 times and fill in the test results in Table 1.

[0132] Table 1 Performance test results of target plates of examples 1-14

[0133]

[0134] Data analysis From Table 1, it can be seen that in each sample target plate style of Examples 1-14, the hydrophobic angles are all 130° and above, indicating that the sample target plates prepared in the present application and the hydrophobic coatings all have good hydrophobic properties; after the friction test, the hydrophobic angles are all above 100°, indicating that the sample target plates prepared in the present application have hydrophobic properties after the hydrophobic coating is worn, and have good wear resistance; the target plate sample barcodes are all easy to distinguish, indicating that the hydrophobic coating of the sample target plates prepared in the present application has good light transmittance, indicating that the sample target plates prepared in the present application and the hydrophobic coating have good light transmittance; after the ink leveling test, no leveling phenomenon occurred around the point circle groove, indicating that the hydrophobic coating prepared in the present application has good adhesion performance to the target plate steel plate and a good restraint effect on the reagent.

[0135] When preparing fluorine-modified silica, when the content of tetraethyl orthosilicate is too little, the particle size of the prepared silica particles is too small, which also affects the hydrophobic effect, so the hydrophobic effect of Example 4 decreases; if the content of tetraethyl orthosilicate is too much, the prepared silica particles will accumulate with each other, so the silica particles will agglomerate, affecting the overall stability of the hydrophobic coating, so the hydrophobic performance and wear resistance of Example 5 are both reduced.

[0136] When preparing fluorine-modified silica, when the amount of ammonia water added is too small, the hydrolysis rate of ethyl orthosilicate is too slow, part of ethyl orthosilicate is not hydrolyzed, the silica particle size decreases, and the hydrophobic improvement effect decreases, so the hydrophobic effect of Example 6 decreases; in Example 7, when there is too much ammonia water, the silica particle size increases too much, which will increase the surface roughness of the prepared hydrophobic coating, and both the hydrophobic performance and the light transmittance performance will be reduced.

[0137] When preparing fluorine-modified silica, the diameter of the added nano-silica particles is too small, making it difficult to further increase the contact angle of the hydrophobic coating, and having little effect on improving the hydrophobic effect, so the hydrophobic performance of Example 8 is reduced; when the diameter of the added nano-silica particles is too large, the surface roughness of the prepared hydrophobic coating is increased, affecting the overall hydrophobic performance and light transmittance of the hydrophobic coating, so the hydrophobic performance and light transmittance of Example 9 are both reduced.

[0138] After no nano-silica particles were added to the fluorine-modified silica, the mechanical properties were reduced, and it was difficult to further improve the hydrophobicity of the system, so the wear resistance and hydrophobicity in Example 10 were reduced.

[0139] When preparing siloxane organic matter, if the content of triethoxymethylsilane is too high, the pH value in the composite coating will increase too much, resulting in highly branched chain oligomers, thereby increasing the surface roughness of the prepared hydrophobic coating. The amino group in triethoxymethylsilane is a hydrophilic group and affects the hydrophobic properties of the hydrophobic coating. Therefore, the hydrophobic properties of Example 11 are reduced.

[0140] When preparing a hydrophobic coating, when the amount of siloxane organic matter added is too small, the hydrophobic effect on the hydrophobic coating is not great, so the hydrophobic performance of Example 12 is reduced. When the proportion of siloxane organic matter is too large, the excessive methyl groups in the siloxane organic matter will increase the surface energy of the prepared hydrophobic coating, and at the same time, different particles in the system will adhere together, resulting in a decrease in the porosity of the coating, thereby affecting the light transmittance, and the stability of the system is reduced, so the performance of Example 13 is reduced.

[0141] In Example 14, the fluorine-modified silica was replaced with a common silica dispersion. The unmodified silica particles agglomerated in the system, thus affecting the overall stability of the system. Therefore, various performances in Example 14 were reduced.

[0142] In comparative example 1, after the surface of the target plate substrate is not plasma treated, the roughness of the surface of the target plate substrate is difficult to improve, the surface energy is small, and the stability of the hydrophobic coating adhering to the target plate surface is reduced. Therefore, the stability of the prepared hydrophobic coating is reduced. Therefore, after the ink is evenly dyed in comparative example 1, even dyeing occurs around the point circle groove.

[0143] This specific embodiment is only an explanation of the present application, and it is not a limitation of the present application. Through the above description, relevant staff can make various changes and modifications without deviating from the technical idea of ​​the present application. The technical scope of the present application is not limited to the content in the specification, and its technical scope must be determined according to the scope of the claims.

Claims

1. A method for preparing a sample target plate for mass spectrometry detection, characterized in that: The invention comprises the following preparation method: (1) Plasma treatment of the surface of the stainless steel target plate substrate; (2) Cutting and processing to obtain point grooves; (3) Carving a barcode to obtain a processed target plate; (4) The surface of the processed target plate is coated with a hydrophobic coating except for the point grooves; (5) curing the processed target plate coated with the hydrophobic coating at high temperature, so that a hydrophobic coating is formed on the surface of the processed target plate, thereby obtaining a sample target plate; The hydrophobic coating comprises fluorine-modified silica, siloxane organic matter and epoxy resin; The fluorine-modified silicon dioxide is prepared by the following method: Mixing tetraethyl orthosilicate, an alkaline catalyst, anhydrous ethanol and deionized water, stirring to obtain a silica particle mixture, adding ethanol and perfluorodecyltrimethylsilane to the silica particle mixture, stirring to obtain fluorine-modified silica; The siloxane organic compound is prepared by the following method: Anhydrous ethanol, acetic acid, triethoxymethylsilane, ethyl orthosilicate and deionized water are mixed and stirred to obtain a siloxane condensate, and water ethanol is continuously added to the siloxane condensate and stirred to obtain a siloxane organic matter; The hydrophobic coating is prepared by the following method: The epoxy resin is mixed with the acetone solution, and then fluorine-modified silica and siloxane organic matter are added, and 3-aminopropyltrimethoxysilane is added after dispersion, and after stirring, a hydrophobic coating is obtained.

2. The method for preparing a sample target plate for mass spectrometry detection according to claim 1, characterized in that: The mass ratio of the fluorine-modified silica, the siloxane organic matter and the epoxy resin is 1:(2.1-2.3):10.

4.

3. The method for preparing a sample target plate for mass spectrometry detection according to claim 1, characterized in that: The mass ratio between the tetraethyl orthosilicate and perfluorodecyltrimethylsilane is (2.9-3.1):

1.

4. The method for preparing a sample target plate for mass spectrometry detection according to claim 1, characterized in that: The alkaline catalyst includes aqueous ammonia.

5. The method for preparing a sample target plate for mass spectrometry detection according to claim 4, characterized in that: The amount of ammonia water added is 2.5-0.3% of the total fluorine-modified silica.

6. The method for preparing a sample target plate for mass spectrometry detection according to claim 1, characterized in that: The fluorine-modified silica is further added with nano-silicon dioxide particles, and the particle size of the nano-silicon dioxide particles is 105-115 nm.

Citation Information

Patent Citations

  • Candle extinguisher

    CA107153A

  • Pigment grinding vehicles containing quaternary ammonium and ternary sulfonium groups

    CA1336216C

  • Target plate and manufacturing method thereof

    CN107907585A

  • Preparation method of hydrophobic silica sol

    CN109987609A